Manufacturing method of polysiloxane porous body, polysiloxane porous body, heat-insulating material, and heat-insulating container

A surfactant-free method using tetraalkoxysilane, methyltrialkoxysilane, and dimethyldialkoxysilane achieves flexible and thermally insulating polysiloxane materials, addressing cost and environmental concerns in silicone monolith production.

JP7576346B2Active Publication Date: 2024-10-31NAT INST FOR MATERIALS SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022578126
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-26
Filing Date
2021-12-14
Publication Date
2024-10-31
Estimated Expiration
2041-12-14

AI Technical Summary

Technical Problem

Existing methods for producing silicone monoliths with flexibility require the use of surfactants, leading to high costs and environmental impact due to solvent washing.

Method used

A method involving the use of tetraalkoxysilane, methyltrialkoxysilane, and dimethyldialkoxysilane without surfactants, with specific mole percentages to achieve a co-continuous structure for flexibility and thermal insulation.

Benefits of technology

Produces a flexible polysiloxane material with excellent thermal insulation properties and reduced environmental impact, suitable for heat-insulating materials and containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576346000005
    Figure 0007576346000005
  • Figure 0007576346000006
    Figure 0007576346000006
  • Figure 0007576346000007
    Figure 0007576346000007
Patent Text Reader

Abstract

The present invention provides a method for producing a polysiloxane porous body, the method making it possible to produce a polysiloxane porous body having exceptional flexibility. The production method according to the present invention includes: preparing a composition including a tetraalkoxysilane, a methyl trialkoxysilane, a dimethyldialkoxysilane, and water, and gelling the composition to form a gel; and drying the gel to obtain a polysiloxane porous body. When the total of the tetraalkoxysilane content, the methyl trialkoxysilane content, and the dimethyldialkoxysilane content in the composition is taken as 100 mol%, the tetraalkoxysilane content is 10.5-20.0 mol%, and the dimethyldialkoxysilane content is 11.0-41.0 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polysiloxane porous body, a polysiloxane porous body, a heat-insulating material, and a heat-insulating container. [Background technology]

[0002] A macroporous body that has flexibility while having a skeleton composed of polysiloxane is known. Patent Document 1 describes a method for producing a monolithic silicone body of aerogel or xerogel having continuous through-flow paths and a silicone skeleton capable of dissolving chemical species, by using both a difunctional alkoxysilane and a trifunctional or higher-functional alkoxysilane as starting materials, copolymerizing these silanes by a sol-gel reaction, forming a network of Si-O bonds, and carrying out phase separation. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-61457 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the manufacturing method described in Patent Document 1, a silicone monolith with excellent flexibility can be manufactured, but in order to form "a silicone skeleton that can form a network of Si-O bonds and simultaneously perform phase separation, and can form continuous through-flow paths and dissolve chemical species," a surfactant for controlling phase separation (phase separation control agent) was required.

[0005] In order to remove the surfactant from the synthesized monolith, washing with a large amount of solvent is usually required, and there is room for improvement in terms of cost, environmental load, etc.

[0006] Therefore, an object of the present invention is to provide a method for producing a polysiloxane porous body that has a skeleton composed of polysiloxane and has excellent flexibility without using a surfactant. Another object of the present invention is to provide a polysiloxane porous body, a heat-insulating material, and a heat-insulating container. [Means for solving the problem]

[0007] As a result of extensive investigations aimed at achieving the above object, the present inventors have found that the above object can be achieved by the following configuration.

[0008] [1] A method for producing a polysiloxane porous body, comprising: preparing a composition containing tetraalkoxysilane, methyltrialkoxysilane, dimethyldialkoxysilane, and water; gelling the composition to form a gel; and drying the gel to obtain a polysiloxane porous body, wherein, when the total content of the tetraalkoxysilane, the methyltrialkoxysilane, and the dimethyldialkoxysilane in the composition is taken as 100 mol %, the content of the tetraalkoxysilane is 10.5 to 20.0 mol % and the content of the dimethyldialkoxysilane is 11.0 to 41.0 mol %. [2] The method for producing a polysiloxane porous body according to [1], wherein the composition does not contain a surfactant. [3] The method for producing a polysiloxane porous body according to [1] or [2], wherein the content of the dimethyldialkoxysilane is 38.0 mol % or less. [4] The method for producing a polysiloxane porous body according to [3], wherein the content of the methyltrialkoxysilane is 50.0 mol % or more and the content of the tetraalkoxysilane is 17.0 mol % or more. [5] The method for producing a polysiloxane porous body according to [3], wherein the content of the methyltrialkoxysilane is 67.0 mol % or more. [6] The bulk density of the polysiloxane porous body is 0.300 gcm -3 The method for producing a polysiloxane porous material according to any one of [1] to [5] below. [7] The method for producing a polysiloxane porous body according to any one of [1] to [6], wherein the thermal conductivity at 20°C is 0.0400 W / (m·K) or less. [8] A polysiloxane porous body obtained by hydrolysis and condensation of a composition containing a tetraalkoxysilane, a methyltrialkoxysilane, a dimethyldialkoxysilane, and water, wherein the content of the tetraalkoxysilane is 10.5 to 20.0 mol % and the content of the dimethyldialkoxysilane is 11.0 to 41.0 mol % when the total content of the tetraalkoxysilane, the methyltrialkoxysilane, and the dimethyldialkoxysilane in the composition is 100 mol %. [9] The polysiloxane porous material according to [8], wherein the content of the dimethyldialkoxysilane in the composition is 38.0 mol % or less.

[10] The polysiloxane porous material according to [9], wherein the content of the methyltrialkoxysilane in the composition is 50.0 mol % or more and the content of the tetraalkoxysilane in the composition is 17.0 mol % or more.

[11] The polysiloxane porous material according to [9], wherein the content of the methyltrialkoxysilane in the composition is 67.0 mol % or more.

[12] Bulk density is 0.300 gcm -3 The polysiloxane porous material according to any one of [8] to

[11] below:

[13] The polysiloxane porous body according to any one of [8] to

[12] , which has a thermal conductivity at 20°C of 0.0400 W / (m K) or less.

[14] A heat-insulating material comprising the polysiloxane porous body according to any one of [8] to

[13] .

[15] An insulated container comprising the insulation material described in

[14] . Effect of the Invention

[0009] According to the present invention, there is provided a method for producing a polysiloxane porous body, which can produce a polysiloxane porous body having a skeleton composed of polysiloxane and excellent flexibility without using a surfactant. The present invention also provides a polysiloxane porous body, a heat-insulating material, and a heat-insulating container. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a ternary diagram showing the content of each silicon alkoxide component in the composition. [Diagram 2] FIG. 1 is a perspective view showing the overall configuration of a thermal insulation container 1 according to one embodiment of the present invention. [Diagram 3] FIG. [Figure 4] FIG. [Diagram 5] FIG. [Figure 6] 10A and 10B are diagrams illustrating a method of attaching a heat-insulating material to a heat-insulating container. [Figure 7] This is a modified example of the thermal insulation container. [Figure 8] Each composition of the examples is plotted on a ternary diagram. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] (Definition of terms) In this specification, the term "cocontinuous structure" refers to a state in which, when a cut surface of a member (polysiloxane porous body) is observed with a scanning electron microscope, a skeletal phase mainly composed of polysiloxane and voids are each continuous and three-dimensionally intertwined with each other.

[0013] In addition, in this specification, the term "macropore" refers to a pore having a pore diameter (pore size) of 50 nm or more according to the IUPAC proposal. The pore size and average pore size of the pores are determined by image analysis of an image observed by an electron microscope.

[0014] [Method for producing polysiloxane porous body] The method for producing a polysiloxane porous body of the present invention (hereinafter also referred to as "the present production method") comprises preparing a composition containing tetraalkoxysilane (TEAS), methyltrialkoxysilane (MTAS), dimethyldialkoxysilane (DMDAS), and water, gelling the composition to form a gel, and drying the gel to obtain a polysiloxane porous body, in which, when TEAS+MTAS+DMDAS=100 mol% in the composition, 10.5≦TEAS≦20.0 and 11.0≦DMDAS≦41.0 are satisfied. In the following description, TEAS, MTAS, and DMDAS may be collectively referred to simply as "silicon alkoxide".

[0015] The present inventors have investigated a method for producing a silicone skeleton monolithic body having excellent flexibility without using a surfactant. The synthesis of silicone-skeleton monolithic bodies proceeds via the so-called sol-gel reaction. Thus, they are produced by preparing a composition containing a polyfunctional silicon alkoxide having a hydrolyzable group, and gradually increasing the amount of the polycondensate of the hydrolysis product of the silicon alkoxide in the composition, that is, the polysiloxane that is the skeleton phase of the gel.

[0016] At this time, the phase separation that occurs between the above-mentioned skeletal phase and the solution phase containing unreacted silicon alkoxide, etc. is adjusted to be a viscoelastic phase separation, so that the skeletal phase and the solution phase each have a continuous three-dimensional network structure and form a co-continuous structure in which they are entangled with each other.

[0017] This bicontinuous structure is one of the factors that gives polysiloxane porous bodies their excellent flexibility. For this reason, it has been thought that surfactants for controlling phase separation (phase separation control agents) are essential for producing silicone-skeleton monoliths with excellent flexibility.

[0018] The present inventors have continued to make intensive studies without being bound by the above-mentioned technical common knowledge, and as a result, after trying a large number of compositions, have finally discovered that by using TEAS, MTAS, and DMDAS in combination as monomers and further setting the content of each monomer in a composition containing the monomers and water within a predetermined range, it is possible to control the phase separation behavior, cause viscoelastic phase separation, and obtain a polysiloxane porous body having excellent flexibility, and have completed the present invention. The method for producing the polysiloxane porous body will be described in detail below.

[0019] (Tetraalkoxysilane: TEAS) First, each monomer component used in this production method will be described. The tetraalkoxysilane used in this production method is R 1 is an alkyl group, the formula is: Si-(OR 1 ) 4 (there are multiple R 1 may be the same or different, but is preferably the same.

[0020] R 1 The alkyl group may be linear, branched, or cyclic, but is preferably a linear or branched alkyl group in that it provides better effects of the present invention. R 1 The number of carbon atoms is not particularly limited, but is preferably 1 to 10, since the alcohol generated by hydrolysis and condensation has superior hydrophilicity.

[0021] Examples of linear or branched alkyl groups having 1 to 10 carbon atoms include the following groups: a methyl group having one carbon atom; an ethyl group having two carbon atoms; a propyl group or an isopropyl group having three carbon atoms; a butyl group, an isobutyl group, a tert-butyl group or a sec-butyl group having four carbon atoms; a pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group or a 1-ethylpropyl group having five carbon atoms; a hexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 4-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 1,4-dimethylbutyl group, a 2,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 3,3-dimethylbutyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, a 1-ethyl-2-methyl-propyl group, a 1 ,1,2-trimethylpropyl group; heptyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 5-methylhexyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 4,4-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 1,4-dimethylpentyl group, 2,3-dimethylpentyl group, 2,4-dimethylpentyl group, 3,4-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1,2,2-trimethylbutyl group, 1,1,2-trimethylbutyl group, 1,3,3-trimethylbutyl group, 1,1,3-trimethylbutyl group, 2,2,3-trimethylbutyl group, 2,3,3-trimethylbutyl group;The alkyl groups that have 8 carbon atoms are octyl, 1-methylheptyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 6-methylheptyl, 1-ethylhexyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 1-propylpentyl, 2-propylpentyl, 1,1-dimethylhexyl, 2,2-dimethylhexyl, 3,3-dimethylhexyl, 4,4-dimethylhexyl, 5,5-dimethylhexyl, 3-ethyl- 3-Methylpentyl, 1,1-diethylbutyl, 2,2-diethylbutyl, 1,1,2,2-tetramethylbutyl, 1,1,3,3-tetramethylbutyl, 2,2,3,3-tetramethylbutyl, 1,1-dimethyl-2-ethylbutyl; and 9-carbon nonyl, 2-methyloctyl, 3-methyloctyl, 4-methyloctyl, 2,2-dimethylheptyl, 2,3-dimethylheptyl, 2,4 dimethylheptyl, 2,6 dimethylheptyl, 3,3 dimethylheptyl. , 3,4-dimethylheptyl, 3,5-dimethylheptyl, 4,4-dimethylheptyl, 3-ethylheptyl, 4-ethylheptyl, 2,2,3-trimethylhexyl, 2,2,4-trimethylhexyl, 2,2,5-trimethylhexyl, 2,3,3-trimethylhexyl, 2,3,4-trimethylhexyl, 2,3,5-trimethylhexyl, 2,4,4-trimethylhexyl, 3,3,4-trimethylhexyl, 2-methyl-3-ethylhexyl, 3-methyl-3-ethylhexyl, ethylhexyl group, 3-ethyl-4-methylhexyl group, 3-ethyl-5-methylhexyl group, 2,2,3,3-tetramethylpentyl group, 2,2,3,4-tetramethylpentyl group, 2,2,4,4-tetramethylpentyl group, 2,3,3,4-tetramethylpentyl group, 2,2-dimethyl-3-ethylpentyl group, 2,3-dimethyl-3-ethylpentyl group, 2,4-dimethyl-3-ethylpentyl group, 3,3-diethylpentyl group; decyl group and isodecyl group having 10 carbon atoms; and the like.

[0022] Examples of the cyclic alkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the cyclic alkenyl group include a cyclopropenyl group, a cyclobutenyl group, a cyclopentenyl group, a cyclopentadienyl group, a cyclohexenyl group, a cyclohexadienyl group, a cycloheptenyl group, a cycloheptadienyl group, a cyclooctenyl group, and a cyclooctadienyl group. Examples of the cyclic alkynyl group include a cycloalkenyl group, a cyclooctynyl group, a cyclononynyl group, a cyclodecynyl group, and a cyclodecadiynyl group.

[0023] Examples of TEAS include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetrakis(2-ethylhexyloxy)silane, and from the standpoints of ease of reaction control and cost, tetramethoxysilane (TMOS) is preferred.

[0024] (Methyltrialkoxysilane: MTAS) The methyltrialkoxysilane used in this production method is R 2 is an alkyl group, formula 2: CH3-Si-(OR 2 ) 3 (there are multiple R 2 may be the same or different, but is preferably the same.

[0025] In addition, R 2 The alkyl group of R 1 The meanings and preferred embodiments of the alkyl group are the same as those of the alkyl group mentioned above.

[0026] Examples of MTAS include methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, and methyltributoxysilane, with methyltrimethoxysilane (MTMS) being preferred.

[0027] (Dimethyldialkoxysilane: DMDAS) The dimethyldialkoxysilane used in this production method is R 3 When the alkyl group is used, the formula is (CH3)2-Si-(OR 3 )2 (there are multiple R 3 They may be the same or different, but it is preferable that they are the same.

[0028] In addition, R 3 The alkyl group of R 1 The meanings and preferred embodiments of the alkyl group are the same as those of the alkyl group mentioned above.

[0029] Examples of DMDAS include dimethyldimethoxysilane and diethoxydimethylsilane, with dimethyldimethoxysilane (DMDMS) being preferred.

[0030] Next, the production steps of the present production method using each of the above monomers will be described. The method includes preparing a composition containing TEAS, MTAS, and DMDAS, and water, gelling the composition to form a gel, and drying the resulting gel.

[0031] The content of TEAS in the above composition is 10.5 to 20.0 mol % (10.5 mol %≦TEAS≦20.0 mol %) when the total of TEAS, MTAS, and DMDAS is taken as 100 mol %. If the TEAS content is less than 10.5 mol % or exceeds 20.0 mol %, in a system in which no surfactant is used, a polysiloxane porous body having excellent flexibility cannot be obtained.

[0032] The content of DMDAS is 11.0 to 41.0 mol % (11.0 mol %≦DMDAS≦41.0 mol %) when the total of TEAS, MTAS, and DMDAS is taken as 100 mol %. If the DMDAS content is less than 11.0 mol % or exceeds 41.0 mol %, in a system in which a surfactant is not used, a polysiloxane porous body having excellent flexibility cannot be obtained.

[0033] The content of MTAS is 39.0 to 78.5 mol % (39.0 mol %≦MTAS≦78.5 mol %) when the total of TEAS, MTAS, and DMDAS is taken as 100 mol %. In summary, the content of silicon alkoxide in the composition is: 10.5 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦41.0 mol%, and 39.0 mol%≦MTAS ≦78.5 mol%, It is. Fig. 1 is a ternary diagram showing the content of each of the silicon alkoxide components in the composition, of which the shaded areas in Fig. 1 satisfy the above numerical ranges.

[0034] In particular, from the viewpoint of providing the resulting polysiloxane porous body with better heat insulating properties (lower thermal conductivity), the content of DMDAS in the composition is preferably 38.0 mol % or less. That is, from the viewpoint of obtaining a polysiloxane porous body having better heat insulation properties, the content of silicon alkoxide in the composition is preferably within the following ranges. 10.5 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 39.0 mol%≦MTAS ≦78.5 mol%

[0035] From the viewpoint of obtaining a polysiloxane porous body having even better heat insulation, it is more preferable that the DMDAS content is 38.0 mol% or less, the MTAS content is 50.0 mol% or less, and the TEAS content is 17.0 mol% or more. In other words, from the viewpoint of obtaining a polysiloxane porous body having even better heat insulation, it is more preferable that the silicon alkoxide content in the composition is within the following ranges. 17.0 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 39.0 mol%≦MTAS ≦50 mol% In this case, the content of DMDAS is preferably 30.0 mol % or more. That is, it is preferable that 30.0 mol %≦DMDAS≦38.0 mol %.

[0036] In another embodiment, when the DMDAS content is 38.0 mol % or less and the MTAS content is 67.0 mol % or more, a polysiloxane porous body having even better heat insulation properties can be obtained. 10.5 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 67.0 mol%≦MTAS ≦78.5 mol%

[0037] The composition contains water. The content of water in the composition is not particularly limited, but is preferably 0.1 to 90% by mass. The composition can be prepared by mixing the components already described. In particular, from the viewpoint of providing the obtained polysiloxane porous body with better heat insulation properties (smaller thermal conductivity), the content of the solvent is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 57% by mass or more, when the total mass of the composition is 100% by mass.

[0038] The composition preferably does not contain a surfactant. The composition does not contain a surfactant means that the content of the surfactant is less than 0.001 moles per mole of silicon (total) of TEAS, MTAS, and DMDAS, preferably 0.0001 moles or less, more preferably 0.00001 moles or less.

[0039] The surfactants include cationic, anionic, amphoteric and nonionic surfactants.

[0040] Examples of the anionic surfactant include hexylbenzenesulfonic acid, octylbenzenesulfonic acid, decylbenzenesulfonic acid, dodecylbenzenesulfonic acid, cetylbenzenesulfonic acid, myristylbenzenesulfonic acid, lauryl sulfate, polyoxyethylene lauryl sulfate, dodecenesulfonic acid, tetradecenesulfonic acid, hexadecenesulfonic acid, hydroxydodecanesulfonic acid, hydroxytetradecanesulfonic acid, hydroxyhexadecanesulfonic acid, and the sodium, potassium, ammonium and triethanolamine salts thereof.

[0041] Examples of cationic surfactants include octyltrimethylammonium hydroxide, lauryltrimethylammonium hydroxide, stearyltrimethylammonium hydroxide, dioctyldimethylammonium hydroxide, distearyldimethylammonium hydroxide, lauryltrimethylammonium chloride, stearyltrimethylammonium chloride, cetyltrimethylammonium chloride, dicocoyldimethylammonium chloride, distearyldimethylammonium chloride, benzalkonium chloride, and stearyldimethylbenzylammonium chloride.

[0042] Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene fatty acid esters, polyoxyethylene sorbitan fatty acid esters, sorbitan fatty acid esters, glycerin fatty acid esters, polyoxyethylene hydrogenated castor oil, polyoxyethylene sorbitol fatty acid esters, polyethylene glycol, polypropylene glycol, and diethylene glycol.

[0043] Examples of amphoteric surfactants include amino acid type and betaine acid type surfactants.

[0044] The composition may contain other components within the scope of the effects of the present invention. Examples of other components include an acid and a base.

[0045] (acid) The composition preferably contains an acid. The acid hydrolyzes the alkoxysilane and catalyzes the curing reaction. When the alkoxysilane is hydrolyzed in the system to produce a hydrolysis product, a polycondensation reaction occurs in sequence. Hydrolysis with acid produces H3O + The reaction proceeds electrophilically by H3O + attacks the oxygen atom of the alkoxy group, producing -Si-OH and an alcohol. This reaction is not affected by steric hindrance, and hydrolysis and polycondensation proceed sequentially, making it easy to synthesize linear polysiloxanes.

[0046] The acid may be an inorganic acid or an organic acid, and examples of the inorganic acid that can be used include hydrochloric acid, sulfuric acid, etc., and examples of the organic acid that can be used include formic acid, acetic acid, propionic acid, oxalic acid, citric acid, etc., with acetic acid being preferred in that the hydrolysis reaction can be more easily controlled.

[0047] The content of the acid in the composition is not particularly limited, but in order to provide the polysiloxane porous body with better shape stability and better flexibility, the content of the acid is preferably 1 to 100 mmol per 1 L of the water content in the composition, and more preferably 5 to 10 mmol.

[0048] (base) The composition preferably contains a base. The base hydrolyzes the alkoxysilane and catalyzes the curing reaction. - The reaction proceeds nucleophilically via OH - attacks silicon atoms directly, and RO - (R is an organic group). Although this reaction does not proceed easily at first due to the influence of steric hindrance, once it has progressed, the steric hindrance is alleviated and the reaction tends to proceed rapidly. As a result, the number of hydroxyl groups that contribute to polycondensation increases, making it easier to synthesize branched polysiloxanes.

[0049] The base is not particularly limited, but examples thereof include alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, and lithium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide, strontium hydroxide, and barium hydroxide; alkali metal carbonates such as potassium carbonate and sodium carbonate; ammonia; and amines such as monomethylamine, dimethylamine, triethylamine, monoethylamine, diethylamine, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine.

[0050] Alternatively, the substance may be one that generates a basic substance through a decomposition reaction. Examples of such substances include urea and hexamine. Of these, urea is preferred because of its high solubility in water and volatility, and therefore ease of removal.

[0051] The content of the base in the composition is not particularly limited, but is preferably from 1 mM to 15 M in order to provide the polysiloxane porous material with better shape stability and better flexibility.

[0052] The polysiloxane porous body includes a process (gelation process) in which a gel composed of a skeletal phase and a solution phase is formed by simultaneously carrying out hydrolysis of silicon alkoxide by a sol-gel method using a composition obtained by mixing the components already described, polycondensation of the hydrolysis product of the silicon alkoxide obtained by the hydrolysis, and phase separation between the polycondensate (polysiloxane) obtained by the polycondensation and a solution system containing unreacted silicon alkoxide and the hydrolysis product.

[0053] The skeletal phase of the gel formed in the gelling step is rich in the polycondensate of the hydrolysis product of the silicon alkoxide, and the solution phase is rich in the solvent of the composition, and the content of the polycondensate in the solution phase is relatively low compared to the content in the skeletal phase. The phase separation is a process that proceeds simultaneously with the hydrolysis of silicon alkoxide and the polycondensation of the hydrolysis product, and is typically a viscoelastic phase separation. The framework phase and the solution phase that are generated through this phase separation process each have a continuous three-dimensional network structure and are entangled with each other.

[0054] The gel formed in the gelation step has a bicontinuous structure of the skeletal phase and the solution phase. The polymer constituting the skeletal phase is a polysiloxane having a network of siloxane bonds (-Si-O-Si-) formed by polycondensation of the hydrolysis product of the silicon alkoxide by the sol-gel reaction. That is, the gel formed in the gelation step is a polysiloxane gel.

[0055] The gelation process proceeds by mixing each component to prepare a composition. The composition may be heated at this time. The heating conditions are not particularly limited, but generally, 40 to 100°C is preferable, and the heating time is preferably 2 to 48 hours.

[0056] The gel obtained by the gelling step is a wet gel of polysiloxane. The drying step is a step of drying the wet gel to obtain a polysiloxane porous body. The drying method is not particularly limited, but examples include a method of maintaining the mixture at room temperature to 120°C for 1 to 24 hours.

[0057] Silicon alkoxides having hydrolyzable groups in the molecule undergo polycondensation of the hydrolysis products in the sol-gel reaction to form a network of siloxane bonds. This composition uses di-, tri-, and tetra-functional alkoxysilanes in combination, resulting in a rigid network formed by tri- and tetra-functional alkoxysilanes, and planar, flexible bonds with a high degree of freedom formed by difunctional alkoxysilanes. As a result, the resulting polysiloxane porous body exhibits flexibility even after drying while having a skeleton constituted by polysiloxane.

[0058] The present production method may include other steps than those described above, as long as the effects of the present invention are not impaired. Examples of such other steps include a step of heating the polysiloxane porous body to dehydrate it. The heating temperature is not particularly limited, but is preferably above 200° C. If silanol (Si-OH) remains in the polysiloxane porous body, it can be dehydrated by heating. The polysiloxane porous body has excellent heat resistance, and the flexibility is not lost by this process.

[0059] (Porous polysiloxane) The polysiloxane porous body prepared by the above method has a co-continuous structure of a skeleton composed of polysiloxane and macropores. The polysiloxane constituting the skeleton is a polysiloxane formed by hydrolysis of silicon alkoxides and polycondensation of the hydrolysis products in a composition containing TEAS, MTAS, and DMDAS. In other words, it is a monolithic macroporous member of a silicone composition in which the skeleton is formed by viscoelastic phase separation accompanying the polycondensation reaction of a specific silicon alkoxide in an aqueous solution.

[0060] The degree of flexibility is, for example, 100 kPa or less in Young's modulus. Due to such high flexibility and the fact that the polysiloxane porous body is white in an uncolored state due to light scattering caused by the presence of macropores, the present inventors have named the polysiloxane porous body "marshmallow gel."

[0061] The polysiloxane porous body has macropores with uniform pore size because macropores having a co-continuous structure with the skeleton are formed through a sol-gel reaction combined with a phase separation process. This structure is completely different from the structure of a porous body obtained through a foaming process using a foaming agent (in which a large number of independent pores are formed by foaming).

[0062] The average diameter of the skeleton is, for example, preferably 500 nm or more and less than 10 μm.The average pore diameter of the macropores is, for example, 500 nm to 200 μm. The average pore diameter of the pores in the polysiloxane porous material is preferably 1 μm or more and less than 100 μm. The skeleton diameter and average pore diameter of the polysiloxane porous material are determined by image analysis of an image observed under an electron microscope.

[0063] The porosity of the polysiloxane porous body is preferably, for example, 75 to 98% as measured by a laser confocal microscope.

[0064] The polysiloxane porous body is stable over a wide temperature range because its skeleton is made of polysiloxane, and can maintain its flexibility from the temperature of liquid nitrogen (-196°C) to the temperature at which polysiloxane decomposes (approximately 320°C).

[0065] The polysiloxane porous body also has excellent heat resistance and excellent heat insulation, and although there is no particular limitation on the thermal conductivity, the thermal conductivity at 20°C (atmospheric pressure, in air) is preferably 0.0400 W / (m K) or less, more preferably 0.0350 W / (m K) or less, and even more preferably 0.0330 W / (m K) or less. There is no particular lower limit, but in general, it is preferably 0.0120 W / (m K) or more. The thermal conductivity is measured by the method described in the examples below.

[0066] The bulk density of the polysiloxane porous body is not particularly limited, but is preferably 0.300 gcm -3 (g / cm 3 ) or less is preferable, and 0.200 gcm -3 Less than 0.110gcm is more preferable. -3 The lower limit is not particularly limited, but generally, it is 0.010 gcm -3 The above is preferred.

[0067] In addition, the present polysiloxane porous body has excellent flex resistance. When a polysiloxane porous body having a thickness of 5 mm is prepared and wound around a cylinder (rod) having a diameter of 10 mm, it is preferable that no cracks occur.

[0068] Furthermore, the present polysiloxane porous body has excellent flexibility, and when a flat-plate-shaped polysiloxane porous body is prepared and uniaxially compressed to 80% of its total height (so that the size becomes 20% of the original size), the compression set remaining after unloading is preferably 10% or less, more preferably 8% or less, and even more preferably 5% or less.

[0069] In addition, it is preferable that the change in thermal conductivity of the polysiloxane porous body is small even when the body is deformed by external compression. Although there are no particular limitations on the rate of change in thermal conductivity, when the compression rate by uniaxial compression is 60% (total height is reduced from 100% to 40%), the rate of change in thermal conductivity compared to the thermal conductivity when not compressed (compression rate 0%) is preferably 10.0% or less, and more preferably 6.0% or less. The rate of change in thermal conductivity is the ratio of the absolute value of the difference between the thermal conductivity after compression and the thermal conductivity before compression, expressed as a percentage, to the thermal conductivity before compression. That is, it is a number expressed by the formula: Rate of change in thermal conductivity = |Thermal conductivity after compression-Thermal conductivity before compression| / Thermal conductivity before compression×100.

[0070] The rate of change in thermal conductivity is preferably 10.0% or less, and more preferably 6.0% or less, over the entire range of the compression ratio from 0 to 60%. The rate of change in thermal conductivity is a value obtained by rounding off to one decimal place.

[0071] (Application) The polysiloxane porous body has excellent flexibility, excellent heat resistance, and excellent heat insulation properties, and can be used as a heat insulating material, etc. In addition, because it maintains its flexibility even at liquid nitrogen temperatures, it can also be used as a liquid nitrogen adsorbent, adsorbing and retaining liquid nitrogen.

[0072] In addition, this polysiloxane porous body has liquid repellency and antifouling properties, and can be used as a liquid repellent substrate, etc. It can also be used as a water / oil separation medium, for producing liposomes, and as a soundproofing and vibration-proofing material. Furthermore, by crushing it, it can be used as an additive in cosmetics, a resin filler, a reflective material, etc.

[0073] [Thermal container] The thermal insulation container according to the embodiment of the present invention is a thermal insulation container provided with a thermal insulation material containing the present polysiloxane porous body. The following describes a thermal container according to an embodiment of the present invention with reference to the drawings. The embodiment shown below is an example that embodies the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the material, shape, structure, and arrangement of the components to the embodiment described below. The drawings are schematic. Therefore, the relationship and ratio between the thickness and the planar dimensions may differ from the actual ones, and the relationship and ratio of the dimensions may differ between the drawings.

[0074] Fig. 2 is a perspective view showing the overall configuration of the thermal insulation container 1 according to one embodiment of the present invention. Fig. 3 is a cross-sectional view of the thermal insulation container 1. Fig. 4 is an exploded cross-sectional view of the thermal insulation container 1. Figs. 3 and 4 are cross-sectional views of the thermal insulation container 1 cut at its radial center along a plane parallel to the XY plane.

[0075] As shown in FIGS. 2 and 3, the thermal insulation container 1 includes a housing 10, a container body 20, a thermal insulation material storage section 30, a support member 40, a thermal insulation material 50 (see FIG. 5), and a container opening / closing section 60.

[0076] The thermal insulation container 1 is used for transporting items that require temperature control, such as human and animal medicines, quasi-drugs, food and beverages, and test and research reagents. The thermal insulation container 1 is formed so that the entire container is cylindrical.

[0077] (Chassis 10) The housing 10 is a member disposed on the outermost side of the thermal insulation container 1, and as shown in FIG. 3, a cross section parallel to the XY plane is formed in a concave shape. The housing 10 has a vacuum insulation layer 13 between the outer surface 11 and the inner surface 12. The vacuum insulation layer 13 is a layer filled with gas at a pressure lower than atmospheric pressure. The vacuum insulation layer 13 is connected to the radial side (X direction) of the housing 10 and the bottom surface of the lower side (Y2 side) of the housing 10. That is, the vacuum insulation layer 13 is formed in the housing 10 so as to have a concave shape except on the container opening / closing part 60 side. The housing 10 is formed of a metal member such as aluminum or stainless steel.

[0078] 4, a threaded portion 11s is provided at the end on the upper side (Y1 side) of the outer surface 11 of the housing 10. The threaded portion 11s is a male screw that engages with a threaded portion 61s of a container opening / closing part 60 (opening / closing part main body 61) described later.

[0079] (Container body 20) The container body 20 is a member provided inside the inner surface 12 of the housing 10, and is formed so that a cross section parallel to the XY plane has a concave shape as shown in Fig. 3. An object to be kept warm (not shown) is accommodated inside the container body 20. The outer diameter of the container body 20 is smaller than the inner diameter of the housing 10, and a gap g1 is formed between the inner surface 12 of the housing 10 and the outer surface 22 of the container body 20. A heat-insulating material storage section 30 (described later) is provided in the space of this gap g1.

[0080] In addition, when a thermal insulation material described later is used as a buffer material, the thermal insulation container 1 does not need to have this container body 20. The polysiloxane porous body has a feature that it does not lose its flexibility even when impregnated with liquid nitrogen, and does not lose its buffering properties even at extremely low temperatures. Therefore, in a form that does not have the container body 20, the thermal insulation material has two functions of heat retention and buffering. The thermal insulation container of this form will be described later.

[0081] The container body 20, like the housing 10, is formed from a metal member such as aluminum or stainless steel.

[0082] The container body 20 is supported by a support member 40 inside the housing 10. The support member 40 is a member that connects between the bottom surface 14 of the housing 10 and the bottom surface 21 of the container body 20. By supporting the container body 20 with the support member 40, a gap g2 is formed between the bottom surface 14 of the housing 10 and the bottom surface 21 of the container body 20. In the heat-insulating container 1 of this embodiment, no heat-insulating material is placed in the space of the gap g2, but when the support member 40 is placed on the side surface of the container body 20, a heat-insulating material 50 can be placed in the space of the gap g2. In this embodiment, as shown in FIG. 3, an example is shown in which two support members 40 are provided along the radial direction (X direction) of the housing 10, but the positions and number of the support members 40 are appropriately set.

[0083] (Thermal insulation storage section 30) The heat-insulating material storage section 30 is a cylindrical space provided between the housing 10 and the container body 20, as shown in Fig. 3 or Fig. 4. The heat-insulating material 50 is removably stored in the heat-insulating material storage section 30. The heat-insulating material 50 is not shown in Figs. 2 to 4. The configuration of the heat-insulating material 50 will be described later.

[0084] (Container opening / closing part 60) 4, the container opening / closing part 60 is a member that opens or closes the opening 23 of the container body 20 and the opening 31 of the heat-insulating material storage part 30. The container opening / closing part 60 is composed of an opening / closing part main body 61. Each part constituting the container opening / closing part 60 may be formed of a metal member like the housing 10, or may be formed of a resin material such as plastic. The opening / closing unit main body 61 is a member that is detachably attached to the housing 10, and is formed so that its cross section is substantially convex. A threaded portion 61s is provided on the inner peripheral surface on the Y2 side, which is the back side, of the opening / closing unit main body 61. The threaded portion 61s is a female thread that engages with a threaded portion 11s provided on the housing 10.

[0085] The opening / closing part body 61 can be attached to the housing 10 by rotating the opening / closing part body 61 so that the threaded portion 61s of the opening / closing part body 61 engages with the threaded portion 11s of the housing 10. By attaching the opening / closing part body 61 to the housing 10, the opening 23 of the container body 20 and the opening 31 of the heat-insulating material storage section 30 are closed as shown in Fig. 3. Moreover, by removing the opening / closing part body 61 from the housing 10, the opening 23 of the container body 20 and the opening 31 of the heat-insulating material storage section 30 are opened as shown in Fig. 4.

[0086] (Heat insulation material) The heat-insulating material contains the present polysiloxane porous body. The present polysiloxane porous body has excellent heat insulation properties, so the heat-insulating container 1 including the present polysiloxane porous body has excellent heat-insulating performance.

[0087] The heat-insulating material may further contain a liquid medium. The polysiloxane porous body has excellent temperature stability and interconnected macropores, and the temperature inside the container can be easily controlled by impregnating the porous body with a heated or cooled liquid medium. Examples of the liquid medium include liquid nitrogen.

[0088] Fig. 5 is a perspective view showing a usage form of the heat retaining material 50. In Fig. 5, the longitudinal direction of the heat retaining material 50 will be described as the up-down direction (Y direction). The heat-insulating material 50 includes the polysiloxane porous body and is cylindrical. The outer diameter D1 and the inner diameter D2 of the heat-insulating material 50 are set to dimensions that allow the heat-insulating material 50 to be stored in the gap g1 (see FIG. 3) of the heat-insulating material storage section 30. A gap may be formed between the heat-insulating material 50 and the heat-insulating material storage section 30.

[0089] FIG. 6 is a diagram for explaining a method of attaching the heat-insulating material 50 to the heat-insulating container 1. As shown in FIG. To store the heat-insulating material 50 in the heat-insulating material storage section 30 (housing 10), as shown in Fig. 6, the container opening / closing section 60 is removed from the housing 10 to open the opening 31 of the heat-insulating material storage section 30. Then, the heat-insulating material 50 is inserted from the opening 31 of the heat-insulating material storage section 30.

[0090] Next, the container opening / closing part 60 can be attached to the housing 10 by engaging the screw portion 11s of the housing 10 with the screw portion 61s of the opening / closing part main body 61 (container opening / closing part 60) and rotating the opening / closing part main body 61.

[0091] In the thermal insulation container 1, the container body 20 is supported by a support member 40 that connects between the bottom surface 14 of the housing 10 and the bottom surface 21 of the container body 20. Therefore, the thermal insulation container 1 can hold the container body 20 more stably inside the housing 10.

[0092] 7 shows a modified example of the thermal insulation container. The thermal insulation container 2 does not have the container body 20 that the thermal insulation container 1 has, but has a cylindrical thermal insulation material 50 with a bottom. In the thermal insulation container 2, the object to be kept warm is held in direct contact with the thermal insulation material 50. As already explained, the thermal insulation material 50 has excellent flexibility and therefore also functions as a cushioning material.

[0093] The thermal insulation container 2 has a thicker thermal insulation material 50 than the thermal insulation container 1. This not only improves the thermal insulation but also improves the shock-absorbing performance of the thermal insulation material 50. The thickness of the thermal insulation container 2 may be appropriately determined, but may be adjusted, for example, so that the object to be kept warm fits snugly into the thermal insulation container 2. In other words, if the object to be kept warm is cylindrical, the thickness of the thermal insulation material 50 may be adjusted so that the cylinder fits snugly into the thermal insulation container 2.

[0094] Furthermore, if the heat-insulating material 50 is impregnated with liquid nitrogen or the like, the inside of the heat-insulating container 2 can be kept at a low temperature while the buffering function of the heat-insulating material 50 is not lost, and it can be preferably used for transporting medicines and the like that need to be transported at low temperatures.

[0095] In addition, the polysiloxane porous body has excellent flexibility and exhibits little change in thermal conductivity due to compression, and therefore has the characteristic that it can provide excellent heat retention (insulation) effects even when used in a form that fills gaps, without being a molded product such as the thermal insulation material 50. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0097] (Preparation of polysiloxane porous bodies) 5 g of urea was dissolved in 15 mL of 5 mM acetic acid, and tetramethoxysilane (TMOS), methyltrimethoxysilane (MTMS), and dimethyldimethoxysilane (DMDMS) were added dropwise to obtain the composition shown in Table 1, followed by stirring for 15 minutes to prepare the composition.

[0098] The composition was transferred to a sealed container (gel type) and kept at 80°C for 24 hours to carry out the reaction (gelation and aging).

[0099] The resulting gel was removed from the mold and immersed in at least five times the amount of pure water once and in industrial alcohol twice, each for at least 6 hours, before being evaporated to dryness at 60°C to obtain a dry cured product (polysiloxane porous body).

[0100] (Evaluation 1: Uniformity of the cured product) Compositions for which a homogeneous cured product was obtained by the above procedure are marked with an "A" in the "Evaluation 1" column in Table 1. On the other hand, compositions for which a homogeneous cured product was not obtained are marked with a "B" in the "Evaluation 1" column.

[0101] (Evaluation 2: Flexibility of the cured product) Next, the obtained cured product (thickness: 5 mm) was wrapped around a cylinder (rod) with a diameter of 10 mm, and observed for the occurrence of cracks. For compositions in which no cracks were observed in the obtained cured product, the obtained cured product was recognized as a "polysiloxane porous body (marshmallow gel)" and an "A" was entered in the "Evaluation 2" column. On the other hand, for compositions in which cracks were observed and the obtained cured product did not have the desired flex resistance, a "B" was entered in the "Evaluation 2" column. For compositions for which a homogeneous cured product was not obtained, the above test could not be carried out, and therefore "-" is entered.

[0102] Figure 8 plots each composition on a ternary diagram. The composition that received an "A" rating for all of the above (marshmallow gel) is marked with a "● (black circle)", those that received an "A" rating for Rating 1 and a "B" rating for Rating 2 are marked with a "◯ (white circle)", and those that received a "B" rating for Rating 1 are marked with a "△ (white triangle)". In addition, the polysiloxane porous body obtained from the composition marked with "●" in Fig. 8 was a monolithic macroporous member (marshmallow gel) made of a silicone composition having a skeleton composed of polysiloxane and a co-continuous structure with macropores. On the other hand, "◯" and "△" were not marshmallow gels.

[0103] For the polysiloxane porous bodies that were rated "A" in both evaluations 1 and 2, synthesis was repeated in the same manner as above, except that the amounts of each of the above raw materials were increased by five times, and a panel of approximately 110 mm x 110 mm x 10 mm was produced, and the thermal conductivity was measured by the following method. Table 2 shows the results.

[0104] (Thermal conductivity measurement) Thermal conductivity was measured using the heat flow meter method (ASTM C518) with a NETZSCH "HFM446Lambda" "small". The temperature of the upper plate was set at 25°C (high temperature side) and the temperature of the lower plate was set at 15°C (low temperature side), and the sample was sandwiched between these two plates and thermal conductivity was measured while applying compressive stress. The test was carried out at 20°C, which is the midpoint temperature between the upper and lower plates. The sample was a panel of marshmallow gel approximately 10 mm thick (size 110 mm x 110 mm).

[0105] [Table 1]

[0106] From the results in Table 1, the content of silicon alkoxide is 10.5 mol%≦TEAS ≦20.0 mol%, and It was found that by using the compositions of Examples 1 to 9, in which 11.0 mol %≦DMDAS≦41.0 mol %, a homogeneous polysiloxane porous body having excellent flexibility was obtained. On the other hand, when the compositions of Examples 10 to 25, which are outside the above range, were used, a homogeneous polysiloxane porous body (dried body) was not obtained, or even if a polysiloxane porous body was obtained, it did not have bicontinuous macropores and did not have the desired flexibility (marshmallow gel was not obtained).

[0107] [Table 2]

[0108] From the results in Table 2, the content of silicon alkoxide is 10.5 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 39.0 mol%≦MTAS ≦78.5 mol%, It was found that the polysiloxane porous body of the composition of Example 2, which is within the above range, has a lower thermal conductivity (higher thermal insulation) than the polysiloxane porous body of the composition of Example 1, which is outside the above range.

[0109] In addition, the content of silicon alkoxide is 17.0 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 39.0 mol%≦MTAS ≦50 mol% It was found that the polysiloxane porous body of the composition of Example 2, which is within the above range, has an even lower thermal conductivity (even higher thermal insulation) than the polysiloxane porous body of the composition of Example 4, which is outside the above range.

[0110] In addition, the content of silicon alkoxide is 10.5 mol%≦TEAS≦20.0 mol%, 11.0 mol%≦DMDAS≦38.0 mol%, and 67.0 mol%≦MTAS ≦78.5 mol% It was found that the polysiloxane porous body of the composition of Example 5, which is within the above range, has an even lower thermal conductivity (even higher thermal insulation) than the polysiloxane porous body of the composition of Example 4, which is outside the above range.

[0111] (Preparation of polysiloxane porous body 2) A polysiloxane porous body was prepared in the same manner as in Example 3 of Table 1, except that the contents of 5 mM acetic acid and urea in the composition were as shown in Table 3 below. As a result, a polysiloxane porous body (marshmallow gel) having excellent flexibility (flex resistance evaluation "A") was obtained. In addition, the thermal conductivity and bulk density were measured in the same manner as above. Table 3 shows the results.

[0112] [Table 3]

[0113] Next, the thermal conductivity of the marshmallow gel of Example 3-C was measured in the same manner as above while applying uniaxial compression and changing the compression ratio. The results are shown in Table 4.

[0114] [Table 4]

[0115] The results in Table 4 show that the change in thermal conductivity of the present polysiloxane porous body due to compression is small. In addition, when compared with the thermal conductivity of the uncompressed sample (Example 3-C), the rate of change in thermal conductivity when the compression rate was 61.0% was 3.3% or less. In addition, over the range of compression rates from 0 to 61.0%, the rate of change in thermal conductivity was 10.0% or less, and 6.0% or less. [Industrial Applicability]

[0116] According to this manufacturing method, a polysiloxane porous body having excellent flexibility can be obtained without using a surfactant. Conventionally, it was considered necessary to use a surfactant to obtain a similar polysiloxane porous body, but the removal of the surfactant required washing with a large amount of organic solvent, which was a large environmental burden. This manufacturing method solves the above problem.

[0117] Furthermore, the polysiloxane porous body obtained by the present production method has excellent flexibility, excellent heat resistance, and excellent heat insulation properties, and can be used as a heat insulating material, etc. In addition, because it maintains its flexibility even at liquid nitrogen temperatures, it can also be used as a liquid nitrogen adsorbent, adsorbing and retaining liquid nitrogen.

[0118] In addition, this polysiloxane porous body has liquid repellency and antifouling properties, and can be used as a liquid repellent substrate, etc. It can also be used as a water / oil separation medium, for producing liposomes, and as a soundproofing and vibration-proofing material. Furthermore, by crushing it, it can be used as an additive in cosmetics, a resin filler, a reflective material, etc. [Explanation of symbols]

[0119] 1, 2: Heat insulation container 10: Housing 11:Outer surface 11s: Threaded part 12 :Inner surface 13: Vacuum insulation layer 14: Bottom 20: Container body 21: Bottom 22 :Outer surface 23: Opening 30: Thermal insulation storage section 31: Opening 40: Support member 50: Heat insulation material 60: Container opening and closing part 61: Opening and closing part body 61s: Threaded part

Claims

1. preparing a composition comprising a tetraalkoxysilane, a methyltrialkoxysilane, a dimethyldialkoxysilane, and water, and gelling the composition to form a gel; and drying the gel to obtain a polysiloxane porous body. when the total content of the tetraalkoxysilane, the methyltrialkoxysilane, and the dimethyldialkoxysilane in the composition is taken as 100 mol %, the content of the tetraalkoxysilane is 10.5 to 20.0 mol % and the content of the dimethyldialkoxysilane is 11.0 to 41.0 mol %, The composition is free of surfactants, The tetraalkoxysilane is at least one selected from the group consisting of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetrakis(2-ethylhexyloxy)silane; The methyltrialkoxysilane is at least one selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, and methyltributoxysilane; The method for producing a polysiloxane porous body, wherein the dimethyldialkoxysilane is at least one selected from the group consisting of dimethyldimethoxysilane and diethoxydimethylsilane.

2. The tetraalkoxysilane is tetramethoxysilane, The methyltrialkoxysilane is methyltrimethoxysilane, 2. The method for producing a polysiloxane porous body according to claim 1, wherein the dimethyldialkoxysilane is dimethyldimethoxysilane.

3. The method for producing a polysiloxane porous body according to claim 1 or 2, wherein the content of the dimethyldialkoxysilane is 38.0 mol % or less.

4. 4. The method for producing a polysiloxane porous body according to claim 3, wherein the content of the methyltrialkoxysilane is 50.0 mol % or more and the content of the tetraalkoxysilane is 17.0 mol % or more.

5. The method for producing a polysiloxane porous body according to claim 3, wherein the content of the methyltrialkoxysilane is 67.0 mol % or more.

6. The bulk density of the polysiloxane porous body is 0.300 g cm -3 The method for producing a polysiloxane porous body according to any one of claims 1 to 5, wherein the method is as follows:

7. The method for producing a polysiloxane porous body according to any one of claims 1 to 6, wherein the thermal conductivity at 20°C is 0.0400 W / (m·K) or less.

8. A polysiloxane porous material which is a hydrolysis condensation product of tetraalkoxysilane, methyltrialkoxysilane, and dimethyldialkoxysilane, When the total content of the tetraalkoxysilane, the methyltrialkoxysilane, and the dimethyldialkoxysilane is taken as 100 mol %, the content of the tetraalkoxysilane is 10.5 to 20.0 mol %, the content of the dimethyldialkoxysilane is 11.0 to 41.0 mol %, and the content of the dimethyldialkoxysilane is 11.0 to 41.0 mol %, The tetraalkoxysilane is at least one selected from the group consisting of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetrakis(2-ethylhexyloxy)silane; The methyltrialkoxysilane is at least one selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, and methyltributoxysilane; The dimethyldialkoxysilane is at least one selected from the group consisting of dimethyldimethoxysilane and diethoxydimethylsilane, The polysiloxane porous body is composed of a skeleton and macropores, The average diameter of the skeleton is 500 nm or more and less than 10 μm; The average pore size of the macropores is 1 μm or more and less than 100 μm.

9. Bulk density is 0.300 gcm -3 The polysiloxane porous body according to claim 8, which is as follows:

10. 10. The polysiloxane porous body according to claim 8, having a thermal conductivity of 0.0400 W / (m·K) or less at 20° C.

11. A heat-insulating material comprising the polysiloxane porous body according to any one of claims 8 to 10.

12. A thermal insulation container comprising the thermal insulation material according to claim 11.

Citation Information

Patent Citations

  • Preparation method and application of three-element siloxane sponge

    CN104194028A

  • Production of transparent silica gel bulk substance containing methyl group

    JP1996165114A

  • Made-of-silicone monolithic body and separation, purification, and concentration method using the same

    JP2014061457A

  • Aerogel composite

    JP2020193316A

  • Composite material, gas adsorbent and method for producing composite material