Film, multi-layer electronic equipment and film manufacturing method

A polyimide layer with tailored properties and manufacturing method addresses the limitations of existing polyimide films, providing enhanced heat resistance, optical properties, and adhesion for use in foldable or rollable displays.

JP7576598B2Active Publication Date: 2024-10-31マイクロワークス ソリューションズ 株式会社
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2022152873
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-09-26
Publication Date
2024-10-31
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

Polyimide films exhibit poor optical properties due to their yellowish color and low transmittance in the visible light region, making them unsuitable for use as optical materials, and they lack the necessary flexibility and resilience for applications in foldable or rollable displays.

Method used

A polyimide layer with specific compositions and properties, including a thickness of 50 μm, loop stiffness of 3-4.5 m/N, heat resistance stability index of 5-15 °C/2 ppm·MPa, thermal expansion coefficient of 35 ppm/°C or less, and adhesion force of 200 gf/inch or more, is developed, using a manufacturing method involving the polymerization of aromatic diamine and dianhydride compounds followed by heat treatment.

Benefits of technology

The polyimide layer achieves excellent heat resistance, optical properties, and adhesion, enabling its use as a support layer in foldable or rollable displays with improved bending resilience and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576598000013
    Figure 0007576598000013
  • Figure 0007576598000014
    Figure 0007576598000014
  • Figure 0007576598000015
    Figure 0007576598000015
Patent Text Reader

Abstract

To provide a film excellent in all of heat resistance, optical properties, and adhesion force and having a high utilization degree as a supporting layer of a foldable display and the like, a multilayer electronic device including the film, and a manufacturing method of the film.SOLUTION: A film includes a polyimide layer 50 including an aromatic diamine compound residue and an aromatic dianhydride compound residue, wherein the polyimide layer 50 has a loop stiffness value of 3 to 4.5 m / N based on a thickness of 50 μm.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiment relates to a film having excellent heat resistance, optical properties, adhesion, etc., due to the polyimide layer, and thus having excellent usability as a support layer for a foldable display, a multilayer electronic device including the same, and a method for manufacturing the film. [Background technology]

[0002] Polyimide films have excellent heat resistance and mechanical properties, and are therefore used in a wide range of applications as coating materials, composite materials, etc. Such polyimide films are generally produced by coating a composition obtained by solution polymerization of aromatic diamines and aromatic dianhydrides into a film, drying the film at high temperatures, and dehydrating the film to cause ring closure.

[0003] Polyimide films have a problem in that they are yellowish due to the high density of aromatic rings, and have low transmittance in the visible light region, making them difficult to use as optical materials. Recently, however, colorless and transparent polyimide films have been produced, and various attempts have been made to apply them as optical materials.

[0004] Related prior art includes Korean Patent Publication No. 10-2007-0017001 and Korean Patent Registration No. 10-1992525. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the embodiment is to provide a film having excellent rigidity for application to a foldable or rollable display and simultaneously improved heat resistance and optical properties, and a multi-layer electronic device using the same. Another object of the embodiment is to provide a film including a polyimide layer having excellent heat resistance, optical properties, adhesive properties, residual stress properties, etc. Still another object of the embodiment is to provide a method for manufacturing the film. [Means for solving the problem]

[0006] To achieve the above object, a film according to an embodiment includes a polyimide layer containing an aromatic diamine compound residue and an aromatic dianhydride compound residue, and the polyimide layer has a loop stiffness value of 3 to 4.5 m / N based on a thickness of 50 μm.

[0007] The polyimide layer has a heat stability index (HS index) of 5 to 15°C according to the following formula 1: 2 / ppm·MPa.

[0008] [Formula 1] JPEG0007576598000001.jpg1044

[0009] In formula 1, The above HS index is the heat stability index (℃ 2 / ppm·MPa).

[0010] The Tg is the glass transition temperature (° C.).

[0011] The H is the thermal expansion coefficient (ppm / ° C.) of the polyimide layer.

[0012] The RS is the value of the residual stress (MPa) of the polyimide layer.

[0013] The polyimide layer may have an adhesion of 200 gf / inch or more.

[0014] The polyimide layer may have a yellowness index of 5.3 or less.

[0015] The polyimide layer has a composite index represented by the following formula 2 of 2° C. 2 / ppm or more.

[0016] [Formula 2] JPEG0007576598000002.jpg1037

[0017] In formula 2, The T Index is a comprehensive index.

[0018] The Tg is the glass transition temperature (° C.).

[0019] The YI is the yellowness value of the polyimide layer at a thickness of 10 μm.

[0020] The H is the thermal expansion coefficient (ppm / ° C.) of the polyimide layer.

[0021] The polyimide layer may contain 5 to 45 moles of biphenyltetracarboxylic acid dianhydride residues when the entire amount of the aromatic dianhydride compound residues is considered to be 100 moles.

[0022] The polyimide layer can include biphenyltetracarboxylic acid dianhydride residues and pyromellitic acid dianhydride residues.

[0023] When the sum of the mole numbers of the biphenyltetracarboxylic acid dianhydride residue and the pyromellitic acid dianhydride residue is viewed as a whole, the content of the biphenyltetracarboxylic acid dianhydride residue may be 15 to 50 mol %.

[0024] The pyromellitic dianhydride residue may be less than 60 mol % when the entire aromatic dianhydride compound residue is considered as 100 mol.

[0025] In order to achieve the above object, a multilayer electronic device according to another embodiment includes a substrate layer; and a light-emitting functional layer disposed on the substrate layer, the substrate layer including a film, and the film is the above-mentioned film.

[0026] In order to achieve the above object, a method for producing a film according to yet another embodiment includes: a polymer solution production step of stirring a raw material composition containing an aromatic diamine compound and an aromatic dianhydride compound to produce a polymer solution having a viscosity of 1,000 to 8,000 cps measured at 25°C; a sheet production step of applying the polymer solution to a sheet and drying it with hot air to produce a sheet; and a film production step of heat-treating the sheet at 360 to 480°C to produce a polyimide layer.

[0027] The film includes the polyimide layer, the polyimide layer contains the aromatic diamine compound residue and the aromatic dianhydride compound residue, and the polyimide layer has a loop stiffness value of 3 to 4.5 m / N based on a thickness of 50 μm.

[0028] The raw material composition or the polymer solution may further include a leveling stabilizer. Effect of the Invention

[0029] The film of the embodiment, the multilayer electronic device including the same, and the method for manufacturing the film provide a film having excellent folding recovery force, which is advantageous for use in a foldable or rollable display. In addition, the film has excellent heat resistance, optical properties, adhesion, etc., and is highly usable as a support layer for a foldable display. The embodiment provides a heat-resistant film including a polyimide layer having improved heat resistance and optical properties at the same time, thereby making it possible to provide a multilayer electronic device that is thinner and lighter while also having improved optical properties. In addition, a reliable manufacturing method can be provided, which can provide a method for manufacturing a film with improved workability. [Brief description of the drawings]

[0030] [Figure 1] 1 is a schematic cross-sectional view illustrating a layer structure of a film according to an embodiment. FIG. [Diagram 2] 1 is a schematic cross-sectional view illustrating a layer structure of a film according to an embodiment. FIG. [Diagram 3] 1 is a schematic cross-sectional view illustrating a layer structure of a multi-layer electronic device according to an embodiment; [Figure 4] 1 is a schematic cross-sectional view illustrating a layer structure of a multi-layer electronic device according to an embodiment; [Diagram 5] 1 is a conceptual diagram illustrating the process of an adhesion test in cross section. [Figure 6] FIG. 1 is a conceptual diagram illustrating a cross-section of the process of a loop stiffness test. BEST MODE FOR CARRYING OUT THEINVENTION

[0031] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the following, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily understand the present invention. However, the present invention may be embodied in many different forms and is not limited to the preferred embodiments described herein. The same reference numerals are used throughout the specification to refer to similar parts.

[0032] In this specification, when a certain configuration "includes" another configuration, this does not mean excluding the other configuration, and means that the other configuration may be further included, unless otherwise specified.

[0033] In this specification, when a certain component is said to be "connected" to another component, this includes not only the case where the component is "directly connected" but also the case where the component is "connected via another component between them."

[0034] In this specification, the term "B is located on A" means that B is located on A in direct contact therewith, or that B is located on A with another structure therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.

[0035] As used herein, the term "combinations thereof" contained in a Markush form expression means a mixture or combination of one or more selected from the group of components set forth in the Markush form expression, and is meant to include one or more selected from the group of components.

[0036] In this specification, the phrase "A and / or B" means "A, B, or A and B."

[0037] In this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from each other, unless otherwise specified.

[0038] In this specification, the term "singular" is to be construed as including the singular or plural as the context requires, unless otherwise specified.

[0039] In this specification, the relative sizes, thicknesses, and the like of components shown in the drawings may be exaggerated for ease of explanation.

[0040] In this specification, the yellowness index (YI) is based on a value calculated according to the ASTM E-313 standard using the CIE color system of a spectrophotometer (UltraScan PRO by Hunter Associates Laboratory).

[0041] In this specification, viscosities given without reference to a specific temperature refer to viscosities measured at room temperature, illustratively viscosities measured at 25°C.

[0042] The embodiments will be described in more detail below.

[0043] When the polyimide film is a film having excellent heat resistance, it has the characteristics of a colored film close to brown, and when it is a transparent film, it has the characteristics of poor heat resistance. In other words, heat resistance and transparency are in a trade-off relationship with each other.

[0044] Polyimide films are used as insulating layers in electronic products based on the insulating properties of the polyimide film. In addition, attempts are ongoing to apply polyimide films to flexible or foldable displays based on the foldable or flexible properties of plastic films themselves and the insulating properties of polyimide films.

[0045] Films used as support layers for displays must be able to withstand harsh environments, such as repeated exposure to high heat during the display manufacturing process, and must also have controlled residual stress and thermal expansion properties to ensure stable physical properties for other layers laminated on the support layer.

[0046] In addition, in order to apply the polyimide layer to a foldable or rollable display, it is necessary for the polyimide layer to have not only the ability to flexibly bend, but also the ability to recover with appropriate elasticity. The inventors have prepared a film having a polyimide layer that satisfies various conflicting characteristics required when applied as a support layer of a display, etc., to an appropriate level or higher, confirmed its characteristics, and presented an embodiment.

[0047] 1 and 2 are conceptual diagrams illustrating the cross-section of a layer structure of a film according to an embodiment, FIGS. 3 and 4 are conceptual diagrams illustrating the cross-section of a layer structure of a multi-layer electronic device according to an embodiment, FIG. 5 is a conceptual diagram illustrating the cross-section of an adhesion test process, and FIG. 6 is a conceptual diagram illustrating the cross-section of a loop stiffness test process.

[0048] The multi-layer electronic device 800 and a film used as the substrate layer 100 will be described in detail below with reference to FIGS. 1 to 6. FIG.

[0049] film The film according to one embodiment includes a polyimide layer 50 (see FIG. 1).

[0050] The polyimide layer 50 contains an aromatic diamine compound residue and an aromatic dianhydride compound residue.

[0051] The polyimide layer 50 can have excellent loop stiffness properties.

[0052] The 50 μm thick polyimide layer 50 may have a loop stiffness value of 3 to 4.5 m / N. The 50 μm thick polyimide layer 50 may have a loop stiffness value of 3.1 to 4.2 m / N. The 50 μm thick polyimide layer 50 may have a loop stiffness value of 3.2 to 4.1 m / N.

[0053] In this case, the polyimide layer has excellent bending recovery, and when applied to a bendable or rollable multi-layer electronic device, the device can have even better recovery force against bending.

[0054] The loop stiffness can be measured using a loop stiffness tester (TOYOSEIKI). A 50μm thick polyimide film sample is fixed at both ends to a fixing part with a width of 15mm and a length of 120mm, and the sample is pressed at a pressing speed of 3.3mm / s using the pressing part until the final separation distance L between the pressing part and the fixing part becomes 20mm, and then the loop stiffness of the sample can be measured using a sensor. In this embodiment, the measurement is based on the MD direction of the film as the longitudinal direction (see Figure 6).

[0055] The polyimide layer 50 has a heat stability index (HS index) of 5 to 15°C according to the following formula 1. 2 / ppm·MPa.

[0056] [Formula 1] JPEG0007576598000003.jpg1044

[0057] In formula 1, The above HS index is the heat stability index (℃ 2 / ppm·MPa).

[0058] The Tg is the glass transition temperature (° C.).

[0059] The H is the thermal expansion coefficient (ppm / ° C.) of the polyimide layer.

[0060] The RS is the value of the residual stress (MPa) of the polyimide layer.

[0061] The heat stability index of the polyimide layer is 5°C 2 The heat stability index may be 6°C / ppm·MPa or more. 2 The heat stability index may be 7°C / ppm·MPa or more. 2 The heat stability index may be 7.3°C / ppm·MPa or more. 2 The polyimide layer may have a heat stability index of 15° C. / ppm·MPa or more. 2 The heat stability index may be 13°C / ppm·MPa or less. 2 / ppm·MPa or less.

[0062] When the polyimide layer has the above heat resistance stability index, it has a relatively high glass transition temperature, a low thermal expansion coefficient, and low residual stress, and is therefore excellent for use as a support layer for a multi-layer electronic device.

[0063] The polyimide layer 50 may have an adhesion of 200 gf / inch or more. The adhesion may be 220 gf / inch or more. The adhesion may be 230 gf / inch or more. The adhesion may be 350 gf / inch or less. The adhesion may be 330 gf / inch or less. The adhesion may be 300 gf / inch or less. The adhesion may be 280 gf / inch or less. When the polyimide layer has an adhesion within the above ranges, the polyimide layer has an appropriate level of adhesion, which is neither excessive nor insufficient, with the components of the light emitting functional layer, etc., as a support layer, and therefore has excellent properties for use as a substrate for a multilayer electronic device.

[0064] The adhesion force can be measured by a method for testing the adhesion force of a polyimide layer. For example, the adhesion force can be measured through a peeling test using a UTM universal testing machine after forming (curing) a polyimide layer on an amorphous silicon-based glass substrate. Specifically, a part of the polyimide layer is lifted using a tape or the like to perform a 180° peeling test, and the adhesion force can be measured using the UTM universal testing machine. More specific conditions may be those presented in the examples described below (see FIG. 5).

[0065] The polyimide layer 50 has a composite index represented by the following formula 2 of 2° C. 2 / ppm or more.

[0066] [Formula 2] JPEG0007576598000004.jpg1037

[0067] In formula 2, The T Index is a comprehensive index.

[0068] The Tg is the glass transition temperature (° C.).

[0069] The YI is the yellowness value of the polyimide layer at a thickness of 10 μm.

[0070] The H is the thermal expansion coefficient (ppm / ° C.) of the polyimide layer.

[0071] The overall index of the polyimide layer 50 is 2° C. 2 / ppm or more. 2 The polyimide layer 50 may have a composite index of 15° C. / ppm or more. 2 The overall index may be 10° C. / ppm or less. 2 The overall index may be 7° C. / ppm or less. 2 / ppm or less.

[0072] The polyimide layer 50 may have a thermal expansion coefficient (ppm / °C) of 35 or less. The thermal expansion coefficient (ppm / °C) may be 30 or less. The polyimide layer 50 may have a thermal expansion coefficient (ppm / °C) of 27 or less. The thermal expansion coefficient (ppm / °C) may be 25 or less. The polyimide layer 50 may have a thermal expansion coefficient (ppm / °C) of 10 or more. The thermal expansion coefficient (ppm / °C) may be 15 or more. When the polyimide layer 50 has such a thermal expansion coefficient, the change in volume due to high temperature change is small, and therefore the polyimide layer 50 is excellent for application to a substrate of a multilayer electronic device.

[0073] Residual stress can be measured by a method for measuring the residual stress of a polyimide film. Specifically, the residual stress can be measured using Frontier Semiconductor's 500TC (FSM128) equipment. Specifically, a polyimide layer is formed on a 6-inch silicon wafer whose warpage has been measured in advance, and the residual stress is measured by comparing the difference in the warpage. A more specific method is based on the method described in the examples below.

[0074] The polyimide layer 50 may have a residual stress of 25 MPa or less. The residual stress may be 22 MPa or less. The residual stress may be 20 MPa or less. The residual stress may be 18 MPa or less. The residual stress may be 16 MPa or less. The residual stress may be 10 MPa or more. When the polyimide layer 50 has such residual stress characteristics, it is highly usable as a support layer for a multilayer electronic device.

[0075] When stacking a multi-layered device, stress due to physical disharmony may occur at the surface of the polyimide layer and the adjacent interface. This may cause problems such as cracks, displacement, or delamination in the laminate. This may cause serious problems not only in the manufacturing process of multi-layered electronic equipment but also in the reliability of the product itself. Therefore, in order for the polyimide layer to be used as a polyimide film, which is a supporting layer, it must have stable properties even in processes where it is repeatedly exposed to temperatures of 350 to 400°C, and residual stress can be used as one of the criteria for evaluating this. This residual stress is thought to be caused by various factors such as high heat applied in the manufacturing process of the polyimide film (polyimide layer), the difference in thermal expansion coefficient with the supporting substrate, and the rigidity of the polymer chain itself. In the embodiment, the generation of residual stress is reduced while maintaining other properties at a certain level or higher by applying the method described below.

[0076] The polyimide layer 50 may have a thickness of 2 to 100 μm. The thickness may be 2 to 55 μm. The thickness may be more than 2 μm and less than 40 μm.

[0077] The polyimide layer 50 has a uniform thickness overall. Specifically, when the polyimide layer 50 is divided into 40 regions having substantially uniform areas, the thickness of the polyimide layer 50 measured at 40 points, one point in each region, is within a range of −5% to +5% of the average value of the thicknesses measured at the 40 points, demonstrating excellent thickness uniformity.

[0078] The polyimide layer 50 has excellent heat resistance properties.

[0079] The polyimide layer 50 may have a glass transition temperature of 365° C. or more. The glass transition temperature may be 370° C. or more. The glass transition temperature may be 375° C. or more. The polyimide layer 50 may have a glass transition temperature of 390° C. or less. The glass transition temperature is based on a result measured using a DMA measuring device. Exemplarily, the DMA measuring device may be a DMA Q800 model manufactured by Texas Instruments, and a measurement mode may be applied in tension mode. Specifically, a heating rate is set to 3° C. / min, and measurements are made from 25 to 450° C., with a frequency of 1 Hz and an amplitude of 20 μm, to obtain a Tg value.

[0080] The polyimide layer 50 has excellent optical properties.

[0081] The yellow index was measured using a spectrophotometer (Hunter Associates Laboratory's UltraScan PRO) with the CIE color system according to the ASTM E-313 standard.

[0082] The polyimide layer 50 may have a yellowness index of 5.3 or less. The yellowness index may be 4.3 or less. The yellowness index may be 4.1 or less. The polyimide layer 50 may have a yellowness index of more than 1. The yellowness index of the polyimide layer is measured based on a value measured on a film having a thickness of 10 μm.

[0083] The in-plane retardation value is measured at room temperature using the RETS-100 model from OTSUKA Electronics, selecting the Alpha / Theta mode with the Rotate Analyzer Method, and the in-plane retardation Re value at 550 nm is taken as the standard. The in-plane retardation of the polyimide layer is measured using a film with a thickness of 10 μm as the standard.

[0084] The polyimide layer 50 may have an in-plane retardation value (Re) of 3.0 or less. The in-plane retardation value (Re) may be 2.0 or less. The in-plane retardation value (Re) may be 1.5 or less. The in-plane retardation value (Re) may be 1.0 or less. The polyimide layer 50 may have an in-plane retardation value (Re) of 0.1 or more. A polyimide layer having an in-plane retardation value in the above-mentioned range has excellent optical properties suitable for application to a display.

[0085] The polyimide layer 50 may have a light transmittance of 85% or more. The light transmittance may be 88% or more. The light transmittance may be 99% or less. The light transmittance is based on the visible light transmittance measured on a film having a thickness of 10 μm.

[0086] The polyimide layer 50 may have a haze of 1% or less. The haze may be 0.6% or less. The haze may be 0.52% or less. The haze may be 0.45% or less. The polyimide layer 50 may have a haze of 0.001% or more. A polyimide layer having such haze characteristics has optical characteristics that appear clear to the naked eye, and is therefore excellent for use as a base film for displays and the like. The haze is based on a value measured on a film having a thickness of 10 μm.

[0087] The polyimide layer 50 includes a polymer formed by polymerizing an aromatic diamine compound and an aromatic dianhydride compound, that is, the polyimide layer includes an aromatic diamine compound residue and an aromatic dianhydride compound residue.

[0088] The aromatic diamine compound can include 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane (HFBAPP), 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether (BTFDPE), 2,2-bis(4-(4-amino-2-(trifluoromethyl)phenoxy)phenyl)hexafluoropropane (HFFAPP), or 3,5-diaminobenzotrifluoride (DATF).

[0089] Specifically, the aromatic diamine compound may be a compound represented by the following formula 1-1.

[0090] [ka]

[0091] The aromatic dianhydride compound may be two or more, preferably three, selected from the group consisting of 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6-FDA), 4,4'-oxydiphthalic anhydride (ODPA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and combinations thereof.

[0092] Specifically, the aromatic dianhydride compound may be any of the compounds represented by the following chemical formulas 2-1 to 2-3.

[0093] [ka] [ka] [ka]

[0094] The aromatic diamine compound and the aromatic dianhydride compound can be reacted in a molar ratio of 1:0.95 to 1.05 to form a polymer.

[0095] The polyimide layer 50 may contain 5 to 45 moles of biphenyltetracarboxylic acid dianhydride residues of chemical formula 2-3 when the total dianhydride residues are considered to be 100 moles. The polyimide layer 50 may contain 8 to 30 moles of biphenyltetracarboxylic acid dianhydride residues of chemical formula 2-3 when the total dianhydride residues are considered to be 100 moles. A polyimide layer having the compound residues of chemical formula 2-3 in such a range may further improve heat resistance, workability, etc.

[0096] The polyimide layer 50 may contain a biphenyltetracarboxylic acid dianhydride residue and a pyromellitic acid dianhydride residue, and when the sum of the moles of the biphenyltetracarboxylic acid dianhydride residue and the pyromellitic acid dianhydride residue is viewed as a whole, the content of the biphenyltetracarboxylic acid dianhydride residue may be 15 to 50 mol%. The polyimide layer 50 may contain a biphenyltetracarboxylic acid dianhydride residue and a pyromellitic acid dianhydride residue, and when the sum of the moles of the biphenyltetracarboxylic acid dianhydride residue and the pyromellitic acid dianhydride residue is viewed as a whole, the content of the biphenyltetracarboxylic acid dianhydride residue may be 18 to 45 mol%. When the residues are contained in such a range, the viscosity can be controlled so that the workability is good in the manufacturing process, and the heat resistance property and the optical property, which are trade-off properties, can be improved at the same time.

[0097] The polyimide layer 50 may have less than 60 mol% of pyromellitic dianhydride residues when the total amount of the aromatic dianhydride residues is 100 mol. The polyimide layer 50 may have 55 mol% or less of pyromellitic dianhydride residues when the total amount of the aromatic dianhydride residues is 100 mol. When the pyromellitic dianhydride residues are contained within such a content range, viscosity control is relatively advantageous, and a polyimide layer having appropriate workability and further improved heat resistance can be obtained.

[0098] The polyimide layer may contain, based on 100 moles of aromatic diamine compound residues, 25 to 55 moles of residues of Chemical Formula 2-1, 35 to 55 moles of residues of Chemical Formula 2-2, and 5 to 25 moles of residues of Chemical Formula 2-3.

[0099] A polyimide layer containing the above residues in such a molar ratio can have excellent heat resistance and excellent optical properties.

[0100] The polyimide layer 50 may contain a compound having a hydroxyl group. This may be detected as a residual compound applied as a leveling stabilizer in the manufacturing process described below. Such a leveling stabilizer helps to facilitate the formation of a more uniform film in the manufacturing process of the polyimide layer, which may contribute to improving the heat resistance of the film, improving residual stress characteristics, and improving adhesion.

[0101] The leveling stabilizer may be any one selected from the group consisting of methanol, ethanol, butanol, propanol, and combinations thereof, and may be methanol or isopropanol. When the above-mentioned compound is used as the leveling stabilizer, the optical properties and heat resistance properties are maintained, and the effects of more stable film formation, improvement of residual stress, etc. can be obtained.

[0102] The film may further include an adhesive layer 60 on one side of the polyimide layer (see FIG. 2).

[0103] An optical adhesive layer having excellent light transmittance and / or transparency may be applied as the adhesive layer 60. For example, a laminate including an OCA (Optically Clear Adhesive), a PSA (Pressure Sensitive Adhesive), or a combination thereof may be applied.

[0104] The film may further include a release film or a reinforcing film on the other surface of the polyimide layer, and the release film or the reinforcing film may be, but is not limited to, a polyethylene terephthalate (PET) film.

[0105] The film contains the polyimide layer, and thus has excellent heat resistance and optical properties while also serving as a support layer, making it highly usable as a substrate layer. In addition, when the film is used as a substrate layer, not only the upper surface of the light-emitting functional layer corresponding to the front surface of the multi-layer electronic device, but also the substrate layer corresponding to the rear surface of the light-emitting functional layer can be made transparent. As a result, it is possible to provide a film that is highly usable in foldable, flexible, and bendable devices and is reliable in terms of heat resistance, thickness, insulating properties, support properties, etc.

[0106] Multi-layer electronic equipment To achieve the above object, a multi-layer electronic device 800 according to an embodiment of the present invention includes a substrate layer 100 and a light-emitting functional layer 300 disposed on the substrate layer (see FIG. 3). The multi-layer electronic device 800 may further include a cover layer 500 disposed on the light-emitting functional layer 300 (see FIG. 4).

[0107] The substrate layer 100 includes the film described above.

[0108] The multi-layer electronic equipment 800 may be a display device.

[0109] The multi-layer electronic equipment 800 may be, for example, a large-area display device, a foldable display device, a bendable display device, or a flexible display device.

[0110] The multi-layer electronic equipment 800 may be, for example, a bendable mobile communication device (eg, a mobile phone) or a bendable notebook computer.

[0111] The light emitting functional layer 300 includes a coloring layer (not shown) having an element that emits light in response to a signal. Exemplarily, the light emitting functional layer may include a signal transmission layer (not shown) that transmits an external electrical signal to the coloring layer, a coloring layer (not shown) that is disposed on the signal transmission layer and emits color in response to a given signal, and an encapsulation layer (not shown) that protects the coloring layer. The signal transmission layer (not shown) may include a thin film transistor (TFT), and may be, for example, but is not limited to, an LTPS, an a-Si TFT, or an Oxide TFT. The encapsulation layer (not shown) may be, but is not limited to, a TFE (Thin Film Encapsulation).

[0112] The color-emitting layer may be a self-luminous color-emitting layer. For example, the color-emitting layer may be, but is not limited to, quantum dot light-emitting diodes (QLEDs) or organic light-emitting diodes (OLEDs).

[0113] The light-emitting functional layer 300 may include a sensor layer (not shown). For example, a touch sensor or the like may be applied. The sensor layer may be disposed above or below the color-emitting layer.

[0114] The light-emitting functional layer 300 may further include a polarizing layer (not shown). The polarizing layer may be disposed above or below the color-emitting layer.

[0115] The light-emitting functional layer 300 may further include a color filter layer (not shown), which may be disposed above or below the color-emitting layer.

[0116] The light-emitting functional layer 300 may be disposed on the substrate layer 100 .

[0117] A cover layer 500 may be disposed on the light emitting functional layer 300 .

[0118] The cover layer 500 may be a plastic film, glass, or the like that is used as a cover layer of a display device.

[0119] An adhesive layer (not shown) may be further applied between the light emitting functional layer 300 and the cover layer 500 .

[0120] The cover layer 500 may further include an electrode layer (not shown) depending on the type of light emitting element applied to the light emitting functional layer. The electrode layer is disposed on one side of the light emitting functional layer, and an optical adhesive layer may or may not be disposed between the electrode layer and the light emitting functional layer. The electrode layer may be a transparent metal layer, and it is preferable to use a transparent metal layer having a sealing function. The electrode layer may induce driving of the light emitting layer of the light emitting functional layer while transmitting light emitted from the light emitting functional layer. Exemplarily, the electrode layer may be applied as a cathode of the light emitting functional layer. In this way, when the signal transmission layer is provided under the other side of the light emitting layer and the electrode layer is provided on one side of the light emitting layer, the structure is suitable for applying a light emitting functional layer such as an OLED.

[0121] The substrate layer 100 includes the film described above.

[0122] The substrate layer 100 includes a polyimide layer 50 .

[0123] The base layer 100 may include a polyimide layer 50 and an adhesive layer 60 located on the polyimide layer.

[0124] An optical adhesive layer having excellent light transmittance and / or transparency may be applied as the adhesive layer 60. Exemplarily, the adhesive layer may be a laminate including an optically clear adhesive (OCA), a pressure sensitive adhesive (PSA), or a combination thereof.

[0125] The specific description of the film and the polyimide layer overlaps with the above description, so a detailed description will be omitted.

[0126] Optionally, the multi-layer electronic device may further include an additional boundary layer (not shown) below the substrate layer, or may further be coupled to a support means (or drive means) of a rollable or bendable display.

[0127] Optionally, the multi-layer electronic equipment may further comprise drive means (or support means) for an additional rollable or bendable display coupled on the cover layer.

[0128] The driving means or supporting means can be applied without any restrictions as long as it is applied to a general rollable or bendable display.

[0129] The multi-layer electronic device 800 may have a light transmittance of 85% or more. The light transmittance may be 90% or more. The light transmittance may be 99% or less. The light transmittance may be measured in a manner similar to that of a polyimide layer.

[0130] Film manufacturing method A method for producing a film according to an embodiment includes the steps of: preparing a polymer solution; preparing a sheet; and preparing a film.

[0131] The step of preparing a polymer solution is a step of preparing a polymer solution by stirring a raw material composition including a diamine and a dianhydride. The step of preparing a polymer solution may include a reaction process and an aging process.

[0132] The diamine may be an aromatic diamine compound.

[0133] The diamine may include one or more aromatic diamine compounds.

[0134] The dianhydride may be an aromatic dianhydride compound.

[0135] The dianhydride can include three or more aromatic dianhydride compounds.

[0136] The raw material composition applied to the production of the polymer solution may contain the aromatic diamine compound and the aromatic dianhydride compound in a molar ratio of 1:0.95 to 1.05.

[0137] The raw material composition may contain the biphenyltetracarboxylic acid dianhydride compound of the chemical formula 2-3 in a molar ratio of 5 to 45 moles when the total dianhydride compound is considered as 100 moles. The raw material composition may contain the biphenyltetracarboxylic acid dianhydride compound of the chemical formula 2-3 in a molar ratio of 8 to 30 moles when the total dianhydride compound is considered as 100 moles. When a polyimide layer having the compound of the chemical formula 2-3 in such a range is produced, the heat resistance, workability, etc. of the polyimide layer can be further improved.

[0138] The raw material composition includes a biphenyltetracarboxylic acid dianhydride compound and a pyromellitic acid dianhydride compound. The raw material composition may have a biphenyltetracarboxylic acid dianhydride compound content of 15 to 50 mol% when the sum of the moles of the biphenyltetracarboxylic acid dianhydride compound and the pyromellitic acid dianhydride compound is viewed as a whole. The raw material composition may have a biphenyltetracarboxylic acid dianhydride compound content of 18 to 45 mol% when the sum of the moles of the biphenyltetracarboxylic acid dianhydride compound and the pyromellitic acid dianhydride compound is viewed as a whole. When the compound is contained in such a range, the viscosity can be controlled so that the workability is improved in the manufacturing process, and the heat resistance and optical properties, which are trade-off characteristics, can be improved at the same time.

[0139] The raw material composition may contain less than 60 mol% of the pyromellitic dianhydride compound when the total amount of the aromatic dianhydride compound is 100 mol. The raw material composition may contain 55 mol% or less of the pyromellitic dianhydride compound when the total amount of the aromatic dianhydride compound is 100 mol. When the raw material composition contains the pyromellitic dianhydride compound in such a content range, it is relatively advantageous to control the viscosity of the raw material composition, and therefore, a polyimide layer having suitable workability and further improved heat resistance can be obtained.

[0140] The raw material composition may contain, based on 100 moles of an aromatic diamine compound, 25 to 55 moles of the compound of the chemical formula 2-1, 35 to 55 moles of the compound of the chemical formula 2-2, and 5 to 25 moles of the compound of the chemical formula 2-3.

[0141] The molar ratio is based on the solids content.

[0142] The reaction process is a process in which the raw material composition is stirred in an organic solvent to induce an imidization reaction, and the product of the reaction process is referred to as a reaction solution for convenience.

[0143] The solid content of the raw material composition in the organic solvent may be 10 to 40 wt %. The content may be 15 to 30 wt %. The content may be 18 to 25 wt %. When the raw material composition has such a solid content, the workability is further excellent.

[0144] The stirring of the raw material composition can be divided into a primary stirring, a secondary stirring, and a tertiary stirring.

[0145] The primary stirring is a step of inducing a reaction between an aromatic diamine compound containing a halogen element in its molecule (e.g., the compound of Chemical Formula 1) and an aromatic dianhydride compound containing a halogen element in its molecule (e.g., the compound of Chemical Formula 2-1) in an organic solvent while stirring them.

[0146] The aromatic diamine compound may be dissolved in an organic solvent (eg, N-Methyl-2-Pyrrolidone, NMP) in an inert atmosphere at 20 to 45° C. before use.

[0147] The aromatic dianhydride compound may be added to the aromatic diamine compound and then first stirred, and the reaction may be carried out at a reaction temperature of 5 to 15° C. for a reaction time of 1 to 7 hours.

[0148] The second stirring is a step of inducing a reaction by stirring the reaction product of the first stirring with an aromatic dianhydride compound (e.g., the compound of Formula 2-3) having no halogen element in the molecule. The second stirring may be performed at a reaction temperature of 30 to 70° C. for a reaction time of 30 minutes to 10 hours.

[0149] The tertiary stirring is a step of inducing a reaction by stirring the reaction product of the secondary stirring with an aromatic dianhydride compound (e.g., compound of formula 2-2) having no halogen element in its molecule. The secondary stirring may be performed at a reaction temperature of 30 to 70° C. for a reaction time of 30 minutes to 10 hours.

[0150] Through this process, a reaction solution can be prepared.

[0151] The reaction solution is subjected to viscosity measurement, and a polymer solution having a viscosity measured at 25° C. of 1,000 to 8,000 cps can be produced.

[0152] The polymer solution may further include a leveling stabilizer.

[0153] The role and type of the leveling stabilizer are as described above.

[0154] The leveling stabilizer may be applied in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the polymer solution. The leveling stabilizer may be applied in an amount of 0.1 to 3 parts by weight. The leveling stabilizer may be applied in an amount of 0.2 to 2 parts by weight.

[0155] The aging process is a process in which the reaction solution is formed into a polymer solution having a certain viscosity and the leveling stabilizer is sufficiently dispersed. The aging process may be a process of stirring at 10 to 35° C. for 2 to 6 hours.

[0156] The completion of the preparation of the polymer solution can be confirmed by measuring the viscosity of the polymer solution. The polymer solution is a precursor of the polyimide layer, and should be easy to coat, suitable for forming a layer of a certain thickness, and should also have excellent optical properties. Therefore, in consideration of workability and physical properties, it is preferable to induce the reaction so that the polymer solution has a viscosity of 1,000 to 8,000 cps based on the value measured at 25°C. It is preferable to prepare a polymer solution having a viscosity of 2,000 cps or more and less than 5,000 cps. It is more preferable that the viscosity is less than 3,000 cps to 4,500 cps. If the viscosity is too low, such as less than 1,000 cps, it may be difficult to prepare a polyimide layer of a certain thickness or an intended thickness, and the heat resistance may be insufficient. If the viscosity exceeds 8,000 cps, gelation may occur, and removal of the film may be substantially difficult.

[0157] If necessary, the polymer solution may contain additional additives, process stabilizers, etc. The additives, process stabilizers, etc. may be used without limitation as long as they are applicable to the polymerization of polyimide.

[0158] The sheet production step is a step of applying the polymer solution to a sheet and then drying the applied solution to produce a dry sheet.

[0159] The polymer solution is applied to a substrate such as a glass plate, and dried at a drying temperature and for a drying time. The drying temperature may be, for example, 100 to 180° C., and the drying time may be 3 to 60 minutes. The drying may be performed in an inert atmosphere or in a vacuum oven to control the optical properties of the polyimide layer.

[0160] The film production step is a step of producing a polyimide film by heat treating the sheet.

[0161] The heat treatment can be carried out by applying a heat treatment temperature and a heat treatment temperature rise rate.

[0162] The heat treatment temperature may be 150 to 450° C. The heat treatment temperature may be 300 to 430° C. The heat treatment temperature may be 360 ​​to 400° C. The temperature rise rate to the heat treatment temperature may be 3 to 25° C. / min. The temperature rise rate may be 10 to 20° C. / min. The temperature rise rate may be 13 to 17° C. / min. When such heat treatment temperatures and temperature rise rates are applied, the degree of polymerization and the like may be controlled so that the produced film has intended physical properties, and the heat treatment can proceed more stably.

[0163] The heat treatment can be advantageously carried out not only in an inert atmosphere but also in an air atmosphere, and the embodiment has the characteristic that the optical properties are excellent even when the heat treatment is carried out in an air atmosphere, thereby further improving the process workability.

[0164] The film produced by the above-mentioned production method includes the polyimide film described above. The polyimide film has the same characteristics as the polyimide layer contained in the above-mentioned film.

[0165] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative for the purpose of aiding understanding of the present invention, and are not intended to limit the scope of the present invention.

[0166] Example: Preparation of polyimide layers Example 1 In a temperature-controllable double-jacketed 1L glass reactor, 458g of NMP (N-Methyl-2-Pyrrolidone) organic solvent was added under a nitrogen atmosphere at 40℃, and then 0.170mol (100mol parts) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFDB) aromatic diamine was gradually added and dissolved. Next, 0.051mol (30mol parts) of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA) was gradually added and stirred at 10℃ for 3 hours (primary stirring).

[0167] 0.034 mol (20 mol parts) of 3,3',4,4'-biphenyltetracarboxylic anhydride (BPDA) was added to the first stirred solution and stirred at 50° C. for 4 hours to prepare a second stirred solution.

[0168] 0.085 mol (50 mol parts) of PMDA (pyromellitic dianhydride) was added to the second stirred solution and stirred at 50° C. for 4 hours to prepare a third stirred solution.

[0169] Based on 100 parts by weight of the third stirred solution, 2 parts by weight of isopropanol was added as a leveling stabilizer, and the mixture was further stirred for 4 hours.

[0170] After the viscosity measurement, additives and process stabilizers were further added and stirred for 4 hours to obtain a polymer solution. The polymer solution was applied to a glass plate and then dried in a vacuum oven at 150°C for 10 minutes. Then, a heat treatment was performed. Specifically, the temperature was raised from 150°C to 400°C at a rate of 15°C / min to harden the solution, and finally a polyimide film having a thickness of 10 μm was obtained, which was used as the polyimide layer of Example 1.

[0171] (Examples 2 and 3 and Comparative Examples 1 to 4) Polyimide layers of Examples 2 and 3 and Comparative Example 1 were prepared by the same method as above, but with different molar ratios of monomers as shown in Table 1 below.

[0172] In the case of Comparative Examples 2 to 4, the molar ratios of the monomers in Table 1 below were the same, but the heat treatment temperature was increased to 350°C in Comparative Example 3 and cured, and increased to 500°C in Comparative Example 4.

[0173] [Table 1] TFMB: 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl 6FDA: 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride PMDA: Pyromellitic dianhydride BPDA: 2,3,3',4'-biphenyltetracarboxylic acid dianhydride *Displayed up to two decimal places. **The film removal evaluation was performed by evaluating the process for producing a polyimide layer from a polymer solution using the same method, with a rating of ◯ indicating that a film-like polyimide layer could be produced, and a rating of △ indicating that the viscosity was too low and therefore workability was reduced.

[0174] In the cases of Examples 1 to 3 and Comparative Example 2, the viscosity measured at room temperature (about 25°C) was about 5000 CPS to about 5500 CPS, and workability was good. In the case of Comparative Example 1, the viscosity# measured at room temperature (about 25°C) was about 2000 CPS, which was excessively low, and in the case of Comparative Example 3, the viscosity was about 1500 CPS, and workability was poor.

[0175] #Viscosity was measured by maintaining the temperature of the polymer solution (Varnish) at 25°C and using a Toki Sangyo BH-II model viscometer. The RPM was set at 4, and spindle number 4 was used to confirm whether the target viscosity was achieved.

[0176] In the following, the physical properties of the samples of Examples 1 to 3 and Comparative Examples 1 to 3 were measured.

[0177] Example: Evaluation of the physical properties of the polyimide layer (polyimide film) A (1) The thickness was measured using a Mitutoyo Digital Micrometer 547547-401 at five randomly positioned points, and the average thickness was calculated.

[0178] (2) Transmittance and haze: Light transmittance (%) and haze (%) were measured using a haze meter NDH-5000W manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with the JIS K 7105 standard.

[0179] (3) Yellowness index (YI) was measured using the CIE color system of a spectrophotometer (Hunter Associates Laboratory's UltraScan PRO). YI was calculated according to the ASTM E-313 standard.

[0180] (4) CTE (Coefficient of Thermal Expansion) was measured using a thermal expansion coefficient measuring instrument, specifically, Seiko Exstar 6000 (TMA6100) model from Seico Inst. (Japan). The measurement method is as follows, and the change in the range of 50 to 250 based on the 2nd Heat was defined as the CTE value. -1st Heating:30℃ start→360℃ heating(10℃ / min↑)→30℃ -2nd Heating:30℃→360℃ heating(5℃ / min↑)

[0181] (5) The glass transition temperature (Tg) was measured using a Texas Instruments DMA Q800 model in tension mode. The temperature was increased at a rate of 3°C / min from 25°C to 450°C, with a frequency of 1Hz and an amplitude of 20μm, and the Tg value at tangent delta was obtained.

[0182] (6) Adhesion force was measured by curing a polyimide layer on an amorphous silicon-based glass substrate, applying the LLO (laser lift off) process to separate a part of the polyimide film from the glass substrate, fixing a tape (T in Figure 5) to the separated polyimide film, and removing the polyimide layer using a UTM universal testing machine. The measurement mode was a 180° peeling test (see Figure 5), and the results were expressed in gf / inch. Specifically, the pre-test and test speeds were 0.83 mm / sec, the post-test speed was 10 mm / sec, the distance from the pre-test to the target mode was 10 mm, and the trigger force was 0.001 N.

[0183] (7) Residual stress was measured using Frontier Semiconductor's 500TC (FSM128) equipment. PI Vanish was applied to a 6-inch silicon wafer, the "warpage" of which had been measured in advance, using a coater, and the wafer was pre-baked at 80°C for 30 minutes. The oxygen concentration in the oven was then adjusted to 10 mass ppm using a high-temperature oven (Koyo Lindberg, model VF-2000B), and heat curing was performed at 350°C for 60 minutes to produce a silicon wafer with a 15 μm-thick polyimide resin film. Residual stress was measured by comparing the degree of warpage caused by the difference in thermal expansion between the silicon wafer and the PI film.

[0184] (8) Loop stiffness was measured using a loop stiffness tester (TOYOSEIKI). Both ends of a polyimide film with a width of 15 mm, length of 120 mm, and thickness of 50 μm were fixed to the fixing parts of the device, and the polyimide film was pressed at a pressing speed of 3.3 mm / s using the pressing part until the final separation distance between the pressing part and the fixing part (L in Figure 6) became 20 mm. The loop stiffness of the polyimide film was then measured using a sensor. The measurement was performed at room temperature with the machine direction of the film as the longitudinal direction.

[0185] The results of the above measurements are shown in Table 2 below.

[0186] [Table 2] *The heat stability index is a value evaluated by Equation 1 above. *The overall index is the value evaluated by Equation 2 above.

[0187] Referring to Tables 1 and 2, it was confirmed that in the case of Examples 1 to 3, the loop stiffness was within an appropriate level range, and that the film had an appropriate recovery force when folded together with flexibility, and was therefore suitable for application as a support layer for foldable or rollable displays, etc. In addition, it was confirmed that the film had a relatively low thermal expansion coefficient, small residual stress, etc., and that, in combination with the optical properties and heat resistance, the film had excellent optical properties such as yellowness, and properties related to processability and reliability required for use as a support, such as adhesion and residual stress.

[0188] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention.

[0189] [Acknowledgements] This invention was made with the support of the Korea Institute for Industrial Technology Assessment and Management's Material and Parts Technology Development Project (package type, project number 20007228). [Explanation of symbols]

[0190] 100 Base material layer 300 Light-emitting functional layer 500 Cover Layer 800 Multi-layer electronic equipment 50 Polyimide layer 60 Adhesive layer G Amorphous Si-based glass plate T-Tape LS-T1 fixed part LS-T2 pressure unit

Claims

1. A polyimide layer containing an aromatic diamine compound residue and an aromatic dianhydride compound residue, The polyimide layer has a loop stiffness value of 3 to 4.5 m / N based on a thickness of 50 μm; The polyimide layer has a yellowness index of 5.3 or less, the polyimide layer contains biphenyltetracarboxylic acid dianhydride residues and pyromellitic acid dianhydride residues; the content of the biphenyltetracarboxylic acid dianhydride residue is 15 to 50 mol % when the sum of the moles of the biphenyltetracarboxylic acid dianhydride residue and the pyromellitic acid dianhydride residue is considered as a whole.

2. The polyimide layer has a heat stability index (HS index) of 5 to 15° C. according to the following formula 1: 2 The film of claim 1, wherein the viscosity is 1 / ppm·MPa. [Formula 1] In Formula 1, The HS index is the heat stability index (°C 2 / ppm·MPa), Tg is the glass transition temperature (° C.); H is the thermal expansion coefficient (ppm / °C) of the polyimide layer, The RS is the value of the residual stress (MPa) of the polyimide layer.

3. The film of claim 1 , wherein the polyimide layer has an adhesion of 200 gf / inch or more.

4. The polyimide layer has a composite index represented by the following formula 2 of 2° C. 2 2. The film of claim 1, wherein the film has a water content of 100 ppm or more. [Formula 2] In formula 2, The T Index is a comprehensive index; Tg is the glass transition temperature (° C.); YI is the yellowness index value of the polyimide layer at a thickness of 10 μm, The H is the thermal expansion coefficient (ppm / ° C.) of the polyimide layer.

5. 2. The film according to claim 1, wherein the polyimide layer contains 5 to 45 moles of biphenyltetracarboxylic acid dianhydride residues when the entire amount of the aromatic dianhydride compound residues is considered to be 100 moles.

6. The film described in claim 1, wherein the pyromellitic dianhydride residues are less than 60 mol% when the total amount of the aromatic dianhydride compound residues is 100 mol.

7. A base layer; a light-emitting functional layer disposed on the base layer, The substrate layer includes a film, A multi-layer electronic device, wherein the film is the film of claim 1.

8. a polymer solution producing step of producing a polymer solution having a viscosity of 1,000 to 8,000 cps measured at 25° C. by stirring a raw material composition including an aromatic diamine compound and an aromatic dianhydride compound; a sheet production step of applying the polymer solution to a sheet and then drying the sheet with hot air; and a film production step of producing a polyimide layer by heat-treating the sheet at 360 to 480° C., The raw material composition or the polymer solution further contains a leveling stabilizer, the film comprises the polyimide layer; The polyimide layer has a yellowness index of 5.3 or less, the polyimide layer contains the aromatic diamine compound residue and the aromatic dianhydride compound residue, and the polyimide layer has a loop stiffness value of 3 to 4.5 m / N based on a thickness of 50 μm.

Citation Information

Patent Citations

  • Polyimide film

    JP2012503701A

  • Polyimide precursor and polyimide

    JP2018172562A

  • Polyimide film, metal-clad laminate, and circuit board

    JP2019065180A

  • Polyimide precursor resin composition having improved resin stability and heat resistance and transparency, method for producing polyimide film using the same, and polyimide film produced by the same

    JP2019528368A

  • Polyimide film

    JP2020139039A