Part for plasma processing apparatus, method for manufacturing part for plasma processing apparatus, electrostatic chuck, and fiber structure for part for plasma processing apparatus
The integration of a fiber-based plasma protection material in a three-member structure enhances the plasma resistance and durability of electrostatic chucks and plasma processing equipment, addressing the limitations of conventional protective layers.
Patent Information
- Application Number
- JP2024058956
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Conventional plasma protective layers in electrostatic chucks and plasma processing equipment are inadequate in terms of plasma resistance, leading to reduced lifespan and airtightness, necessitating improvements for enhanced durability and performance.
A plasma-resistant structure comprising a first member, a second member, and an intermediate member with a plasma protection material containing fibers, arranged along the outer periphery to provide enhanced plasma resistance, stress relief, and improved durability.
The proposed structure extends the lifespan of electrostatic chucks and plasma processing equipment by providing superior plasma resistance, stress relief, and reduced particle generation, thereby improving the overall durability and performance.
Smart Images

Figure 0007576723000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a plasma-resistant structure, a method for manufacturing a plasma-resistant structure, an electrostatic chuck, an edge ring, a fiber structure, a member for a plasma processing apparatus, and a method for repairing a member for a plasma processing apparatus. [Background technology]
[0002] Conventionally, an etching apparatus that performs dry etching of an object by plasma has been used as a semiconductor manufacturing apparatus, and an electrostatic chuck is used in the etching apparatus to fix the object by using static electricity. In the electrostatic chuck, a holding member that fixes and holds the object and a base that holds the holding member are joined by a bonding layer, and a plasma protection layer that reduces damage to the bonding layer by plasma is bonded to the outer surface of the bonding layer (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-165776 A [Patent Document 2] JP 2021-44303 A Summary of the Invention [Problem to be solved by the invention]
[0004] The plasma protective layers described in Patent Documents 1 and 2 are made of a thermosetting resin or an elastomer, and further improvements are required from the viewpoint of plasma resistance, etc. Similarly, in order to maintain the hermeticity in a sealed space using plasma in a plasma processing device or the like, further improvements are required from the viewpoint of plasma resistance, etc. Such improvements are expected to extend the life of electrostatic chucks, plasma processing devices, etc.
[0005] An object of the present invention is to provide a long-life plasma-resistant structure, an electrostatic chuck, an edge ring, a fiber structure, and a member for a plasma processing apparatus, as well as a method for manufacturing such a plasma-resistant structure and a method for repairing a member for a plasma processing apparatus. [Means for solving the problem]
[0006] The plasma-resistant structure of the present disclosure is A plasma-resistant structure including a first member, a second member, an intermediate member disposed between the first member and the second member, and a plasma protective material including fibers, At least one of the first member and the second member has plasma resistance, The plasma protective material containing the fibers is characterized in that it is disposed on the outer surface side of the plasma resistant structure at the end of the intermediate member.
[0007] In the plasma-resistant structure of the present disclosure, The plasma protective material including the fiber may be disposed on the outer periphery of the intermediate member.
[0008] In the plasma-resistant structure of the present disclosure, The direction in which the fibers extend may be along an outer periphery of the intermediate member.
[0009] In the plasma-resistant structure of the present disclosure, The plasma protective material containing fibers may include a fiber structure made of fibers.
[0010] In the plasma-resistant structure of the present disclosure, The extension direction of the fiber structure may be along an outer periphery of the intermediate member.
[0011] In the plasma-resistant structure of the present disclosure, The intermediate member may be a bonding layer.
[0012] In the plasma-resistant structure of the present disclosure, The length of the fiber in the extending direction is longer than the outer periphery of the intermediate member, The fiber may be wound around an outer periphery of the intermediate member.
[0013] In the plasma-resistant structure of the present disclosure, The length of the fiber structure in the extending direction is longer than the outer periphery of the intermediate member, The fiber structure may be wound around an outer periphery of the intermediate member.
[0014] In the plasma-resistant structure of the present disclosure, The fibers may be inorganic fibers.
[0015] In the plasma-resistant structure of the present disclosure, The textile structure may include at least one of a twisted yarn, a nonwoven fabric, a mesh, or a woven fabric.
[0016] The electrostatic chuck of the present disclosure comprises: Equipped with the plasma-resistant structure of the present disclosure, The first member is a holding member that holds an object to be held, and the second member is a base that holds the holding member.
[0017] In the electrostatic chuck of the present disclosure, The outermost periphery of the holding member may be located outside the outermost point of the plasma protection material.
[0018] In the electrostatic chuck of the present disclosure, The outermost periphery of the base may be located outside the outermost point of the plasma protection material.
[0019] The edge ring of the present disclosure is The present invention is characterized by being provided with a plasma-resistant structure according to the present disclosure.
[0020] The plasma processing apparatus member of the present disclosure includes: The present invention is characterized by being provided with a plasma-resistant structure according to the present disclosure.
[0021] The fiber structure of the present disclosure comprises: A fiber structure having fibers, A plasma-resistant structure including a first member, a second member, an intermediate member disposed between the first member and the second member, and the fiber structure of the present disclosure, The intermediate member is characterized in that it is disposed along the outer periphery of the intermediate member.
[0022] The method for manufacturing a plasma-resistant structure according to the present disclosure includes the steps of: A method for manufacturing a plasma-resistant structure according to the present disclosure, comprising: a first member; a second member; an intermediate member disposed between the first member and the second member; and a fiber structure having fibers, the method comprising the steps of: disposing an intermediate member between the first member and the second member; and winding the fiber structure around an outer periphery of the intermediate member.
[0023] The method for repairing a member for a plasma processing apparatus according to the present disclosure includes: A method for repairing a member for a plasma processing apparatus, the method comprising: a first member; a second member; and an intermediate member disposed between the first member and the second member, the method comprising the steps of: The method includes a step of winding a fiber structure having fibers around the outer periphery of the intermediate member. Effect of the Invention
[0024] According to the present disclosure, there are provided a long-life plasma-resistant structure, an electrostatic chuck, an edge ring, a fiber structure, a member for a plasma processing apparatus, a method for manufacturing such a plasma-resistant structure, and a method for repairing a member for a plasma processing apparatus. [Brief description of the drawings]
[0025] [Figure 1] 1 is a cross-sectional view showing a schematic configuration of a plasma-resistant structure according to an embodiment of the present disclosure. [Diagram 2] 10 is a cross-sectional view showing another schematic configuration of a plasma-resistant structure according to an embodiment of the present disclosure. [Diagram 3] 1 is a diagram showing an outline of a method for repairing a plasma-resistant structure (electrostatic chuck) according to an embodiment of the present disclosure. [Figure 4]1 is a cross-sectional view showing a schematic configuration of an electrostatic chuck according to an embodiment of the present disclosure. [Diagram 5] FIG. 11 is a cross-sectional view showing another schematic configuration of an electrostatic chuck according to an embodiment of the present disclosure. [Figure 6] FIG. 1 is a diagram showing a schematic configuration of an edge ring according to an embodiment of the present disclosure. [Figure 7] FIG. 1 is a schematic configuration diagram in which an edge ring is disposed to surround an electrostatic chuck according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings, but the present disclosure is not limited thereto.
[0027] [Plasma-resistant structure] 1 and 2 are cross-sectional views showing a schematic configuration of a plasma-resistant structure according to an embodiment of the present disclosure. As shown in FIG. 1, the plasma-resistant structure 1 includes a first member 2, a second member 3, an intermediate member 4 disposed between the first member 2 and the second member 3, and a plasma protective material 5 containing fibers. At least one of the first member 2 and the second member 3 has plasma resistance. The plasma protective material 5 containing fibers (hereinafter also simply referred to as the plasma protective material 5) is disposed on the outer surface side of the plasma-resistant structure 1 at the end of the intermediate member 4. Here, the "outer surface side" of the plasma-resistant structure 1 means the side in contact with the external atmosphere. In FIG. 6(B), which is a cross-sectional view showing a schematic configuration of an edge ring according to an embodiment of the present disclosure, the plasma protective materials 45a and 45b (plasma protective materials 5) are disposed on the outer periphery and inner periphery of the edge ring 41 (plasma-resistant structure 1) at the end of the intermediate member 44, and both of these outer periphery and inner periphery are located on the outer surface side of the plasma-resistant structure 1 (edge ring 41) in contact with the external atmosphere.
[0028] (First member 2 and second member 3) In the plasma-resistant structure 1, either the first member 2 or the second member 3 may have plasma resistance. That is, only the first member 2 may be formed from a material having plasma resistance (plasma-resistant material), or only the second member 3 may be formed from a plasma-resistant material. If both the first member 2 and the second member 3 are formed from a plasma-resistant material, the intermediate member 4 disposed therebetween can be more effectively protected from plasma, which is preferable. The first member 2 and / or the second member 3 may be a plasma protection material 5 containing fibers, which will be described later. As in the first member 2a of the plasma-resistant structure 1a shown in FIG. 2, the first member 2 and / or the second member 3 may be a plasma protection material 5 containing fibers. The first member 2 and / or the second member 3 may be composed of a plurality of components.
[0029] Examples of plasma-resistant materials include organic materials and inorganic materials. As organic materials, nylon, polyimide, polyamide, polyester, acrylic, polyolefin, aromatic polyether ketone, polyphenylene sulfide, fluororesin, polyvinyl alcohol, ethylene-vinyl alcohol resin, phenol resin, vinyl chloride, and silicone resin are preferred, but are not limited to these. As inorganic materials, metals and ceramics are preferred, but are not limited to these. Examples of inorganic materials include those containing at least one of yttrium, aluminum, zirconium, hafnium, calcium, magnesium, nickel, titanium, and silicon, and may be oxides, hydroxides, carbides, or mixtures (minerals, etc.) of these elements, and the mixture may contain hydroxyapatite.
[0030] (Intermediate part 4) The intermediate member 4 is not particularly limited, and may be a member having functions such as bonding, sealing, insulation, heat insulation, heat conduction, and conductivity (hereinafter also referred to as a "functional member"), or may be a filler or space with no intended function. Therefore, the material of the intermediate member 4 is also not limited. The shape of the intermediate member 4 is also not particularly limited, and may be hollow, layered, etc. Specific examples of the intermediate member 4 include a sealing material (O-ring), a bonding layer (bonding layer 14 in FIG. 4), etc.
[0031] (Joining layer) The bonding layer, which is one of the functional members, is not particularly limited, and may be a metal, an adhesive material (resin), etc. As the metal, from the viewpoint of workability, a brazing material (silver brazing, copper brazing, copper alloy brazing, aluminum brazing, nickel brazing, activated silver brazing, titanium brazing, solder material, etc.) may be used. Among these, a more appropriate one may be selected in relation to the properties (thermal expansion, thermal conductivity, etc.) of the first member 2 and the second member 3 to be bonded.
[0032] (Adhesive material) The bonding layer (functional member) may be an adhesive material. Examples of adhesive materials include silicone resin, fluororesin, acrylic resin, polyimide resin, polyamide resin, polyester resin, polyolefin resin, and adhesive materials mixed with fillers. From the viewpoint of adhesiveness and heat resistance, silicone resin, fluororesin, acrylic resin, polyimide resin, and adhesive materials mixed with fillers are preferred, silicone resin, acrylic resin, epoxy resin, and adhesive materials mixed with fillers are more preferred, and silicone resin and silicone resin mixed with fillers are even more preferred, but are not limited to these.
[0033] (Sealing material) The intermediate member 4 may be a sealing material. Examples of the sealing material include silicone, polyimide, aromatic polyether ketone, fluororesin, elastomer, and a mixture of these sealing materials with a filler. From the viewpoint of plasma resistance and heat resistance, fluororesin and a mixture of fluororesin with a filler are preferable, but are not limited to these. The shape of the sealing material may be a ring shape (for example, an O-ring), and the sealing material may be formed by pouring uncured curable liquid resin into any shape.
[0034] (Plasma protection material 5) The plasma protective material 5 includes fibers and is formed from a plasma-resistant material. The plasma protective material 5 protects the intermediate member 4, such as a resin material, from the plasma space, and can isolate or keep the resin material away from the plasma space. The plasma protective material 5 blocks the path to the intermediate member 4, increasing the distance the plasma reaches the intermediate member 4, deactivating the plasma, and reducing the effect on the intermediate member 4. When the plasma protective material 5 is made of fibers, voids are formed between the fibers and around the fibers, and such voids allow the material to follow dimensional changes in the outside world and relieve stress (cushioning properties). For example, the material can follow dimensional changes in the first member 2 and the second member 3 due to heating and relieve stress caused by the dimensional changes, resulting in a longer life for the plasma-resistant structure 1. When the plasma protective material 5 is made by mixing fibers with ceramics, the fibers become aggregates for the ceramics, and the strength of the plasma protective material 5 against stress is increased. As a result, the stress resistance against external dimensional changes is increased, and the life span of the plasma-resistant structure 1 is extended.
[0035] The fibers constituting the plasma protective material 5 are preferably inorganic fibers, examples of which include at least one of yttrium, aluminum, zirconium, hafnium, calcium, magnesium, nickel, titanium, and silicon. The plasma protective material 5 may be made of oxides, hydroxides, carbides, fibers in which the surface of organic fibers is coated with these inorganic compounds, or mixtures thereof, but is not limited to these. Furthermore, examples of commercially available inorganic fibers include Fineflex manufactured by Nichias Corporation, Isowool manufactured by Isolite Industries Co., Ltd., Ibiwool manufactured by Ibiden Co., Ltd., Superwool manufactured by Shin-Nichika Thermal Ceramics Co., Ltd., Nextel manufactured by 3M Corporation, N-Silica manufactured by Nippon Glass Fiber Industries Co., Ltd., BelCo Tex manufactured by BelChem Co., Ltd., Nichibi Alf manufactured by Nichibi Co., Ltd., Almax manufactured by Mitsui Mining Materials Co., Ltd., Saffi Examples of such fibers include SAFFIL manufactured by Denka Fibres, DENKA ALCENSE manufactured by Denka, RUBILE manufactured by Nichias Corporation, MAFTEC manufactured by Mitsubishi Chemical Industrial Products, ARTEX manufactured by Sumitomo Chemical Co., Ltd., ROCKFIBER manufactured by Nitto Boseki Co., Ltd., MG Mighty Wool manufactured by Nichias Corporation, S-FIBER manufactured by Nippon Rockwool Industries Co., Ltd., ROCKFIL manufactured by Lapinas Co., Ltd., NICALON manufactured by Nippon Carbon Co., Ltd., TYRANNO FIBERS manufactured by Ube Industries, LASRON manufactured by Nippon Seisen Co., Ltd., BEIPORD manufactured by Bekaert, BOLFUR manufactured by Unitika Ltd., SENCY manufactured by Unitika Ltd., UNITIKA GLASS FIBER manufactured by Unitika Ltd., NITTOBO GLASS FIBER manufactured by Nitto Boseki Co., Ltd., E-Glass manufactured by Nippon Electric Glass Co., Ltd., ARG manufactured by Nippon Electric Glass Co., Ltd., and ALUFIBER manufactured by Asahi Glass Co., Ltd.
[0036] The plasma protective material 5 is disposed on the outer surface side of the plasma-resistant structure 1 at the end of the intermediate member 4. The plasma protective material 5 may be disposed on the outer periphery of the intermediate member 4, and the plasma protective material 5 is preferably provided along the outer periphery of the intermediate member 4. The extension direction of the fibers of the plasma protective material 5 is preferably along the outer periphery of the intermediate member 4.
[0037] The length of the plasma protective material 5 in the direction in which the fibers extend is longer than the outer periphery of the intermediate member 4, and the fibers may be wound around the outer periphery of the intermediate member 4 or may be (tightly) wound around the outer periphery of the intermediate member 4 (including the result of being present around the intermediate member once or multiple times). Here, the plasma protective material 5 may be directly wound around the intermediate member 4, or may be sandwiched and wound between the first member 2 and the second member 3 (i.e., the plasma protective material 5 may be separated from the intermediate member 4). In this specification, the term "fiber" refers to a thread-like substance, and its structure (shape) is not particularly limited, but the diameter of the fibers of the plasma protective material 5 is preferably 0.01 mm to 0.2 mm, more preferably 0.02 mm to 0.1 mm. It is preferable that the average fiber diameter is within these ranges from the viewpoint of stress relaxation property and plasma resistance. The aspect ratio (length / diameter) of the fiber depends on the application, but is preferably 1,000 to 2,200,000, more preferably 28,000 to 2,200,000, and even more preferably 140,000 to 1,200,000. This is because the longer the fiber length (aspect ratio), the better the plasma resistance, durability, and particle resistance tend to be obtained.
[0038] The structure (shape) of the plasma protective material 5 containing fibers is not particularly limited, but the plasma protective material 5 may be a fiber structure made of fibers. The fiber structure may be a twisted yarn, a nonwoven fabric, a woven fabric, or a mesh-like structure, and may be composed of a plurality of components (fibers, etc.) having gaps (voids). A known method for manufacturing these fiber structures can be adopted according to the intended use. For example, the twisted yarn can be manufactured by combining and twisting a plurality of fibers, and the nonwoven fabric can be manufactured by a dry method or a wet method, but is not limited thereto. The above-mentioned "voids" of the plasma protective material 5 are also not particularly limited as long as the above-mentioned stress relaxation properties and long life can be achieved. For example, the plasma protective material 5 may be one in which a single fiber formed from the above-mentioned plasma-resistant material is wound around the outer periphery of the intermediate member 4. In this case, too, the voids between the wound fibers can follow the dimensional changes of the first member 2 and the second member 3, and can exert the effect of relaxing the stress caused by the dimensional changes. As a result, a plasma-resistant structure 1 with a long life can be provided.
[0039] In addition, the plasma protective material 5 (fiber structure) preferably includes a fiber bundle. That is, by bundling, stress relaxation, strength, and ease of handling (including arrangement and removal) are improved compared to when only fibers are included. The materials and dimensions of each fiber in the fiber bundle may be the same or different, but it is preferable that the direction and orientation are the same and the dimensions are approximately the same. The number of fibers to be bundled is not particularly limited, and can be appropriately set in consideration of the thickness of the intermediate member 4 and the diameter of the fiber. For example, it is preferable that the fiber bundle made of inorganic fibers is sandwiched between the first member 2 and the second member 3. That is, by being sandwiched between the first member 2 and the second member 3, the intermediate member 4 is isolated from the plasma atmosphere, and the fiber bundle is less likely to fall off. By selecting and setting the number of fibers in this way, the life of the plasma-resistant structure 1 can be extended. In addition, it is preferable that the fibers in the fiber bundle are bonded to each other to a degree that can maintain the shape and provide cushioning properties at the same time.
[0040] The extending (extending) direction of the fiber structure is also preferably along the outer periphery of the intermediate member 4, i.e., the fiber bundles constituting the plasma protective material 5 also preferably extend along the outer periphery of the intermediate member 4. The direction of each fiber of the fiber bundle is also preferably along the outer periphery of the intermediate member 4. In this way, since the fiber direction is aligned, the fiber bundles as the plasma protective material 5 can be uniformly inserted between the first member 2 and the second member 3, so that the gaps between the first member 2 and the plasma protective material 5 and between the second member 3 and the plasma protective material 5 are reduced, improving the plasma resistance. As a result, the life of the plasma-resistant structure 1 can be extended.
[0041] In addition, the length of the plasma protective material 5 in the extending direction of the fiber structure may be longer than the outer periphery of the intermediate member 4, and the fiber structure may be wound around the outer periphery of the intermediate member 4 (FIG. 3). Note that FIGS. 3(A) and (B) are examples of a top view and a perspective view of the plasma-resistant structure 1 when the plasma protective material 5 is wound around the outer periphery of the intermediate member 4.
[0042] In addition, the fiber bundle contained in the plasma protective material 5 preferably includes a twisted yarn shape. If the twisted fibers can move relative to each other in the fiber bundle, both high strength and cushioning properties can be achieved. In addition, the high strength of the twisted yarn can increase the strength of the plasma protective material 5, and it also becomes easy to remove the plasma protective material 5 from the plasma-resistant structure 1. In addition, the twisted yarn can also relax the stress by the fibers being loosened in the fiber bundle. There is no particular limitation on the twisting method, but it can be 5 to 360 turns per meter, and is preferably in the range of 20 to 300 turns. In the twisting method, if it is in the above range, not only the strength and stress relaxation of the fiber bundle but also the suppression of particle generation during plasma treatment can be realized in a balanced manner. As a result, it is possible to provide a plasma-resistant structure 1 with a long life. Here, "particles" mainly mean small pieces generated from the plasma-resistant structure 1 during plasma treatment. There is a risk that the particles will become impurities of the held object W. For example, if the strength of the plasma protective material 5 is low, the fibers may be destroyed by the plasma treatment and adhere to the held object W as particles. Furthermore, if the intermediate member 4 is not isolated or kept away from the plasma atmosphere by the plasma protection material 5, the intermediate layer may be deteriorated or destroyed by the plasma atmosphere, and may adhere to the held object W as particles.
[0043] The diameter of each fiber in the fiber bundle is preferably 0.01 mm to 0.2 mm, more preferably 0.02 mm to 0.1 mm. It is preferable that the average fiber diameter is within these ranges from the viewpoint of stress relaxation and plasma resistance. In addition, the aspect ratio of each fiber in the fiber bundle is preferably 500 or more, more preferably 1000 or more, and even more preferably 8000 or more. When each fiber is a long fiber in this way, the stress relaxation of the plasma protective material 5 is improved, and as a result, a plasma-resistant structure 1 with a long life can be provided. In addition, the "diameter" in this specification is the average value of the area diameter (for example, the average value of 20 fibers or fiber bundles) derived by calculating the cross-sectional area in any vertical cross section with respect to the extension direction of the fiber or fiber bundle imaged by a microscope (for example, calculated by known software), and calculating the diameter of a circle having the same area as the cross-sectional area. In addition, the "length" of the fiber bundle in this specification is, for example, the average value of the lengths of any 10 fibers in the fiber bundle.
[0044] The plasma protective material 5 does not have to be bonded to the first member 2, the second member 3, or the intermediate member 4. For example, a fiber structure (twisted yarn, mesh, nonwoven fabric, metal wire, etc.) may be pushed between the first member 2 and the second member 3 toward the intermediate member 4 as the plasma protective material 5.
[0045] It is preferable that the plasma protective material 5 and the intermediate member 4 are at least partially separated, and it is more preferable that they are partially separated and the other parts are in close contact with each other (for example, in an electrostatic chuck 21 having a plasma-resistant structure shown in FIG. 5, the side of the plasma protective material 25 that contacts the first member 22 and the side that contacts the second member 23 are separated from the outer peripheral portion 24a of the bonding layer 24, which is the intermediate member). If the plasma protective material 5 is completely separated from the intermediate member 4, there is a risk of it falling off, but by separating a part of it and in close contact with another part, it is possible to improve the stress relaxation property. As a result, it is possible to provide a plasma-resistant structure 1 with a long life.
[0046] Other embodiments of the present disclosure are described below, with the reference numbers of components that are the same as or similar to the components of the plasma-resistant structure 1 being numbered with 10, 20, 30, 40, etc. (i.e., for example, the plasma protection material 15 in FIG. 4 is the same as or similar to the plasma protection material 5). Also, in particularly preferred embodiments, the same or similar components may be given different names (for example, the edge ring portion 42 and the edge ring portion 43 in FIG. 6 correspond to the first member 2 and the second member 3, respectively, and may be formed from a plasma-resistant material, but are given different names). The description of these will be omitted as appropriate.
[0047] [Electrostatic chuck 11] According to the present disclosure, an electrostatic chuck 11 having a plasma-resistant structure 1 as shown in FIG. 4 is provided. That is, in FIG. 4, the plasma-resistant structure 1 can be a holding member 12 that holds an object W to be held, and a base 13 that holds the holding member 12. More specifically, the electrostatic chuck 11 has the holding member 12 that holds the object W to be held, the base 13 that holds the holding member 12, a bonding layer 14 disposed between the holding member 12 and the base 13, and a plasma protective material 15 containing fibers, and the plasma protective material 15 containing fibers is disposed on the outer surface side of the electrostatic chuck 11 at the end of the bonding layer 14. The plasma protective material 15 has resistance to plasma as described later, and the plasma protective material 15 can be provided at a desired position of the electrostatic chuck 11 other than the bonding layer 14.
[0048] (Retaining member 12) The holding member 12 is for adsorbing and holding the object to be held W. The shape of the holding member 12 is not limited, and it can be disk-shaped or rectangular according to the shape of the object to be held W. The dimensions of the holding member 12 can also be set appropriately according to the object to be held W. The "object to be held W" is also not limited, and can include workpieces such as wafers (silicon wafers, quartz wafers, SiC wafers, etc.), flat panel display (FPD) panels and substrates, metal members, film members, resin members (automotive interior materials, etc.), glass members, etc.
[0049] Examples of the holding member 12 include ceramic substrates (alumina, aluminum nitride, yttrium oxide, silicon carbide, etc.), resin substrates, and metal substrates made of aluminum, stainless steel, etc. From the viewpoints of plasma resistance and heat resistance, examples of the resin substrate include polyimide, polyamide, polyamideimide, aromatic polyether ketone, and fluorine-based polymer. The holding member 12 may be a substrate made of two or more types of materials. From the viewpoints of plasma resistance and heat resistance, the holding member 12 is preferably a ceramic substrate, a resin substrate, or a composite substrate made of ceramic and resin.
[0050] The thickness of the holding member 12 is not particularly limited and can be within a range of 0.2 mm to 7 mm. In addition, when an internal electrode is provided in the holding member 12 as described later, the thickness of the holding member 12 may be within a range of 3 mm to 10 mm.
[0051] In addition, a plurality of protrusions may be provided on the surface of the holding member 12 that holds the object W. The contact area between the holding member 12 and the object W is reduced by holding (adsorbing) the object W on the upper surfaces of these protrusions. As a result, the quality of the object W can be maintained and the life of the electrostatic chuck 11 can be extended. The number, arrangement, shape, height, dimensions, etc. of the protrusions are not particularly limited. From the viewpoint of maintaining the quality of the object W, the shape of the protrusions is preferably disk-like or cylindrical, and the upper surface of each protrusion is preferably flat. If the shape and height of the protrusions are as described above, the quality of the object W can be maintained well and an electrostatic chuck 11 with a longer life can be provided.
[0052] (Base 13) The base 13 holds the holding member 12 and also has a cooling function. The shape, material, thickness, etc. of the base 13 can be appropriately designed to suit the application. For example, the material of the base 13 can be ceramic, metal, or a combination thereof. Examples of ceramics include alumina, aluminum nitride, yttrium oxide, silicon carbide, etc., and examples of metals include aluminum, stainless steel, etc., but are not limited to these.
[0053] (Joining layer 14) The bonding layer 14 bonds together the various members such as the holding member 12 and the base 13. The thickness (height) of the bonding layer 14 is not particularly limited, but is preferably 20 μm to 1000 μm, more preferably 50 μm to 800 μm, and further preferably 100 μm to 500 μm. If the thickness of the bonding layer 14 is within this range, the bonding layer 14 can favorably withstand the stress of the dimensional change of the holding member 12 and the base 13 during heating, and can limit the contact between the bonding layer 14 and the plasma atmosphere in the plasma treatment step. As a result, an electrostatic chuck 11 with a longer life can be provided.
[0054] Examples of the material of the bonding layer 14 include metals and adhesive materials (resins). As the metal, from the viewpoint of workability, brazing materials (silver brazing, copper brazing, copper alloy brazing, aluminum brazing, nickel brazing, activated silver brazing, titanium brazing, solder materials, etc.) can be used, but are not limited to these. A more appropriate brazing material can be selected in relation to the properties (thermal expansion, thermal conductivity, etc.) of the holding member 12 and the base 13 to be bonded. In addition, examples of the adhesive material include thermoplastic elastomers, thermosetting elastomers, epoxy resins, urethane resins, polyester resins, polyimide resins, polyamide resins, fluororesins, acrylic resins, silicone resins, urethane resins, and mixtures of these with fillers. From the viewpoint of adhesion and heat resistance, silicone resins, acrylic resins, epoxy resins, and mixtures of these with fillers are preferred, and silicone resins and mixtures of silicone resins with fillers are more preferred.
[0055] The bonding layer 14 may contain a thermally conductive filler. By containing the thermally conductive filler, both adhesiveness and thermal conductivity can be achieved, and thermal deterioration of the bonding layer 14 can be suppressed. As a result, it is possible to provide an electrostatic chuck 11 with a long life. Examples of the thermally conductive filler include, but are not limited to, metal, alumina, aluminum nitride, silicon carbide, boron nitride, carbon black, carbon nanotubes, diamond, and the like. The amount, shape, and the like of the thermally conductive filler are also not particularly limited.
[0056] According to the present disclosure, an electrostatic chuck 21 as shown in Fig. 5 can also be provided. The bonding layer 24 may be different depending on the position in the surface direction. For example, different types of materials may be used for the central portion 24b and the outer peripheral portion 24a of the bonding layer 24 (Fig. 5). This can favorably withstand the stress caused by the dimensional change of the holding member 22 and the base 23 when heated.
[0057] (Plasma protection material 15) The plasma protection material 15 isolates or keeps the bonding layer 14 away from the plasma atmosphere in order to protect the bonding layer 14, and is preferably provided along the outer periphery of the bonding layer 14.
[0058] The plasma protective material 15 may be a combination of different materials. The plasma protective material 15 may also be a fibrous structure such as a twisted yarn as described above.
[0059] (Protective material) The electrostatic chuck 11 may further include a protective material (not shown) provided along the outer periphery of the plasma protective material 15. This protective material improves the strength of the plasma protective material 15 and can suppress particles generated from the plasma protective material 15. The protective material can also fix the plasma protective material 15 and hold the plasma protective material 15. For stress relief, it is preferable that at least a part of the protective material is separated from the plasma protective material 15.
[0060] As the material of the protective material, an organic substance such as a resin can be used to hold and fix the plasma protective material 15. Examples of the resin include silicone resin, fluororesin, epoxy resin, polyimide resin, acrylic resin, etc. Also, a plasma-resistant material can be used to protect the bonding layer 14 and the plasma protective material 15, and it is particularly preferable to use alumina, silicon carbide, metal oxide, etc.
[0061] The protective material can also be formed by applying a paste containing inorganic particles, a metal organic compound solution, a metal complex solution, or the like, followed by sintering, or can be formed by thermal spraying an inorganic material.
[0062] (others) In the electrostatic chuck 11 according to the present embodiment, an internal electrode (not shown) can be provided in the holding member 12 in order to apply a voltage to generate an electrostatic force (Coulomb force) to adsorb the workpiece W. Alternatively, such an internal electrode may be provided in the base 13.
[0063] The internal electrode is not particularly limited as long as it is made of a conductive material that can exhibit an electrostatic adsorption force when a voltage is applied. For example, a thin film made of a metal such as copper, aluminum, gold, silver, platinum, chromium, nickel, or tungsten, or a thin film made of at least two metals selected from the above metals is preferably used as the internal electrode, and such a conductive material may be contained in a ceramic material. Examples of such a thin film of a conductive material include a film formed by deposition, plating, sputtering, spraying, etc., a film formed by applying and drying a conductive paste, and specifically, a metal foil such as copper foil.
[0064] Moreover, it is preferable that the outermost periphery of the holding member 12 is located outside the outermost point of the plasma protective material 15 (or protective material), and it is more preferable that the outermost periphery of the base 13 is located outside the outermost point of the plasma protective material 15 (or protective material) (FIG. 4). This is because deterioration of the plasma protective material 15 and the protective material due to plasma is suppressed. Furthermore, if the outermost periphery of the holding member 12 is located outside the outermost periphery of the base 13, it is preferable because the base 13 does not interfere with other members such as an edge ring 41 (FIGS. 6 and 7) used together with the electrostatic chuck 11.
[0065] (Manufacturing method and uses of electrostatic chuck 11) The electrostatic chuck 11 can be manufactured, for example, as follows. First, the holding member 12 and the base 13 are prepared. At this time, as described above, a metal such as copper is patterned on either the holding member 12 or the base 13 to form an internal electrode. Next, the holding member 12 and the base 13 are bonded via a bonding layer 14. This is also performed in the conventional electrostatic chuck manufacturing method. In the conventional electrostatic chuck, after the holding member and the base are bonded via a bonding layer, an O-ring or an adhesive (elastomer, acrylic rubber, silicone rubber, fluororubber, thermosetting resin, etc.) is provided. In contrast, in the embodiment of the present disclosure, the plasma protective material 15 as described above is provided on the outer surface side of the electrostatic chuck 11 at the end of the bonding layer 14. Furthermore, a protective material is appropriately provided along the outer periphery of the plasma protective material 15 (FIG. 4).
[0066] The electrostatic chuck 11 according to the present embodiment applies a voltage to the internal electrodes embedded in the holding member 12 or the base 13 to generate a Coulomb force and adsorb the object W to be held. For example, the electrostatic chuck 11 can be used to adsorb a wafer (object W) in a dry etching or CVD process in a semiconductor manufacturing process. In particular, in an apparatus or method using plasma, if the electrostatic chuck 11 according to the present embodiment is used, even if the holding member 12 or the base 13 becomes hot and expands due to plasma irradiation, for example, when the plasma protective material 5 includes an inorganic fiber structure, voids are generated between the inorganic fibers, and the stress due to the difference in expansion and contraction between the holding member 12 and the base 13 can be absorbed, and as a result, the life of the electrostatic chuck 11 can be extended. In addition, when the plasma protective material 15 is formed by mixing the above-mentioned fibers with ceramics or the like, the fibers become aggregates of the ceramics, and the strength of the plasma protective material 15 against stress is increased. As a result, the stress resistance against dimensional changes in the outside world is increased, and the life of the electrostatic chuck 11 can be extended.
[0067] Furthermore, compared to conventional electrostatic chucks, the manufacturing method of electrostatic chuck 11 generally differs in whether or not a plasma protective material 15 is provided, and therefore, when repairing a conventional electrostatic chuck, it can be easily manufactured into electrostatic chuck 11 according to the present disclosure ( FIG. 3 ).
[0068] [Edge Ring 41] In addition, as an embodiment of the present disclosure, an edge ring 41 having a plasma-resistant structure as shown in FIG. 6(A)(B) is provided. FIG. 6(A) and (B) are a perspective view and a cross-sectional view of the edge ring 41, respectively. The edge ring 41 of the present disclosure is formed to surround the outer periphery of the electrostatic chuck and is formed in a ring shape. It is also used in a plasma processing step to uniformly perform plasma processing on a held object W such as a wafer attracted to the upper surface of a holding member of the electrostatic chuck (FIG. 7). In FIG. 6, more specifically, the edge ring 41 has an edge ring portion 42, an edge ring portion 43, a bonding layer (intermediate member) 44 disposed between the edge ring portion 42 and the edge ring portion 43, and a plasma protective material 45 containing fibers, and the plasma protective material 45 is disposed on the outer surface side of the edge ring 41 in the bonding layer 44. The plasma protective material 45 has resistance to plasma, and the plasma protective material 45 can be provided at a desired position of the edge ring 41 other than the bonding layer 44.
[0069] (Edge ring parts 42 and 43) The edge ring parts 42 and 43 are parts that constitute the edge ring 41. The edge ring parts 42 and 43 may be made of a material such as a semiconductor, a conductor, an insulator, or a combination of two or more of these, but are not limited to these. By combining these materials as desired, the dielectric characteristics can be controlled, and the workpiece W, such as a wafer, attracted to the upper surface of the holding member of the electrostatic chuck can be uniformly plasma-processed. As a result, the edge ring 41 can be provided with a long life.
[0070] (Joining layer 44) The bonding layer 44 bonds each component such as the edge ring portion 42 and the edge ring portion 43 together. The thickness (height) of the bonding layer 14 is not particularly limited, but is preferably 20 μm to 1000 μm, more preferably 50 μm to 800 μm, and even more preferably 100 μm to 500 μm. If the thickness of the bonding layer 14 is within this range, the bonding layer 44 can favorably withstand the stress of the dimensional change of the edge ring portion 42 and the edge ring portion 43 during heating, and can limit the contact between the bonding layer 44 and the plasma atmosphere in the plasma treatment process. As a result, an edge ring 41 with a longer life can be provided.
[0071] The bonding layer 44 and the plasma protective material 45 may be the same as the bonding layer 14 and the plasma protective material 15. The edge ring 41 may also be provided with a protective material.
[0072] (Edge Ring 41 manufacturing method and uses) The edge ring 41 can be manufactured, for example, as follows. First, the edge ring portion 42 and the edge ring portion 43 are prepared. At this time, as described above, the edge ring portion 42 and the edge ring portion 43 are bonded via the bonding layer 44. This is also performed in the conventional edge ring manufacturing method. In the conventional edge ring, after the edge ring portion 42 and the edge ring portion 43 are bonded via the bonding layer, an O-ring or adhesive (elastomer, acrylic rubber, silicone rubber, fluororubber, thermosetting resin, etc.) is provided. In contrast, in the embodiment of the present disclosure, the plasma protective material 45 as described above is provided on the outer surface side of the edge ring 41 at the end of the bonding layer 44. Furthermore, a protective material is appropriately provided along the outer periphery of the plasma protective material 45 (not shown).
[0073] The edge ring 41 according to the present embodiment has a long life as described above. In addition, in an apparatus or method using plasma, even if the edge ring portion 42 or the edge ring portion 43 becomes hot and expands due to plasma irradiation, for example, when the plasma protective material 45 includes an inorganic fiber structure, voids are generated between the inorganic fibers, and the stress caused by the difference in expansion and contraction between the edge ring portion 42 and the edge ring portion 43 can be absorbed, and as a result, the edge ring 41 can have a long life. In addition, when the plasma protective material 45 is configured by mixing the above-mentioned fibers with ceramics or the like, the fibers become aggregates for the ceramics, and the strength of the plasma protective material 45 against stress is increased. As a result, the stress resistance against dimensional changes in the outside world is increased, and the edge ring 41 can have a long life.
[0074] Furthermore, compared with the conventional edge ring, the manufacturing method of the edge ring 41 generally differs in whether or not the plasma protection material 45 is provided. Edge Ring When repairing the edge ring 41, the edge ring 41 according to the present disclosure can be easily manufactured.
[0075] [Plasma treatment equipment components] Although not shown, as an embodiment of the present disclosure, a member for a plasma processing apparatus having a plasma-resistant structure can be provided. In a plasma processing apparatus, since it is exposed to a plasma atmosphere, the housing and the parts installed inside the apparatus (electrostatic chuck, edge ring, inner wall of the apparatus, etc.) are also required to have plasma resistance. For example, in a plasma processing apparatus used in a semiconductor device manufacturing process, in order to balance the loading and unloading of a workpiece such as a wafer and the securing of a vacuum state inside, the housing is detachable, and a sealing material (sealing material) such as an O-ring is used in the detachable part. If these detachable parts are provided with the plasma-resistant structure of the present disclosure, the life of the plasma processing apparatus can be extended. In the present disclosure, the "member" for a plasma processing apparatus is a plasma processing apparatus that has the plasma-resistant structure of the present disclosure. For example, a housing and a detachable part can be mentioned. In addition, the plasma processing apparatus itself may have the plasma-resistant structure of the present disclosure as a part thereof. That is, as an embodiment of the present disclosure, a plasma processing apparatus having a plasma-resistant structure can be provided.
[0076] When a crack exists in a plasma-resistant wall of a plasma processing apparatus, the wall can be made into a first member 2 and a second member 3, and the plasma protective material 5 and the intermediate member 4 can be inserted into the crack between the first member 2 and the second member 3 as a filler or adhesive (to bond the plasma protective material 5 to the first member 2 and the second member 3). In this manner, the plasma protective material 5 of the present disclosure can also be used as a repair material.
[0077] (Method of manufacturing and repairing members for plasma processing equipment) The member for plasma processing apparatus (plasma-resistant structure 1) can be manufactured, for example, as follows. First, the first member 2 and the second member 3 are prepared. At this time, as described above, the intermediate member 4 is disposed between the first member 2 and the second member 3. This is also performed in the conventional manufacturing method for the member for plasma processing apparatus. In the conventional member for plasma processing apparatus, the first member and the second member are joined via a joining layer, and then an O-ring or an adhesive (elastomer, acrylic rubber, silicone rubber, fluororubber, thermosetting resin, etc.) is provided. In contrast, in the embodiment of the present disclosure, the plasma protective material 5 as described above is provided on the outer surface side of the member for plasma processing apparatus at the end of the intermediate member 4. For example, the plasma protective material 5 can be installed by winding a fiber structure having fibers around the outer periphery of the intermediate member 4. Furthermore, a protective material is appropriately provided around the outer periphery of the plasma protective material 5 (not shown). The repair method for the member for plasma processing apparatus (plasma-resistant structure 1) includes a step of winding a fiber structure around the outer periphery of the intermediate member, as in the manufacturing method for the member for plasma processing apparatus.
[0078] The plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, and member for a plasma processing apparatus according to the present embodiment configured as described above include a first member 2, a second member 3, an intermediate member 4 disposed between the first member 2 and the second member 3, and a plasma protective material 5 containing fibers. At least one of the first member 2 and the second member 3 has plasma resistance, and the plasma protective material 5 containing fibers is disposed on the outer surface side of the plasma-resistant structure 1 at the end of the intermediate member 4.
[0079] Furthermore, a fiber structure which is one embodiment of the present disclosure has fibers, and in a plasma-resistant structure 1 which includes a first member 2, a second member 3, and an intermediate member 4 arranged between the first member 2 and the second member 3, this fiber structure is arranged along the outer periphery of the intermediate member 4.
[0080] In addition, a manufacturing method for the plasma-resistant structure 1 according to one embodiment of the present disclosure includes a step of placing an intermediate member between the first member 2 and the second member 3, and a step of winding a fiber structure around the outer periphery of the intermediate member 4.
[0081] Furthermore, according to a method for repairing a member for a plasma processing apparatus which is one embodiment of the present disclosure, the member for a plasma processing apparatus comprises a first member 2, a second member 3, and an intermediate member 4 disposed between the first member 2 and the second member 3, and this repair method includes a step of winding a fiber structure having fibers around the outer periphery of the intermediate member 4.
[0082] As described above, in the plasma-resistant structure 1, the plasma protective material 5 and the first member 2, etc. have plasma resistance, so that the intermediate member 4 and therefore the plasma-resistant structure 1 are extended in life. In addition, the voids in the plasma protective material 5 allow it to follow, for example, dimensional changes in the holding member 12 and the base 13 and relieve stress, thereby extending the life of the electrostatic chuck 11. In addition, when the plasma protective material 5 is formed by mixing fibers with ceramics, etc., the fibers become aggregates for the ceramics, which increases the strength of the plasma protective material 5 against stress, and for example, increases the stress resistance against dimensional changes in the holding member 12 and the base 13, thereby extending the life of the electrostatic chuck 11.
[0083] In the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, member for plasma processing apparatus, fiber structure, method for manufacturing plasma-resistant structure 1, and method for repairing member for plasma processing apparatus of the present embodiment, plasma protective material 5 containing fibers may be disposed on the outer periphery of intermediate member 4. The extending direction of the fibers may be along the outer periphery of intermediate member 4.
[0084] In the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus of the present embodiment, the plasma protective material 5 including fibers may include a fiber structure made of fibers. In other words, the fiber structure may be formed from a plasma-resistant material like the plasma protective material 5.
[0085] In the plasma-resistant structure 1 , the electrostatic chuck 11 , the edge ring 41 and the member for a plasma processing apparatus according to the present embodiment, the extending direction of the fiber structure may be along the outer periphery of the intermediate member 4 .
[0086] In addition, in the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, and member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus of the present embodiment, intermediate member 4 may be a bonding layer.
[0087] In addition, in the plasma-resistant structure 1, electrostatic chuck 11, edge ring and member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus of this embodiment, the length in the extension direction of the fibers is longer than the outer periphery of intermediate member 4, and the fibers may be wound around the outer periphery of intermediate member 4.
[0088] In addition, in the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, and member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus of this embodiment, the length in the extension direction of the fiber structure is longer than the outer periphery of intermediate member 4, and the fiber structure may be wound around the outer periphery of intermediate member 4.
[0089] In addition, in the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, and member for a plasma processing apparatus, fiber structure, manufacturing method for the plasma-resistant structure 1, and repair method for a member for a plasma processing apparatus of the present embodiment, the fibers may be inorganic fibers.
[0090] In addition, in the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, and member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus of this embodiment, the fiber structure may include at least one of twisted yarn, nonwoven fabric, mesh, or woven fabric.
[0091] In the electrostatic chuck 11 of the present embodiment, the first member 2 may be a holding member 12 that holds an object to be held, and the second member 3 may be a base 13 that holds the holding member 12.
[0092] In addition, in the electrostatic chuck 11 of this embodiment, the outermost periphery of the holding member 12 may be located outside the outermost point of the plasma protective material 5, and the outermost periphery of the base 13 may be located outside the outermost point of the plasma protective material 5.
[0093] It should be noted that the plasma-resistant structure 1, electrostatic chuck 11, edge ring 41, member for plasma processing apparatus, fiber structure, manufacturing method for plasma-resistant structure 1, and repair method for member for plasma processing apparatus according to the present embodiment are not limited to the above-mentioned aspects and combinations.
[0094] For example, the number of internal electrodes provided on the holding member 12 or the base 13 may be two, rather than just one.
[0095] For example, an electrode may be provided on the edge ring portion 42 or within the edge ring portion 42 .
[0096] For example, edge ring 41 may further include one or more members in addition to edge ring portion 42 and edge ring portion 43, and intermediate member 4 may be disposed between these members, and plasma protection material 5 may be provided on the outer periphery of intermediate member 4.
[0097] The present disclosure will be described in more detail below using examples and comparative examples.
[0098] [Electrostatic chuck manufacturing method]
[0099] Example 1 An electrostatic chuck-shaped plasma-resistant structure (hereinafter, electrostatic chuck) was fabricated so as to have the configuration shown in Table 1. That is, a silicone adhesive (intermediate member, bonding layer) was applied to the upper surface of an aluminum base (second member, diameter 296 mm, thickness 30 mm) except for the outer periphery width of 20 mm so as to have a thickness of 0.2 mm after application, and an alumina plate (diameter 297 mm, thickness 4 mm) was bonded as a holding member (first member) to the upper surface of the base via this silicone adhesive. Next, an alumina fiber bundle (plasma protection material) made of alumina fibers shown in Table 1 was wound around the outer peripheral end of the silicone adhesive (bonding layer), the alumina plate, and the recess (outer periphery of the bonding layer) surrounded by the base, and fixed between the alumina plate and the base. Then, the end point of the alumina fiber bundle was bonded to a part of the alumina fiber bundle that overlapped the position by firing using a burner. The alumina fiber bundle was in contact with the bonding layer, and the alumina fiber bundle did not protrude from the outer peripheral end of the base and the alumina plate. Thereafter, the substrate was placed in a thermostatic chamber set at 120° C. for 2 hours to harden the silicone adhesive, thereby producing an electrostatic chuck.
[0100] (Examples 2 and 3) The electrostatic chucks of Examples 2 and 3 were fabricated in the same manner as the electrostatic chuck of Example 1 so as to have the configuration shown in Table 1. Instead of wrapping around the outer peripheral end of the bonding layer, the alumina plate, and the recess surrounded by the base, the alumina fiber bundles (fiber length 15 mm or 200 mm) shown in Table 1 were inserted along the entire outer periphery of the bonding layer so that three alumina fiber bundles were arranged next to each other and the extension direction of the alumina fiber bundles was along the outer periphery of the bonding layer.
[0101] (Examples 4 to 13) Electrostatic chucks of Examples 4 to 13 were fabricated in the same manner as the electrostatic chuck of Example 1 so as to have the configuration shown in Table 1. In Table 1, "fiber bundle 1" is CY-640D manufactured by Ceramic Wool Industries Co., Ltd., "fiber bundle 2" is CY-1280D manufactured by Ceramic Wool Industries Co., Ltd., "fiber bundle 3" is CT-2560D manufactured by NITVI Co., Ltd., "fiber bundle 4" is Naslon 12-100 / 2 manufactured by Nippon Seisen Co., Ltd., and "fiber bundle 5" is T300-1000 manufactured by Toray Industries, Inc. (the same applies to Table 2).
[0102] Comparative Example 1 An electrostatic chuck of Comparative Example 1 was fabricated in the same manner as the electrostatic chuck of Example 1 so as to have the configuration shown in Table 1. The silicone adhesive was applied so as to have a thickness of 3.0 mm after application, and as the plasma protective material of Comparative Example 1, a fluororubber-based O-ring (AS568-277-D manufactured by NOK, wire diameter 3.5 mm, outer diameter 299 mm, inner diameter 292 mm) was used and inserted into a recess surrounded by the outer circumferential end of the bonding layer, the alumina plate, and the base.
[0103] Comparative Example 2 An electrostatic chuck of Comparative Example 2 was fabricated in the same manner as the electrostatic chuck of Example 1 so as to have the configuration shown in Table 1. The plasma protective material of Comparative Example 2 was formed by spraying alumina particles (manufactured by Fujimi Co., Ltd., SURPREX AHP50, particle size 45 μm (manufacturer's nominal value)) from the outside of the bonding layer onto the outer peripheral end of the bonding layer, the alumina plate, and the recess surrounded by the base.
[0104] Example 14 An edge ring was produced so as to have the configuration shown in Table 2. That is, a silicone adhesive (intermediate member, bonding layer; Shin-Etsu Chemical Co., Ltd., addition curing type silicone rubber KE-8101) was applied to the surface of a ring-shaped alumina plate (first member; outer diameter 340 mm, inner diameter 300 mm, thickness 16 mm) so as to be 0.2 mm thick after application, and to the surface except for the outer periphery and inner periphery width of 10 mm of the alumina plate, and a ring-shaped aluminum plate (second member) of the same dimensions as this alumina plate was attached from the upper side of the silicone adhesive. Next, an alumina fiber bundle (plasma protection material) made of alumina fibers shown in Table 2 was inserted along the outer periphery and inner periphery of the bonding layer into the recess surrounded by the outer periphery and inner periphery ends of the silicone adhesive (bonding layer), the alumina plate, and the aluminum plate. Then, the end point of the alumina fiber bundle was bonded to a part of the overlapping alumina fiber bundle by firing using a burner. Note that the alumina fiber bundle was in contact with the bonding layer, and the alumina fiber bundle did not protrude from the outer periphery and inner periphery ends of the alumina plate and the aluminum plate. Thereafter, the substrate was left in a thermostatic chamber set at 120° C. for 2 hours to harden the silicone adhesive, thereby producing an edge ring.
[0105] (Examples 15 and 16) The edge rings of Examples 15 and 16 were fabricated in the same manner as the edge ring of Example 14 so as to have the configuration shown in Table 2. Instead of inserting alumina fiber bundles made of alumina fibers into the outer and inner peripheral ends of the bonding layer, the plasma protective material was inserted along the entire outer and inner peripheral ends of the bonding layer so that three alumina fiber bundles shown in Table 2 were lined up next to each other and the extension direction of the alumina fiber bundles was along the outer and inner peripheral sides of the bonding layer.
[0106] (Examples 17 to 22) The edge rings of Examples 17 to 22 were fabricated in the same manner as the edge ring of Example 14 so as to have the configuration shown in Table 2.
[0107] Comparative Example 3 The edge ring of Comparative Example 3 was produced in the same manner as the edge ring of Example 14 so as to have the configuration shown in Table 2. In Comparative Example 3, the silicone adhesive was applied so as to have a thickness of 3.0 mm after application, and as the plasma protective material, a fluororubber-based O-ring (AS568-279-D manufactured by NOK, wire diameter 3.5 mm, outer diameter 337 mm, inner diameter 330 mm) was used on the outer periphery of the silicone adhesive, and a fluororubber-based O-ring (AS568-278-D manufactured by NOK, wire diameter 3.5 mm, outer diameter 311 mm, inner diameter 304 mm) was used on the inner periphery, and these were inserted into the outer and inner periphery ends of the silicone adhesive (bonding layer), and into the recess surrounded by the alumina plate and the aluminum plate.
[0108] Comparative Example 4 The edge ring of Comparative Example 4 was produced in the same manner as the edge ring of Example 14 so as to have the configuration shown in Table 2. The plasma protective material of Comparative Example 4 was formed by plasma spraying alumina particles (SURPREX AHP50 manufactured by Fujimi Co., Ltd., particle size 45 μm (manufacturer's nominal value)) from the outside and inside of the bonding layer toward the inner and outer periphery ends of the bonding layer, and the recess surrounded by the alumina plate and the aluminum plate.
[0109] [Evaluation method] (Measurement of the number of cross-sectional fibers after installation) The number of fibers in a cross section after installation in the electrostatic chuck and edge ring of Examples 1 to 22 was measured under the conditions shown below. That is, the plasma protective material installed on each electrostatic chuck and edge ring was cut in the vertical direction, and the number of fibers in a cross section was measured from the obtained cross section using a microscope (Keyence Corporation, VHX-5000). (Evaluation of plasma resistance) The electrostatic chucks and edge rings of Examples 1 to 22 and Comparative Examples 1 to 4 were subjected to plasma treatment under the conditions shown below. Thereafter, the plasma protective material was removed, and the end of the silicone adhesive was observed at a magnification of 100 times using a digital microscope (Keyence VHX-6000). The evaluation of plasma resistance was as follows: "A+" if there was no change in the appearance of the silicone adhesive before and after plasma treatment; "A" if the outer or inner end surface of the silicone adhesive retreated toward the inside of the silicone adhesive by a maximum of less than 2 mm; "B" if the outer or inner end surface of the silicone adhesive retreated toward the inside of the silicone adhesive by a maximum of 2 mm or more and less than 5 mm; "C" if the silicone adhesive remained and the outer or inner end surface of the silicone adhesive retreated toward the inside of the silicone adhesive by a maximum of 5 mm or more and less than 8 mm; and "D" if the outer or inner end surface of the silicone adhesive retreated toward the inside of the silicone adhesive by 8 mm or more, or the silicone adhesive was completely lost.
[0110] Plasma processing equipment: Unity Me (Tokyo Electron Ltd.) High frequency power output: 1000W High frequency power supply frequency: 13.56MHz Bias power output: None Vacuum degree: 300mTorr Oxygen gas flow rate: 400sccm Fluorine gas flow rate: 200sccm Temperature of the mounting surface: 25℃ Plasma treatment time: 24 hours
[0111] (Durability evaluation) The electrostatic chucks and edge rings of Examples 1 to 22 and Comparative Examples 1 to 4 were subjected to durability evaluation. Specifically, a thermal cycle and a plasma treatment were performed under the following conditions, and the electrostatic chucks and edge rings were evaluated for cracking or peeling of the bonding layer and the plasma protective material. In the thermal cycle test, the electrostatic chucks and edge rings were placed in a thermostatic chamber (TCC-151W manufactured by Espec Corp.) set at 0°C, and the temperature was increased to 120°C at a heating rate of 10°C / min, and then the process of holding at 120°C for 30 minutes and decreasing to 0°C at a heating rate of 10°C / min was performed 200 cycles. Then, the electrostatic chucks and edge rings were taken out of the thermostatic chamber and placed in a plasma device, and plasma treatment was performed for 10 hours. Then, the appearances of the electrostatic chucks and edge rings were observed and evaluated. The durability of the electrostatic chuck and edge ring was evaluated as follows: "A" if neither cracking nor peeling occurred in the bonding layer nor the plasma protective material, "B" if cracking or peeling occurred only in the plasma protective material, "C" if cracking or peeling occurred only in the bonding layer, and "D" if cracking or peeling occurred in both the bonding layer and the plasma protective material. The plasma treatment conditions are shown below.
[0112] Plasma processing equipment: Unity Me (Tokyo Electron Ltd.) High frequency power output: 1000W High frequency power supply frequency: 13.56MHz Bias power output: None Vacuum degree: 300mTorr Oxygen gas flow rate: 400sccm Fluorine gas flow rate: 200sccm Temperature of the mounting surface: 25℃ Plasma treatment time: 10 hours
[0113] (Particle resistance rating 1) The electrostatic chucks of Examples 1 to 13 and Comparative Examples 1 and 2 were evaluated for particle resistance (particle generation ability). Specifically, a dummy wafer was placed on the mounting surface (holding member) of the electrostatic chuck, and the number of particles attached to the surface of the dummy wafer that had been in contact with the mounting surface after plasma processing was calculated. That is, a dummy wafer (diameter 300 mm, thickness 775 mm, material silicon) was placed on the mounting surface of the electrostatic chuck, and then the dummy wafer was placed in a plasma device and plasma processing was performed for 24 hours. Thereafter, the electrostatic chuck was removed, the dummy wafer was lifted from the mounting surface, and the number and size of particles attached to the surface that had been in contact with the mounting surface of the dummy wafer were measured using a wafer surface inspection device (WM-10 manufactured by TOPCON Corporation), and the number of particles with a diameter of 0.5 μm or more and less than 1.0 μm and the number of particles with a diameter of 1.0 μm or more were measured. The particle resistance was evaluated as follows: "A" if the total particle number was less than 1000, "B" if the particle number was 1000 or more and less than 5000, "C" if the particle number was 5000 or more and less than 10000, and "D" if the particle number was 10000 or more. The plasma treatment conditions are shown below.
[0114] Plasma processing equipment: Unity Me (Tokyo Electron Ltd.) High frequency power output: 1000W High frequency power supply frequency: 13.56MHz Bias power output: None Vacuum degree: 300mTorr Oxygen gas flow rate: 400sccm Fluorine gas flow rate: 200sccm Temperature of the mounting surface: 25℃ Plasma treatment time: 24 hours
[0115] (Particle resistance rating 2) The edge rings of Examples 14 to 22 and Comparative Examples 3 and 4 were evaluated for particle resistance. Specifically, the electrostatic chuck of Example 1 was installed on the inner periphery of the edge ring, a dummy wafer was placed on the mounting surface of the electrostatic chuck, and then plasma processing was performed. The number of particles attached to the surface of the dummy wafer that was in contact with the mounting surface was then calculated. That is, the electrostatic chuck of Example 1 was installed on the inner periphery of the edge ring, and a dummy wafer (diameter 300 mm, thickness 775 mm, material silicon) was placed on the mounting surface of the electrostatic chuck to prepare an evaluation sample. The evaluation sample was then placed in a plasma device, and plasma processing was performed for 24 hours. After the plasma processing was completed, the evaluation sample was removed, the dummy wafer was lifted from the mounting surface, and the number and size of particles attached to the surface that was in contact with the mounting surface of the dummy wafer were measured using a wafer surface inspection device (WM-10 manufactured by TOPCON Corporation), and the number of particles with a diameter of 0.5 μm or more and less than 1.0 μm and the number of particles with a diameter of 1.0 μm or more were measured. The particle resistance was evaluated as follows: "A" if the total particle number was less than 1500, "B" if the particle number was 1500 or more and less than 5500, "C" if the particle number was 5500 or more and less than 10500, and "D" if the particle number was 10500 or more. The plasma treatment conditions are shown below.
[0116] Plasma processing equipment: Unity Me (Tokyo Electron Ltd.) High frequency power output: 1000W High frequency power supply frequency: 13.56MHz Bias power output: None Vacuum degree: 300mTorr Oxygen gas flow rate: 400sccm Fluorine gas flow rate: 200sccm Temperature of the mounting surface: 25℃ Plasma treatment time: 24 hours
[0117] [Table 1]
[0118] [Table 2]
[0119] (comprehensive evaluation) As shown in Tables 1 and 2, the plasma-resistant structures (electrostatic chuck, edge ring) of the present disclosure equipped with a plasma protective material containing fiber exhibit a well-balanced combination of plasma resistance, durability, and particle resistance compared to the plasma-resistant structures of Comparative Examples 1 to 4 which do not contain fiber, and have an overall longer life.
[0120] Comparative Examples 1 and 3, which were provided with an O-ring made of fluororubber, were durable but vulnerable to plasma. In the case of twisted yarn as in the examples, multiple fibers are not bonded but entangled, so it is believed that when stress is applied, the positional relationship is changed and the stress is alleviated. In contrast, in the case of Comparative Example 3, since it has an integrated structure (bulk body), it cannot deform when the positional relationship is changed, and as a result, it is believed to have cracked. In addition, Comparative Examples 2 and 4, in which the plasma protective material is formed by plasma spraying alumina particles instead of fibers, are not only inferior in particle resistance, but are also vulnerable to thermal stress, especially in terms of durability, and the plasma protective material was cracked after evaluation.
[0121] From the results of Examples 1 to 5 and 14 to 18, it can be seen that the longer the fiber length (aspect ratio), the better the evaluation. It was also found that when the fiber length is short, not only the plasma resistance is poor, but also the particle resistance is reduced. In addition, the durability was good regardless of the fiber length.
[0122] From the results of Examples 6 to 9 and 20 to 22, it was found that if the number of twists is too large, the durability and plasma resistance are reduced. This is thought to be because the fibers are fixed, making it difficult to relieve stress, and because insufficient stress relief increases gaps between the base and the holding member and the plasma protective material. On the other hand, it was found that if the number of twists is small, the plasma resistance and particle resistance are reduced. From the above, it was suggested that the preferable number of twists (calculated per 1 meter) is 20 to 300 times. In other words, by setting the number of twists in the above range, it is possible to achieve both stress relief and particle generation suppression.
[0123] From the results of Examples 10 to 11, it was found that the plasma resistance decreased as the fiber bundle became thicker (the number of fibers in the fiber bundle increased). This is thought to be because the increased number of fibers reduces the fiber's movable area, making stress relaxation difficult, and as a result, the gaps between the base and the fiber bundle and between the holding member and the fiber bundle become larger.
[0124] In Example 12, which used SUS fiber, the plasma resistance was low. This is thought to be due to the low resilience of the material, which led to a gap occurring between the base and the holding member. The durability was good, which is thought to be due to the high stress relaxation of the fiber. In Example 13, which used carbon fiber, the durability and particle resistance were low. This is thought to be due to the high resilience of the fiber, which is easily broken by even a small amount of stress. [Explanation of symbols]
[0125] 1, 1a, 11, 21, 41 Plasma-resistant structure (electrostatic chuck, edge ring) 2, 2a, 12, 22, 42 First member (holding member, edge ring portion) 3, 13, 23, 43 Second member (base, edge ring part) 4, 14, 24a, 24b, 44 Intermediate member (joint layer) 5, 15, 25, 45, 45a, 45b Plasma protection material W Object to be held
Claims
1. A part for a plasma processing apparatus used inside a plasma processing apparatus in a semiconductor device manufacturing process, The plasma protection device includes a first member, a second member, an intermediate member disposed between the first member and the second member, and a plasma protection material including fibers; At least one of the first member and the second member has plasma resistance, the plasma protective material including the fiber is disposed on the outer surface side of the component at the end of the intermediate member; The plasma protective material containing the fiber includes a fiber structure made of fiber, The part for a plasma processing apparatus, wherein the direction in which the fibrous structure extends is along the outer periphery of the intermediate member.
2. 2. The part for a plasma processing apparatus according to claim 1, wherein the plasma protective material containing the fibers is disposed on an outer periphery of the intermediate member.
3. 2. The part for a plasma processing apparatus according to claim 1, wherein the direction in which the fibers extend is along the outer periphery of the intermediate member.
4. 2. The part for a plasma processing apparatus according to claim 1, wherein the intermediate member is a bonding layer.
5. The length of the fiber in the extending direction is longer than the outer periphery of the intermediate member, 2. The part for a plasma processing apparatus according to claim 1, wherein the fiber is wound around the outer periphery of the intermediate member.
6. a length of the fiber structure in an extending direction is longer than an outer periphery of the intermediate member; 2. The part for a plasma processing apparatus according to claim 1, wherein the fiber structure is wound around the outer periphery of the intermediate member.
7. 2. The part for a plasma processing apparatus according to claim 1, wherein the fibers are inorganic fibers.
8. The component for a plasma processing apparatus according to claim 1 , wherein the fiber structure includes at least one of a twisted yarn, a nonwoven fabric, a mesh, and a woven fabric.
9. The part for a plasma processing apparatus according to claim 1 is an electrostatic chuck, An electrostatic chuck, wherein the first member is a holding member that holds an object to be held, and the second member is a base that holds the holding member.
10. 10. The electrostatic chuck according to claim 9, wherein the outermost periphery of the holding member is located outside the outermost point of the plasma protection material.
11. 10. The electrostatic chuck according to claim 9, wherein the outermost periphery of the base is located outside the outermost point of the plasma protection material.
12. A fiber structure having fibers used in a plasma processing device part installed inside a plasma processing device in a semiconductor device manufacturing process, comprising: The fiber structure has plasma resistance, In the component including a first member, a second member, an intermediate member disposed between the first member and the second member, and the fiber structure, disposed along the outer periphery of the intermediate member, A fibrous structure for a part of a plasma processing apparatus, wherein the extending direction of the fibrous structure is along the outer periphery of the intermediate member.
13. A method for manufacturing a part for a plasma processing apparatus to be used inside a plasma processing apparatus in a semiconductor device manufacturing process, the part including a first member, a second member, an intermediate member disposed between the first member and the second member, and a fiber structure having fibers, disposing an intermediate member between the first member and the second member; and winding the fiber structure around an outer periphery of the intermediate member, The fiber structure has plasma resistance, The method for manufacturing a part for a plasma processing apparatus, wherein the direction in which the fiber structure extends is along the outer periphery of the intermediate member.
Citation Information
Patent Citations
Repairing method and repairing device of electrostatic chuck device, and electrostatic chuck device
JP2010165776A
Holding device
JP2020027914A
Holding device
JP2020047746A
Electrostatic chuck
JP2020109803A
Holding device
JP2021044303A