Manufacturing method of filler granules
The production of filler granules with a polymer and dispersant mixture addresses issues of concentration, dispersibility, and productivity, resulting in improved thermoplastic resin compositions with enhanced performance and safety.
Patent Information
- Application Number
- JP2023174273
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-06
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-09-11
AI Technical Summary
Existing thermoplastic resin compositions face challenges with high filler concentration, productivity, versatility of fillers, and dispersibility, necessitating improvements in filler granules for better performance and environmental safety.
The production of filler granules involves a mixture of a polymer, filler, and a dispersant, including polyhydric alcohol fatty acid ester, fatty acid amide, polyglycerol fatty acid ester, and alcohol ester of condensed hydroxy fatty acid, with a high filler content and a semi-wet granulation method using a disk pelleter to create cylindrical granules with improved dispersibility.
The resulting filler granules offer high filler concentration, enhanced dispersibility, and improved productivity, reducing environmental pollution and equipment downtime while maintaining mechanical performance and moldability, thus enhancing the quality and efficiency of thermoplastic resin compositions.
Smart Images

Figure 0007576675000001 
Figure 0007576675000002 
Figure 0007576675000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a filler granule. [Background technology]
[0002] In recent years, high functionality and high performance are required for thermoplastic resin compositions, and therefore, fillers are often mixed and provided. Thermoplastic resin compositions containing fillers (hereinafter also referred to as "filler-containing resin compositions") are usually produced by melt-kneading a filler and a thermoplastic resin, but in recent years, the use of filler granules of a predetermined concentration (e.g., 50 to 80% by weight of filler) has been proposed (e.g., Patent Documents 1 to 4). In the production of filler-containing resin compositions, the use of filler granules is expected to be advantageous in terms of cost, safety and health, working environment, material management, etc. However, the filler granules are still insufficient in terms of high filler concentration, productivity of the filler granules, versatility of the applied filler, dispersibility of the filler in the thermoplastic resin composition, etc., and improvements in these properties are required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-70856 A [Patent Document 2] International Publication No. 2017 / 147465 [Patent Document 3] Patent No. 6482755 [Patent Document 4] JP 2014-101423 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above problems, and an object of the present invention is to provide a filler granule that is excellent in terms of a high filler concentration in the filler granule, productivity of the filler granule, versatility of applicable fillers, dispersibility of the filler in a thermoplastic resin composition, etc. [Means for solving the problem]
[0005] The filler granule of the present invention contains a polymer, a filler, and a dispersant, the dispersant being at least one selected from the group consisting of polyhydric alcohol fatty acid esters, fatty acid amides, polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids, and the content of the filler is 80 parts by weight to 99.9 parts by weight per 100 parts by weight of the total amount of the polymer and the filler. In one embodiment, the content of the filler is 90 parts by weight to 99.9 parts by weight with respect to 100 parts by weight of the total amount of the polymer and the filler. In one embodiment, the content of the dispersant is 0.1 parts by weight to 15 parts by weight with respect to 100 parts by weight of the total amount of the polymer and the filler. In one embodiment, the dispersant is at least one selected from the group consisting of polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids. In one embodiment, the polymer is a polyolefin resin. According to another aspect of the present invention, there is provided a method for producing a filler granule, comprising a mixing step of mixing a polymer liquid, a filler, and a dispersant, a granulation step of granulating the mixture obtained through the mixing step to obtain a granule precursor, and a drying step of drying the granule precursor. In one embodiment, the granulation step includes granulation by a semi-wet granulation method. In one embodiment, the granulation step includes carrying out granulation by a disk pelleter method. Effect of the Invention
[0006] According to the present invention, it is possible to provide a filler granule that is excellent in terms of a high concentration of the filler in the filler granule, productivity of the filler granule, versatility of the applicable filler, dispersibility of the filler in a thermoplastic resin composition, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] A. Overview of filler granulation materials The filler granule of the present invention contains a polymer, a filler, and a dispersant. The dispersant is at least one selected from the group consisting of polyhydric alcohol fatty acid esters, fatty acid amides, polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids. The content of the filler is preferably 80 to 99.9 parts by weight based on 100 parts by weight of the total amount of the polymer and the filler.
[0008] The filler granules of the present invention are used in the production of a filler-containing resin composition, and can be added during melt-kneading of the resin composition.
[0009] In one embodiment, the filler granules can be obtained by processing a mixture containing a polymer liquid (polymer solution or polymer dispersion) containing the polymer, the filler, and the dispersant by any suitable method.
[0010] In the present invention, by producing a filler granule by adding the above-mentioned dispersant, a high concentration (80% by weight or more) of filler can be added to the filler granule. Moreover, the filler granule of the present invention can be produced with excellent production efficiency even though it contains a large amount of filler, and has excellent quality stability (shape stability, uniformity of pellet hardness, low fine powder mixing). In addition, by preparing the filler-containing resin composition using the above-mentioned filler granule, the productivity of the resin composition can be improved. Specifically, since the above-mentioned filler granule has a remarkably excellent stability in feeding into an apparatus such as an extruder, the productivity (compound processing speed per hour) of the filler-containing resin composition can be dramatically improved by using the filler granule. In addition, the working environment pollution due to dust can be significantly improved, the occupational safety and health environment of the workers can be improved, and the time required for cleaning the equipment to be changed over can be significantly reduced. Furthermore, although the filler granules of the present invention contain a high concentration of filler, the filler-containing resin composition obtained using the filler granules has excellent filler dispersibility. In addition, since the filler granules of the present invention have the effect of increasing molding processability (high fluidity), the load on the extruder can be reduced even while containing a high concentration of filler, and melt kneading with suppressed thermal deterioration of the resin by suppressing excessive heat generation of the resin can be performed, and the obtained filler-containing resin composition can be given excellent mechanical properties and molding processability. By using the filler granules of the present invention that have such effects, not only can the production of a filler-containing resin composition be reduced in cost, but also high performance can be achieved.
[0011] In one embodiment, the filler granules are produced by a semi-wet granulation method. The semi-wet granulation method makes the above-mentioned effects more pronounced.
[0012] The filler granules may have any suitable shape. Typically, the filler granules are cylindrical (pellet-shaped).
[0013] When the filler granules are cylindrical, the diameter of the filler granules is, for example, 2 mm to 5 mm. The length (height) of the filler granules is, for example, 1 mm to 5 mm. With such a shape, a filler granule that can be preferably combined with a resin (particularly a thermoplastic resin) can be obtained. The diameter of the filler granules can be adjusted by the diameter of the die hole of the disk plate during granulation, and the length can be adjusted by the distance between the disk plate and the cutter. By adjusting the filler granules to the pellet size of the resin (particularly a thermoplastic resin) to be combined, the handling property is improved, and the dispersibility of the filler in the molten compound is improved.
[0014] The breaking stress of the filler granules measured with a Kiya hardness tester is preferably 0.05 kg to 10 kg, more preferably 0.5 kg to 7 kg, and further preferably 1.0 kg to 5 kg. Within such ranges, the handling property and the filler dispersibility are excellent. Here, the breaking stress refers to the average disintegration stress measured for 20 or more particles.
[0015] The water content of the filler granules may be any suitable water content, and is preferably 10% by weight or less, more preferably 5% by weight or less, even more preferably 3% by weight or less, particularly preferably 1% by weight or less, and most preferably 0.5% by weight or less.
[0016] The bulk density of the filler granules may be any appropriate bulk density depending on the type of filler. When the filler is a mineral (natural mineral), the bulk density of the filler granules is preferably 0.5 g / cm 3 ~2.0g / cm 3 By increasing the bulk density, the supply speed and supply stability of the filler granules are increased when melt-kneading with a resin (particularly a thermoplastic resin).
[0017] A-1. Polymer The filler granules are granulated using a polymer as a binder.
[0018] Any suitable polymer can be used as the polymer. Specific examples of the polymer include high density polyethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), polyolefin elastomer (POE), functional polyolefin copolymer including polyolefin-based ionomer, polypropylene (PP), polyolefin copolymer (e.g., ethylene-butene, ethylene-octene, ethylene vinyl alcohol, etc.), polystyrene, polystyrene copolymer (e.g., high impact polystyrene, acrylonitrile-butadiene-styrene copolymer), polyacrylate, polymethacrylate, polyester, polyvinyl chloride (PVC), fluoropolymer, polyamide, polyetherimide, polyphenylene sulfide, polysulfone, polyacetal, polycarbonate, polyphenylene oxide, polyurethane, thermoplastic elastomer (e.g., SIS, SEBS, SEPS, SBS), etc. These polymers may be used alone or in combination of two or more.
[0019] In one embodiment, a polyolefin resin is used as the polymer. By using a polyolefin resin, a filler granule containing a large amount of filler with good dispersibility can be obtained. Polyolefins usually have a melting point in the range of 50 to 150°C, and in the semi-wet granulation method, they are particularly preferred because they become molten or semi-molten due to shear heat generated when passing through a die hole during granulation, allowing the polymer to permeate the filler particles and increase the binding property of the filler granule.
[0020] Commercially available products may be used as the polymer. Examples of commercially available products include Chemipearl (registered trademark) manufactured by Mitsui Chemicals, HYPOD (registered trademark) manufactured by Dow Chemical Company, AQUACER (registered trademark) manufactured by BYK Japan, ZAIKXEN (registered trademark) manufactured by Sumitomo Seika Chemicals, and Michem (registered trademark) manufactured by Michaelman Japan. Other preferred examples include ethylene-vinyl alcohol copolymer (EVOH; EVAL (registered trademark) manufactured by Kuraray Co., Ltd.), butenediol-vinyl alcohol copolymer (BVOH; Nichigo G-Polymer (registered trademark) manufactured by Mitsubishi Chemical Co., Ltd.). Other preferred examples include aqueous sulfopolyester dispersions sold under the name Eastman AQ (registered trademark) manufactured by Eastman Chemical Co., and salts of hexane-1,6-diamine and adipic acid (AH salts) sold by Ascend Performance, which are diluted with water to form aqueous polymer dispersions.
[0021] The content ratio of the polymer in the filler granules can be any appropriate ratio depending on the size, shape, water absorption, oil absorption, bulk specific gravity, etc. of the filler. The content ratio of the polymer in the filler granules is preferably 0.1 to 20 parts by weight, preferably 0.5 to 18 parts by weight, more preferably 1 to 18 parts by weight, and even more preferably 3 to 15 parts by weight, relative to 100 parts by weight of the total amount of the polymer and the filler. Within such a range, a filler granule can be obtained that exhibits a favorable binding force as a binder and has excellent dispersibility of the filler.
[0022] As described above, the filler granules can be obtained from a mixture containing a polymer liquid (polymer solution or polymer dispersion) containing the polymer, the filler, and the dispersant. If a liquid polymer dispersion is used, the viscosity of the mixture can be reduced when granulating the filler granules, making it possible to easily granulate the filler. Furthermore, since the polymer liquid can efficiently and uniformly coat the filler surface, a filler granule with little powder falling, high disintegration hardness, and high bulk density can be obtained. Furthermore, when blended with a thermoplastic resin, the dispersibility of the filler can be greatly improved. The details of the polymer liquid will be described later.
[0023] A-2. Filler As described above, the content of the filler is 80 parts by weight to 99.9 parts by weight relative to 100 parts by weight of the total amount of the polymer and the filler. The content of the filler is preferably 82 parts by weight to 99 parts by weight, more preferably 85 parts by weight to 98 parts by weight, even more preferably 87 parts by weight to 97 parts by weight, and even more preferably 90 parts by weight to 96 parts by weight relative to 100 parts by weight of the total amount of the polymer and the filler. In one embodiment, the content of the filler is 90 parts by weight to 99.9 parts by weight relative to 100 parts by weight of the filler granules.
[0024] The volume content of the filler in the filler granules is preferably 40% by volume to 95% by volume, more preferably 50% by volume to 90% by volume, and further preferably 60% by volume to 85% by volume.
[0025] As the filler, any appropriate filler can be used depending on the properties required for the filler-containing resin composition and / or the molded article obtained from the filler-containing resin composition.
[0026] Examples of properties and effects that can be imparted by the above-mentioned fillers include weight increase or weight reduction, reinforcement (increased rigidity, increased elastic modulus, increased strength), dimensional stability, molding cycle (crystallization rate), degree of crystallinity, thermal conductivity, electrical conductivity, magnetism, piezoelectricity, vibration damping, sound insulation, sliding properties, heat insulation, electromagnetic wave absorption, light reflectivity, light scattering, heat radiation, flame retardancy, radiation protection, ultraviolet protection, moisture removal, dehydration, deodorization, gas absorption, gas barrier, anti-blocking, oil absorption, antibacterial properties, promotion of biodegradation, improved bio content (increased ratio of components derived from natural products), and the like.
[0027] For example, calcium carbonate, talc, silica, and clay are suitable for increasing the weight. For reinforcing purposes, wollastonite, potassium titanate, xonotlite, gypsum fiber, aluminum borate, fibrous magnesium compound (MOS), aramid fiber, various fiber systems, carbon fiber, glass fiber, talc, mica, glass flakes, polyoxybenzoyl whiskers, and the like are suitable. For providing antibacterial properties, catechin, silver ion-supported zeolite, copper phthalocyanine, and the like are suitable. For providing gas barrier properties, synthetic mica systems, clay / synthetic mica nanofillers, and the like are suitable. For reducing weight, balloon systems such as silica balloons, glass balloons, cenospheres, perlite, and shirasu balloons are suitable. For providing electrical conductivity, carbon black, graphite, carbon fiber, metal powder, metal fiber, and metal foil are suitable. For the purpose of imparting magnetism, various magnetic materials, various ferrites, magnetic iron oxide, samacobalt (Sm-Co), Nd-Fe-B, etc. are suitable. For the purpose of imparting thermal conductivity, alumina, AlN, BN, BeO, etc. are suitable. For the purpose of imparting piezoelectricity, barium titanate, lead zirconate titanate (PZT), etc. are suitable. For the purpose of imparting vibration damping properties, mica, graphite, potassium titanate, xonotlite, carbon fiber, ferrite, etc. are suitable. For the purpose of imparting sound insulation properties, iron powder, lead powder, barium sulfate, etc. are suitable. For the purpose of imparting sliding properties, graphite, hexagonal BN, molybdenum sulfide, Teflon (registered trademark) powder, talc, high molecular weight polyethylene, etc. are suitable. For the purpose of imparting electromagnetic wave absorption, electromagnetic wave absorbing ferrite, graphite, charcoal powder, carbon microcoil (CMC), carbon nanotube (CNT), PZT, etc. are suitable. For the purpose of imparting light reflection and light scattering, titanium oxide, glass beads, calcium carbonate, aluminum powder, mica, etc. are suitable. For the purpose of imparting heat radiation, magnesium oxide, hydrotalcite, MOS, alumina, charcoal powder, etc. are suitable. For the purpose of flame retardancy, antimony oxide, aluminum hydroxide, magnesium hydroxide, zinc borate, red phosphorus, zinc carbonate, hydrotalcite, dawsonite, bromine-based flame retardants, phosphorus-based flame retardants, etc. are suitable. For the purpose of radiation protection, lead powder, barium sulfate, etc. are suitable.For the purpose of "ultraviolet protection", titanium oxide, zinc oxide, iron oxide, etc. are suitable. For the purpose of dehumidification and dehydration, calcium oxide, magnesium oxide, etc. are suitable. For the purpose of deodorization and gas absorption, zeolite, activated clay, etc. are suitable. For the purpose of anti-blocking (prevention of film pressure adhesion), silica, calcium carbonate, talc, spherical microparticles (silicone or acrylic beads), etc. are suitable. For the purpose of oil absorption (printing ink absorption, quick drying, etc.), algae-shaped calcium carbonate, algae-shaped xonotlite, etc. are suitable. For the purpose of water absorption, water-absorbing polymer gel, calcium oxide, magnesium oxide, etc. are suitable. For the purpose of increasing the bio content, cellulosic materials (wood flour, wood fiber, sawdust, wood chips, newsprint, paper, flax, hemp, wheat straw, rice husks, kenaf, jute, sisal, peanut shells, soybean hulls, etc.), starch, natural rubber, etc. are suitable.
[0028] The size of the filler can be any appropriate size, and the particle size of the filler is, for example, 10 nm to 100 μm.
[0029] The blending ratio of the polymer and the filler can be any suitable blending ratio. In general, the smaller the particle size of the filler, the more preferable the blending ratio of the polymer, the lower the shape symmetry of the filler (for example, scale-like or needle-like), the more preferable the blending ratio of the polymer, and the broader the filler particle size distribution, the more preferable the blending ratio of the polymer. This is because it becomes possible to preferably cover the filler surface with the polymer. In addition, in mixing the polymer and the filler, a strong mechanical stress is applied within a range in which the filler particles do not collapse, and distributive mixing is performed for a long time, thereby increasing the uniformity of the mixture and improving the granulation characteristics.
[0030] A-3. Dispersants As described above, the dispersant is at least one selected from the group consisting of polyhydric alcohol fatty acid ester, fatty acid amide, polyglycerin fatty acid ester, condensed hydroxy fatty acid, and alcohol ester of condensed hydroxy fatty acid. Among them, at least one selected from the group consisting of polyglycerin fatty acid ester, condensed hydroxy fatty acid, and alcohol ester of condensed hydroxy fatty acid is particularly preferably used.
[0031] The dispersant is a compound composed of a hydrophobic group and a hydrophilic group. The hydrophilic / hydrophobic balance can be controlled by adjusting the degree of esterification of the dispersant compound, the type of fatty acid (presence or absence of a hydroxyl group, saturated or unsaturated fatty acid, alkyl chain length), and the degree of polymerization. The hydrophilic / hydrophobic balance can be any appropriate balance depending on the type of the filler, the type of resin to be combined with the filler granule, and the like.
[0032] The polyhydric alcohol fatty acid ester is an ester compound composed of a polyhydric alcohol and a fatty acid, and can be obtained by esterification of the polyhydric alcohol and a fatty acid.
[0033] Examples of the polyhydric alcohol include alkane polyols such as pentaerythritol and glycerin; polyalkane polyols which are polymers of the alkane polyols; sugars such as sucrose; and sugar derivatives represented by sugar alcohols such as sorbitol and mannitol. These alcohols may be used alone or in combination of two or more. Any appropriate fatty acid may be used as the fatty acid. In one embodiment, a fatty acid having 8 or more carbon atoms (preferably 8 to 24 carbon atoms, more preferably 10 to 22 carbon atoms) is used. Specific examples of fatty acids include caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, palmitoleic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, nonadecanoic acid, arachic acid, gadoleic acid, eicosadienoic acid, arachidonic acid, behenic acid, erucic acid, docosadienoic acid, lignoceric acid, isostearic acid, ricinoleic acid, 12-hydroxystearic acid, 9-hydroxystearic acid, 10-hydroxystearic acid, hydrogenated castor oil fatty acid (a fatty acid containing a small amount of stearic acid and palmitic acid in addition to 12-hydroxystearic acid), etc. Among them, palmitic acid and stearic acid are preferable. Only one type of fatty acid may be used, or two or more types may be used in combination.
[0034] The fatty acid amide is a compound having a structure in which a fatty acid and ammonia or a primary or secondary amine are dehydrated and condensed. The fatty acid amide is not particularly limited, but specifically includes saturated fatty acid monoamides such as lauric acid amide, palmitic acid amide, stearic acid amide, and behenic acid amide, unsaturated fatty acid monoamides such as oleic acid amide, erucic acid amide, and ricinoleic acid amide, substituted amides such as N-stearyl stearic acid amide, N-oleyl oleic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, and N-oleyl palmitic acid amide, methylol amides such as methylol stearic acid amide and methylol behenic acid amide, methylene bis stearic acid amide, ethylene bis capric acid amide, ethylene bis lauryl ... Examples of the fatty acid amides include saturated fatty acid bisamides such as uric acid amide, ethylene bisstearic acid amide, ethylene bisisostearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene bishydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacic acid amide, unsaturated fatty acid bisamides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, and N,N'-dioleyl adipic acid amide, and aromatic bisamides such as m-xylylene bisstearic acid amide. These fatty acid amides may be used alone or in combination of two or more. Among these, those having a melting temperature in the range of about 70°C to 120°C are particularly preferred.
[0035] The polyglycerol fatty acid ester is an ester compound composed of polyglycerol and a fatty acid.
[0036] As the polyglycerin, any suitable polyglycerin can be used.Specific examples of the polyglycerin include diglycerin, triglycerin, tetraglycerin, pentaglycerin, hexaglycerin, heptaglycerin, octaglycerin, nonaglycerin, decaglycerin, eicosaglycerin, and tetracontaglycerin.Of these, diglycerin, triglycerin, pentaglycerin, or decaglycerin is preferred.Only one type of polyglycerin may be used, or two or more types may be used in combination.
[0037] Any appropriate fatty acid may be used as the fatty acid. In one embodiment, a fatty acid having 8 or more carbon atoms (preferably 8 to 24, more preferably 10 to 22) is used. Specific examples of fatty acids include caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, palmitoleic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, nonadecanoic acid, arachic acid, gadoleic acid, eicosadienoic acid, arachidonic acid, behenic acid, erucic acid, docosadienoic acid, lignoceric acid, isostearic acid, ricinoleic acid, 12-hydroxystearic acid, 9-hydroxystearic acid, 10-hydroxystearic acid, and hydrogenated castor oil fatty acid (a fatty acid containing small amounts of stearic acid and palmitic acid in addition to 12-hydroxystearic acid). Among these, palmitic acid and stearic acid are preferred. Only one type of fatty acid may be used, or two or more types may be used in combination.
[0038] Specific examples of the polyglycerol fatty acid ester include diglycerol palmitate, diglycerol stearate, diglycerol oleate, decaglycerol palmitate, decaglycerol stearate, decaglycerol oleate, etc. These may be used alone or in combination of two or more.
[0039] The fatty acid esterification rate of the polyglycerol fatty acid ester is preferably 35% or more, more preferably 50% to 70%. Within this range, a filler granule having excellent production stability can be obtained. In addition, the filler granule has excellent dispersibility in resins (especially thermoplastic resins). The esterification rate (%) is expressed by the formula: esterification rate (%) = (mol number of constituent fatty acids / number of hydroxyl groups of polyglycerol) x 100.
[0040] The polyglycerol fatty acid ester can be obtained by any suitable method. For example, it can be obtained by reacting polyglycerol with a fatty acid in the presence or absence of a catalyst (e.g., phosphoric acid, p-toluenesulfonic acid, caustic soda) at 100°C to 300°C (preferably 120°C to 260°C) while removing the generated water from the system. The reaction is preferably carried out in the presence of an inert gas. It may also be carried out in an azeotropic solvent such as toluene or xylene.
[0041] The condensed hydroxy fatty acid can be obtained by dehydration condensation of a hydroxy fatty acid. The condensed hydroxy fatty acid can be obtained, for example, by adding an alkali catalyst such as caustic soda to a hydroxy fatty acid and removing reaction water under heating to perform dehydration condensation.
[0042] The condensed hydroxy fatty acid is a condensation product of a hydroxy fatty acid, and the degree of condensation is preferably not less than 2, more preferably not less than 4. The upper limit of the degree of condensation of the condensed hydroxy fatty acid is, for example, 20. The degree of condensation can be calculated from the acid value of the raw hydroxy fatty acid and the acid value after the condensation reaction.
[0043] The above-mentioned hydroxy fatty acid is a fatty acid having one or more hydroxyl groups in the molecule.Specific examples of hydroxy fatty acid include ricinoleic acid, 12-hydroxystearic acid, savinic acid, 2-hydroxytetradecanoic acid, iprolic acid, 2-hydroxyhexadecanoic acid, yarapinolic acid, uniperilic acid, ambrettolic acid, aluritic acid, 2-hydroxyoctadecanoic acid, 18-hydroxyoctadecanoic acid, 9,10-dihydroxyoctadecanoic acid, camrolenoic acid, ferronic acid, and cerebronic acid.Hydroxy fatty acid may be used alone or in combination of two or more.
[0044] The alcohol ester of the condensed hydroxy fatty acid can be obtained by esterification reaction of the condensed hydroxy fatty acid with alcohol. The alcohol ester of the condensed hydroxy fatty acid can be obtained, for example, by mixing the condensed hydroxy fatty acid with alcohol, adding an alkali catalyst such as caustic soda or an acid catalyst such as phosphoric acid to the resulting mixture, and removing reaction water under heating. The progress of esterification during this reaction can be confirmed by measuring the acid value, saponification value, hydroxyl value, etc. In the condensed hydroxy fatty acid used here, the condensation degree is preferably 2 or more, more preferably 4 or more, as described above.
[0045] Examples of the alcohol include monohydric alcohols such as methyl alcohol, ethyl alcohol, and isopropyl alcohol; dihydric alcohols such as ethylene glycol and propylene glycol. In addition, polyhydric alcohols may be used as the alcohol. Examples of the polyhydric alcohol include alkane polyols such as pentaerythritol and glycerin; polyalkane polyols which are polymers of the alkane polyols; sugars such as sucrose; and sugar derivatives represented by sugar alcohols such as sorbitol and mannitol. These alcohols may be used alone or in combination of two or more.
[0046] Specific examples of the condensed hydroxy fatty acid and its alcohol ester include condensed ricinoleic acid obtained by dehydration condensation of ricinoleic acid, condensed 12-hydroxystearic acid obtained by dehydration condensation of 12-hydroxystearic acid, condensed ricinoleic acid hexaglycerin ester which is an ester of condensed ricinoleic acid and hexaglycerin of glycerin 6 polymer, condensed ricinoleic acid tetraglycerin ester which is an ester of condensed ricinoleic acid and tetraglycerin of glycerin 4 polymer, condensed 12-hydroxystearic acid propylene glycol ester which is an ester of condensed 12-hydroxystearic acid and propylene glycol, and condensed linoleic acid propylene glycol ester which is an ester of condensed ricinoleic acid and propylene glycol, etc. These may be used alone or in combination of two or more.
[0047] The polyglycerol fatty acid ester, condensed hydroxy fatty acid, and alcohol ester of condensed hydroxy fatty acid may be commercially available. Examples of commercially available products include "Chirabazol P-4", "Chirabazol VR-01", "Chirabazol VR-08" (polyglycerol fatty acid ester), "Chirabazol H-818" (alcohol ester of condensed hydroxy fatty acid), etc., manufactured by Taiyo Kagaku Co., Ltd.
[0048] The weight average molecular weight of the dispersant is preferably 800 or more, more preferably 800 to 4000. Within such a range, a filler granule having excellent granulation properties, thermal stability, and dispersibility can be obtained. The weight average molecular weight can be measured by the intrinsic viscosity method.
[0049] The content of the dispersant is preferably 0.1 to 15 parts by weight, more preferably 1 to 10 parts by weight, and even more preferably 1 to 5 parts by weight, relative to 100 parts by weight of the total amount of the polymer and the filler. If the content is within such a range, a filler granule having excellent productivity and dispersibility can be obtained.
[0050] A-4. Other ingredients The filler granules may further contain any other appropriate components (additives) as necessary. Examples of additives include antioxidants, light stabilizers, foaming agents, UV absorbers, foaming agents, antiblocking agents, heat stabilizers, impact modifiers, antibacterial agents, compatibilizers, plasticizers, tackifiers, processing aids, lubricants, coupling agents, flame retardants, oxygen scavengers, colorants, and the like. The additives may be blended in the form of liquid, powder, pellets, granules, or in the form of master batches, etc., during filler granulation or in the resin compounding process. In one embodiment, the additives may be blended into a polymer liquid, granulated with a semi-wet granulator, and blended into the filler granules.
[0051] B. Method for manufacturing filler granules The filler granules can be produced by any suitable method. For example, the filler granules can be obtained by subjecting a mixture containing a polymer liquid containing the polymer, the filler, and the dispersant to a semi-wet granulation method.
[0052] In one embodiment, the method for producing the filler granules includes a mixing step of mixing a polymer liquid containing the polymer, the filler, and the dispersant, a granulation step of granulating the mixture obtained through the mixing step to obtain a granule precursor, and a drying step of drying the granule precursor.
[0053] The polymer liquid may include aqueous and / or non-aqueous solvents. The non-aqueous solvent may be an organic solvent, mineral oil, or other hydrocarbon-based oil, silicone-based oil, etc. The polymer liquid may include water and an organic solvent such as alcohol. The polymer liquid may also be a water-in-oil emulsion or an oil-in-water emulsion.
[0054] The polymer liquid is preferably a polymer dispersion, more preferably an aqueous polyolefin dispersion.
[0055] The polymer content of the polymer liquid is preferably 1 to 70 parts by weight, more preferably 3 to 60 parts by weight, and even more preferably 5 to 50 parts by weight, relative to 100 parts by weight of the polymer liquid. In one embodiment, the solid content concentration of the polymer liquid is preferably 1 to 70% by weight, more preferably 3 to 60% by weight, and even more preferably 5 to 50% by weight. By setting the amount of polymer in the polymer liquid within the above range, the polymer exerts sufficient adhesive force as a binder, and a granulated product can be stably produced, and a filler granulated product having excellent filler uniformity can be obtained.
[0056] The mixing ratio of the above polymer liquid is preferably 1 to 70 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 10 to 30 parts by weight, relative to 100 parts by weight of the total amount of the polymer liquid and the filler.
[0057] When the polymer liquid is an aqueous polyolefin dispersion, the average particle size of the aqueous polyolefin in the polymer liquid is preferably 0.1 μm to 100 μm, more preferably 0.5 μm to 50 μm, and even more preferably 1 μm to 25 μm. Within such a range, the polymer can uniformly cover the surface of the filler powder over a wide range, exhibit sufficient adhesive strength as a binder, and can stably produce a granulated product, and can obtain a filler granulated product with excellent filler uniformity. In this specification, the average particle size means the weight average particle size measured by the Coulter count method.
[0058] The polymer liquid may further contain any suitable additive. In one embodiment, the polymer liquid contains a surfactant (e.g., a nonionic surfactant, an anionic surfactant, a cationic surfactant, an amphoteric surfactant, etc.) and / or a basic substance. If these additives are contained, the dispersibility of the polymer in the polymer liquid can be improved. On the other hand, when the filler granules are applied to a resin composition, the surfactant or the basic substance may cause deterioration and decomposition of the resin. From the viewpoint of preventing resin deterioration, it is preferable to suppress the amount of surfactant and basic substance added. From this viewpoint, Chemipearl (registered trademark) manufactured by Mitsui Chemicals, Inc. is soap-free and can be preferably used. When the polymer liquid (e.g., an aqueous polyolefin dispersion) contains a basic substance, the pH of the polymer liquid is not particularly limited, but is preferably, for example, 7.0 to 12.0, more preferably 7.5 to 11.5, and even more preferably 8.0 to 11.0.
[0059] In the mixing step, other components (e.g., the above-mentioned additives), a solvent (preferably, water), etc. may be further mixed in. The water to be added is not particularly limited, and for example, tap water, distilled water, ion-exchanged water, hard water, soft water, etc. can be used.
[0060] In the mixing step, it is preferable to mix the components at room temperature and homogenize them using any suitable mixer, such as a Henschel mixer, a powder kneader (KDH, KDA, CKD, CPM) (Dalton), a Spartan mixer (SPM) (Dalton), or a SP granulator (SPG) (Dalton).
[0061] The mixing time in the mixing step can be any appropriate mixing time depending on the type of components, the type of mixer, the component blending ratio, etc. Preferably, the mixing time is set so that the surface of the filler is sufficiently and uniformly covered with the polymer. A high-speed mixer such as a Henschel mixer or a Spartan mixer can perform the mixing for 1 to 10 minutes. On the other hand, a powder kneader may require a processing time of several minutes to 60 minutes.
[0062] In the granulation step, a compression granulation method is preferably used. In addition, in the granulation step, a semi-wet granulation method can be preferably used. Examples of the compression granulation method / semi-wet granulation method include a disk pelleter method, a tableting method, and a briquetting method. From the viewpoint of the balance between productivity and the quality of the obtained filler granules, the disk pelleter method is preferably used.
[0063] The basic structure of a disk pelletizer is one or two disks with many holes of 2 mm to 30 mm, and a roller for pressure-feeding the raw material into the holes of the disk. The raw material supplied between the disk and the roller, or between two disks, is pressed into the holes of the disk as the roller rotates, and a cylindrical extrudate is formed. Here, the disk hole is tapered, and a compressive stress is applied from the outer periphery of the die hole in the process of the filler mixture passing through the hole. The length of this tapered hole is called the effective length. The extruded granulated material precursor is cut by a cutter or the like on the back side of the disk to obtain a pellet-shaped filler granulated material. The length of the granulated material precursor (resulting in a filler granulated material) can be adjusted by the distance between the back side of the disk and the cutter and the number of rotations of the roller.
[0064] More specifically, the disc pelleter type includes a roller disc die type, a roller ring die type, a double die type, a flat die type, etc. An example of a commercially available disc pelleter type granulator is the Disc Pelletter F Series manufactured by Dalton.
[0065] Although disk pelletizers do not usually have a heating system, they are heated by shear heat generated during operation. In the granulation process, the temperature during granulation is preferably raised to a temperature equal to or higher than the melting point of the polymer component of the polymer liquid, since the molten polymer penetrates between the fillers and a strong binder effect can be obtained. For example, in a polymer liquid (polymer dispersion) containing aqueous polyolefin as the polymer, the temperature during granulation is usually in the range of 40°C to 100°C, preferably 50°C to 90°C, and more preferably 60°C to 80°C as the pellet temperature immediately after granulation.
[0066] Any suitable drying method can be used in the drying step. After the drying step, a filler granule from which fine powder has been removed can be obtained by processing with a vibrating sieve or the like. Any suitable drying equipment can be used in the drying step. For example, a vibrating fluidized dryer is preferred because it can perform drying efficiently in a short time, and examples of such equipment include the VDF series vibrating fluidized dryers manufactured by Dalton.
[0067] C. Melt compounding of resin and filler granules In one embodiment, a melt compound of the filler granules and a resin is provided. As the resin, a thermoplastic resin is preferably used. The thermoplastic resin is not particularly limited, and examples thereof include general-purpose resins such as high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), polypropylene (PP), polyvinyl chloride (PVC), polyvinylidene chloride, polystyrene (PS), polyvinyl acetate (PVAc), polyurethane (PUR), fluorine-based resin, ABS resin (acrylonitrile butadiene styrene resin), AS resin, and acrylic resin (PMMA), polyamide (PA), nylon, polyacetal (POM), polycarbonate (PC), modified polyphenylene sulfide (DE), and the like. Examples of suitable materials include engineering plastics such as m-PPE, modified PPE, PPO, polyesters (PET, PBT, etc.), and cyclic polyolefin (COP), as well as super engineering plastics such as polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), liquid crystal polymer (LCP), polyetheretherketone (PEEK), thermoplastic polyimide (PI), and polyamideimide (PAI).
[0068] Moreover, a biodegradable resin may be used as the resin. Examples of the biodegradable resin include aliphatic polyester resins (e.g., homopolymers or copolymers of polycaprolactone, polylactic acid, polyethylene succinate, polybutylene succinate-adipate, polyhydroxyvalerate, etc., and modified homopolymers or copolymers thereof), aliphatic / aromatic polyester resins (e.g., block polymers or random polymers of aliphatic carboxylic acids or hydroxy acids, aromatic dicarboxylic acids and 1,3-propanediol, etc.), and polyvinyl alcohol resins (e.g., polyvinyl alcohol, polyvinyl acetate, polyvinyl butyrate, ethylene-vinyl alcohol copolymers, etc.). Examples of naturally derived biodegradable resins include natural rubber, etc.
[0069] Any suitable method can be used as a method for producing the molten compound. For example, a kneader, a Banbury mixer, a roll, a single-screw extruder or a multi-screw extruder having two or more screws can be used. A twin-screw extruder is preferably used. The melt-kneaded composition is pelletized. EXAMPLES
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, parts and percentages are based on weight unless otherwise specified.
[0071] [Example 1] 20 parts by weight of polymer dispersion (polyolefin dispersion (aqueous PE dispersion); Mitsui Chemicals, Inc., product name "Chemipearl A100"; polyolefin solids concentration: 40% by weight; average particle size of polyolefin particles: 4 μm; in the table, "A-1") and 1 part by weight of dispersant (polyglycerol condensed hydroxy fatty acid ester; Taiyo Kagaku, Inc., product name "Chirabazol H818"; in the table, "C-1") were added to a 1L plastic container and stirred for 20 minutes at room temperature using a stirring blade to obtain mixture A. Next, 80 parts by weight of filler (untreated magnesium hydroxide powder; Fimatec, Inc., product name "Junmag BF"; average particle size: 12 μm; in the table, "B-1") were added to a powder kneader (Dalton, product name "KDHJ-10"; processing capacity: 6L), and mixture A was added to the powder kneader while stirring with a stirring blade at a rotation speed of 30 rpm. Thereafter, the mixture was stirred for 6 minutes to obtain mixture B. Mixture B was put into a disk pelleter (manufactured by Dalton, product name "Disc Pelleter F-5 / 11-175; capacity: 5 L") to obtain a pellet-shaped granulated precursor. At this time, the hole diameter of the die was 3 mmφ, the thickness of the die plate was 15 mm, the effective length of the die hole was 10 mm, and the rotation speed of the roller of the disk pelleter was 108 rpm. The obtained granulated precursor was dried at 140°C for 4 hours using a hot air circulation type dryer to obtain filler granulated product MB-1. The temperature of the filler granulated product immediately after granulation was measured with a contact thermocouple and was 50 to 60°C.
[0072] [Examples 2 to 10, Comparative Examples 1 to 2, Reference Examples 1 to 3] Filler granules MB-2 to MB-10 and MB-C1 to MB-C5 were obtained in the same manner as in Example 1, except that the polymer liquid, filler and dispersant shown in Table 1 were used in the amounts shown in Table 1. In addition, in Reference Example 3, 12 parts by weight of water was added as another component. The specific contents of each component used in Examples 1 to 10, Comparative Examples 1 and 2, and Reference Examples 1 to 3 are as shown in Table 2.
[0073] [Table 1]
[0074] [Table 2]
[0075] <Evaluation> The filler granules obtained in Examples 1 to 10, Comparative Examples 1 and 2, and Reference Examples 1 to 3 were subjected to the following evaluations. The results are shown in Table 3. (1) Granulation property The obtained filler granules were checked, and the granulation properties were evaluated according to the following criteria. ○: Granules with a diameter of 3 mm are obtained. △: The filler is in the form of granules, but the binding force is insufficient and it easily crumbles. ×: The filler clogs the die, or the filler has no cohesiveness and does not become granular. (2) Granulation speed The production rate of the filler granules per hour (kg / Hr) was calculated. (3) Bulk density The dried filler granules were weighed out in a 1-liter measure to a volume of exactly 1 liter, and the weight was measured to calculate the bulk density (unit: kg / L) of the filler granules. (4) Pellet size 20 particles of the filler granules were taken out, and the average length and diameter of the particles were measured using a caliper. (5) Moisture content The amount of moisture (unit: weight %) remaining in the filler granules was measured using an infrared moisture meter (FD-660, manufactured by Kett Electric Laboratory). (6) Collapse strength measurement The collapse stress (unit: kg) of the dried filler granules was measured using a Kiya hardness tester (manufactured by Shiro Sangyo Co., Ltd., product name "WPF1600-B") The measured value was the average value of 20 filler granules. (7) Fine powder amount measurement 1 kg of the filler granules was weighed out and sieved through a 14 mesh sieve to measure the mass proportion of fine powder (unit: weight %). (8) Filler concentration 1 to 3 g of the filler granules were collected and kept in a crucible in an electric furnace at 600°C for 3 hours, the binder components were removed, and the filler concentration in the filler granules was calculated from the change in weight (unit: weight %).
[0076] [Table 3]
[0077] As shown in Table 3, MB-1 to MB-10 can obtain pellet-shaped filler granules with stable pellet shape, high granulation speed, and appropriate hardness. On the other hand, MB-C1 and MB-C2 can obtain pellet-shaped filler granules, but when melt-kneaded with a thermoplastic resin, the filler dispersibility is insufficient as shown in the comparison between Example 13 and Comparative Example 4 and the comparison between Example 14 and Comparative Example 5 described later. In addition, the comparison between Example 5 and Comparative Example 2 shows that the granulation property of the filler granules is poor when the dispersant is lacking. In MB-C3 to MB-C5, the quality of the filler granules is poor, and the pellet-shaped filler granules cannot be obtained stably with high productivity.
[0078] [Example 11] 70 parts by weight of the filler granules MB-1 and 30 parts by weight of a thermoplastic resin (homopolypropylene; manufactured by Japan Polypropylene Corporation, trade name "Novatec MA1B", MFR 21g / 10min) were charged into a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., trade name "TEM37SS", L / D = 48) and continuously melt-kneaded to produce pellets of a thermoplastic resin composition. The filler granules MB-1 and the thermoplastic resin were each independently charged into the twin-screw extruder quantitatively from the hopper position at the most upstream part of the extruder via a gravimetric feeder. The cylinder temperature of the extruder was set to 180 ° C. from the middle stage of the extruder onwards. The rotation speed of the main screw of the twin-screw extruder was set to 200 rpm. The melt-kneaded resin composition was extruded into a strand shape, cooled in a water-cooled bath, and made into pellets with a length of about 3 mm.
[0079] [Example 12] Pellets of the thermoplastic resin composition were produced in the same manner as in Example 11, except that the filler granules shown in Table 4 were used in the amounts shown in Table 4 and the extrusion speed of the extruder was set as shown in Table 4.
[0080] [Example 13] Mixture I obtained by mixing 70 parts by weight of filler granule MB-1 with 30 parts by weight of thermoplastic resin (homopolypropylene; manufactured by Japan Polypropylene Corporation, trade name "Novatec MA1B", MFR 21g / 10min) was fed into a 40mm single screw extruder (manufactured by Isuzu Processing Machinery Co., Ltd., model number "SV-40-32-EXT"; with dulmage, L / D=32) to produce pellets of thermoplastic resin composition. The cylinder temperature of the extruder was set to 180°C from the middle stage of the extruder onwards. The rotation speed of the main screw of the single screw extruder was set to 100 rpm. The melt-kneaded resin composition was extruded in the form of a strand, cooled in a water-cooled bath, and made into pellets with a length of about 3 mm.
[0081] [Comparative Example 3] Thermoplastic resin composition pellets were produced using magnesium hydroxide powder B-1 without using the filler granules MB-1, in the same manner as in Example 12. In Comparative Example 3, the content of magnesium hydroxide powder B-1 in the resin composition was 65% by weight, and the discharge speed was 30 kg / Hr. In Comparative Example 3, the magnesium hydroxide powder B-1 formed bridges in the hopper, causing poor bite into the extruder screw, and stable production was not possible. Comparing Example 12 with Comparative Example 3, it can be seen that the use of filler granules MB-1 eliminates the feed neck of magnesium hydroxide powder B-1, dramatically improves productivity, and at the same time enables a molten compound that satisfies good filler dispersion in the resin.
[0082] [Examples 14 to 22, Comparative Examples 4 to 7] Pellets of a thermoplastic resin composition were produced in the same manner as in Example 13, except that the filler granules shown in Table 4 were used in the amounts shown in Table 4 and the thermoplastic resin was added in the amounts shown in Table 4. In Comparative Examples 6 and 7, a filler was added to the powder mixture.
[0083] <Evaluation> The pellets of the thermoplastic resin compositions obtained in Examples 14 to 22 and Comparative Examples 4 to 7 were subjected to the following evaluations. The results are shown in Table 4. (a) Resin composition discharge speed (unit: kg / Hr) It is the amount of compound resin composition discharged per hour. (b) Extruder load (unit: %) This is the displayed value of the actual measured power load percentage (percentage of the maximum allowable motor load) of a twin screw extruder or single screw extruder. (c) Temperature of molten resin at the die (unit: °C) The temperature of the resin composition extruded from the die was measured with a contact thermocouple. (d) MFR (unit: g / 10 min) The melt mass flow rate (MFR) was measured and the fluidity was evaluated using a "Melt Indexer" manufactured by Toyo Seiki Seisakusho Co., Ltd. The test conditions in the MFR test of the resin composition were as follows, depending on the type of resin added. Polypropylene resin: 230℃, 2.16kg load Polyethylene resin: 190℃, 5kg load PC / PET resin: 270℃, 2.16kg load (e) Filler content (unit: weight %) 1 to 3 g of pellets of the resin composition were dried at 80°C for 4 hours, and then held in a crucible in an electric furnace at 600°C for 3 hours to remove the thermoplastic resin components. The filler concentration in the resin composition was calculated from the change in weight. (f) Dispersibility of filler in resin composition The pellets of the resin composition were rolled by a hot press to form a sheet having a thickness of about 0.5 mm. The remaining filler aggregates were visually observed through the sheet and evaluated according to the following criteria. AA: Good dispersion state with almost no filler agglomerates observed A: A state in which a small amount of relatively small filler aggregates remain BB: A state in which a considerable number of relatively small filler aggregates remain. B: Large filler aggregates (Distribution order: AA>A>BB>B (left good))
[0084] [Table 4]
[0085] As is clear from Table 4, according to the present invention, it is possible to obtain a resin composition that has excellent fluidity and filler dispersibility even though it contains a high concentration of filler. When magnesium hydroxide powder (B-1) was used instead of the filler granules (Comparative Example 3), poor feeding of the magnesium hydroxide powder (B-1) occurred even at a discharge rate of 30 kg / Hr, and stable production was not possible.
[0086] In addition, even if a single screw extruder, which has a poorer filler dispersion function than a twin screw extruder, is used, it is possible to obtain a resin composition having excellent fluidity and filler dispersibility even though it contains a high concentration of filler (Examples 13 to 22). Examples 13 to 16 show that the fluidity and filler dispersibility improve as the amount of dispersant increases. Furthermore, by using the filler granules of the present invention, it is possible to suppress the rise in resin temperature during melt kneading. This fact indicates that, even in a resin composition with a high filler content, heat generation is suppressed, and thermal decomposition of the resin is suppressed, making it possible to perform molding processing, which leads to the suppression of coloring and discoloration caused by heat generation of the resin and the maintenance of the strength of the processed product, thereby providing extremely useful effects.
[0087] [Examples 23 to 30] Filler granules MB-11 to MB-18 were obtained in the same manner as in Example 1, except that the polymer liquid, filler, and dispersant shown in Table 5 were used in the amounts shown in Table 5. Here, for MB-13, the diameter of the die hole of the disc pelletizer was changed to 5 mmφ, the thickness of the die plate was changed to 15 mm, and the effective length of the die hole was changed to 10 mm. The polymer solution "A-2" in Examples 27 and 28 used a water-soluble vinyl alcohol resin (BVOH) (manufactured by Mitsubishi Chemical Corporation, product name "Nichigo G-polymer"; saponification degree 98.0 mol% or more, melting point: 172°C). BVOH was dissolved in tap water and used at a concentration of 2.5% by weight (Example 27) and 5.0% by mass (Example 28). The specific contents of each component used in Examples 23 to 30 are as shown in Table 2. The obtained filler granules were subjected to the above evaluations (1) to (8). The results are shown in Table 6.
[0088] [Table 5]
[0089] [Table 6]
[0090] [Examples 31 to 33] Pellets of thermoplastic resin compositions were produced in the same manner as in Example 13, except that the filler granules shown in Table 7 were used in the blending amounts shown in Table 7, and the thermoplastic resins shown in Table 7 were used in the blending amounts shown in Table 7. In each case, a resin composition with excellent filler dispersibility was obtained.
[0091] [Examples 34 to 37] Pellets of a thermoplastic resin composition were produced in the same manner as in Example 11, except that the filler granules shown in Table 7 were used in the amounts shown in Table 7, the thermoplastic resins shown in Table 7 were used in the amounts shown in Table 7, and the cylinder temperature of the extruder was set to 250°C from the middle stage of the extruder onwards. In Examples 34 to 37, polycarbonate (PC; manufactured by Mitsubishi Engineering Plastics Corporation, product name "Novarex 7022PJ"; MVR (300°C, 1.2 kg load): 11 cm 3A mixture of polyethylene terephthalate (PET; Mitsubishi Engineering Plastics Corporation, product name "PBK1") (weight ratio PC:PET = 65 / 35) was used as the resin composition. In both cases, a resin composition with excellent filler dispersion was obtained.
[0092] [Table 7]
Claims
1. a mixing step of mixing a polymer liquid, a filler, and a dispersant; a granulation step of granulating the mixture obtained through the mixing step to obtain a granulated product precursor; A method for producing a filler granule, comprising: drying the granule precursor, The filler granules are A composition comprising a polymer, a filler, and a dispersant, the dispersant is at least one selected from the group consisting of fatty acid amides, polyglycerol fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids; The content of the filler is 80 parts by weight to 99.9 parts by weight based on 100 parts by weight of the total amount of the polymer and the filler. A method for producing a filler granule.
2. The method for producing a filler granule according to claim 1, wherein the content of the filler is 90 parts by weight to 99.9 parts by weight per 100 parts by weight of the total amount of the polymer and the filler.
3. The method for producing a filler granule according to claim 1 or 2, wherein the content of the dispersant is 0.1 to 15 parts by weight based on 100 parts by weight of the total amount of the polymer and the filler.
4. The method for producing a filler granule according to any one of claims 1 to 3, wherein the dispersing agent is at least one selected from the group consisting of polyglycerol fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids.
5. The method for producing a filler granule according to claim 1 , wherein the polymer is a polyolefin resin.
6. The method for producing a filler granulated product according to claim 1 , further comprising the step of granulating the filler by a semi-wet granulation method.
7. The method for producing a filler granulated product according to claim 1 , wherein the granulation step comprises granulation by a disk pelleter method.
Citation Information
Patent Citations
JP1975017453A
Process for manufacturing granular coloring agent for thermoplastic resin
JP1977105948A
Facsimile exchanging device
JP1989082755A
Production of resin composition for coloring and resin composition for coloring
JP1995247367A
Thermoplastic resin composition and resin molded article
JP2007284502A