Thermally conductive silicone grease composition and method for producing same

The thermally conductive silicone grease composition addresses the issue of hardening in dispensers by using a two-part system with a hardened joint and uncured sections, ensuring efficient application and improved drop resistance for electronic components.

JP7576733B1Active Publication Date: 2024-10-31FUJI POLYMER INDUSTRIES CO LTD

Patent Information

Application Number
JP2024549223
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-09-08
Filing Date
2024-05-23
Publication Date
2024-10-31
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Conventional thermally conductive materials used in electronic components tend to harden within dispensers due to curing, leading to storage issues and inefficiencies in application, and they lack sufficient drop resistance.

Method used

A thermally conductive silicone grease composition comprising a first silicone grease with a curing reaction catalyst and no crosslinking agent, and a second silicone grease with a crosslinking agent but no curing reaction catalyst, joined via a joint portion that hardens after application, allowing for uncured states elsewhere, enhancing drop resistance and application flexibility.

Benefits of technology

The composition prevents hardening in the dispenser, maintains good drop resistance, and can be easily applied, adhering well to irregular surfaces while providing effective thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576733000006
    Figure 0007576733000006
  • Figure 0007576733000007
    Figure 0007576733000007
  • Figure 0007576733000008
    Figure 0007576733000008
Patent Text Reader

Abstract

The thermally conductive silicone grease composition 10 comprises a first thermally conductive silicone grease, a second thermally conductive silicone grease, and a joint therebetween, wherein the first thermally conductive silicone grease 7a, 7b contains a curing reaction catalyst but does not contain a crosslinking agent, and the second thermally conductive silicone grease 8a, 8b does not contain a curing reaction catalyst but does contain a crosslinking agent, the first and second thermally conductive silicone greases are joined via the joint on at least one opposing surface, and the joints 9a, 9b, 9c are cured, with the rest of the composition being uncured.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive silicone grease composition in which first and second thermally conductive silicone greases are joined via a bond formed by curing, and to a method for producing the same. [Background technology]

[0002] In recent years, the performance of semiconductors such as CPUs has improved remarkably, and the amount of heat generated has also increased dramatically. For this reason, heat sinks are attached to electronic components that generate heat, and thermally conductive grease is used to improve the adhesion between the heat sink and the heat source such as semiconductors. As devices become smaller, more powerful, and more highly integrated, thermally conductive grease is required to have high thermal conductivity as well as drop resistance.

[0003] Japanese Patent Application Laid-Open No. 2020-104078 proposes filling two syringes with one-liquid and two-liquid thermally conductive grease, with the discharge port serving as a mixing section, and discharging the one-liquid and two-liquid mixed together. In Japanese Patent Application No. 6674590, the present inventors have proposed a thermally conductive sheet in which a cured sheet and an uncured sheet are laminated in the planar direction. Summary of the Invention

[0004] The present invention provides a thermally conductive silicone grease composition comprising a first thermally conductive silicone grease, a second thermally conductive silicone grease, and a joint therebetween, The first thermally conductive silicone grease contains a curing reaction catalyst and does not contain a crosslinking agent, the second thermally conductive silicone grease does not contain a curing reaction catalyst and contains a crosslinking agent; the first and second thermally conductive silicone greases are joined via the joint at at least one opposing surface of the first and second thermally conductive silicone greases; The joint is hardened, In areas other than the joint, the first and second thermally conductive silicone greases are in an uncured state, forming a thermally conductive silicone grease composition. [Brief description of the drawings]

[0005] [Figure 1] FIG. 1A is a schematic plan view of a state in which first and second thermally conductive silicone greases in one embodiment of the present invention are applied alternately in a cylindrical shape from respective dispensers, and FIG. 1B is a schematic plan view of the compression molded state. [Diagram 2] FIG. 2A is a schematic plan view of a state in which first and second thermally conductive silicone greases in another embodiment of the present invention are applied in alternate dot form from respective dispensers, and FIG. 2B is a schematic plan view of the state after compression molding. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a method of using the thermally conductive sheet in one embodiment of the present invention. [Figure 4] 4A-B are schematic explanatory views showing a method for measuring the thermal conductivity of a sample in one embodiment of the present invention. [Diagram 5] 5A to 5D are schematic explanatory views illustrating a drop test used in an embodiment of the present invention. [Figure 6] FIG. 6 is a 5000x photograph of amorphous alumina (surface treated with octyltrimethoxysilane) with a D50 of 0.3 μm used in one embodiment of the present invention. [Figure 7] FIG. 7 is a 2000-fold magnification photograph of D50=2.3 μm amorphous alumina (surface treated with decyltrimethoxysilane) used in one embodiment of the present invention. [Figure 8] FIG. 8 is a 2000x photograph of amorphous aluminum nitride (without surface treatment) with D50=15 μm used in one embodiment of the present invention. [Figure 9] FIG. 9 is a 100-fold photograph of spherical alumina (without surface treatment) with D50=105 μm used in one embodiment of the present invention. [Figure 10] FIG. 10 is a photograph of spherical agglomerated boron nitride, D50=25 μm (without surface treatment), used in one embodiment of the present invention. [Figure 11] FIG. 11 is a photograph of spherical agglomerated boron nitride, D50=60 μm (without surface treatment), used in one embodiment of the present invention. Detailed Description of the Invention

[0006] However, in the above-mentioned conventional technology, a two-component curing type thermally conductive material is used in the hope of drop resistance, but since the two components are mixed in the dispenser and then applied, if application is not completed immediately after mixing, the thermally conductive material may harden in the dispenser. To avoid this, the thermally conductive material cannot be stored in the dispenser for a long time after mixing, which causes a problem of time required for cleaning the device.

[0007] In order to solve the above-mentioned problems in the conventional art, the present invention provides a thermally conductive silicone grease composition that can be applied with a dispenser, has good drop resistance, and cures after application so that curing does not progress within the dispenser, and a method for producing the same.

[0008] The thermally conductive silicone grease composition of the present invention is a thermally conductive silicone grease composition comprising a first thermally conductive silicone grease, a second thermally conductive silicone grease, and a junction therebetween, wherein the first thermally conductive silicone grease contains a curing reaction catalyst but does not contain a crosslinking agent, and the second thermally conductive silicone grease does not contain a curing reaction catalyst but does contain a crosslinking agent, the first and second thermally conductive silicone greases are joined via the junction on at least one opposing surface, the junction being cured, and the first and second thermally conductive silicone greases are in an uncured state apart from the junction.

[0009] The method for producing a thermally conductive silicone grease composition of the present invention is a method for producing the thermally conductive silicone grease composition, and includes the steps of filling a dispenser with each of the first and second thermally conductive silicone greases, discharging and applying the first and second thermally conductive silicone greases alternately from the discharge holes of the dispensers while leaving a gap of 10% to 90% of the application thickness so that the respective thermally conductive silicone greases do not come into contact with each other, and compression molding the applied first and second thermally conductive silicone greases at a compression rate of 10% to 90% of the application thickness, thereby causing an addition reaction at the contact portions of the first and second thermally conductive silicone greases to form joints, and joining the first and second thermally conductive silicone greases via these joints to produce a thermally conductive silicone grease composition.

[0010] The thermally conductive silicone grease composition of the present invention can be prepared by the steps of: filling a dispenser with the first thermally conductive silicone grease and the second thermally conductive silicone grease; a step of alternately applying and arranging the first and second thermally conductive silicone greases from the discharge holes of the dispenser, while leaving a gap of 10% to 90% of the applied thickness so that the respective thermally conductive silicone greases do not come into contact with each other; The thermal conductive silicone grease composition is manufactured by a method including a step of compressing and molding the applied first and second thermal conductive silicone greases at a compression rate of 10 to 90% of the applied thickness to cause an addition reaction at the contact portion of the first and second thermal conductive silicone greases to form joints, and bonding the first and second thermal conductive silicone greases through the joints to produce a thermal conductive silicone grease composition. That is, the joints are cured by the addition reaction, but the first and second thermal conductive silicone greases are in an uncured state except for the joints. According to this manufacturing method, the first and second thermal conductive silicone greases can be applied by a dispenser, have good drop resistance, and the first and second thermal conductive silicone greases are cured after application, so that curing does not proceed in the dispenser before application.

[0011] Furthermore, in the thermally conductive silicone grease composition of the present invention, the joints are cured by an addition reaction, and the areas other than the joints are uncured, so that while the cured areas have a high hardness, the uncured areas have a low hardness and are therefore able to deform freely and easily conform to the irregularities of the heat generating and / or heat dissipating areas. For this reason, the thermally conductive silicone grease composition of the present invention is suitable as a thermal interface material (TIM) to be placed between the heat generating parts of electric or electronic components and heat dissipating bodies.

[0012] The present invention is a thermally conductive silicone grease composition comprising a first thermally conductive silicone grease and a second thermally conductive silicone grease and a joint therebetween, the first thermally conductive silicone grease containing a curing reaction catalyst and not containing a crosslinking agent, the second thermally conductive silicone grease not containing a curing reaction catalyst and containing a crosslinking agent, the first and second thermally conductive silicone greases being joined via the joint at at least one opposing surface, the joint being cured, and the first and second thermally conductive silicone greases being in an uncured state except for the joint. The first and second thermally conductive silicone greases in an uncured state can freely deform and are easy to follow the unevenness of the heat generating part and / or heat dissipating part. In addition, since the joint is cured by an addition reaction, it has shape retention and good drop resistance. It is presumed that the good drop resistance of the thermally conductive silicone grease composition of the present invention is due to the fact that the leaching components are trapped by the cured joint.

[0013] [First and second thermally conductive silicone greases] The first and second thermally conductive silicone greases contain a matrix resin and thermally conductive particles, and the matrix resin preferably contains the following components (A) and (C), and the thermally conductive particles preferably contain the following component (B). The following compositions allow the first and second thermally conductive silicone greases to be smoothly applied by a dispenser. The first and second thermally conductive silicone greases each contain a matrix resin and thermally conductive particles, but the matrix resin of the first thermally conductive silicone grease and the matrix resin of the second thermally conductive silicone grease may be the same or different. If they are different, the type and / or content of at least one of the following components (A) and (C) contained in the first and second thermally conductive silicone greases may be different. The thermally conductive particles of the first thermally conductive silicone grease and the thermally conductive particles of the second thermally conductive silicone grease may be the same or different. When they are different, the type and / or content of the below-described component (B) contained in the first and second thermally conductive silicone greases may be different. (A) Kinematic viscosity at 40°C is 100 to 3000 mm 2 / s addition reaction curable organopolysiloxane: 100 parts by weight (B) Thermally conductive filler: 200 to 3,000 parts by mass relative to 100 parts by mass of the matrix resin (C)R a Si(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1): 0 to 10 parts by mass

[0014] <Matrix resin> Here, the matrix resin includes the curing reaction catalyst or the crosslinking agent. The matrix resin includes the components (A) and (C), and also includes the below-described component (D) (non-reactive silicone oil) when it is added.

[0015] (1) Curing reaction catalyst As the curing reaction catalyst, a catalyst used in a hydrosilylation reaction can be used. Examples of the curing reaction catalyst include platinum black, platinum (II) chloride, chloroplatinic acid, a reaction product of chloroplatinic acid with a monohydric alcohol, a complex of chloroplatinic acid with an olefin or vinylsiloxane, platinum-based catalysts such as platinum bisacetoacetate, palladium-based catalysts, and rhodium-based catalysts, and platinum-based metal catalysts are preferred. The curing reaction catalyst is preferably added in an amount of 1 to 3,500 ppm (10 to 35,000 times the effective curing amount) by weight, more preferably 5 to 2000 ppm, and even more preferably 7 to 700 ppm, based on the matrix resin.

[0016] (2) Crosslinking agent An example of the crosslinking agent is organohydrogenpolysiloxane. Organohydrogenpolysiloxane acts as a crosslinking agent, and is cured by addition reaction (hydrosilylation) between the SiH group in this component and the alkenyl group of the organopolysiloxane (component A). Such organohydrogenpolysiloxane can be used as a crosslinking agent as long as it has two or more hydrogen atoms (i.e., SiH groups) bonded to silicon atoms in one molecule. The molecular structure of this organohydrogenpolysiloxane may be any of linear, cyclic, branched, and three-dimensional network structures. In addition, organohydrogenpolysiloxanes having a number of silicon atoms (i.e., degree of polymerization) of 2 to 1000, particularly about 2 to 300, can be preferably used as a crosslinking agent.

[0017] The organohydrogenpolysiloxane contains a SiH group as described above. In the organohydrogenpolysiloxane, the position of the SiH group is not particularly limited, and may be at the end of the molecular chain or at a non-end of the molecular chain (in the middle of the molecular chain). In addition, the organic group bonded to the silicon atom other than a hydrogen atom is R in the general formula (I). 1 and the like. Examples of the substituted or unsubstituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds include those shown below.

[0018] An example of the organohydrogenpolysiloxane is represented by the following formula (I).

[0019] [ka]

[0020] In the above formula (I), R 6 may be the same or different and are hydrogen, an alkyl group, a phenyl group, an epoxy group, an acryloyl group, a methacryloyl group, or an alkoxy group, and at least two of them are hydrogen. L is an integer from 0 to 1,000, particularly an integer from 0 to 300; M is an integer from 1 to 200.

[0021] (3) Organopolysiloxane (component (A)) Organopolysiloxane is a main component (base polymer component) in a matrix resin, and contains, for example, two or more alkenyl groups bonded to silicon atoms in one molecule. This organopolysiloxane has, as the alkenyl group, two alkenyl groups bonded to silicon atoms, such as vinyl groups and allyl groups, having 2 to 8 carbon atoms, particularly 2 to 6 carbon atoms, in one molecule. From the viewpoint of workability, curability, etc., it is desirable that the viscosity of the organopolysiloxane is 10 to 1,000,000 mPa·s, particularly 100 to 100,000 mPa·s, and more preferably 100 to 3,000 mPa·s at 25°C. The kinetic viscosity of the organopolysiloxane at 40°C is 100 to 3,000 mm 2 / s, preferably 100 to 2,000 mm 2 / s, more preferably 100 to 1,000 mm 2 / s.

[0022] Specifically, a linear organopolysiloxane containing an average of two or more alkenyl groups per molecule, bonded to silicon atoms at the molecular chain ends, represented by the following general formula (II) can be used. From the viewpoints of workability, curability, etc., a viscosity of 10 to 1,000,000 mPa·s at 25°C is desirable. Note that this linear organopolysiloxane may contain a small amount of a branched structure (trifunctional siloxane unit) in the molecular chain.

[0023] [ka]

[0024] In formula (II), R 1 are the same or different unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds, R 2 is an alkenyl group, k is 0 or a positive integer.

[0025] Here, in the general formula (II), R 1 The unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond is preferably, for example, one having 1 to 10 carbon atoms, particularly preferably 1 to 6 carbon atoms. Specific examples of the unsubstituted monovalent hydrocarbon group having no aliphatic unsaturated bond include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups, aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups, and aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups. Examples of the substituted monovalent hydrocarbon group having no aliphatic unsaturated bond include those in which some or all of the hydrogen atoms of the unsubstituted monovalent hydrocarbon group are substituted with halogen atoms such as fluorine, bromine, and chlorine, or cyano groups, for example, halogen-substituted alkyl groups such as chloromethyl, chloropropyl, bromoethyl, and trifluoropropyl groups, and cyanoethyl groups.

[0026] In the general formula (II), R 2 The alkenyl group preferably has, for example, 2 to 6 carbon atoms, particularly 2 to 3 carbon atoms. Specific examples include vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, hexenyl, and cyclohexenyl groups, with vinyl being preferred.

[0027] In general formula (II), k is 0 or a positive integer, for example, 0 or a positive integer satisfying 0≦k≦10000, preferably 5≦k≦2000, more preferably 10≦k≦1200.

[0028] The organopolysiloxane may be used in combination with an organopolysiloxane having, in one molecule, at least three, usually about 3 to 30, and preferably about 3 to 20 alkenyl groups, such as vinyl groups and allyl groups, bonded to silicon atoms having 2 to 8 carbon atoms, particularly 2 to 6 carbon atoms. The molecular structure may be any of linear, cyclic, branched, and three-dimensional network molecular structures. A preferred example is a linear organopolysiloxane whose main chain is made of repeated diorganosiloxane units and whose both molecular chain terminals are blocked with triorganosiloxy groups, and whose viscosity at 25°C is 10 to 1,000,000 mPa·s, particularly 100 to 100,000 mPa·s.

[0029] In organopolysiloxanes containing two or more alkenyl groups bonded to silicon atoms in one molecule, the alkenyl groups may be bonded to any part of the molecule. For example, they may be bonded to silicon atoms at the molecular chain terminals or non-terminals (in the middle of the molecular chain). Among them, linear organopolysiloxanes represented by the following general formula (III) having 1 to 3 alkenyl groups on each of the silicon atoms at both molecular chain terminals and having a viscosity of 10 to 1,000,000 mPa·s at 25°C are desirable in terms of workability, curability, etc. However, when the number of alkenyl groups bonded to silicon atoms at the molecular chain terminals of this linear organopolysiloxane is less than 3 in total at both terminals, linear organopolysiloxanes having at least one alkenyl group bonded to a silicon atom at a non-terminal (in the middle of the molecular chain) of the molecular chain (for example, as a substituent in a diorganosiloxane unit) are preferred. As mentioned above, such linear organopolysiloxanes preferably have a viscosity of 10 to 1,000,000 mPa s at 25°C in terms of workability, curing properties, etc. The linear organopolysiloxanes may contain a small amount of branched structures (trifunctional siloxane units) in the molecular chain.

[0030] [ka]

[0031] In formula (III), R 3 may be the same or different and are unsubstituted or substituted monovalent hydrocarbon groups, with at least one being an alkenyl group. R 4 may be the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds, R 5 is an alkenyl group, l and m are each independently 0 or a positive integer.

[0032] In the general formula (III), R 3The unsubstituted or substituted monovalent hydrocarbon group preferably has 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms. Specific examples of the unsubstituted monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups; and alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl groups. Examples of the substituted monovalent hydrocarbon group include those in which some or all of the hydrogen atoms of the unsubstituted monovalent hydrocarbon group have been substituted with halogen atoms such as fluorine, bromine, chlorine, etc.; or with a cyano group, etc., such as halogen-substituted alkyl groups such as a chloromethyl group, a chloropropyl group, a bromoethyl group, or a trifluoropropyl group; and a cyanoethyl group.

[0033] In addition, in the general formula (III), R 4 As the unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond, those having 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms, are preferred. 4 The unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond is preferably the above-mentioned R 1 Specific examples of the unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond are the same as those of the substituted or unsubstituted monovalent hydrocarbon group having no aliphatic unsaturated bond, except that alkenyl groups are not included.

[0034] In the general formula (III), R 5 The alkenyl group in the formula (1) is preferably an alkenyl group having 2 to 6 carbon atoms, particularly preferably an alkenyl group having 2 to 3 carbon atoms. 2 The preferred is a vinyl group.

[0035] In general formula (III), l and m are 0 or positive integers, for example, 0 or positive integers satisfying 0 < l + m ≤ 10000, preferably 5 ≤ l + m ≤ 2000, more preferably 10 ≤ l + m ≤ 1200, and are integers satisfying 0 < l / (l + m) ≤ 0.2, preferably 0.0011 ≤ l / (l + m) ≤ 0.1.

[0036] (4) R a Si(OR') 4-a alkoxysilane ((C) component) In the formula of the (C) component, R a Si(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1) alkoxysilane functions as a viscosity modifier. By including the (C) component, the thermal conductive silicone grease has better dischargeability, which is preferable.

[0037] (C) In the formula of the component, R a Si(OR’) 4-a (R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R’ is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1) alkoxysilane includes, for example, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, etc. The alkoxysilane can be used alone or in combination of two or more. As the surface treatment agent, the alkoxysilane and a mono-terminal silanol siloxane may be used in combination.

[0038] (5) Non-reactive silicone oil ((D) component) The matrix resin of the first and second thermally conductive silicone greases may further contain 1 to 50 mass % of (D) non-reactive silicone oil in the component (A). This allows smooth application using a dispenser. The (D) non-reactive silicone oils contained in the matrix resins of the first and second thermally conductive silicone greases may be the same or different. If different, the type and / or content of the (D) component contained in the first and second thermally conductive silicone greases may be different.

[0039] The non-reactive silicone oil has a kinetic viscosity of, for example, 50 to 3,000 mm at 25°C. 2 / s, preferably 70 to 2,500 mm 2 / s. Viscosity is measured using a Brooklyn Field type rotational viscometer SP No.2. If the kinetic viscosity is within the above range, oil bleeding is suppressed to a low level and the filling property of the thermally conductive particles is also good. The non-reactive silicone oil is a silicone polymer that does not have a reactive group, and examples of the non-reactive silicone oil include dimethylpolysiloxane and diphenylpolysiloxane.

[0040] <Thermal conductive particles> The thermally conductive particles are preferably added in an amount of 200 to 3,000 parts by mass per 100 parts by mass of the matrix resin. This allows the thermal conductivity of the thermally conductive silicone grease composition to be maintained at a high level. The material of the thermally conductive particles is preferably at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, quartz, and silica, and more preferably at least one selected from the group consisting of aluminum nitride, boron nitride, and alumina. Various shapes such as spherical, scaly, and polyhedral shapes can be used. When alumina is used, α-alumina with a purity of 99.5% by weight or more is preferred. The specific surface area of ​​the thermally conductive particles is 0.06 to 10 m 2 / g is preferable. The specific surface area is a BET specific surface area, and the measurement method is in accordance with JIS R1626. The average particle size of the thermally conductive particles is preferably in the range of 0.1 to 100 μm. The particle size is measured by measuring the median size using a laser diffraction light scattering method. An example of the measuring device is the LA-950S2 laser diffraction / scattering type particle distribution measuring device manufactured by Horiba, Ltd.

[0041] At least two thermally conductive particles with different average particle sizes may be used in combination, because in this case, the thermally conductive particles with smaller particle sizes are filled between the larger particles, allowing for a state of nearly closest packing, thereby increasing the thermal conductivity.

[0042] The thermally conductive particles have the formula R a Si(OR') 4-a (R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1), or a partial hydrolyzate thereof. a Si(OR') 4-a Examples of alkoxysilanes represented by the formula (R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1) include octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane. The alkoxysilanes may be used alone or in combination of two or more. As a surface treatment agent, the alkoxysilanes may be used in combination with one-terminated silanol siloxane. The surface treatment here includes adsorption as well as covalent bonding. The surface treatment is preferably performed on thermally conductive particles having an average particle size D of 10 μm or less. Thermally conductive particles having D of 10 μm or less have a high specific surface area and are prone to adsorb platinum catalysts, which can cause curing inhibition, but this can be prevented by surface treatment.

[0043] The thermally conductive particles include a thermally conductive filler (component (B)). (1) Thermally conductive filler (component (B)) The thermally conductive filler may be an electrically conductive filler, an electrically insulating filler, or the like, and any of these may be used. The electrically conductive filler may be a carbon powder such as carbon black or a metal powder. In the case of a metal powder, a metal powder having a surface resistance of 1Ω / □ or less is preferable, specifically, a powder of metals such as gold, silver, platinum, copper, nickel, iron, palladium, cobalt, chromium, aluminum, or an alloy such as stainless steel, or a metal powder whose surface is coated with a precious metal such as gold or silver to reduce the electrical resistance is preferable. As the electrically insulating filler, a filler of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, quartz, or silica is preferable, and at least one selected from the group consisting of aluminum nitride, boron nitride, and alumina is more preferable. The thermally conductive filler may have various shapes such as a spherical shape, a scaly shape, a polyhedral shape, or the like. When alumina is used as the thermally conductive filler, α-alumina having a purity of 99.5% by weight or more is preferable. The specific surface area of ​​the thermally conductive filler is 0.06 to 10 m 2 / g is preferable. The specific surface area is a BET specific surface area, and the measurement method is in accordance with JIS R1626. The average particle size of the thermally conductive filler is preferably in the range of 0.1 to 100 μm. The average particle size is the D50 (median size) of the cumulative particle size distribution based on volume in particle size distribution measurement by laser diffraction light scattering method. An example of this measurement device is the laser diffraction / scattering type particle distribution measurement device LA-950S2 manufactured by Horiba, Ltd.

[0044] The thermally conductive filler may be a mixture of fillers having different particle sizes. Specifically, the following two types of filler mixtures can be exemplified:

[0045] (i) Filler mixture 1 The thermally conductive filler (B) preferably includes a thermally conductive filler (B1) having a median particle size (D50) of 0.01 to 10 μm, a thermally conductive filler (B2) having a median particle size (D50) of more than 10 μm and not more than 80 μm, and a thermally conductive filler (B3) having a median particle size (D50) of more than 80 μm and not more than 150 μm. By using the thermally conductive filler (B) having such a configuration, the thermally conductive filler (B) can be filled in the thermally conductive silicone grease composition in a state close to closest packing, and as a result, the thermal conductivity of the thermally conductive silicone grease composition can be increased. The median particle size is the D50 (median diameter) of the cumulative particle size distribution based on volume measured by a laser diffraction light scattering method. An example of the measuring device is the LA-950S2 laser diffraction / scattering type particle size distribution measuring device manufactured by Horiba, Ltd.

[0046] The thermally conductive filler (B1) is preferably amorphous alumina. This is because alumina is inexpensive. The thermally conductive filler (B2) is preferably at least one thermally conductive filler selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, and silicon carbide. The shape of the thermally conductive filler (B2) is preferably amorphous. The thermally conductive filler (B3) is preferably spherical alumina. When the proportion of spherical alumina added as the thermally conductive filler (B3) is high, the thermal conductivity of the thermally conductive silicone grease composition can be increased and the cost can be reduced. In addition, when alumina is used as the thermally conductive filler (B), it is preferable to use a combination of so-called submicron particles (B1-1) having a D50 (median diameter) of 0.01 μm or more and less than 1 μm, small particles (B1-2) having a D50 (median diameter) of 1 μm or more and 10 μm or less, and large particles (B3) having a D50 of more than 80 μm and 150 μm or less. By using a thermally conductive filler (B) having such a configuration, the thermally conductive filler (B) can be closely packed in the thermally conductive silicone grease composition, and as a result, the thermal conductivity of the thermally conductive silicone grease composition can be increased. In addition, amorphous alumina is produced by pulverization or crushing, and commercially available products can be used. These thermally conductive fillers (B1), (B2) and (B3) have high thermal conductivity.

[0047] The mass ratios of the thermally conductive fillers (B1), (B2), and (B3) preferably satisfy the relationship (B2)≦(B1)≦(B3), because by satisfying this ratio, the thermally conductive fillers can be packed in a state close to closest packing within the thermally conductive silicone grease composition, thereby enabling the thermal conductivity of the thermally conductive silicone grease composition to be increased.

[0048] The thermally conductive filler (B) preferably contains 100 to 1,000 parts by mass of the thermally conductive filler (B1), more preferably 150 to 1,000 parts by mass, and even more preferably 300 to 850 parts by mass, relative to 100 parts by mass of the matrix resin. The thermally conductive filler (B) preferably contains 100 to 500 parts by mass of the thermally conductive filler (B2), more preferably 150 to 500 parts by mass, and even more preferably 200 to 450 parts by mass, relative to 100 parts by mass of the matrix resin. The thermally conductive filler (B) preferably contains 300 to 1,400 parts by mass of the thermally conductive filler (B3), more preferably 300 to 1,300 parts by mass, and even more preferably 500 to 1,200 parts by mass, relative to 100 parts by mass of the matrix resin. This makes it possible to obtain a thermally conductive silicone grease composition that has high thermal conductivity, is relatively resistant to dripping, and has good dischargeability. For the same reason, the thermally conductive filler (B) preferably contains 100 to 1,000 parts by mass of the thermally conductive filler (B1), 100 to 500 parts by mass of the thermally conductive filler (B2), and 300 to 1,400 parts by mass of the thermally conductive filler (B3) relative to 100 parts by mass of the matrix resin, more preferably contains 150 to 1,000 parts by mass of the thermally conductive filler (B1), 150 to 500 parts by mass of the thermally conductive filler (B2), and 300 to 1,300 parts by mass of the thermally conductive filler (B3), and further preferably contains 300 to 850 parts by mass of the thermally conductive filler (B1), 200 to 450 parts by mass of the thermally conductive filler (B2), and 500 to 1,200 parts by mass of the thermally conductive filler (B3).

[0049] The thermally conductive filler (B1) having a median particle diameter (D50) of 0.01 to 10 μm, the thermally conductive filler (B2) having a median particle diameter (D50) of more than 10 μm and not more than 80 μm, and the thermally conductive filler (B3) having a median particle diameter (D50) of more than 80 μm and not more than 150 μm may each contain two or more types of thermally conductive fillers having different median particle diameters (D50). By using a thermally conductive filler (B) having such a configuration, the thermally conductive filler (B) can be closely packed in the thermally conductive silicone grease composition, and as a result, the thermal conductivity of the thermally conductive silicone grease composition can be increased. For example, it is preferable that the thermally conductive filler (B1) contains two or more types of thermally conductive fillers having different median particle diameters (D50). Specifically, the thermally conductive filler (B1) preferably includes a thermally conductive filler (B1-1) having a median particle size (D50) of 0.01 μm or more and less than 1 μm and a thermally conductive filler (B1-2) having a median particle size (D50) of 1 μm or more and 10 μm or less, more preferably includes a thermally conductive filler (B1-1) having a median particle size (D50) of 0.05 μm or more and less than 1 μm and a thermally conductive filler (B1-2) having a median particle size (D50) of 1 μm or more and 8 μm or less, and even more preferably includes a thermally conductive filler (B1-1) having a median particle size (D50) of 0.1 μm or more and less than 1 μm and a thermally conductive filler (B1-2) having a median particle size (D50) of 1 μm or more and 5 μm or less. By using a thermally conductive filler (B) with such a configuration, the thermally conductive filler (B) can be closely packed within the thermally conductive silicone grease composition, and as a result, the thermal conductivity of the thermally conductive silicone grease composition can be increased. When the thermally conductive filler (B1) contains the thermally conductive filler (B1-1) and the thermally conductive filler (B1-2), the thermally conductive inorganic particles (B1) preferably contain 50 to 400 parts by mass of the thermally conductive filler (B1-1) and 50 to 600 parts by mass of the thermally conductive filler (B1-2) relative to 100 parts by mass of the matrix resin, more preferably contain 50 to 400 parts by mass of the thermally conductive filler (B1-1) and 100 to 600 parts by mass of the thermally conductive filler (B1-2), and even more preferably contain 100 to 350 parts by mass of the thermally conductive filler (B1-1) and 200 to 500 parts by mass of the thermally conductive filler (B1-2).By using a thermally conductive filler (B) with such a configuration, the thermally conductive filler (B) can be closely packed within the thermally conductive silicone grease composition, and as a result, the thermal conductivity of the thermally conductive silicone grease composition can be increased.

[0050] A part or all of the thermally conductive filler (B1) having a median particle size (D50) of 0.01 to 10 μm is represented by the formula R a Si(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1). Surface treatment in advance means pretreating before mixing. By surface treating the thermally conductive filler (B1) in advance, it becomes easier to fill the thermally conductive filler (B1) into the matrix resin, and it is effective in preventing the thermally conductive filler (B1) from adsorbing a curing reaction catalyst (e.g., a platinum-based catalyst) and preventing curing inhibition. This is useful for storage stability. In particular, small particles having a D50 (median diameter) of 10 μm or less tend to adsorb a curing reaction catalyst, so it is preferable to surface treat a thermally conductive filler having a D50 (median diameter) of 10 μm or less. The surface treatment here includes adsorption as well as covalent bonding. The surface-treated thermally conductive filler (B1) has good mixability with the matrix resin. The non-reactive silicone oil is preferably added in an amount of 0.01 to 10 parts by mass relative to 100 parts by mass of the thermally conductive filler.

[0051] The content of the filler mixture 1 is 400 to 3000 parts by mass, preferably 500 to 2900 parts by mass, and more preferably 600 to 2800 parts by mass, relative to 100 parts by mass of the matrix resin.

[0052] (ii) Filler mixture 2 The thermally conductive filler (B) preferably comprises spherically agglomerated boron nitride particles. The spherical agglomerated boron nitride particles include spherical agglomerated boron nitride particles (B4) having a median particle diameter D50 of 10 μm or more and 30 μm or less, and spherical agglomerated boron nitride particles (B5) having a median particle diameter D50 that is at least twice that of B1 and is more than 30 μm and 100 μm or less. The ratio of the amount of the spherical agglomerated boron nitride particles (B5) to the amount of the spherical agglomerated boron nitride particles (B4) (B5 / B4, mass ratio) is 1.00 to 6.00. The ratio of the amounts (B5 / B4, mass ratio) is preferably 1.20 to 5.50, more preferably 1.40 to 5.50, and even more preferably 1.60 to 5.40.

[0053] An example of the spherical agglomerated boron nitride particles (B4) that can be used is product name "PTX25" manufactured by Momentive Corp., and an example of the spherical agglomerated boron nitride particles (B5) that can be used is product name "PTX60" manufactured by Momentive Corp. Catalogs for "PTX25" and "PTX60" are available on the Internet at the following URL: https: / / www.tomo-e.co.jp / upload / newsJA / 29SVF8R-newsJA#content-012.pdf.

[0054] The content of the filler mixture 2 is 10 to 300 parts by mass, preferably 50 to 250 parts by mass, and more preferably 60 to 200 parts by mass, relative to 100 parts by mass of the matrix resin.

[0055] <Other ingredients> The heat conductive silicone grease composition of the present invention can be blended with other components as necessary.The heat conductive silicone grease composition may contain, for example, heat resistance improvers such as red iron oxide, titanium oxide, and cerium oxide, flame retardant assistants, and alkyltrialkoxysilanes for the purpose of surface treatment of fillers.The heat conductive silicone grease composition may contain alkoxy group-containing silicones as materials added for the purpose of surface treatment of fillers.The heat conductive silicone grease composition may contain adhesion promoters such as silane coupling agents.The heat conductive silicone grease composition may contain organic or inorganic pigments for the purpose of coloring and color matching.

[0056] At least one of the first and second thermally conductive silicone greases has a thermal conductivity of preferably 2.0 W / m K or more, more preferably 3.0 W / m K or more, and even more preferably 4.0 W / m K or more. The upper limit is 20.0 W / m K or less.

[0057] The first and second thermally conductive silicone greases each preferably have an absolute viscosity in the range of 1,000 to 20,000 Pa·s, more preferably 1,500 to 18,000 Pa·s, and even more preferably 2,000 to 15,000 Pa·s, as measured by a Brookfield viscometer at 23° C. If the absolute viscosity is within this range, the thermally conductive silicone grease can be smoothly applied using a dispenser.

[0058] The first and second thermally conductive silicone greases are preferably each filled into a 30 mL syringe, and discharged in an amount of 2 to 10 g when discharged for 9 seconds with a discharge hole diameter of 2.5 mm and a discharge pressure of 0.5 MPa, allowing smooth application by a dispenser.

[0059] [Joint part] The first and second thermally conductive silicone greases are joined via the joints on at least one of the opposing surfaces. The joints are formed by the first and second thermally conductive silicone greases coming into contact with each other, causing an addition reaction between the curing reaction catalyst of the first thermally conductive silicone grease and the crosslinking agent of the second thermally conductive silicone grease to harden. When the first and second thermally conductive silicone greases come into contact in the thickness direction, the curing reaction catalyst contained in the first thermally conductive silicone grease penetrates and then diffuses into the uncured second thermally conductive silicone grease, causing an addition reaction between the curing reaction catalyst and the crosslinking agent to harden it. The first and second thermally conductive silicone greases are joined via the joints formed by this hardening. The first and second thermally conductive silicone greases are in an uncured state except for the joints.

[0060] [Thermal conductive silicone grease composition] The thermally conductive silicone grease composition of the present invention will now be described with reference to the accompanying drawings, in which like reference numerals denote like parts. 1A and 1B are schematic plan views of a heat conductive silicone grease composition according to an embodiment of the present invention. In FIG. 1A, the first heat conductive silicone grease 2a, 2b and the second heat conductive silicone grease 3a, 3b are alternately discharged from the respective dispensers in a cylindrical shape and applied to form a cylindrical array 1. In FIG. 1B, the cylindrical array 1 is compression molded to form a molded body 4. In FIG. 1B, the first heat conductive silicone grease 2a, 2b and the second heat conductive silicone grease 3a, 3b come into contact with each other, causing an addition reaction and curing to form joints 5a, 5b, 5c, and the other first heat conductive silicone greases 2a, 2b and the second heat conductive silicone greases 3a, 3b are in an uncured state.

[0061] 2A and 2B are schematic plan views of a heat conductive silicone grease composition in another embodiment of the present invention. In FIG. 2A, the first heat conductive silicone grease 7a, 7b and the second heat conductive silicone grease 8a, 8b are alternately discharged from the respective dispensers in a dot shape and applied to form a dot array 6. In FIG. 2B, the dot array 6 is compression molded to form a molded body 10. In FIG. 2B, the first heat conductive silicone grease 7a, 7b and the second heat conductive silicone grease 8a, 8b come into contact with each other, causing an addition reaction and curing to form joints 9a, 9b, 9c, and the other first heat conductive silicone grease 7a, 7b and second heat conductive silicone grease 8a, 8b are in an uncured state.

[0062] The heat conductive silicone grease composition is placed between two plates in an amount of 1.0 g, compressed to a thickness of 1.0 mm, and the two plates are vertically held and placed in a heat shock tester, and held at -40°C and 125°C for 30 minutes each, and in a heat shock test in which 500 cycles are allowed to pass, it is preferable that the heat conductive silicone grease composition falls within 5 mm. This allows the drop resistance of the heat conductive silicone grease composition to be well maintained. If the drop resistance of the heat conductive silicone grease composition is high, it is preferable that the composition does not seep out, and contamination of the surroundings can be prevented after being incorporated into a heat generating component.

[0063] [Method of producing thermally conductive silicone grease composition] The method for producing the thermally conductive silicone grease composition of the present invention includes the steps of filling a dispenser with the first thermally conductive silicone grease and the second thermally conductive silicone grease, alternately discharging and applying the first and second thermally conductive silicone greases from the discharge holes of the dispensers while leaving a gap of 10% to 90% of the application thickness so that the respective thermally conductive silicone greases do not come into contact, and compression molding the applied first and second thermally conductive silicone greases at a compression rate of 10% to 90% of the application thickness, thereby causing an addition reaction at the contact points between the first and second thermally conductive silicone greases to form joints, and joining the first and second thermally conductive silicone greases via these joints to produce the thermally conductive silicone grease composition. For example, when the gap is 10% of the coating thickness, the first and second thermally conductive silicone greases are compression molded at a compression rate of 10%, and when the gap is 90% of the coating thickness, the first and second thermally conductive silicone greases are compression molded at a compression rate of 90%. This makes it possible to obtain a thermally conductive silicone grease composition without voids.

[0064] In the coating step of the manufacturing method, the coating step may be performed by alternately discharging the first and second thermally conductive silicone greases in a cylindrical shape, or may be performed by alternately discharging the first and second thermally conductive silicone greases in a dot shape. The manufacturing method may be performed when mounting the thermally conductive silicone grease composition on a heat-generating component. In the case of a cylindrical shape, the diameter of the cylinder is preferably 0.5 to 3.0 mm and the length of the cylinder is preferably 50 to 1000 mm. In the case of a dot shape, the dot is preferably 0.5 to 30 mm in diameter. The thermally conductive silicone grease composition in the above range is convenient for incorporating into a heat-generating electric or electronic component. The thermally conductive silicone grease composition may be a thermally conductive sheet formed into a sheet shape. The thickness of the thermally conductive sheet is preferably 0.1 to 5 mm.

[0065] The compression molding in the above-mentioned manufacturing method is preferably carried out at a temperature in the range of 80 to 150° C. for a period of 5 to 60 minutes. If it is within this range, the efficiency of mounting the thermally conductive silicone grease composition can be improved.

[0066] [Thermal conductive sheet] The present invention relates to a thermally conductive sheet in which the thermally conductive silicone grease composition of the present invention is formed into a sheet. 3 is a schematic cross-sectional view of a heat dissipation structure 16 incorporating a heat conductive sheet according to an embodiment of the present invention. The heat conductive sheet 11b dissipates heat generated by an electronic component 13 such as a semiconductor element, and is fixed to a main surface 12a of the heat spreader 12 facing the electronic component 13, and is sandwiched between the electronic component 13 and the heat spreader 12. The heat conductive sheet 11a is sandwiched between the heat spreader 12 and a heat sink 15. The heat conductive sheets 11a and 11b, together with the heat spreader 12, constitute a heat dissipation member that dissipates heat from the electronic component 13. The heat spreader 12 is formed, for example, in a rectangular plate shape, and has a main surface 12a facing the electronic component 13 and a side wall 12b erected along the outer periphery of the main surface 12a. The heat spreader 12 has a thermally conductive sheet 11b provided on a main surface 12a surrounded by side walls 12b, and a heat sink 15 provided on another surface 12c opposite to the main surface 12a via the thermally conductive sheet 11a. The electronic component 13 is, for example, a semiconductor element such as a BGA, and is mounted on a wiring board 14.

[0067] In one embodiment, the present invention is a method for producing a thermally conductive sheet, which comprises forming the thermally conductive silicone grease composition of the present invention into a sheet and then curing the composition. The thermally conductive silicone grease composition of the present invention is suitable as a thermal interface material (TIM (Thermal Interface Material)) when formed into a sheet and cured. The sheet forming method may be a rolling method or a press molding method (mold clamping method). The sheet forming is preferably performed by sandwiching the compound thermally conductive silicone grease composition between polyethylene terephthalate (PET) films and rolling the composition, and the curing is preferably performed by heating at 80 to 150°C for 10 to 120 minutes.

[0068] In one aspect, the present invention relates to use of the thermally conductive sheet of the present invention, in which the thermally conductive sheet of the present invention is interposed between a heat generating body and a heat dissipating body. Examples of the heat generating body include electronic components such as semiconductor elements or electric components, and examples of the heat dissipating body include a heat spreader and a heat sink.

[0069] The present invention includes the following aspects.

[0070] [Item 1] A thermally conductive silicone grease composition comprising a first thermally conductive silicone grease, a second thermally conductive silicone grease, and a joint therebetween, The first thermally conductive silicone grease contains a curing reaction catalyst and does not contain a crosslinking agent, the second thermally conductive silicone grease does not contain a curing reaction catalyst and contains a crosslinking agent; the first and second thermally conductive silicone greases are joined via the joint at at least one opposing surface of the first and second thermally conductive silicone greases; The joint is hardened, a thermally conductive silicone grease composition, wherein the first and second thermally conductive silicone greases are in an uncured state except at the joint portion.

[0071] [Item 2] The thermally conductive silicone grease composition according to Item 1, wherein the curing reaction catalyst is a catalyst used in a hydrosilylation reaction.

[0072] [Item 3] The thermally conductive silicone grease composition according to Item 1 or 2, wherein the curing reaction catalyst is a platinum-based catalyst such as platinum black, platinic chloride, chloroplatinic acid, a reaction product of chloroplatinic acid with a monohydric alcohol, a complex of chloroplatinic acid with an olefin or a vinylsiloxane, platinum bisacetoacetate, or another platinum group metal catalyst such as a palladium-based catalyst or a rhodium-based catalyst, and preferably a platinum-based metal catalyst.

[0073] [Item 4] The thermally conductive silicone grease composition according to any one of Items 1 to 3, wherein the crosslinking agent is an organohydrogenpolysiloxane.

[0074] [Item 5] The thermally conductive silicone grease composition according to Item 4, wherein the organohydrogenpolysiloxane has two or more hydrogen atoms bonded to silicon atoms (i.e., SiH groups) in one molecule.

[0075] [Item 6] The thermally conductive silicone grease composition according to any one of Items 1 to 5, wherein the first and second thermally conductive silicone greases contain a matrix resin and thermally conductive particles.

[0076] [Item 7] The thermally conductive silicone grease composition according to Item 6, wherein the matrix resin contains the following components (A) and (C): (A) Kinematic viscosity at 40°C is 100 to 3000 mm 2 / s addition reaction curable organopolysiloxane: 100 parts by weight (C)R a Si(OR') 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1): 0 to 10 parts by mass

[0077] [Item 8] The thermally conductive silicone grease composition according to Item 7, wherein the organopolysiloxane has, per molecule, two alkenyl groups bonded to silicon atoms, the alkenyl groups being vinyl groups, allyl groups or the like and having 2 to 8, and particularly 2 to 6, carbon atoms.

[0078] [Item 9] The thermally conductive silicone grease composition according to Item 7 or 8, wherein the alkoxysilane is one or more selected from the group consisting of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, and dodecyltriethoxysilane.

[0079] [Item 10] The matrix resin of the first and second thermally conductive silicone greases further comprises (D) The thermally conductive silicone grease composition according to any one of items 7 to 9, wherein the component (A) contains 1 to 50 mass % of a non-reactive silicone oil.

[0080] [Item 11] The non-reactive silicone oil has a kinetic viscosity at 25°C of, for example, 50 to 3,000 mm 2 / s, preferably 70 to 2,500 mm 2Item 11. The thermally conductive silicone grease composition according to item 10, wherein the R 1 / s.

[0081] [Item 12] The thermally conductive silicone grease composition according to Item 10 or 11, wherein the non-reactive silicone oil is dimethylpolysiloxane and / or diphenylpolysiloxane.

[0082] [Item 13] The thermally conductive particles contain the following component (B): Item 13. The thermally conductive silicone grease composition according to any one of items 6 to 12. (B) Thermally conductive filler: 200 to 3,000 parts by mass relative to 100 parts by mass of the matrix resin

[0083] [Item 14] The thermally conductive silicone grease composition according to any one of Items 6 to 13, wherein the material of the thermally conductive particles is preferably at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, quartz, and silica, and more preferably at least one selected from the group consisting of aluminum nitride, boron nitride, and alumina.

[0084] [Item 15] The thermally conductive silicone grease composition according to Item 13 or 14, wherein the thermally conductive filler (B) comprises a thermally conductive filler (B1) having a median particle size (D50) of 0.01 to 10 μm, a thermally conductive filler (B2) having a median particle size (D50) of more than 10 μm and not more than 80 μm, and a thermally conductive filler (B3) having a median particle size (D50) of more than 80 μm and not more than 150 μm.

[0085] [Item 16] The thermally conductive silicone grease composition according to Item 15, wherein the thermally conductive filler (B) contains preferably 100 to 1,000 parts by mass, more preferably 150 to 1,000 parts by mass, and even more preferably 300 to 850 parts by mass of the thermally conductive filler (B1) per 100 parts by mass of the matrix resin; the thermally conductive filler (B) contains preferably 100 to 500 parts by mass, more preferably 150 to 500 parts by mass, and even more preferably 200 to 450 parts by mass of the thermally conductive filler (B2) per 100 parts by mass of the matrix resin; and the thermally conductive filler (B) contains preferably 300 to 1,400 parts by mass, more preferably 300 to 1,300 parts by mass, and even more preferably 500 to 1,200 parts by mass of the thermally conductive filler (B3) per 100 parts by mass of the matrix resin.

[0086] [Item 17] The thermally conductive silicone grease composition according to Item 13, wherein the thermally conductive filler (B) comprises spherical agglomerated boron nitride particles.

[0087] [Item 18] The thermally conductive silicone grease composition according to Item 17, wherein the spherical agglomerated boron nitride particles include spherical agglomerated boron nitride particles (B4) having a median particle diameter D50 of 10 μm or more and 30 μm or less, and spherical agglomerated boron nitride particles (B5) having a median particle diameter D50 that is at least twice that of B1 and exceeds 30 μm and is 100 μm or less.

[0088] [Item 19] The thermally conductive silicone grease composition according to any one of Items 1 to 18, wherein at least one of the first and second thermally conductive silicone greases has a thermal conductivity of preferably 2.0 W / m K or more, more preferably 3.0 W / m K or more, even more preferably 4.0 W / m K or more, and preferably 20.0 W / m K or less.

[0089] [Item 20] The thermally conductive silicone grease composition according to any one of Items 1 to 19, wherein the first and second thermally conductive silicone greases each have an absolute viscosity at 23°C as measured using a Brookfield viscometer in the range of preferably 1,000 to 20,000 Pa s, more preferably 1,500 to 18,000 Pa s, and even more preferably 2,000 to 15,000 Pa s.

[0090] [Item 21] The thermally conductive silicone grease composition according to any one of Items 1 to 20, wherein the first and second thermally conductive silicone greases are each filled into a 30 mL syringe and discharged in an amount of 2 to 10 g when the composition is discharged for 9 seconds with a discharge hole diameter of 2.5 mm and a discharge pressure of 0.5 MPa.

[0091] [Item 22] The thermally conductive silicone grease composition according to any one of Items 1 to 21, wherein 1.0 g of the thermally conductive silicone grease composition is placed between two plates, compressed and held to a thickness of 1.0 mm, the two plates are held vertically and placed in a heat shock tester, and held at -40°C and 125°C for 30 minutes each, for 500 cycles, in which the thermally conductive silicone grease composition falls no more than 5 mm.

[0092] [Item 23] A method for producing the thermally conductive silicone grease composition according to any one of items 1 to 22, comprising the steps of: filling the first thermally conductive silicone grease and the second thermally conductive silicone grease into dispensers; a step of alternately discharging and applying the first and second thermally conductive silicone greases from the discharge holes of the dispenser, while leaving a gap of 10% to 90% of the applied thickness so that the respective thermally conductive silicone greases do not come into contact with each other; A method for producing a thermally conductive silicone grease composition, comprising the steps of: compressing and molding the applied first and second thermally conductive silicone greases at a compression rate of 10 to 90% of the applied thickness, thereby causing an addition reaction at the contact portions of the first and second thermally conductive silicone greases to form joints, and joining the first and second thermally conductive silicone greases via these joints to produce a thermally conductive silicone grease composition.

[0093] [Item 24] The method for producing a thermally conductive silicone grease according to Item 23, wherein the applying step is carried out by alternately discharging the first and second thermally conductive silicone greases in cylindrical shapes and applying them.

[0094] [Item 25] The method for producing thermally conductive silicone grease according to Item 24, wherein the cylindrical shape has a diameter of 0.5 to 3.0 mm and a length of 50 to 1000 mm.

[0095] [Item 26] The method for producing a thermally conductive silicone grease composition according to Item 23, wherein the applying step is carried out by alternately discharging and applying the first and second thermally conductive silicone greases in the form of dots.

[0096] [Item 27] ​​The method for producing a thermally conductive silicone grease composition according to Item 26, wherein the dots have a diameter of 0.5 to 30 mm.

[0097] [Item 28] The method for producing a thermally conductive silicone grease composition according to any one of Items 23 to 27, wherein the compression molding is carried out at a temperature in the range of 80 to 150°C for a period of 5 to 60 minutes.

[0098] [Item 29] The method for producing the thermally conductive silicone grease composition according to any one of Items 23 to 28, which is carried out when mounting the thermally conductive silicone grease composition on a heat-generating component.

[0099] [Item 30] A thermally conductive sheet obtained by forming the thermally conductive silicone grease composition according to any one of items 1 to 22 into a sheet shape.

[0100] [Item 31] A method for producing a thermally conductive sheet, comprising forming the thermally conductive silicone grease composition according to any one of items 1 to 22 into a sheet, and then curing the sheet.

[0101] [Item 32] The method for producing a thermally conductive sheet according to Item 31, wherein the forming into a sheet is preferably carried out by sandwiching the thermally conductive silicone grease composition in a compound form between polyethylene terephthalate (PET) films and rolling the resulting film, and the curing is preferably carried out by heating at 80 to 150°C for 10 to 120 minutes.

[0102] [Item 33] Use of a thermally conductive sheet by interposing the thermally conductive sheet of Item 30 between a heat generating body and a heat sink.

[0103] [Example] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the measurement method will be described.

[0104] <Thermal conductivity> The thermal conductivity of the thermally conductive silicone grease was measured using a hot disk (compliant with ISO 22007-2:2008). As shown in FIG. 4A, this thermal conductivity measuring device 19 sandwiches a polyimide film sensor 17 between two samples 18a and 18b, applies a constant power to the sensor 17, and generates a constant amount of heat, analyzing the thermal characteristics from the temperature rise of the sensor 17. As shown in FIG. 4B, the tip 20 of the sensor 17 has a diameter of 7 mm and has a double spiral electrode structure, with an applied current electrode 21 and a resistance value electrode (temperature measurement electrode) 22 arranged at the bottom. The thermal conductivity is calculated using the following formula (Math. 1).

[0105]

number

[0106] <Drop test> The measurements were performed using the drop test shown in Figures 5A-D. 1.0 g of thermally conductive silicone grease 26 was applied between an aluminum plate 24 measuring 40 mm in length, 100 mm in width, and 5 mm in thickness and a glass plate 23 measuring 40 mm in length, 100 mm in width, and 5 mm in thickness (FIG. 5A), and compressed to a thickness of 1.0 mm with a spacer 25 interposed (FIG. 5B). 27 is the thermally conductive silicone grease compressed to a thickness of 1.0 mm. Next, the aluminum plate 24 and the glass plate 23 were placed in a heat cycle tester so that the gap between them was vertical (FIG. 5C). 28 is the test piece before the test. In this state, a heat cycle test was performed in which the plate was held at -40°C and 125°C for 30 minutes each. After 500 cycles, the test piece was removed and observed to see if the thermally conductive silicone grease 27 had fallen off. 29 is the test piece after the test (FIG. 5D), and 30 is the fall distance. The drop test for the thermally conductive silicone grease composition was carried out in the same manner as above, except that the "thermally conductive silicone grease" was changed to the "thermally conductive silicone grease composition". Judgment criteria A: Grease drop is within 5mm B: If it exceeds 5mm

[0107] <Absolute viscosity of thermally conductive silicone grease> The absolute viscosity of the thermally conductive silicone grease was measured using a Brookfield HBDV2T viscometer. The spindle used was a TE spindle, and the absolute viscosity was measured at a rotation speed of 5 rpm and 23°C.

[0108] <Discharge test> The thermally conductive silicone grease was filled into a 30 mL syringe PSY-30F manufactured by Musashi Engineering Co., Ltd., and the amount of the grease discharged was measured when the grease was discharged for 9 seconds at a discharge pressure of 0.5 MPa.

[0109] 1. Matrix resin (1) Organopolysiloxane (component A), curing reaction catalyst, crosslinking agent A commercially available two-liquid addition reaction curing silicone liquid was used as component (A). One liquid (liquid A) was an organopolysiloxane (base polymer component, component A, kinetic viscosity at 40°C 450 mm 2 The other liquid (liquid B) contains organopolysiloxane (base polymer component, component A, kinetic viscosity at 40°C 450mm 2 / s) and organohydrogenpolysiloxane (crosslinking agent), but does not contain a platinum group metal catalyst (curing reaction catalyst). In the examples, liquid (i) contains liquid A, and in the examples, liquid (ii) contains liquid B. The ratio of liquid A to liquid B in the examples is A:B=100:100 by mass. (2) Non-reactive silicone oil (Component D) Dimethylpolysiloxane was used as a non-reactive silicone oil (Kinematic viscosity at 25°C: 110 mm using a Brooklyn Field type rotational viscometer SP No. 2). 2 / s) was used. (3) Alkoxysilane (Component C) Decyltrimethoxysilane was used as component (C).

[0110] 2. Thermally conductive particles (component B) The thermally conductive particles shown in Table 1 were used as component (B). The average particle size is the D50 (median size) of the cumulative particle size distribution based on volume in particle size distribution measurement by laser diffraction light scattering method. An example of the measuring device is the LA-950S2 laser diffraction / scattering particle distribution measuring device manufactured by Horiba, Ltd. The number before μm in the table is the average particle size of each particle. - Irregular alumina (D50 = 0.3 μm) (Figure 6): Surface treated with octyltrimethoxysilane. - Irregular alumina (D50=2.3μm) (Figure 7): Surface treated with decyltrimethoxysilane. Spherical alumina (D50=105μm) (Fig. 9): No surface treatment. Aluminum nitride (D50=15μm) (Fig. 8): No surface treatment. Spherical agglomerated boron nitride (D50=25μm) (Fig. 10): No surface treatment. Spherical agglomerated boron nitride (D50=60μm) (Fig. 11): No surface treatment.

[0111] [Example 1] (a) Thermally conductive silicone grease composition shown in FIG. 1B The amounts of each material shown in Table 1 were measured, and then they were mixed uniformly in a mixing device to prepare two types of thermally conductive silicone grease: liquid (i) (first thermally conductive silicone grease) and liquid (ii) (second thermally conductive silicone grease). Liquids (i) and (ii) of the thermally conductive silicone grease were filled into a 30 mL syringe PSY-30F manufactured by Musashi Engineering Co., Ltd., and alternately discharged onto the plate at a discharge pressure of 0.3 MPa as shown in Figure 1A. The discharged thermally conductive silicone grease liquids (i) and (ii) were cylindrical with an average diameter of 3 mm and an average length of 15 mm. A gap of 20% of the coating thickness was provided.

[0112] As shown in Figure 1A, the cylindrical thermally conductive silicone grease liquids (i) and (ii) were discharged and compressed to a thickness of 1.0 mm using a spacer, and then compression molded by leaving it in an oven at 100°C for 10 minutes. The compression ratio of the cylindrical body was 66%. The thickness of the obtained thermally conductive silicone grease composition was 1 mm.

[0113] (b) The thermally conductive silicone grease composition shown in FIG. 2B The amounts of each material shown in Table 1 were measured, and they were mixed uniformly in a mixing device to prepare two types of thermally conductive silicone grease: liquid (i) (first thermally conductive silicone grease) and liquid (ii) (second thermally conductive silicone grease). Liquids (i) and (ii) of this thermally conductive silicone grease were filled into a 30 mL syringe PSY-30F manufactured by Musashi Engineering Co., Ltd., and discharged at a discharge pressure of 0.3 MPa as shown in Figure 2A. Figure 2A shows dots (spherical bodies) with an average diameter of 3 mm. A gap of 20% was provided relative to the coating thickness.

[0114] As shown in Figure 2A, the dot-shaped (spherical) thermally conductive silicone grease liquid (i) and liquid (ii) were discharged and compressed to a thickness of 1.0 mm using a spacer, and then compression molded by leaving it in an oven at 100°C for 10 minutes. The compression ratio of the dot-shaped (spherical) bodies was 66%. The thickness of the obtained thermally conductive silicone grease composition was 1 mm.

[0115] [Example 2] (a) Thermally conductive silicone grease composition shown in FIG. 1B A thermally conductive silicone grease composition was produced in the same manner as in Example 1(a), except that the amounts of each material were changed to those shown in Table 1 above. (b) The thermally conductive silicone grease composition shown in FIG. 2B A thermally conductive silicone grease composition was produced in the same manner as in Example 1(b), except that the amounts of each material were changed to those shown in Table 1 above.

[0116] [Comparative Examples 1 to 2] The amounts of each material shown in Table 1 above were weighed out and placed in a mixer to mix uniformly to prepare a thermally conductive silicone grease.

[0117] The above conditions and results are summarized in Table 1. In Table 1, the amount of each material is shown in parts by mass when the matrix resin is taken as 100 parts by mass (100 g).

[0118] [Table 1]

[0119] The above results reveal the following: (1) From the results of Example 1 and Example 2, the drop test results for the first thermally conductive silicone grease (liquid i) and the second thermally conductive silicone grease (liquid ii) were both rated B, but the drop test results for the thermally conductive silicone grease composition shown in Figures 1B and 2B were rated A. This is presumably because the junction between the first and second thermally conductive silicone greases is cured, resulting in the seepage components being trapped in the first and second thermally conductive silicone greases. (2) From the results of Examples 1 and 2, the first thermally conductive silicone grease (liquid I) and the second thermally conductive silicone grease (liquid II) had good dischargeability. This means that the first and second thermally conductive silicone greases can be stored for long periods of time because they do not harden in the dispenser. (3) Comparative Example 1 was rated a B in the drop test. This result is presumably because the non-reactive silicone oil is the main component of the matrix resin in Comparative Example 1, and therefore it is not expected that the leaching components will be contained by the hardening of the matrix resin.

[0120] The thermally conductive silicone grease composition of the present invention is suitable as a thermal interface material (TIM) that is a heat dissipation sheet to be placed between the heat generating parts of electric or electronic parts and the like and a heat sink. [Explanation of symbols]

[0121] 1. Cylindrical array 2a, 2b, 7a, 7b First thermally conductive silicone grease 3a, 3b, 8a, 8b Secondary thermally conductive silicone grease 4,10 Molded body 5a,5b,5c,9a,9b,9c joint 6 Dot array 11a, 11b Thermally conductive sheet 12 Heat spreader 13. Electronic Components 14 Wiring board 15 Heat sink 16 Heat dissipation structure 17 Sensors Samples 18a and 18b 19 Thermal conductivity measuring device 20 Sensor tip 21 Electrode for applied current 22 Resistance electrode (temperature measurement electrode) 23 Glass Plate 24 Aluminum Plate 25 Spacer 26 Thermally conductive silicone grease 27 Compressed thermally conductive silicone grease 28 Test specimen before testing 29 Test piece after test 30 Fall Distance

Claims

1. A thermally conductive silicone grease composition comprising a first thermally conductive silicone grease, a second thermally conductive silicone grease, and a joint therebetween, The first thermally conductive silicone grease contains a curing reaction catalyst and does not contain a crosslinking agent, the second thermally conductive silicone grease does not contain a curing reaction catalyst and contains a crosslinking agent; the first and second thermally conductive silicone greases are joined via the joint on at least one opposing surface of the first and second thermally conductive silicone greases; The joint is hardened, a thermally conductive silicone grease composition, wherein the first and second thermally conductive silicone greases are in an uncured state except at the joint portion.

2. The first and second thermally conductive silicone greases each contain a matrix resin and thermally conductive particles, The matrix resin contains the following components (A) and (C): The thermally conductive particles contain the following component (B): The thermally conductive silicone grease composition according to claim 1. (A) Kinematic viscosity at 40°C is 100 to 3000 mm 2 / s addition reaction curable organopolysiloxane: 100 parts by mass (B) Thermally conductive filler: 200 to 3,000 parts by mass relative to 100 parts by mass of the matrix resin (C) R a Si(OR′) 4-a (wherein R is an unsubstituted or substituted organic group having 8 to 12 carbon atoms, R' is an alkyl group having 1 to 4 carbon atoms, and a is 0 or 1): 0 to 10 parts by mass of alkoxysilane

3. The matrix resin of the first and second thermally conductive silicone greases further comprises 3. The thermally conductive silicone grease composition according to claim 2, wherein component (A) contains 1 to 50 mass % of a non-reactive silicone oil.

4. 3. The thermally conductive silicone grease composition according to claim 2, wherein the material of the thermally conductive particles is at least one selected from the group consisting of alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, aluminum hydroxide, quartz, and silica.

5. 2. The thermally conductive silicone grease composition according to claim 1, wherein at least one of the first and second thermally conductive silicone greases has a thermal conductivity of 2.0 W / m·K or higher.

6. 2. The thermally conductive silicone grease composition according to claim 1, wherein the first and second thermally conductive silicone greases each have an absolute viscosity, as measured by a B-type viscometer at 23° C., in the range of 1,000 to 20,000 Pa s.

7. The thermally conductive silicone grease composition according to claim 1, wherein the first and second thermally conductive silicone greases are each filled into a 30 mL syringe and discharged in an amount of 2 to 10 g when discharged for 9 seconds with a discharge hole diameter of 2.5 mm and a discharge pressure of 0.5 MPa.

8. The thermally conductive silicone grease composition according to claim 1, wherein 1.0 g of the thermally conductive silicone grease composition is placed between two plates, compressed and held to a thickness of 1.0 mm, and the two plates are held vertically and placed in a heat shock tester, and held at -40°C and 125°C for 30 minutes each, over a heat shock test of 500 cycles, in which the thermally conductive silicone grease composition falls no more than 5 mm.

9. A method for producing the thermally conductive silicone grease composition according to claim 1, comprising the steps of: filling the first thermally conductive silicone grease and the second thermally conductive silicone grease into dispensers; a step of alternately discharging and applying the first and second thermally conductive silicone greases from the discharge holes of the dispenser, while leaving a gap of 10% to 90% of the applied thickness so that the respective thermally conductive silicone greases do not come into contact with each other; A method for producing a thermally conductive silicone grease composition, comprising the steps of: compressing and molding the applied first and second thermally conductive silicone greases at a compression rate of 10 to 90% of the applied thickness, thereby causing an addition reaction at the contact portions of the first and second thermally conductive silicone greases to form joints, and joining the first and second thermally conductive silicone greases via these joints to produce a thermally conductive silicone grease composition.

10. 10. The method for producing a thermally conductive silicone grease according to claim 9, wherein the applying step is carried out by alternately discharging the first and second thermally conductive silicone greases in cylindrical shapes and applying them.

11. 10. The method for producing a thermally conductive silicone grease composition according to claim 9, wherein the applying step is carried out by discharging and applying the first and second thermally conductive silicone greases alternately in the form of dots.

12. 10. The method for producing a thermally conductive silicone grease composition according to claim 9, wherein the method is carried out when the thermally conductive silicone grease composition is mounted on a heat-generating component.

13. 9. A thermally conductive sheet in which the thermally conductive silicone grease composition according to any one of claims 1 to 8 is formed into a sheet.

Citation Information

Patent Citations

  • Manufacture of heat conductive / Composite sheet

    JP1994155517A

  • Extrusible crosslinked grease-like radiation material, container in which the material is filled and enclosed, manufacturing method of the container and radiation method using these

    JP2002294269A

  • Silicone composition

    JP2014080546A

  • Composition for thermal conducive grease, thermal conductive grease and heat dissipating member

    JP2016216523A

  • Thermal GEL composition

    WO2022187569A1

Cited By

  • Heat-conducting silicone grease with core-shell structure as well as preparation method and application of heat-conducting silicone grease