Optical semiconductor devices

The compositionally graded AlGaN layer in optical semiconductor devices addresses the limitations of AlN substrates by maintaining high crystal quality and reducing electrical resistance, resulting in improved light emission and reception efficiencies at lower operating voltages.

JP7576386B2Active Publication Date: 2024-10-31STANLEY ELECTRIC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2017240978
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2017-12-15
Publication Date
2024-10-31
Estimated Expiration
2037-12-15

AI Technical Summary

Technical Problem

Optical semiconductor devices, particularly those operating in the deep ultraviolet region, face challenges with low light emission and reception efficiencies due to high crystal defect densities and increased electrical resistance, which are exacerbated by the limitations of growing AlGaN layers on AlN substrates, leading to compressive strain and limited film thickness.

Method used

The device employs a pseudolattice-matched AlGaN layer with a compositionally graded structure, where the Al composition gradually decreases from the AlN substrate to the active layer, using first and second compositionally graded layers to alleviate strain and maintain high crystal quality, thereby allowing for thicker layers with reduced electrical resistance.

Benefits of technology

This approach results in optical semiconductor devices with improved light extraction and reception efficiencies, operating at lower voltages by maintaining high crystal quality and reducing Fresnel reflection, thus enhancing overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576386000001
    Figure 0007576386000001
  • Figure 0007576386000002
    Figure 0007576386000002
  • Figure 0007576386000003
    Figure 0007576386000003
Patent Text Reader

Abstract

To provide an optical semiconductor element in a deep ultraviolet region which includes an n-type AlGaN layer of high quality and high Al composition of a desired layer thickness, is operated in a low operation voltage, and includes a luminous reception efficacy.SOLUTION: An optical semiconductor element includes: an AlN substrate 11; an n-type semiconductor layer 13 grown onto the AlN substrate, pseudo-lattice matched to the AlN substrate, and formed by an AlGaN layer of which an Al composition becomes small as being farther from the AlN substrate; an active layer 14 grown onto the n-type semiconductor layer; and a p-type semiconductor layer grown onto the active layer.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to optical semiconductor elements such as semiconductor light emitting elements and semiconductor light receiving elements. [Background technology]

[0002] In recent years, AlGaN-based semiconductor light-emitting devices having an emission peak wavelength in the deep ultraviolet region (e.g., 200 nm to 300 nm) have been attracting attention in the field of air and water sterilization applications as a new light source to replace mercury lamps that have been mainly used as ultraviolet light sources. For example, Patent Documents 1 and 2 disclose deep ultraviolet light-emitting devices in which an AlGaN-based semiconductor layer is laminated on single crystal sapphire that has been generally used as a substrate for blue light-emitting diodes. In addition, for example, Patent Document 3 discloses a pseudomorphic semiconductor heterostructure in which an AlGaN-based semiconductor layer is epitaxially grown using aluminum nitride single crystal (AlN) as a substrate material, and a deep ultraviolet light-emitting device including the heterostructure. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4063520 [Patent Document 2] Patent No. 5641173 [Patent Document 3] Patent No. 5730484 [Non-patent literature]

[0004] [Non-Patent Document 1] Journal of Crystal Growth 311 (2009)2864-2866 Summary of the Invention [Problem to be solved by the invention]

[0005] In optical semiconductor elements such as semiconductor light emitting elements, it is preferable that they have high light emission efficiency or light receiving efficiency. For this purpose, for example, it is preferable that the optical semiconductor layer that receives and emits light has high crystal quality, specifically, it is preferable to reduce the density of crystal defects such as threading dislocations that cause a decrease in light emission efficiency or light receiving efficiency. In addition, from the viewpoint of power conversion efficiency, it is preferable that the operating voltage when driving the optical semiconductor element is low, and for this purpose, it is preferable that the optical semiconductor layer has low electrical resistance.

[0006] In particular, optical semiconductor elements that receive and emit light in the deep ultraviolet region have much room for improvement in terms of at least light emission efficiency and light receiving efficiency. For example, optical semiconductor elements in the deep ultraviolet region have optical semiconductor layers including an active layer that are made of AlGaN layers having a high Al composition.

[0007] When an AlGaN layer with a high Al composition is grown on an AlN substrate, it grows in a state where the lattice constant is the same as that of the AlN substrate, i.e., in a pseudomorphic state. Therefore, an AlGaN layer with high crystal quality can be formed. However, when an AlGaN layer with a high Al composition is grown on an AlN substrate, the AlGaN layer is subjected to compressive strain, and the maximum film thickness (critical film thickness) at which the pseudomorphic state can be maintained becomes very small.

[0008] For example, in Non-Patent Document 1, AlGaN with an Al composition of 50% (Al 0.5 Ga 0.5 It has been shown that the critical thickness for an AlGaN layer grown on an AlN substrate is only 0.5 μm or less. Thus, it is often difficult to epitaxially grow an AlGaN layer of the desired thickness while maintaining a pseudomorphic state.

[0009] When the thickness of the AlGaN layer used in an optical semiconductor device is smaller than the desired thickness, the electrical resistance in the direction parallel to the growth surface of the AlGaN layer (hereinafter sometimes referred to as the lateral direction) becomes large, which causes the operating voltage to increase and the current spreading in the semiconductor layer to be hindered, resulting in a decrease in the light emission efficiency.

[0010] In particular, in the n-type AlGaN layer grown on the AlN substrate, the layer thickness becomes small from the viewpoint of the critical film thickness described above, and the operating voltage of the optical semiconductor device increases significantly due to the increase in lateral resistance. Also, in an optical semiconductor device in which both an n-electrode and a p-electrode are provided on one surface side of the optical semiconductor layer, the increase in operating voltage becomes significant. Also, the deterioration of the crystal quality of the n-type AlGaN layer affects the crystal quality of the active layer and the p-type semiconductor layer grown thereafter.

[0011] Furthermore, when mounting an optical semiconductor element on a mounting substrate by flip-chip mounting, for example, light is extracted or taken in through the n-type AlGaN layer and the AlN substrate. In this case, Fresnel reflection occurs at the interface between the AlN substrate and the n-type AlGaN layer due to the difference in refractive index, and the light extraction efficiency or light intake efficiency decreases.

[0012] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a deep ultraviolet optical semiconductor device which has a high-quality n-type AlGaN layer with a desired layer thickness and a high Al composition, which operates at a low operating voltage, and which has high light receiving and emitting efficiency. [Means for solving the problem]

[0013] An optical semiconductor device according to the present invention is characterized by having an AlN substrate, an n-type semiconductor layer grown on the AlN substrate, pseudomorphic to the AlN substrate, and made of an AlGaN layer having an Al composition decreasing with increasing distance from the AlN substrate, an active layer grown on the n-type semiconductor layer, and a p-type semiconductor layer grown on the active layer.

[0014] Furthermore, an optical semiconductor element according to the present invention comprises an AlN substrate, an n-type semiconductor layer grown on the AlN substrate, pseudo lattice matched to the AlN substrate, and made of an AlGaN layer having an Al composition that decreases with increasing distance from the AlN substrate, an active layer grown on the n-type semiconductor layer, and a p-type semiconductor layer grown on the active layer, wherein the n-type semiconductor layer is grown on the AlN substrate, a first composition gradient layer having an Al composition in the range of 0.95 to 1 on the AlN substrate side, and the Al composition gradually decreases from the AlN substrate to the active layer at a first ratio to 0.7 to 0.8, and a second composition gradient layer grown on the first composition gradient layer, and the Al composition gradually decreases from the first composition gradient layer to the active layer at a second ratio smaller than the first ratio.

[0015] Moreover, an optical semiconductor element according to the present invention comprises an AlN substrate, an n-type semiconductor layer grown on the AlN substrate, pseudo lattice matched to the AlN substrate, and made of an AlGaN layer having an Al composition that decreases with increasing distance from the AlN substrate, an active layer grown on the n-type semiconductor layer, and a p-type semiconductor layer grown on the active layer, wherein the n-type semiconductor layer is grown on the AlN substrate, a first composition gradient layer having an Al composition in the range of 0.95 to 1 on the AlN substrate side and whose Al composition gradually decreases at a rate in the range of 0.5 to 2 / μm from the AlN substrate toward the active layer, and a second composition gradient layer grown on the first composition gradient layer and whose Al composition gradually decreases at a rate of 0.1 to 1 / μm from the first composition gradient layer toward the active layer. [Brief description of the drawings]

[0016] [Figure 1] 1 is a cross-sectional view of an optical semiconductor element in accordance with a first embodiment. [Diagram 2] 1 is a band diagram of an optical semiconductor element in accordance with a first embodiment. [Diagram 3] 1 is a diagram illustrating a configuration example of an optical semiconductor element according to a first embodiment. [Figure 4] 1 is a diagram showing the reflectance at the interface between an n-type AlGaN layer and an AlN layer versus the layer thickness of the first composition gradient layer in the optical semiconductor element according to Example 1. FIG. [Diagram 5]4 is a diagram showing the relationship between the layer thickness of the first composition gradient layer in the optical semiconductor element in accordance with Example 1 and the amount of light in the AlN substrate. [Figure 6] 4 is a diagram showing the relationship between the layer thickness of the first composition gradient layer and the optical output in the optical semiconductor element according to Example 1. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, examples of the present invention will be described in detail. EXAMPLES

[0018] Fig. 1 is a cross-sectional view of an optical semiconductor element 10 according to a first embodiment. Fig. 2 is a band diagram of the optical semiconductor element 10. The optical semiconductor element 10 is a semiconductor element that performs photoelectric conversion, for example, a semiconductor light-emitting element. In the following, a case where the optical semiconductor element 10 is a semiconductor light-emitting element will be described, and the optical semiconductor element 10 will be referred to as a light-emitting element. The light-emitting element 10 is, for example, a deep ultraviolet light-emitting element having a peak emission wavelength in the range of 200 nm to 300 nm.

[0019] The light emitting element 10 has an AlN single crystal substrate (hereinafter referred to as AlN substrate) 11, and a buffer layer 12, an n-type semiconductor layer 13, an active layer 14, and a p-type semiconductor layer 15 formed on the AlN substrate 11.

[0020] The light emitting device 10 can be fabricated by using an AlN substrate 11 as a growth substrate and successively growing a buffer layer 12, an n-type semiconductor layer 13, an active layer 14, and a p-type semiconductor layer 15 on the AlN substrate 11 in this order.

[0021] The configuration of each layer of the light-emitting element 10 will be described with reference to FIGS.

[0022] First, although there is no particular limitation, it is preferable to use an AlN substrate 11 having a low dislocation density. 6 cm -2 It is preferable that the value is 10 or less, and more preferably 10 4 cm-2 By using an AlN substrate 11 with a low dislocation density, the dislocation density of the semiconductor layers laminated on the AlN substrate 11 can also be reduced, resulting in improved light emission efficiency or light receiving efficiency. The lower limit of the dislocation density is 0 cm -2 The dislocation density can be measured by a known method, such as measuring the number of dislocations from a transmission electron microscope image or measuring the number of etch pits after immersion in a heated acid mixed solution.

[0023] In the present invention, the crystal growth surface of the AlN substrate 11 is the C-plane. The surface may be slightly inclined (off-angled) from the C-plane, and in this case, the off-angle is preferably 0.1 to 0.5°, and more preferably 0.3 to 0.4°. The direction in which the crystal plane is inclined is not particularly limited, but from the viewpoint of smoothness, it is preferable that the crystal plane is inclined toward the M-axis direction. Since the present invention uses a C-plane AlN substrate, the semiconductor layer grown on the substrate also has the same C-plane as the substrate as its crystal growth surface.

[0024] In addition, the crystal growth surface of the AlN substrate 11 is preferably smooth in order to suppress the generation of new dislocations at the interface between the AlN substrate and the semiconductor layer. 2 The root mean square roughness (RMS) in this region is preferably 5 nm or less, more preferably 1 nm or less, and even more preferably 0.5 nm or less. Such a smooth surface can be obtained by a known chemical mechanical polish (CMP) process. The lower limit of the RMS is preferably 0 nm, but considering industrial production, the lower limit is 0.05 nm with current technology.

[0025] In addition, it is preferable that the AlN substrate 11 has high transparency to the light of the light emitting element or light receiving element to be finally formed. For this reason, it is preferable that the absorption coefficient in the deep ultraviolet region, specifically, in the wavelength of 210 nm or more, is 25 cm -1 The lower limit of the absorption coefficient is preferably 0 cm. -1However, taking into consideration industrial production and measurement accuracy, the lower limit of the absorption coefficient at 210 nm is 15 cm -1 The lower limit of the absorption coefficient at wavelengths of 250 nm or more is 5 cm -1 By using an AlN substrate with such a low absorption coefficient, it is possible to suppress deterioration of characteristics due to ultraviolet light absorption in the AlN substrate 11.

[0026] In addition, the thickness of the AlN substrate 11 used in the present invention is not particularly limited. If the thickness of the AlN substrate is thin, the amount of light absorbed in the substrate can be reduced even if the absorption coefficient is high. However, if the AlN substrate is too thin, it is difficult to handle and there is a risk of reducing the yield of the device. Therefore, the thickness is usually preferably 50 to 1000 μm. The AlN substrate 11 described above can be produced by, for example, the sublimation method or hydride vapor phase epitaxy described in the literature J. Cryst. Growth 312, 58-63 (2009) and the literature Appl. Phys. Express 5, 055504 (2011).

[0027] The crystal growth surface of the AlN substrate 11 is the C-plane (C + The present invention is not limited to a surface (face), and may be, for example, an M surface or an A surface.

[0028] The buffer layer 12 is a single crystal AlN layer provided between the AlN substrate 11 and the n-type semiconductor layer 13. The buffer layer 12 is not essential for the function of the light emitting device or the light receiving device, but is preferably provided from the viewpoint of suppressing lattice relaxation of the n-type semiconductor layer 13 and increasing the yield of the crystal growth process. The thickness of the buffer layer 12 is not particularly limited, but is preferably 5 to 1000 nm, more preferably 30 to 100 nm, in order to obtain the above-mentioned effect of suppressing lattice relaxation. The buffer layer 12 is in a state of lattice matching with the AlN single crystal substrate 11. Here, the lattice matching state refers to a state in which the lattice constant of the a-axis of the AlN single crystal substrate 11 is almost equal to that of the buffer layer 12, and the lattice relaxation rate is ±5% or less. The lower limit of the lattice relaxation rate is 0, which means that the lattice constants of the AlN single crystal substrate 11 and the semiconductor layer are completely the same. The lattice relaxation rate can be measured by X-ray reciprocal lattice mapping measurement.

[0029] The n-type semiconductor layer 13 is a single crystal AlN layer having a band gap equal to or smaller than that of the AlN substrate 11 and the buffer layer 12. x Ga 1-x N (0.5≦x≦1) layer. Since n-type semiconductor layer 13 is lattice-matched with AlN substrate 11, lattice relaxation accompanied by generation of dislocations does not occur in n-type semiconductor layer 13. Therefore, the dislocation density in n-type semiconductor layer 13 is equivalent to the dislocation density on the surface of AlN substrate 11. Therefore, the dislocation density of n-type semiconductor layer 13 is the same as that of AlN substrate 11, and 6 cm -2 It is preferable that the value is 10 or less, and more preferably 10 4 cm -2 It is to be noted that even when the n-type semiconductor layer 13 of the present invention is formed from a plurality of layers, all of these layers are lattice-matched, and therefore the dislocation density is the same in each layer.

[0030] The n-type semiconductor layer 13 contains, for example, Si as an n-type dopant. The dopant concentration of the n-type semiconductor layer 13 is not particularly limited and may be appropriately determined depending on the purpose. In particular, in order to achieve high conductivity, the Si concentration is, for example, 1×1018 cm -3 ~5×10 19 cm -3 Even when the n-type semiconductor layer 13 is formed of a plurality of layers, the Si concentration of each layer is preferably 1×10 18 cm -3 ~5×10 19 cm -3 It is preferable that the Si concentration of each layer is constant, or may be different depending on the device design, etc. Also, the Si concentration at the interface between each layer may be relatively high.

[0031] In this embodiment, the n-type semiconductor layer 13 is made of an AlGaN layer in which the Al composition decreases in the growth direction, that is, in the direction away from the AlN substrate 11 (direction toward the active layer 14).

[0032] In this embodiment, the n-type semiconductor layer 13 includes first and second composition gradient layers 13A and 13B in which the Al composition gradually decreases at different ratios. Specifically, the first composition gradient layer 13A is grown on the AlN substrate 11 and is made of an AlGaN layer in which the Al composition gradually decreases at a first ratio (decrease rate) from the AlN substrate 11 toward the active layer 14.

[0033] The second compositional gradient layer 13B is grown on the first compositional gradient layer 13A and is made of an AlGaN layer having an Al composition equal to or lower than that of the first compositional gradient layer 13A. The second compositional gradient layer 13B is made of an AlGaN layer in which the Al composition gradually decreases at a second ratio (decrease rate) smaller than the first ratio from the first compositional gradient layer 13A toward the active layer 14. Therefore, the n-type semiconductor layer 13 has a band gap as shown in FIG.

[0034] 1, the second composition gradient layer 13B has a layer thickness larger than that of the first composition gradient layer 13A. Specifically, the first composition gradient layer 13A has a first layer thickness d1, and the second composition gradient layer 13A has a second layer thickness d2 larger than the first layer thickness d1. In this embodiment, the entire n-type semiconductor layer 13 is a composition gradient layer and has a layer thickness D.

[0035] The active layer 14 is made of an AlGaN layer having a band gap equal to or smaller than that of the n-type semiconductor layer 13. In this embodiment, the active layer 14 has a multiple quantum well structure made of a plurality of well layers and barrier layers. The active layer 14 emits light in the deep ultraviolet region. Note that the configuration of the active layer 14 is not limited to this, and it may be made of a single layer or may have a single quantum well structure.

[0036] The p-type semiconductor layer 15 is made of an AlN layer, an AlGaN layer, or a GaN layer containing, for example, Mg as a p-type dopant. In this embodiment, the p-type semiconductor layer 15 has a structure in which an electron block layer 15A made of an AlN layer, a p-type cladding layer 15B made of an AlGaN layer, and a p-type contact layer 15C made of a GaN layer are grown on the active layer 14. Therefore, the p-type semiconductor layer 15 has a band gap as shown in FIG.

[0037] It should be noted that there is no limitation to this configuration of p-type semiconductor layer 15. For example, electron blocking layer 15A does not need to have a p-type dopant, and electron blocking layer 15A does not need to be provided.

[0038] Furthermore, the light-emitting element 10 has an n-electrode 16 formed on the n-type semiconductor layer 13, and a p-electrode 17 formed on the p-type semiconductor layer 15. In this embodiment, as shown in Fig. 1, a portion of the active layer 14 and the p-type semiconductor layer 15 are removed, and the upper surface of the n-type semiconductor layer 13 is exposed from the removed portion. The n-electrode 16 is formed on the exposed upper surface of the n-type semiconductor layer 13. Furthermore, the p-electrode 17 is formed on the p-type semiconductor layer 15.

[0039] For example, the n-electrode is made of a laminate of a Ti layer, an Al layer, and an Au layer, and the p-electrode 17 is made of a laminate of a Ni layer and an Au layer.

[0040] In this embodiment, light emitted from the active layer 14 is extracted to the outside through the AlN substrate 11. That is, the surface of the AlN substrate 11 opposite to the n-type semiconductor layer 13 functions as a light extraction surface. The light emitting element 10 has a flip-chip mounting structure in which the n-electrode 16 and p-electrode 17 sides are mounted on a mounting substrate (not shown).

[0041] 3 is a diagram showing a schematic configuration example of the n-type semiconductor layer 13 and the active layer 14 of the light emitting element 10. The detailed configuration of the n-type semiconductor layer 13 will be described with reference to FIG. 3. First, the n-type semiconductor layer 13 is made of Al x Ga 1-x It has a composition of N (0.5≦x≦1). In this embodiment, the n-type semiconductor layer 13 is configured so that the Al composition x gradually decreases from 1 to 0.65.

[0042] The first composition gradient layer 13A of the n-type semiconductor layer 13 is Al x1 Ga 1-x1 The second composition gradient layer 13B has a composition of AlN (0.75≦x1≦1), and is configured so that the Al composition x1 decreases linearly from the AlN substrate 11 toward the active layer 14. x2 Ga 1-x2 It has a composition of N (0.65≦x2≦0.75), and is configured so that the Al composition x2 decreases linearly from the first composition gradient layer 13A toward the active layer .

[0043] First, the n-type semiconductor layer 13 is configured so that the Al composition gradually decreases from the AlN substrate 11 (buffer layer 12), thereby realizing a layer thickness suitable for a deep ultraviolet light emitting device while maintaining high quality. Specifically, the inventors of the present application have fabricated an AlGaN layer having a high Al composition (for example, an Al composition x of 0.5 or more) that is pseudo lattice matched on the AlN substrate 11. Critical Film Thickness noted that the size remained at around 1 μm.

[0044] This is believed to be due to the large strain that occurs in the AlGaN layer (especially at the interface with AlN) during the growth of AlGaN due to the difference in lattice constant between AlN and AlGaN. However, in consideration of suppressing an increase in the operating voltage (lateral electrical resistance), it is preferable that the AlGaN layer as the n-type semiconductor layer 13 in the light emitting device 10 as a deep ultraviolet light emitting device has a thickness greater than this. On the other hand, it is preferable to suppress a deterioration in crystal quality.

[0045] In contrast, the n-type semiconductor layer 13 suppresses abrupt changes in the lattice constant by gradually changing the Al composition within the layer. For example, if the AlGaN layer has a uniform Al composition, strain is concentrated at the interface with the AlN layer (buffer layer 12). However, in the present invention, the AlGaN layer (n-type semiconductor layer 13) is configured such that small strain is gradually generated from the interface with the AlN layer (buffer layer 12). Therefore, strain is relaxed throughout the entire n-type semiconductor layer 13.

[0046] Therefore, the n-type semiconductor layer 13 can be configured as an AlGaN layer having a layer thickness of 1 μm or more while being pseudomorphic. The inventor of the present application predicts that it is possible to form a pseudomorphic n-type semiconductor layer 13 even if the layer thickness D is 2 μm or more. Therefore, the electrical resistance in the n-type semiconductor layer 13 in the direction parallel to the n-type semiconductor layer 13 is reduced, and an increase in the operating voltage is suppressed. Furthermore, in the n-type semiconductor layer 13 with high crystal quality, the absorption of the emitted light from the active layer 14 is small. Therefore, a high light extraction efficiency can be obtained.

[0047] In this embodiment, the first composition gradient layer 13A is configured such that the Al composition x1 decreases from 1 to 0.75 within a relatively small layer thickness d1. This is because, in the AlGaN layer serving as the n-type semiconductor layer 13, the electrical conductivity drops sharply when the Al composition x exceeds 0.8. Specifically, when the n-type semiconductor layer 13 has a large region in which the Al composition x is 0.8 or more, the electrical conductivity of the n-type semiconductor layer 13 as a whole, i.e., the electrical resistance, increases. Therefore, it is preferable that the layer thickness is small at least until the Al composition falls below 0.8.

[0048] In this embodiment, the first composition gradient layer 13A has a thickness d1 smaller than the thickness d2 of the second composition gradient layer 13B. Therefore, the ratio of the thickness d1 of the first composition gradient layer 13A to the total thickness D of the n-type semiconductor layer 13 is small. Therefore, an increase in electrical resistance is suppressed throughout the n-type semiconductor layer 13, and an increase in operating voltage is suppressed.

[0049] In addition, it is preferable that the first composition gradient layer 13A, which is provided on the AlN substrate 11 side of the second composition gradient layer 13B, has an Al composition x1 that decreases from at least 0.95 to less than 0.8 from the AlN substrate 11 toward the second composition gradient layer 13B, regardless of the relationship between the layer thicknesses d1 and d2 described above.

[0050] Moreover, when the upper limit of the Al composition x1 is below 0.95, the difference in the Al composition at the interface between the first composition gradient layer 13A and the AlN substrate 11 (buffer layer 12) becomes large. This increases the difference in refractive index between the AlN substrate 11 and the AlN layer that is the buffer layer 11, and the n-type semiconductor layer 13. This makes it easier for Fresnel reflection of light to occur between the buffer layer 11 and the n-type semiconductor layer 13 in this embodiment. Therefore, it becomes difficult for the emitted light from the active layer 14 to be extracted to the outside from the AlN substrate 11, and the light extraction efficiency decreases. Furthermore, when the lower limit of the Al composition x1 exceeds 0.8, the region in which the electrical conductivity decreases as described above becomes large.

[0051] The lower limit of the Al composition in the interface between the first composition gradient layer 13A and the second composition gradient layer 13B may be determined appropriately depending on the design of the element, but is preferably 0.7 from the viewpoint of reducing distortion within the crystal.

[0052] Therefore, the first composition gradient layer 13A is Al x1 Ga 1-x1 It is preferable that the first compositionally graded layer 13A has a composition of N (0.7≦x1≦1), and that the composition x1 decreases linearly from the AlN substrate 11 toward the active layer 14. It is also preferable that the first compositionally graded layer 13A is configured such that the Al composition x1 on the AlN substrate 11 side is within a range of 1 to 0.95, and that the Al composition x1 decreases from at least 0.95 to below 0.8.

[0053] Next, the second composition gradient layer 13B has a layer thickness d2 larger than that of the first composition gradient layer 13A as described above. The second composition gradient layer 13B is configured so that the Al composition x2 gradually decreases compared to the first composition gradient layer 13A. This increases the ratio of the portion with high conductivity in the n-type semiconductor layer 13. In this embodiment, the n-electrode 16 is in contact with the second composition gradient layer 13B. Therefore, a large current flows between the n-electrode 16 and the active layer 14 through the second composition gradient layer 13B. In addition, the second composition gradient layer 13B, for example, 500 nm or more, preferably 1 μm or more, is interposed between the n-electrode 16 and the first composition gradient layer 13A. This makes it possible to suppress an increase in the operating voltage.

[0054] For example, the thickness d1 of the first composition gradient layer 13A is preferably within a range of 50 to 500 nm. For example, the thickness d2 of the second composition gradient layer 13B is preferably within a range of 0.5 to 2 μm. An example of the configuration of the first and second composition gradient layers 13A and 13B is that the thickness d1 of the first composition gradient layer 13A is less than half the thickness d2 of the second composition gradient layer 13B, for example, the first composition gradient layer 13A is 300 nm, and the second composition gradient layer 13B is 700 nm. This means that when the entire n-type semiconductor layer 13 is considered, 2 / 3 or more of the entire Al composition gradient occurs in 1 / 3 of the region on the AlN substrate 11 side.

[0055] Considering the above, for example, the preferable decrease rate (first ratio) of the Al composition x1 in the first composition gradient layer 13A is within the range of 0.5 to 2 / μm, and for example, the preferable decrease rate (second ratio) of the Al composition x2 in the second composition gradient layer 13B is within the range of 0.1 to 1 / μm.

[0056] 3, the second composition gradient layer 13B preferably has the same Al composition as the Al composition x1 of the first composition gradient layer 13A on the second composition gradient layer 13B side at the interface with the first composition gradient layer 13A. This makes it possible to suppress abrupt composition changes at the interface between the first and second composition gradient layers 13A and 13B and the resulting refractive index changes. Therefore, it is possible to improve the crystal quality while suppressing an increase in the operating voltage.

[0057] In this embodiment, the active layer 14 is made of four Al 0.65 Ga 0.35 The barrier layer has a composition of N and three Al 0.5 Ga 0.5 It has a multiple quantum well structure made up of well layers having a composition of N. Therefore, in this embodiment, the light emitting device 10 emits light with a wavelength of about 265 nm.

[0058] The barrier layer of the active layer 14 has an Al composition equal to or less than the Al composition of the interface with the barrier layer in the second composition gradient layer 13B. 0.8 Ga 0.2 A GaN layer is grown on the N layer as the p-type contact layer 15C. The p-type cladding layer 15B has an Al composition at the interface with the electron blocking layer 15A that is equal to or exceeds the Al composition at the interface with the active layer 14 (barrier layer) of the second composition gradient layer 13B.

[0059] Next, a more preferable layer thickness d1 of the first composition gradient layer 13A will be described with reference to Figures 4 and 5. Figure 4 is a diagram showing the reflectance of light at the interface between the n-type semiconductor layer 13 (AlGaN layer) and the buffer layer 12 (AlN layer) versus the layer thickness d1 of the first composition gradient layer 13A. Figure 4 shows the calculation results of the reflectance at the interface when the active layer 14 emits light with a wavelength of about 265 nm and the light is perpendicularly incident on the interface.

[0060] 4, it can be seen that the reflectance drops sharply when the layer thickness d1 of the first composition gradient layer 13A exceeds 50 nm. This 50 nm corresponds to half the optical wavelength of the light emitted from the active layer 14 in the first composition gradient layer 13A.

[0061] Therefore, the layer thickness d1 of the first composition gradient layer 13A is preferably equal to or greater than half the optical wavelength in the first composition gradient layer 13A of the light emitted from the active layer 14. This significantly suppresses the reflection of light (Fresnel reflection) at the interface between the first composition gradient layer 13A and the buffer layer 12. This improves the light extraction efficiency.

[0062] 5 shows the calculation results of plotting the increase rate (d1=0 nm is used as a reference, i.e., the increase rate is 0%) of the amount of light penetrating into the AlN substrate against the layer thickness d1 when ultraviolet light with a wavelength of 265 nm is incident from the first composition gradient layer 13A side at an incident angle in the range of 0 to 90°. As shown in FIG. 5, the increase rate improves as the layer thickness d1 of the first composition gradient layer 13A increases, and the increase rate tends to saturate when it exceeds about 200 nm.

[0063] 6 shows the increase rate of the light output from the ultraviolet light-emitting device 10 having the same structure as that calculated in FIG. 5. As shown in FIG. 6, the same results as the calculation results in FIG. 5 were obtained in the experiment, and the light output was improved by 10% or more when the layer thickness d1 of the first composition gradient layer 13A was 200 nm and 300 nm. The difference between the calculation results in FIG. 5 and the experimental results in FIG. 6 is believed to be due to the fact that the calculation estimates the amount of light penetrating one path from the n-type semiconductor layer 13 into the AlN substrate 11, whereas in the actual light-emitting device, the effect of multiple reflections inside the semiconductor layer is added, and the effect of suppressing Fresnel reflection becomes more prominent.

[0064] Therefore, the layer thickness d1 of the first composition gradient layer 13A is preferably 200 nm or more. Therefore, for example, the layer thickness d1 of the first composition gradient layer 13A is preferably within a range of 200 to 500 nm, and more preferably 200 to 350 nm. If the layer thickness d1 is 500 nm or more, the layer thickness D of the entire n-type semiconductor layer 13 becomes large, and the risk of lattice relaxation increases. Also, from the viewpoint of suppressing Fresnel reflection, the effect obtained is the same even if the layer thickness d1 is 350 nm or more, so from the viewpoint of productivity, the layer thickness d1 is preferably 350 nm or less.

[0065] An example of the thicknesses of the other layers in the light-emitting device 10 is shown below. For example, each of the well layers in the active layer 14 has a thickness of 3 nm. Each of the barrier layers in the active layer 14 has a thickness of 7 nm, except for the barrier layer closest to the p-type semiconductor layer 15. The barrier layer in the active layer 14 closest to the p-type semiconductor layer 15 has a thickness of 20 nm. The electron blocking layer 15A has a thickness of 9 nm. The p-type cladding layer 15B has a thickness of 50 nm. The p-type contact layer 15C has a thickness of 250 nm.

[0066] In this embodiment, the first and second composition gradient layers 13A and 13B each have a linear Al composition. However, the Al composition may change stepwise. That is, the Al composition of the n-type semiconductor layer 13 gradually decreases means that the Al composition decreases linearly or decreases stepwise.

[0067] In this embodiment, a compositionally graded layer is grown on the buffer layer 12 as the n-type semiconductor layer 13. However, the compositionally graded layer may have a layer that does not contain an n-type dopant in a part thereof. For example, a compositionally graded layer that does not contain an n-type dopant may be provided between the buffer layer 12 and the n-type semiconductor layer 13. That is, the non-doped compositionally graded layer and a compositionally graded layer that contains an n-type dopant may be stacked.

[0068] In this embodiment, the first and second composition gradient layers 13A and 13B are each composed of an AlGaN layer having a continuously decreasing Al composition. However, the first and second composition gradient layers 13A and 13B may be an AlGaN layer having an equivalently decreasing Al composition. Specifically, the first and second composition gradient layers 13A and 13B may have a superlattice structure in which pairs of well layers and barrier layers made of AlGaN are stacked multiple times, and the Al composition of the well layers may be gradually decreased toward the active layer 14.

[0069] In addition, in this embodiment, the optical semiconductor element 10 is a semiconductor light emitting element, but the optical semiconductor element 10 may be a light receiving element that receives light in the deep ultraviolet region and generates an electrical signal. In this case, for example, the surface of the AlN substrate 11 opposite to the n-type semiconductor layer 13 functions as a light intake surface (light receiving surface). In this case as well, the n-type semiconductor layer 13 with high crystal quality is formed with the desired layer thickness D, so that a semiconductor light receiving element with low operating voltage and high light receiving efficiency can be provided.

[0070] Furthermore, when the optical semiconductor element 10 is a semiconductor light receiving element, the layer thickness d1 of the first composition gradient layer 13A only needs to be equal to or greater than the optical wavelength in the first composition gradient layer 13A of the light received by the active layer 14. This suppresses the reflection of light (Fresnel reflection) at the interface between the first composition gradient layer 13A and the buffer layer 12. This increases the amount of light that is taken in through the AlN substrate 11, the buffer layer 12, and the n-type semiconductor layer 13. This improves the light receiving efficiency (light taking-in efficiency).

[0071] Therefore, the layer thickness d1 of the first composition gradient layer 13A is preferably equal to or greater than the optical wavelength in the first composition gradient layer 13A of the light emitted from or received by the active layer 14. Note that the light emitted from or received by the active layer 14 refers to light having a wavelength corresponding to the band gap of the active layer 14 and a wavelength band including that wavelength.

[0072] As described above, the optical semiconductor device 10 has the AlN substrate 11, the n-type semiconductor layer 13 made of an AlGaN layer grown on the AlN substrate 11, pseudo lattice matched to the AlN substrate 11, and having a decreasing Al composition with increasing distance from the AlN substrate 11, the active layer 14 grown on the n-type semiconductor layer 13, and the p-type semiconductor layer 15 grown on the active layer 14. Therefore, it is possible to provide an optical semiconductor device 10 in the deep ultraviolet region that has a high-quality n-type AlGaN layer with a desired layer thickness D and that operates at a low operating voltage. [Explanation of symbols]

[0073] 10 Optical semiconductor elements 11 AlN substrate (growth substrate) 12 AlN buffer layer 13 n-type semiconductor layer 13A First compositionally graded layer 13B Second compositionally graded layer 14 Active layer 15 p-type semiconductor layer

Claims

1. An AlN substrate having a C+ surface; an n-type semiconductor layer made of an AlGaN layer grown on and in contact with the C+ plane of the AlN substrate, pseudomorphically lattice-matched to the AlN substrate, and having an Al composition that decreases with increasing distance from the AlN substrate; an active layer grown on the n-type semiconductor layer; a p-type semiconductor layer grown on the active layer; The n-type semiconductor layer is a first composition gradient layer grown on a C+ plane of the AlN substrate, the first composition gradient layer having an Al composition in a range of 0.95 to 1 on the AlN substrate side, and the Al composition gradually decreasing at a first ratio in a range of 0.5 to 2 / μm from the AlN substrate toward the active layer; a second compositional gradient layer grown on the first compositional gradient layer, having an Al composition equal to or lower than that of the first compositional gradient layer, and the Al composition gradually decreasing from the first compositional gradient layer toward the active layer at a second ratio in a range of 0.1 to 1 / μm; The second ratio is less than the first ratio. An optical semiconductor element comprising:

2. The first composition gradient layer is Al x1 G 1-x1 N (0.7≦x1≦1), 2. The optical semiconductor device according to claim 1, wherein the Al composition x1 decreases linearly from the AlN substrate toward the active layer.

3. 3. The optical semiconductor device according to claim 2, wherein the first compositionally graded layer has a thickness smaller than that of the second compositionally graded layer.

4. 4. The optical semiconductor element according to claim 1, wherein the first composition gradient layer has a layer thickness equal to or greater than an optical wavelength in the first composition gradient layer of light emitted from the active layer or light received by the active layer.

5. 4. The optical semiconductor device according to claim 1, wherein the first composition gradient layer has a thickness of 200 nm or more.

6. 6. The optical semiconductor element according to claim 1, wherein the second compositionally graded layer has the same Al composition as the first compositionally graded layer on the side of the first compositionally graded layer.

7. An AlN substrate having a C+ surface; a buffer layer made of single crystal AlN grown on the C+ face of the AlN substrate, the buffer layer having the C+ face as a main surface and lattice-matched with the AlN substrate; an n-type semiconductor layer made of an AlGaN layer grown on and in contact with the C+ plane of the buffer layer, pseudomorphically matching the buffer layer, and having an Al composition that decreases with increasing distance from the AlN substrate; an active layer grown on the n-type semiconductor layer; a p-type semiconductor layer grown on the active layer; The n-type semiconductor layer is a first composition gradient layer grown on the C+ plane of the buffer layer, the first composition gradient layer having an Al composition in the range of 0.95 to 1 on the AlN substrate side, and the Al composition gradually decreasing from the AlN substrate to the active layer at a first ratio to 0.7 to 0.8; a second composition gradient layer grown on the first composition gradient layer, the second composition gradient layer having an Al composition that gradually decreases from the first composition gradient layer to the active layer at a second ratio that is smaller than the first ratio.

8. An AlN substrate having a C+ surface; a buffer layer made of single crystal AlN grown on the C+ face of the AlN substrate, the buffer layer having the C+ face as a main surface and lattice-matched with the AlN substrate; an n-type semiconductor layer made of an AlGaN layer grown on and in contact with the C+ plane of the buffer layer, pseudomorphically matching the buffer layer, and having an Al composition that decreases with increasing distance from the AlN substrate; an active layer grown on the n-type semiconductor layer; a p-type semiconductor layer grown on the active layer; The n-type semiconductor layer is a first composition gradient layer grown on the C+ plane of the buffer layer, the first composition gradient layer having an Al composition in a range of 0.95 to 1 on the AlN substrate side, and the Al composition gradually decreasing at a first ratio in a range of 0.5 to 2 / μm from the AlN substrate toward the active layer; a second composition gradient layer grown on the first composition gradient layer, the second composition gradient layer having an Al composition that gradually decreases from the first composition gradient layer toward the active layer at a second ratio within a range of 0.1 to 1 / μm; The second ratio is less than the first ratio. An optical semiconductor element comprising:

9. 9. The optical semiconductor element according to claim 1, wherein the AlN substrate having the C+ plane has an off angle, the off angle being 0.1 to 0.5°.

10. 9. The optical semiconductor element according to claim 1, wherein the off angle is a tilt toward an M-axis direction.

Citation Information

Patent Citations

  • Method and device for welding and assembling bottom plate of tank

    JP1981041173A

  • Compensation system for speed error of reproduced video signal

    JP1982030484A

  • Nitride semiconductor light-emitting element and semiconductor optical device

    JP2012146847A

  • semiconductor light emitting device

    JP4063520B2

  • Nitride semiconductor light-emitting element

    WO2017057149A1