Hot stamping parts

The hot-stamping member with a controlled plating layer composition and distribution of Zn-based oxides addresses chemical conversion and LME issues, enhancing the quality and reliability of Al-based plated steel sheets in hot-stamping processes.

JP7575701B2Active Publication Date: 2024-10-30NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022575645
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-14
Filing Date
2022-01-14
Publication Date
2024-10-30
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Existing hot-stamping methods using Al-based plated steel sheets face issues with insufficient chemical conversion treatment properties and susceptibility to Liquid Metal Embrittlement (LME) during spot welding, which compromises the quality and reliability of the hot-stamped members.

Method used

A hot-stamping member with a plating layer composed of specific chemical elements (Zn: 0.5 to 15.0%, Mg: 0~10.0%, Si:0.05~10.0%, Fe:20.0~60.0%, and others) and a controlled distribution of Zn-based oxides, ensuring a ratio of ΣLi/Le≧0.10 and ΣLai/ΣLi≧0.50, enhances chemical conversion treatment properties and suppresses LME during spot welding.

Benefits of technology

The solution provides hot-stamped members with excellent chemical conversion treatment properties and robust LME resistance, improving both the quality and reliability of the hot-stamped components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575701000004
    Figure 0007575701000004
  • Figure 0007575701000005
    Figure 0007575701000005
  • Figure 0007575701000006
    Figure 0007575701000006
Patent Text Reader

Abstract

This hot stamp member comprises a steel material and a plated layer formed on the steel material, wherein: the plated layer has a predetermined chemical composition; the plated layer contains a Zn-based oxide which is composed of one or two types of oxides among a Zn oxide and a Zn-Mg oxide and has a size of 1.0-10.0 μm in the thickness direction of the plated layer and at least 0.1 μm in a direction perpendicular to the thickness direction; and in the cross section of the plated layer in the thickness direction, when the length of the boundary surface between the plated layer and the steel material is defined as Le, the total length of the Zn-based oxide projected onto the boundary surface from the upper surface of the plated layer is defined as ΣLi, and the total length of the portion, projected onto the boundary surface from the upper surface of the plated layer, of the Zn-based oxide in contact with the plated layer is defined as ΣLai, ΣLi / Le≥0.10 and ΣLai / ΣLi≥0.50 are satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot stamped component. This application claims priority based on Japanese Patent Application No. 2021-004022, filed on January 14, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, in order to protect the environment and prevent global warming, there has been a demand to reduce the consumption of chemical fuels. For example, automobiles, which are indispensable in daily life and activities as a means of transportation, are no exception to this demand. In response to this demand, improvements in fuel efficiency, such as by reducing the weight of the automobile body, have been considered for automobiles. Since most automobile structures are formed of iron, particularly steel plates, reducing the weight of the steel plates by making them thinner is highly effective in reducing the weight of the automobile body. However, there is a concern that simply reducing the thickness of the steel plates to reduce the weight of the steel plates will reduce the strength of the structure and reduce safety. Therefore, in order to reduce the thickness of the steel plates, it is necessary to increase the mechanical strength of the steel plates used so as not to reduce the strength of the structure. Therefore, research and development is being conducted on steel sheets that can maintain or increase their mechanical strength even when made thinner than previously used steel sheets by increasing their mechanical strength. Such steel sheets are required not only in the automobile manufacturing industry but also in various other manufacturing industries.

[0003] Generally, materials with high mechanical strength tend to have low shape fixability in forming processes such as bending, and when they are processed into complex shapes, the processing itself becomes difficult. One of the means for solving the problem of formability is the application of the so-called hot stamping method. In the hot stamping method, the material to be formed is once heated to a high temperature to be austenitized, and the material softened by heating is pressed to be formed, or simultaneously with forming, it is rapidly cooled in a die to cause martensite transformation, and a high-strength processed product can be obtained after forming.

[0004] According to the hot stamping method, the material is first heated to a high temperature to soften it, and then pressed in the softened state, so that the material can be easily pressed. Therefore, this hot press processing can produce a press-formed product that has both good shape fixability and high mechanical strength. In particular, when the material is steel, the mechanical strength of the press-formed product can be increased by the quenching effect caused by cooling after forming.

[0005] However, when hot stamping is applied to steel sheets, the surface iron and other components are oxidized by heating to high temperatures of, for example, 800 to 850°C or higher, resulting in the formation of scale (oxide). Therefore, after hot press processing, a process for removing this scale (descaling process) is required, which reduces productivity. In addition, for components that require corrosion resistance, it is necessary to perform rust prevention treatment or metal coating on the component surface after processing, which requires a surface cleaning process and a surface treatment process, which also reduces productivity.

[0006] An example of a method for suppressing such a decrease in productivity is a method of coating a steel sheet. Generally, various materials such as organic materials and inorganic materials are used as coatings on steel sheets. Among them, zinc-based plating, which has a sacrificial anticorrosive effect, is often applied to steel sheets from the viewpoint of its anticorrosive performance and steel sheet production technology. On the other hand, the heating temperature during pressing is often performed at a temperature higher than the Ac3 transformation point of steel in order to obtain a quenching effect, for example, the heating temperature is about 800 to 1000 ° C. However, this heating temperature is higher than the decomposition temperature of organic materials and the boiling point of metal materials such as Zn. For this reason, when a steel sheet coated with an organic material or a Zn-based metal material is heated for hot pressing, the plating layer on the surface of the steel sheet may evaporate, which may cause a significant deterioration in the surface properties.

[0007] In order to avoid such deterioration of surface properties, it is preferable to coat steel sheets that are to be subjected to hot press working in which the steel sheets are heated to high temperatures with, for example, an Al-based metal, which has a higher boiling point than organic material coatings or Zn-based metal coatings. By using steel sheets coated with an Al-based metal, so-called Al-plated steel sheets, it is possible to prevent scale from adhering to the steel sheet surface, and since processes such as descaling are unnecessary, productivity is improved. In addition, since the Al-based metal coating has a rust-preventing effect, corrosion resistance after painting is also improved.

[0008] For these reasons, Al-based plated steel sheets having an Al-based plating on the surface have begun to be used as steel sheets for hot stamping. However, when an Al-based plated steel sheet is hot stamped, there is a problem that the hot stamped member (steel sheet after hot stamping) does not have sufficient chemical conversion treatability. In order to improve the chemical treatability of steel sheets after hot stamping, it has been proposed to add Zn or Mg to the coating layer. However, if the coating layer contains Zn or Mg, it can cause cracks due to LME during spot welding.

[0009] For example, Patent Document 1 discloses a steel sheet coated with a metal coating containing 2.0 to 24.0 wt. % zinc, 7.1 to 12.0 wt. % silicon, optional 1.1 to 8.0 wt. % magnesium, and an additional element optionally selected from Pb, Ni, Zr, or Hf, wherein the weight content of each additional element is less than 0.3 wt. %, with the balance being aluminum and optional unavoidable impurities and residual elements, and having an Al / Zn ratio of more than 2.9.

[0010] Patent Document 2 discloses a method for producing a hardened part, which provides a part that does not have the problem of LME caused by hot forming when hot forming a steel sheet that has been pre-coated with a metal coating containing 2.0 to 24.0% by weight of zinc, 1.1 to 7.0% by weight of silicon, and when the amount of silicon is between 1.1 and 4.0% by weight, optionally containing 1.1 to 8.0% by weight of magnesium, and optionally containing an additional element selected from Pb, Ni, Zr or Hf, the weight content of each additional element being less than 0.3% by weight, with the remainder being aluminum and unavoidable impurities and residual elements. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2017 / 017513 [Patent Document 2] International Publication No. 2017 / 017514 Summary of the Invention [Problem to be solved by the invention]

[0012] However, Patent Document 1 does not consider LME at all. In addition, although the method of Patent Document 2 is effective in suppressing LME during hot forming such as hot stamping, the inventors have found through their investigations that LME occurs when spot welding is performed on parts obtained by this method. As described above, no hot stamped member that is excellent in chemical conversion treatability and can suppress LME during spot welding has been proposed in the past. Therefore, an object of the present invention is to provide a hot stamped member that is excellent in chemical conversion treatability and can suppress LME during spot welding (excellent LME resistance), on the premise that the hot stamped member uses an Al-based plated steel material (a steel material having a plating layer containing Al) as a raw material. [Means for solving the problem]

[0013] The present inventors have conducted studies to improve the chemical conversion treatability and LME resistance during spot welding in hot stamped members obtained by hot stamping an aluminum-plated steel sheet. As a result, they have found that by limiting the chemical composition of the plating layer and allowing the plating layer to contain Zn oxides and / or Zn-Mg oxides of a predetermined size in a predetermined distribution state, the plating layer can have excellent chemical conversion treatability and suppress LME during spot welding.

[0014] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [1] A hot stamped member according to one aspect of the present invention comprises a steel material and a plating layer formed on the steel material, the plating layer containing, in mass%, 0.5 to 15.0% Zn, 0 to 10.0% Mg, 0.05 to 10.0% Si, 20.0 to 60.0% Fe, 0 to 3.00% Ca, 0 to 0.50% Sb, 0 to 0.50% Pb, and %, Sr: 0-0.50%, Sn: 0-1.00%, Cu: 0-1.00%, Ti: 0-1.00%, Ni: 0-1.00%, Mn: 0-1.00%, Cr: 0-1.00%, La: 0-1.00%, Ce: 0-1.00%, Zr: 0-1.00%, and Hf: 0-1.00%, with a total of 0-5.0% or more of these selected from the above. The plating layer has a chemical composition of 0.0%, with the balance consisting of Al and impurities, and the plating layer contains Zn-based oxides consisting of one or both of Zn oxide and Zn-Mg oxide, having a size of 1.0 μm or more and 10.0 μm or less in the thickness direction of the plating layer and 0.1 μm or more in the direction perpendicular to the thickness direction, and the following formulas (1) and (2) are satisfied when a length of an interface between the plating layer and the steel material in a cross section of the plating layer in the thickness direction is Le, a sum of lengths of the Zn-based oxides projected from an upper surface of the plating layer onto the interface is ΣLi, and a sum of lengths of portions of the Zn-based oxides in contact with the plating layer, projected from the upper surface of the plating layer onto the interface is ΣLai. ΣLi / Le≧0.10 (1) ΣLai / ΣLi≧0.50 (2) [2] The hot-stamped member according to the above [1] may have a chemical composition containing, in mass%, 0.2 to 7.0% Mg. [3] The hot-stamped member described in [1] may have a chemical composition, in mass%, of 3.0 to 7.0% Mg and 7.0 to 15.0% Zn. Effect of the Invention

[0015] According to the above-described aspect of the present invention, it is possible to provide a hot stamped member having excellent chemical conversion treatability and excellent LME resistance during spot welding. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a diagram showing an example of a cross section of a plating layer of a hot-stamped member according to the embodiment. [Diagram 2] FIG. 2 is a diagram illustrating a method for measuring the ratio of the projected length of a Zn-based oxide to the interface length. [Diagram 3] FIG. 1 is a diagram for explaining a method for measuring ΣLai. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A hot-stamped member according to one embodiment of the present invention (a hot-stamped member according to the present embodiment) will be described. As shown in FIG. 1 , the hot stamped member according to the present embodiment includes a steel material 1 and a plating layer 2 formed on the steel material 1. The plating layer 2 has a predetermined chemical composition and contains Zn-based oxide 101 (comprising one or two of Zn oxide and Zn-Mg oxide) having a size of 1.0 μm or more and 10.0 μm or less in a thickness direction of the plating layer 2 and 0.1 μm or more in a direction perpendicular to the thickness direction. In a cross section in the thickness direction of the plating layer 2, when a length of an interface between the plating layer 2 and the steel material 1 is Le and a sum of lengths of the Zn-based oxide 101 projected from an upper surface of the plating layer 2 to the interface between the plating layer 2 and the steel material 1 is ΣLi, ΣLi / Le ≧ 0.10 (ΣLi / Le is 0.10 or more) is satisfied. When a sum of lengths of a portion of the Zn-based oxide 101 in contact with the plating layer projected from the upper surface of the plating layer 2 to the interface between the plating layer 2 and the steel material 1 is ΣLai, ΣLai / ΣLi ≧ 0.50 is satisfied. Zn-based oxides are mainly formed by hot stamping, and therefore mainly form near the surface layer, as shown in FIG.

[0018] <Steel> In the hot stamped member according to this embodiment, the coating layer 2 is important, and the type of the steel material 1 is not particularly limited. It may be determined depending on the product to which it is applied, the required strength, plate thickness, etc. For example, a steel sheet such as a hot rolled steel sheet described in JIS G3131:2018 or a cold rolled steel sheet described in JIS G3141:2017 can be used.

[0019] <Plating layer> The hot stamped member according to this embodiment has a plating layer 2 on (on the surface of) a steel material 1. The plating layer 2 may be formed on one side of the steel material 1, or on both sides.

[0020] [Chemical composition] The reasons for limiting the content of each element contained in the chemical composition of the plating layer 2 of the hot stamped member according to this embodiment will be described below. The "%" for the content of each element is mass %.

[0021] Zn: 0.5-15.0% Zn is an element that forms Zn-based oxides (Zn oxides, or Zn-Mg oxides when the plating layer contains Mg) on ​​the surface of the steel material by hot stamping. When Zn oxide is present on the surface of the hot stamped member, the chemical conversion treatability is improved. Zn is also an element that contributes to improving the corrosion resistance of the plating layer by improving sacrificial corrosion protection. To obtain these effects, the Zn content is set to 0.5% or more. The Zn content is preferably 1.0% or more, more preferably 5.0% or more, and even more preferably 7.0% or more. On the other hand, if the Zn content exceeds 15.0%, it becomes difficult to suppress LME, so the Zn content is set to 15.0% or less, and preferably 10.0% or less.

[0022] Magnesium: 0 to 10.0% Mg is an element that forms Zn-Mg oxide together with Zn on the surface of the steel material during hot stamping, and has the effect of improving the chemical conversion treatability of the hot stamped member. In terms of improving the chemical conversion treatability, Zn-Mg oxide is more effective than Zn oxide. Mg does not necessarily have to be contained, but may be contained in order to obtain the above-mentioned effect. To obtain the above-mentioned effect sufficiently, the Mg content is preferably 0.2% or more. The Mg content is more preferably 0.5% or more, and further preferably 2.0% or more. On the other hand, in order to make the Mg content of the hot stamped member exceed 10.0%, it is necessary to make the Mg content of the plated steel sheet exceed 15.0%. In this case, problems in production arise, such as an increase in the amount of dross generated in the plating bath. Therefore, the Mg content is set to 10.0% or less. The Mg content is preferably 7.0% or less, and more preferably 5.0% or less.

[0023] Silicon: 0.05 to 10.0% Si is an element that has the effect of suppressing the formation of an excessively thick alloy layer between the steel sheet and the plating layer when a plating layer is formed on the steel sheet, thereby enhancing the adhesion between the steel sheet and the plating layer. When Si is contained together with Mg, it also forms a compound with Mg and contributes to improving corrosion resistance after painting. To obtain the above effect, the Si content is set to 0.05% or more. The Si content is preferably 0.1% or more, more preferably 1.0% or more. On the other hand, if the Si content exceeds 10.0%, the workability of the plating layer decreases. Therefore, the Si content is set to 10.0% or less. The Si content is preferably 8.0% or less.

[0024] Fe: 20.0 to 60.0% Fe diffuses from the steel material into the coating layer when the coating layer is formed, and also diffuses from the steel material into the coating layer during hot stamping and is included in the coating layer. Part of Fe combines with Al and other elements in the coating layer to form an alloy. If the Fe content is less than 20.0%, unalloyed Al phase remains in the plating layer, which may cause the plating layer to adhere to the mold, resulting in reduced manufacturability. On the other hand, if the Fe content exceeds 60.0%, the Fe concentration is excessive, and red rust may form early in a corrosive environment.

[0025] Ca: 0-3.00%, Sb: 0-0.50%, Pb: 0-0.50%, Sr: 0-0.50%, Sn: 0-1.00%, Cu: 0-1.00%, Ti: 0-1.00%, Ni: 0-1.00%, Mn: 0-1.00%, Cr: 0-1.00%, La: 0-1.00%, Ce: 0-1.00%, Zr: 0-1.00%, Hf: 0-1.00%, one or more selected from the above, total 0-5.00% The plating layer of the hot stamped member according to this embodiment may contain one or more of Ca, Sb, Pb, Sr, Sn, Cu, Ti, Ni, Mn, Cr, La, Ce, Zr, and Hf as an impurity or by intentional addition, so long as the elements are within the above-mentioned ranges.

[0026] If the Ca content is high, the coating layer will contain CaZn 11 The Ca content is set to 3.00% or less because Ca-based intermetallic compounds such as Ca-Fe-Fe-P ... On the other hand, when Ca is contained in the coating layer, the amount of dross that is easily formed during coating operation decreases with an increase in the Mg content, improving coating manufacturability. Therefore, Ca may be contained within the range of 3.00% or less.

[0027] If the Sb content, Sr content, or Pb content is excessive, the viscosity of the plating bath increases, making it difficult to prepare the plating bath itself, and it is not possible to produce a plated steel sheet with good plating properties. Therefore, the Sr content is set to 0.50% or less, the Sb content is set to 0.50% or less, and the Pb content is set to 0.50% or less. When Sr, Sb, or Pb is contained in the plating layer, the appearance of the plating layer changes, spangles are formed, and an improvement in metallic luster is confirmed. Therefore, these elements may be contained as long as their content is within the range of 0.50% or less.

[0028] Sn is an element that increases the Mg dissolution rate in a plating layer that contains Zn, Al, and Mg. If the Mg dissolution rate increases, the corrosion resistance of the flat surface deteriorates. Therefore, the Sn content is set to 1.00% or less.

[0029] If the Cu, Ti, Ni, or Mn content is excessive, the viscosity of the plating bath increases, making it difficult to prepare the plating bath itself, and it is not possible to produce a plated steel sheet with good plating properties. Therefore, the content of each element is set to 1.00% or less. On the other hand, these elements contribute to improving corrosion resistance, and therefore may be contained within a range of 1.00% or less.

[0030] If the La content or Ce content is excessive, the viscosity of the plating bath increases, making it difficult to prepare the plating bath itself, and it is not possible to produce plated steel products with good plating properties. Therefore, the La content and Ce content are each set to 1.00% or less.

[0031] If the Zr content or Hf content is excessive, the corrosion resistance may decrease, so the Zr content and Hf content are each set to 1.00% or less.

[0032] The chemical composition of the plating layer of the plated steel sheet according to this embodiment has the above-mentioned chemical composition, with the balance being Al and impurities.

[0033] The chemical composition of the plating layer is measured by the following method. First, the plating layer is stripped and dissolved using an acid containing an inhibitor that suppresses corrosion of the base steel (steel material) to obtain an acid solution. The obtained acid solution is then measured using ICP analysis to obtain the chemical composition of the plating layer. There are no particular restrictions on the type of acid, so long as it is an acid that can dissolve the plating layer. The chemical composition is measured as an average chemical composition. Since ICP analysis cannot analyze O, the above chemical composition is the content of elements that does not take into account the presence of O in the plating layer.

[0034] [Organization] The plating layer provided on the hot stamped member according to this embodiment contains a Zn-based oxide composed of one or both of Zn oxide and Zn-Mg oxide, having a size of 1.0 μm or more and 10.0 μm or less in the thickness direction of the plating layer and 0.1 μm or more in the direction perpendicular to the thickness direction (plane direction). In addition, in a cross section in the thickness direction of this plating layer, when the length of the interface between the plating layer and the steel material is Le, the sum of the lengths of Zn-based oxides having the above-mentioned size projected from the upper surface of the plating layer onto the interface is ΣLi, and the sum of the lengths of the portions of the Zn-based oxides in contact with the plating layer projected from the upper surface of the plating layer onto the interface between the plating layer and the steel material is ΣLai, ΣLi / Le ≧ 0.10 and ΣLai / ΣLi ≧ 0.50. When a Zn-based oxide consisting of one or both of Zn oxide and Zn-Mg oxide is present in the coating layer, a zinc phosphate crystal (zinc phosphate crystal containing Mg in the case of Zn-Mg) is formed during chemical conversion treatment, resulting in excellent chemical conversion treatment properties. However, if the projected length of a Zn-based oxide (Zn oxide or Zn-Mg oxide) of a given size projected onto the interface is smaller than the length of the interface between the plating layer and the steel material (when viewed from above, the interface is not covered sufficiently), the effect of improving the chemical conversion treatability cannot be sufficiently obtained. Therefore, when viewed in a cross section in the thickness direction, the ratio of the total projected length of Zn-based oxides having a size of 1.0 μm or more and 10.0 μm or less in the thickness direction and 0.1 μm or more in the surface direction to the length of the interface (in other words, the total length of the interface above which oxides exist) is set to 0.10 (10%) or more. It is preferably 0.30 (30%) or more, and more preferably 0.50 (50%) or more. Furthermore, if the plating layer does not contain Zn-based oxides consisting of one or both of Zn oxide and Zn-Mg oxide and having a size of 1.0 μm or more and 10.0 μm or less in the thickness direction of the plating layer and 0.1 μm or more in the direction perpendicular to the thickness direction, this can cause a decrease in chemical conversion treatability. Even if the plating layer contains Zn-based oxides, if there are gaps (voids) between the plating layer and the Zn-based oxides, gaps will remain between the chemical conversion layer and the plating layer even after chemical conversion treatment. In this case, the adhesion of the chemical conversion layer decreases, making it easier for scale to occur. Therefore, in the plating layer of the hot stamped member according to the present embodiment, the ratio of the portion of the oxide in contact with the plating layer is increased. Specifically, the ratio of the portion of the oxide in contact with the plating layer is calculated as follows. First, in a cross section of the plating layer in the thickness direction, the length of the entire interface between the plating layer and the steel material is Le, and the sum of the lengths of the Zn-based oxides projected from the top surface of the plating layer onto the interface is ΣLi. Then, the sum of the lengths of the oxides in contact with the plating layer, projected from the top surface of the plating layer onto the interface, is ΣLai. Therefore, if the proportion of the oxides in contact with the plating layer is increased, the proportion of ΣLai to ΣLi will increase. "The part of the oxide in contact with the plating layer" refers to the whole oxide excluding the part that is "not in contact with the plating layer." The part of the oxide that is not in contact with the plating layer refers to the part where a gap (void) of more than 0.5 mm exists between the plating layer and the Zn-based oxide in cross-sectional SEM observation. On the other hand, if no gap is observed between the plating layer and the Zn-based oxide in cross-sectional SEM observation, or if a gap is observed, but it is 0.5 mm or less, it is considered to be the part of the oxide in contact with the plating layer. In addition, for the portion of the oxide in contact with the plating layer, when a plating layer is present on both sides of the oxide in the thickness direction, this means that the gap between the plating layer and the oxide is 0.5 mm or less (including 0) on both sides in the thickness direction. When a plating layer is present only on one side of the oxide in the thickness direction (such as when the oxide is the outermost layer), this means that the gap between the plating layer and the oxide is 0.5 mm or less in the direction in which the plating layer is present. In other words, even if an oxide is present, the portion in which the plating layer is present with a gap of more than 0.5 mm between the oxide and the oxide in the thickness direction is excluded from the target for measuring the projected length when calculating ΣLai.

[0035] It is believed that such gaps between the plating layer and the oxide are caused by the evaporation of Zn. In the hot stamped member according to this embodiment, as described later, the Zn phase is dispersed in the dendrites and oxygen diffusion into the plating layer is promoted, so that these elements can be fixed as oxides before Zn (and Mg, if Mg is included) evaporates. In this case, by suppressing the formation of gaps, ΣLai / ΣLi can be made 0.50 (50%) or more. ΣLai / ΣLi is preferably 0.60 or more, more preferably 0.70 or more, and further preferably 0.80 or more.

[0036] The presence of Zn-based oxides (Zn oxides and / or Zn-Mg oxides) having a size of 1.0 μm or more and 10.0 μm or less in the thickness direction of the plating layer and 0.1 μm or more in the direction perpendicular to the thickness direction can be confirmed by the following method. A sample is taken and the cross section of the plated steel sheet is polished while embedded in resin so that the cross section of the plated layer including the interface between the steel material and the plated layer can be observed. After polishing to a mirror finish, an element map image is taken using a scanning electron microscope (SEM) and SEM-EDS with a field of view of, for example, 50 μm × 50 μm. In the obtained element map image, a region where O (oxygen) and Zn coexist is determined to be Zn oxide, and a region where O, Zn, and Mg coexist is determined to be Zn-Mg oxide. By measuring the dimensions of the Zn oxide and Zn-Mg oxide identified by this method, it is possible to identify Zn-based oxides (Zn oxide and / or Zn-Mg oxide) having a size of 1.0 μm to 10.0 μm in the thickness direction of the plated layer and 0.1 μm or more in the direction perpendicular to the thickness direction.

[0037] In addition, the ratio of the total projected length to the length of the interface (ΣLi / Le) is calculated by the following method. The Zn-based oxides are identified by the above-mentioned method. Then, for example, as shown in Figure 2, when multiple Zn-based oxides are present in the coating layer 2, the lengths (L1, L2, L3, L4, L5 (L1 to L5 in the figure, but L1 to Li if there are i inclusions) of each Zn-based oxide projected from the top surface of the coating layer 2 to the interface are measured with respect to the length Le of the interface between the steel material 1 and the coating layer 2 in the measurement area. The total value (ΣL5) of L1 to L5 (ΣLi if L1 to Li) is the total projected length. However, any overlapping projected portions are deducted from the total length (the overlapping portions are included in the length only once). The ratio of the total projected length to the interface length (ΣLi / Le) is obtained by dividing the total projected length (ΣLi) by the interface length (Le). On the other hand, the ratio of the projected length of the part of the oxide that is in contact with the plating layer to the projected length of the oxide (ΣLai / ΣLi) is calculated by the following method. For example, when multiple Zn-based oxides 101 are present in the plating layer 2 as shown in Fig. 3, if plating layers are present on both sides of the oxide in the thickness direction (vertical direction in the drawing), the projected length (e.g., La1) of the portion (contacting the plating layers on both sides) where no gap is observed between the plating layers or where a gap is observed but is 0.5 mm or less is obtained. When a plating layer is present only on one side of the oxide in the thickness direction, the projected length (e.g., La2, La3) of the portion (contacting the plating layers) where no gap is observed between the plating layers or where a gap is observed but is 0.5 mm or less is obtained. The sum of these La1, La2, La3, ...Lai is ΣLai. However, the overlapping parts of the projections are subtracted from the total length (the overlapping parts are included in the length only once). ΣLai / ΣLi is calculated from this ΣLai and ΣLi obtained by the above method.

[0038] Moreover, the structure of the plating layer 2 of the hot stamped member according to this embodiment preferably contains an Fe-Al based intermetallic compound, an Fe-Al-Si based intermetallic compound, and an Fe-Zn based intermetallic compound. In particular, in the hot stamped member according to this embodiment, it is preferable that the plating layer contains an Fe2Al5 phase and the amount of Zn dissolved in the Fe2Al5 phase is 3.00 to 8.00 mass %, which improves corrosion resistance. The Mg-based IMC (intermetallic compound phase) is preferably 5% by area or less in order to avoid LME cracking during hot stamping.

[0039] In this embodiment, the area ratio of each phase in the plating layer is determined by the following method. First, the prepared sample is cut into pieces measuring 25 mm x 25 mm, embedded in resin, and polished to a mirror finish. Then, an SEM-EDS elemental map image of the cross section of the plating layer is obtained at a magnification of 1500x. The elemental map image is taken so that the entire thickness of the hot-dip plating layer is in the field of view. The photographing position is selected randomly. The photographing position should not be arbitrarily reselected based on the results of the area ratio calculation. Each structure and each phase is identified from the element map image. Then, the total cross-sectional area of ​​each structure and each phase appearing in all the cross-sectional photographs is measured by computer image analysis, and this is divided by the cross-sectional area of ​​the hot-dip plated layer appearing in all the cross-sectional photographs to calculate the area ratio of each structure and each phase.

[0040] <Manufacturing method> Next, a preferred method for manufacturing the hot stamped component according to the present embodiment will be described. The hot stamped component according to the present embodiment can obtain the above-mentioned effects regardless of the manufacturing method. However, the method including the following steps is preferable because it can be manufactured stably. (I) A plating process in which a steel material is immersed in a plating bath to produce a base sheet for plating; (II) a cooling step of cooling the plated original sheet to a temperature range of 200° C. or less; (III) a holding step of reheating the plated original sheet after the cooling step, if necessary, and holding it in a temperature range of 100 to 200° C. for 100 seconds or more to obtain a plated steel material; (IV) A hot stamping step of hot stamping the plated steel material to obtain a hot stamped member. In a preferred method for producing the hot stamped member according to the present embodiment, a plating layer having a predetermined chemical composition is provided by (I) to (III), the structure of the plating layer includes an α phase which is a solid solution of Al and Zn, and the α phase contains Zn phases having grain sizes of 10 to 200 nm at a number density of 10 particles / 100 μm 2 A plated steel material having the above-mentioned contents can be obtained. This plated steel material is then hot stamped to obtain the hot stamped member according to the present embodiment.

[0041] [Plating process] In the plating process, a steel material is immersed in a plating bath to form a plating layer on the surface of the steel material, thereby producing an original sheet for plating. The composition of the plating layer to be formed can be predicted from the composition of the plating bath, and therefore, the composition may be adjusted according to the chemical composition of the plating layer to be obtained. The steel material to be subjected to the plating process is not particularly limited, but for example, a hot-rolled steel sheet as described in JIS G3131:2018 or a cold-rolled steel sheet as described in JIS G3141:2017 can be used. Prior to the plating process, the steel material may be subjected to reduction annealing under known conditions, for example, by heating to 750 to 900°C in a 5% H2-N2 gas atmosphere with a dew point of -10°C or higher and holding for 30 to 240 seconds.

[0042] The plating bath composition preferably contains, in mass%, Zn: 1.0 to 30.0%, Mg: 0 to 10.0%, Si: 0.05 to 10.0%, Fe: 0 to 10.0%, and one or more selected from Ca: 0 to 3.00%, Sb: 0 to 0.50%, Pb: 0 to 0.50%, Sr: 0 to 0.50%, Sn: 0 to 1.00%, Cu: 0 to 1.00%, Ti: 0 to 1.00%, Ni: 0 to 1.00%, Mn: 0 to 1.00%, Cr: 0 to 1.00%, La: 0 to 1.00%, Ce: 0 to 1.00%, Zr: 0 to 1.00%, and Hf: 0 to 1.00%, in a total amount of 0 to 5.00%, with the remainder being Al and impurities. By immersing the plated base sheet in such a plating bath, a plated layer having a chemical composition similar to that of the plating bath can be obtained. Since the contents of Zn, Mg, and Fe change due to heating during hot stamping, it is preferable to control the chemical composition of the plated base sheet in consideration of this change so as to control the chemical composition of the hot stamped member as described above.

[0043] [Cooling process] In the cooling process, the original plate after the plating process (pulled out of the plating bath) is cooled after adjusting the plating adhesion amount with wiping gas such as N2. During cooling, after being removed from the plating bath, the steel sheet is cooled to 380°C at an average cooling rate of 20°C / sec or more and less than 40°C / sec (first cooling), and then cooled to 200°C or less at an average cooling rate of 40°C / sec or more from 380 to 200°C (second cooling). By setting the average cooling rate (of the first cooling) to 380°C to 20°C / s or more and less than 40°C / s, Zn is dissolved in the α phase. This promotes the formation of a Zn phase of 10 to 200 nm in the α phase in the subsequent holding step. If the average cooling rate to 380°C after removal from the plating bath is 40°C / s or more, Zn cannot be sufficiently dissolved in the solid solution. On the other hand, if the average cooling rate is less than 20°C / s, Zn precipitates at high temperature, and fine Zn phases cannot be precipitated in the α phase in the subsequent holding step. By limiting the average cooling rate in the temperature range of 380 to 200°C and cooling to 200°C or less (second cooling), the solid-dissolved Zn phase is kept in a supersaturated state while being cooled to a temperature range of 200°C or less. This promotes the formation of a Zn phase of 10 to 200 nm in the α phase in the subsequent holding step. If the average cooling rate in this temperature range is less than 40°C / sec, the precipitation of fine Zn phase into the α phase at the plated steel material stage will be insufficient, and the formation of Zn-based oxides will be insufficient in the hot stamped member. The average cooling rate in the second cooling is preferably 60°C / sec or more, more preferably 70°C / sec or more, and even more preferably 80°C / sec or more. The cooling start temperature for cooling from 380 to 200°C (the temperature at which the first cooling and second cooling are switched over) is preferably close to 380°C, but as long as the average cooling rate to 200°C is 40°C / sec or faster, it may be between 300 and 380°C.

[0044] [Holding process] In the holding step, the plated original sheet after the cooling step is held in a temperature range of 100 to 200° C. for 100 seconds or more to obtain a plated steel material. When the plated original sheet is held, reheating may be performed as necessary, for example, when the original sheet is cooled to 100° C. or lower in the cooling step. After the above cooling, the material is held in a temperature range of 100 to 200° C. for 100 seconds or more, whereby Zn phase having a grain size of 10 to 200 nm is sufficiently precipitated in the α phase. In this case, Zn-based oxides are sufficiently formed in the hot stamped member. If the holding temperature is low or the holding time is short, the amount of Zn phase precipitated becomes insufficient, and the formation of Zn-based oxides in the hot stamped member becomes insufficient. On the other hand, if the holding temperature is high, it becomes difficult to form a Zn phase of 10 to 200 nm in the α phase. Also, if the holding time is long, it causes the Zn phase to grow coarsely, so the holding time is set to 1000 seconds or less.

[0045] Moreover, the holding step is preferably carried out within 5 minutes after the completion of the cooling steps (first cooling and second cooling). "Completion of the cooling step" refers to the point in time when the temperature of the steel material reaches 200°C. If the time from the completion of the cooling step to the start of the holding step is more than 5 minutes, the metastable phase α R phase precipitation begins, making it difficult to meet the number density of the Zn phase in the α phase. After the cooling step is completed, the time until the holding step is started is preferably within 1 minute.

[0046] [Hot stamping process] In the hot stamping process, the plated steel sheet obtained through the above-mentioned processes is heated and cooled during or after forming. In the hot stamping process, in order to impart a predetermined strength to the steel sheet, the sheet is heated to, for example, 840° C. to 1000° C., held at that temperature for 1 to 4 minutes, and then press-formed in a die and quenched. EXAMPLES

[0047] A cold-rolled steel sheet (0.2%C-2.0%Si-2.3%Mn) having a thickness of 1.6 mm was prepared as the steel sheet to be plated. This steel sheet was cut into a size of 100 mm x 200 mm, and then annealed and hot-dipped in succession using a batch-type hot-dip galvanizing test device. The annealing was performed in a furnace with an oxygen concentration of 20 ppm or less in an atmosphere containing 5% H2 gas and the remainder N2 gas with a dew point of 0° C. at 860° C. for 120 seconds. After annealing, the steel sheet was air-cooled with N2 gas, and when the steel sheet temperature reached bath temperature + 20°C, it was immersed in a plating bath having a bath temperature shown in Table 1 for approximately 3 seconds. The plating layer is applied to the plated base sheet, and the plating adhesion is increased to 40 to 80 g / m2 using N2 gas. 2 After adjusting the temperature to 100°C, the steel sheet was cooled under the conditions shown in Table 1. Thereafter, the steel sheet was reheated as necessary and held under the conditions shown in Table 1. The temperature of the steel sheet was measured using a thermocouple spot-welded to the center of the original steel sheet.

[0048] In addition, the obtained plated steel material was inserted into a muffle furnace in an air atmosphere set at 900°C, and then removed after 4 minutes. Hot stamping was then performed by pressing the material with a flat die and quenching the material to obtain a hot stamped part.

[0049] For the obtained hot stamped parts, the chemical composition of the coating layer, whether or not the coating layer contained Zn-based oxides (Zn oxides and / or Zn-Mg oxides) with a size of 1.0 μm to 10.0 μm in the thickness direction and 0.1 μm or more in the direction perpendicular to the thickness direction (plane direction), and if so, the projected length ratios ΣLi / Le and ΣLai / ΣLi of the Zn-based oxides at the interface with the steel were examined by the above-mentioned method. The results are shown in Tables 1 and 2.

[0050] In addition, spot welding was performed on these hot stamped components under the following conditions, and the cross sections of the welds were observed and evaluated based on the length of the cracks (LME cracks). That is, 50mm x 50mm (x sheet thickness) samples were taken from the No. 1 to 26 hot stamped members in the table, and were overlapped with commercially available galvannealed steel sheets of the same size, and the current-carrying electrode was pressed against them with an impact angle of 7° (axial deviation of the electrode from the direction perpendicular to the steel sheet surface) and a load of 400 kgf, and the current pattern was set so that the nugget diameter was 3.5 x √t to 5.5 x √t (t: sheet thickness), and spot welding was performed. A JIS standard DR6φ type Cu-Cr electrode was used as the current-carrying electrode. After spot welding, the steel plate was cut parallel to the direction of the strike angle so that the cross section in the thickness direction of the plate could be observed. After cutting, the cross section of the welded part was mirror-polished by mechanical and chemical polishing, and observed under an optical microscope to measure the LME crack length of the internal crack. The presence or absence of cracks and their length were judged as follows, with AA or A being judged to have excellent LME resistance. (evaluation) AA: No cracks A: Crack length 100μm or less B: Crack length over 100 μm

[0051] In addition, a sample of 50 mm x 100 mm (x plate thickness) was taken from the hot stamped component, and this sample was treated with zinc phosphate (SD5350 system: Nippon Paint Industrial Coating Co., Ltd. standard) to form a chemical conversion coating. The surface of the plated steel sheet on which this chemical conversion coating was formed was observed with an SEM to measure the proportion (area %) of lack of hiding in the chemical conversion coating. The proportion of white paint was judged as follows, with AA or A being judged to have excellent chemical conversion treatability. AA: 5% or less A: More than 5%, less than 10% B: More than 10%

[0052] In addition, the corrosion resistance (corrosion resistance after painting) of the obtained hot stamped members was evaluated. That is, a 50 x 100 mm sample was taken from the hot stamped part and subjected to Zn phosphate treatment (SD5350 system: Nippon Paint Industrial Coating Co., Ltd. standard), then electrocoating (PN110 Powernix (registered trademark) gray: Nippon Paint Industrial Coating Co., Ltd. standard) was applied to a thickness of 20 μm, and baking was performed at a baking temperature of 150 ° C for 20 minutes. Then, a cut was made in the electrocoating film that reached the base steel, and the film was subjected to the JASO test. If the paint film blister width at the 90th cycle in the JASO test was 1 mm or less, it was evaluated as "A", and if it was more than 1 mm, it was evaluated as "B".

[0053] In addition, the spot weldability of the obtained hot stamped members was evaluated based on the appropriate current range during spot welding. That is, a 50mm x 50mm (x plate thickness) sample was taken from the flat surface of the hot stamped component, and the plated surfaces of two of these samples were placed together and pressed together to a pressure of 200kgf between the electrodes. Spot welding was then performed while keeping the electrodes in contact, changing the welding current from 4 to 12kA in 0.5kA increments. The power source was single-phase AC (50Hz), and the current flow time was 12 cycles. A DENGENSHA Resister welder was used as the spot welding machine, and a dome radius type Cr-Cu electrode (tip diameter φ6mm) was used as the electrode. After spot welding, the nugget diameter was measured by observing the cross section of the welded part with an optical microscope, and the relationship between the welding current and the nugget diameter (weld lobe) was investigated. Furthermore, the appropriate current range (unit: kA) was measured, with the current value at which the nugget diameter was 4√t or more (nugget formation current) as the lower limit and the current value at which expulsion occurred (explosion generation current) as the upper limit. The appropriate current range was evaluated as follows: AA: 2kA or more A: Less than 1 to 2 kA B: Less than 1kA

[0054] [Table 1]

[0055] [Table 2]

[0056] [Table 3]

[0057] As can be seen from Tables 1 to 3, Nos. 2 to 7 and Nos. 9 to 19, which have a predetermined chemical composition, a coating layer containing Zn-based oxides consisting of one or both of Zn oxide and Zn-Mg oxide, with a size of 1.0 μm to 10.0 μm in the thickness direction of the coating layer and 0.1 μm or more in the direction perpendicular to the thickness direction, and ΣLi / Le≧0.10 and ΣLai / ΣLi≧0.50, are excellent in chemical conversion treatability or LME resistance during spot welding. In contrast, Comparative Examples Nos. 1, 8, and 20 to 26, in which one or more of the chemical composition of the coating layer and the state of the Zn-based oxide are outside the range of the present invention, were inferior in chemical conversion treatability or LME resistance during spot welding. Furthermore, among the inventive examples, Nos. 2 to 19 had excellent corrosion resistance since the amount of Zn dissolved in the Fe2Al5 phase was within the preferred range of 3.00 mass % or more. In addition, for Nos. 3 to 19, the contact projected length ratio ΣLai / ΣLi of the Zn oxide or Zn-Mg oxide to the plating layer was 0.60 or more, which was within the preferable range, and therefore the appropriate current range was also wide. [Explanation of symbols]

[0058] 1 Steel material 2. Plating layer 101 Zn-based oxide

Claims

1. Steel and A plating layer formed on the steel material; Equipped with The plating layer comprises, in mass %, Zn: 0.5-15.0%, Mg: 0-10.0%, Si: 0.05-10.0%, Fe: 20.0 to 60.0%, and Ca: 0-3.00%, Sb: 0 to 0.50%, Pb: 0 to 0.50%, Sr: 0 to 0.50%, Sn: 0-1.00%, Cu: 0 to 1.00%, Ti: 0 to 1.00%, Ni: 0 to 1.00%, Mn: 0 to 1.00%, Cr: 0-1.00%, La: 0 to 1.00%, Ce: 0-1.00%, Zr: 0 to 1.00%, and Hf: 0-1.00%, Contains 0 to 5.00% in total of one or more selected from the following: The balance is Al and impurities. the plating layer contains a Zn-based oxide consisting of one or both of Zn oxide and Zn-Mg oxide, the Zn-based oxide having a size of 1.0 μm or more and 10.0 μm or less in a thickness direction of the plating layer and 0.1 μm or more in a direction perpendicular to the thickness direction, In a cross section of the plating layer in the thickness direction, when a length of an interface between the plating layer and the steel material is Le, a sum of lengths of the Zn-based oxides projected from an upper surface of the plating layer onto the interface is ΣLi, and a sum of lengths of portions of the Zn-based oxides in contact with the plating layer projected from the upper surface of the plating layer onto the interface is ΣLai, the following formulas (1) and (2) are satisfied. A hot stamped member comprising: ΣLi / Le≧0.10 (1) ΣLai / ΣLi≧0.50 (2)

2. In the chemical composition, in mass%, Mg: 0.2 to 7.0%; The hot stamped component of claim 1 .

3. In the chemical composition, in mass%, Mg: 3.0-7.0%, Zn: 7.0 to 15.0%; The hot stamped component of claim 1 .

Citation Information

Patent Citations

  • Plating steel sheet for hot press forming, forming member using same, and manufacturing method therefor

    EP3733922A1

  • Sowing of plant seed and apparatus therefor

    JP1989039906A

  • Method For Producing A Steel Component By Hot Forming And Steel Component Produced By Hot Forming

    US20120085466A1

  • Steel sheet coated with a metallic coating based on aluminum

    WO2017017513A1

  • Method for the manufacture of a hardened part which does not have LME issues

    WO2017017514A1