Polyurethane urea resin composition and coating agent
The polyurethaneurea resin composition, utilizing polycarbonate diol and alicyclic diisocyanate, addresses issues of workability, shape stability, and weather resistance, offering high softening temperature and improved handling properties.
Patent Information
- Application Number
- JP2018049081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-03-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2038-03-16
AI Technical Summary
Existing polyurethane resins exhibit insufficient workability during processing, shape stability under high-temperature environments, and weather resistance.
A polyurethaneurea resin composition is developed using specific polycarbonate diol, alicyclic diisocyanate, and alicyclic diamine, with a number average molecular weight ranging from 30,000 to 90,000, achieving a softening temperature of 150°C or higher.
The composition provides high softening temperature, excellent weather resistance, and good handling properties, maintaining shape and function under high-temperature conditions.
Smart Images

Figure 0007576903000001 
Figure 0007576903000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyurethane urea resin composition having high heat resistance, a coating agent using said composition, and use thereof. [Background technology]
[0002] Traditionally, polyurethane resins have excellent physical properties such as abrasion resistance, flexibility, softness, processability, adhesion and chemical resistance, and are also well suited to a variety of processing methods. As a result, they have been widely used as resin components in coatings, inks, adhesives and paints for electronic device parts, clothing, furniture, home appliances, daily necessities, construction and civil engineering, and automotive parts, as well as in various molded articles such as films and sheets.
[0003] Such polyurethane resins are also used in synthetic leather, and because their appearance and texture are similar to natural leather, they are widely used in the fields of clothing, bags, sacks, footwear, etc. For example, it has been proposed to use polyurethane obtained from 4,4'-diphenylmethane diisocyanate (hereinafter also referred to as MDI), polyether, and 4,4'-diaminodiphenylmethane as a leather sheet material (see Patent Document 1). Also, in order to improve the solubility of polyurethane resins in solvents and reduce the viscosity of the resin solution to improve workability, a urethane resin composition containing an isomer other than 4,4'-diphenylmethane diisocyanate has been proposed (see Patent Document 2).
[0004] However, the method was insufficient in terms of workability during processing, shape stability when the molded product was exposed to a high-temperature environment, and weather resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 4-80141 [Patent Document 2] Japanese Patent Application Publication No. 10-8383 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above-mentioned background art, and an object of the present invention is to provide a resin composition having a high softening temperature, excellent weather resistance and good handleability. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by a polyurethane urea resin composition using a specific polycarbonate diol and a specific polyisocyanate, thereby completing the present invention.
[0008] That is, the present invention includes the embodiments shown below.
[0009] [1] A polyurethane urea resin composition obtained from a polyol (A), a polyisocyanate (B), a diamine (C), and a monoamine (M), characterized in that the polyol (A) contains a polycarbonate diol (a1) having a number average molecular weight of 2,200 to 6,000, the polyisocyanate (B) contains an alicyclic diisocyanate (b1), and the polyurethane urea resin composition has a number average molecular weight of 30,000 to 90,000.
[0010] [2] The polyurethane urea resin composition according to the above [1], wherein the polyol (A) contains the polycarbonate diol (a1) and a chain extender (a2), and the chain extender (a2) is a diol having 2 to 8 carbon atoms.
[0011] [3] The polyurethane urea resin composition according to the above [1] or [2], characterized in that the alicyclic diisocyanate (b1) contains dicyclohexylmethane-4,4'-diisocyanate and isophorone diisocyanate.
[0012] [4] The polyurethane urea resin composition according to any one of the above [1] to [3], wherein the diamine (C) includes an alicyclic diamine.
[0013] [5] The polyurethane urea resin composition according to any one of [1] to [4] above, which has a softening temperature of 150°C or higher.
[0014] [6] A coating agent comprising the polyurethane urea resin composition according to any one of [1] to [5] above.
[0015] [7] The coating agent according to the above item 6, characterized in that the polyurethane urea resin composition is used in a one-component system.
[0016] [8] A coating film obtained from the coating agent described in [6] or [7] above.
[0017] [9] A molded product using the coating agent described in [6] or [7] above.
[0018]
[10] A method for producing a polyurethane urea resin composition obtained by reacting an isocyanate-terminated prepolymer (P) obtained from a polyol (A) and a polyisocyanate (B) with a diamine (C) and a monoamine (M), wherein the polyol (A) contains a polycarbonate diol (a1) having a number average molecular weight of 2,200 to 6,000, the polyisocyanate (B) contains an alicyclic diisocyanate (b1), and the polyurethane urea resin composition has a number average molecular weight of 30,000 to 90,000.
[0019] In the present invention, the softening temperature is one of the indices of the heat resistance of the obtained resin composition, and a higher softening temperature means higher heat resistance. Effect of the Invention
[0020] According to the present invention, it is possible to obtain a polyurethane urea resin composition having a high softening temperature, excellent weather resistance, and good handleability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The polyurethane urea resin composition of the present invention is characterized in that it is a polyurethane urea resin composition obtained from a polyol (A), a polyisocyanate (B), a diamine (C), and a monoamine (M).
[0022] The polyol (A) of the present invention contains a polycarbonate diol (a1) having a number average molecular weight of 2,200 to 6,000.
[0023] The polycarbonate diol (a1) can be obtained, for example, by reacting a carbonate such as a dialkyl carbonate, e.g., dimethyl carbonate, diethyl carbonate, etc., an alkylene carbonate, e.g., ethylene carbonate, propylene carbonate, etc., or a diaryl carbonate, e.g., diphenyl carbonate, dinaphthyl carbonate, dianthryl carbonate, diphenanthryl carbonate, diindanyl carbonate, tetrahydronaphthyl carbonate, etc., with a glycol.
[0024] The glycol is selected from the group of low molecular weight diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, diethylene glycol, dipropylene glycol, neopentyl glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, diol dimer acid, ethylene oxide or propylene oxide adduct of bisphenol A, bis(β-hydroxyethyl)benzene, and xylylene glycol. These may be used alone or in combination of two or more.
[0025] As the polycarbonate diol (a1) in the present invention, an alkylene carbonate is used as the carbonate, and as the glycol, 1,6-hexanediol is preferred in view of the ease of availability and the ability to increase the softening temperature of the resulting polyurethane urea resin.
[0026] In the present invention, a copolymer polyol obtained by subjecting a polycarbonate diol (a1) to an ester exchange reaction with a polyester polyol (a3) can be used in place of the polycarbonate diol (a1).
[0027] Examples of the polyester polyol (a3) include polyester polyols obtained from glycol and dicarboxylic acid components, and those obtained by ring-opening addition polymerization of cyclic ester compounds such as lactones using glycol as an initiator.
[0028] Examples of the glycol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, diethylene glycol, dipropylene glycol, neopentyl glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, diol dimer acid, ethylene oxide or propylene oxide adduct of bisphenol A, bis(β-hydroxyethyl)benzene, xylylene glycol, and the like. Trimethylolpropane, glycerin, pentaerythritol, sorbitol, and the like can be used in combination.
[0029] Polyester polyols prepared by a known condensation method between these alcohols and dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, adipic acid, tartaric acid, pimelic acid, sebacic acid, phthalic acid, and terephthalic acid can be used.
[0030] In addition, preferred lactones include, for example, β-propiolactone, β-butyrolactone, γ-butyrolactone, β-valerolactone, γ-valerolactone, δ-valerolactone, α-caprolactone, β-caprolactone, γ-caprolactone, δ-caprolactone, ε-caprolactone, α-methyl-ε-caprolactone, β-methyl-ε-caprolactone, 4-methylcaprolactone, γ-caprylolactone, ε-caprylolactone, ε-palmitolactone, etc., and one or more selected from these can be used in combination. Among these, a ring-opening addition polymer of ε-caprolactone using ethylene glycol as an initiator is preferred from the standpoint of stability during polymerization and economic efficiency.
[0031] When using a copolymer polyol obtained by subjecting a polycarbonate diol (a1) and a polyester polyol (a3) to an ester exchange reaction, the mass ratio of the polycarbonate diol (a1) to the polyester polyol (a3) is preferably in the range of (a1) / (a3)=95 / 5 to 50 / 50, more preferably in the range of (a1) / (a3)=90 / 10 to 60 / 40.
[0032] By setting the mass ratio within these ranges, it is possible to improve both flexibility and adhesion to a substrate by achieving a balance between the cohesive force of the polycarbonate diol, the urethane group concentration, and the polyester polyol content.
[0033] The number average molecular weight of the polycarbonate diol (a1) is in the range of 2200 to 6000, and in consideration of the high softening temperature characteristic, ease of synthesis, and ease of handling, it is preferably in the range of 2500 to 4000, and more preferably in the range of 2800 to 3500. The number average molecular weight of the copolymer polyol obtained by subjecting the polycarbonate diol (a1) to an ester exchange reaction with the polyester polyol (a3) is the same.
[0034] The polyisocyanate (B) in the present invention includes an alicyclic diisocyanate from the viewpoint of weather resistance. Examples of the alicyclic diisocyanate include isophorone diisocyanate (hereinafter referred to as IPDI), cyclohexane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate (hereinafter referred to as hydrogenated diphenylmethane diisocyanate or hydrogenated MDI), norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, and hydrogenated tetramethylxylene diisocyanate. Among these alicyclic diisocyanates, IPDI and hydrogenated MDI are preferred, and it is particularly preferred to use the two in combination from the viewpoints of flexibility, durability, and productivity.
[0035] When IPDI and hydrogenated MDI are used in combination, the mass ratio of IPDI to hydrogenated MDI is preferably in the range of 10 / 90 to 75 / 25, and more preferably in the range of 10 / 90 to 40 / 60.
[0036] Furthermore, within the range in which performance is not reduced, aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, araliphatic diisocyanates, isocyanurate group-containing polyisocyanates obtained using these polyisocyanates as raw materials, uretdione group-containing polyisocyanates, uretdione group- and isocyanurate group-containing polyisocyanates, urethane group-containing polyisocyanates, allophanate group-containing polyisocyanates, biuret group-containing polyisocyanates, urethimine group-containing polyisocyanates, and the like can be used in combination.
[0037] Examples of the diamine (C) of the present invention include alicyclic diamines such as isophoronediamine, cyclohexanediamine, norbornanediamine, hydrogenated tolylenediamine, hydrogenated xylenediamine, and hydrogenated tetramethylxylenediamine, and diamines other than alicyclic diamines such as ethylenediamine, butylenediamine, hexamethylenediamine, diphenylmethanediamine, tolylenediamine, xylylenediamine, 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, and 2-hydroxy-1,3-propanediamine, and these can be used alone or in combination of two or more kinds.
[0038] Of these diamines, it is preferable to use alicyclic diamines, and it is more preferable to use isophorone diamine in view of the balance between flexibility and durability.
[0039] The monoamine (M) of the present invention is not particularly limited, and examples thereof include ethylamine, morpholine, propylamine, dibutylamine, diethylamine, monoethanolamine, dibutylamine monoethanolamine, diethanolamine, N-methylethanolamine, N-ethylethanolamine, Nn-butylethanolamine, Nt-butylethanolamine, hydroxyethylpiperazine, N-(3-aminopropyl)diethanolamine, N-cyclohexylethanolamine, etc. Among these, monoethanolamine is preferred from the viewpoint of reactivity and molecular weight control.
[0040] In the present invention, a chain extender (a2) may be used as necessary. The chain extender is not particularly limited, but examples thereof include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,4-bis(β-hydroxyethoxy)benzene, neopentyl glycol, methyloctanediol, 1,9-nonanediol, bisphenol, cyclohexanedimethanol, dimethylolheptane, and polypropylene glycol. Among these, diols having 2 to 8 carbon atoms are preferred, and 1,4-butanediol and 1,6-hexanediol are preferred from the perspective of the balance between durability and flexibility.
[0041] The molar ratio of the polycarbonate diol (A) to the chain extender (a2), (a2) / (A), is preferably 0.05-7, more preferably 0.1-5, and particularly preferably 0.2-4.
[0042] The polyurethane urea resin in the present invention has a number average molecular weight of 30,000 to 90,000, and preferably 40,000 to 80,000. If the number average molecular weight is less than the lower limit, the softening temperature of the resin composition may decrease. If the number average molecular weight exceeds the upper limit, the viscosity of the resin solution may increase, and the handling properties may decrease.
[0043] Next, a general method for producing the polyurethane urea resin composition of the present invention will be described with reference to the following examples.
[0044] First step: Polyol (A) and polyisocyanate (B) are charged so that there is an excess of isocyanate groups, and are subjected to a urethane reaction in the presence or absence of an organic solvent to produce an isocyanate-terminated prepolymer (P).
[0045] Second step: The isocyanate-terminated prepolymer (P) is subjected to a urea-forming reaction with a diamine (C) and a monoamine (M).
[0046] In the series of production steps, it is preferable to carry out the reaction in a nitrogen gas or dry air stream in order to suppress the reaction between the isocyanate group and moisture.
[0047] In the first step, "so that there is an excess of isocyanate groups" means that when the raw materials are charged, the raw materials are preferably charged so that the molar ratio of the isocyanate groups of the polyisocyanate (B) to the hydroxyl groups of the polyol (A) is R = isocyanate groups / hydroxyl groups, which is 1.5 to 3.0, and more preferably R = 1.8 to 2.7.
[0048] The reaction temperature of the urethanization reaction is preferably 20 to 120° C., and more preferably 50 to 100° C. Although this urethanization reaction proceeds without a catalyst, the reaction can be accelerated by using a known urethanization reaction catalyst.
[0049] As the catalyst that can be used in the urethanization reaction, for example, an organometallic compound such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, or an organic amine such as triethylenediamine or triethylamine, or a salt thereof can be selected and used.
[0050] The reaction time for the urethane reaction varies depending on the presence or absence, type, and temperature of a catalyst, but is generally within 10 hours, preferably 1 to 5 hours. However, as the reaction time increases, problems such as coloring may occur.
[0051] As the organic solvent used in the production of the polyurethane urea resin composition, a solvent that does not affect the reaction in the presence of the organic solvent is appropriately selected.
[0052] Examples of organic solvents include aliphatic hydrocarbons such as octane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, ketones such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, esters such as butyl acetate and isobutyl acetate, glycol ether esters such as ethylene glycol ethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methyl-3-methoxybutyl acetate, and ethyl-3-ethoxypropionate, ethers such as dioxane, halogenated hydrocarbons such as methylene iodide and monochlorobenzene, and polar aprotic solvents such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethylsulfoxide, and hexamethylphosphonylamide. These solvents can be used alone or in combination of two or more.
[0053] In the second step, the isocyanate-terminated prepolymer (P) produced in the first step is subjected to a urea-forming reaction with a diamine (C) and a monoamine (M) at 20 to 60° C. to obtain the polyurethane urea resin of the present invention.
[0054] When using the polyurethane urea resin composition of the present invention, since it has a high softening temperature even without using a hardener, it is preferable to use it in a one-liquid system that does not use a hardener such as polyisocyanate. The softening temperature can be further increased by using a hardener, but since there is a risk of impairing flexibility, the amount of the hardener used is preferably 10 parts by mass or less, more preferably 3 parts by mass or less, per 100 parts by mass of the polyurethane urea resin composition.
[0055] As the curing agent, for example, the above-mentioned aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, araliphatic diisocyanates, isocyanurate group-containing polyisocyanates obtained using these polyisocyanates as raw materials, uretdione group-containing polyisocyanates, uretdione group- and isocyanurate group-containing polyisocyanates, urethane group-containing polyisocyanates, allophanate group-containing polyisocyanates, biuret group-containing polyisocyanates, urethimine group-containing polyisocyanates, and the like can be used.
[0056] The polyurethane urea resin composition obtained by the present invention may be appropriately blended with additives, such as antioxidants, ultraviolet absorbers, pigments, dyes, solvents, flame retardants, hydrolysis inhibitors, lubricants, plasticizers, fillers, antistatic agents, dispersants, catalysts, storage stabilizers, surfactants, and leveling agents, as necessary.
[0057] The polyurethane urea resin composition of the present invention thus obtained can have a softening temperature of 150° C. or higher. By achieving a softening temperature of 150° C. or higher, the composition can maintain its shape and function under high temperature conditions, and can be more useful in electronic device components, furniture and home appliance components, daily necessities, automobile components, and the like.
[0058] Next, a coating agent using the polyurethane urea resin composition of the present invention, and a coating film and a molded article obtained from the coating agent will be described.
[0059] The polyurethane urea resin composition of the present invention is suitably used as a coating agent, coating film, or molded product for electronic device components such as communication tablets, synthetic leather for clothing, bags, sacks, footwear, etc., furniture and home appliance components, daily necessities, and automobile components.
[0060] The coating agent is a composition obtained by blending the polyurethane urea resin composition of the present invention with a solvent, additives, etc., as necessary, and can be suitably used as, for example, a paint, an adhesive, etc.
[0061] The coating film is a coating film formed on a substrate by mixing a coating agent containing at least the polyurethane urea resin composition of the present invention with the above-mentioned crosslinking agent and additives as necessary, stirring the mixture uniformly, and then using a known technique such as spray coating, knife coating, wire bar coating, doctor blade coating, reverse roll coating, or calendar coating.
[0062] The molded products include members, structures, films, and sheets, and examples of the molded products include those molded by known techniques such as casting and coating.
[0063] The substrate may be stainless steel, phosphate-treated steel, galvanized steel, iron, copper, aluminum, brass, glass, acrylic resin, polycarbonate resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene phthalate resin, polystyrene resin, AS resin, ABS resin, polycarbonate-ABS resin, 6-nylon resin, 6,6-nylon resin, MXD6 nylon resin, polyvinyl chloride resin, polyvinyl alcohol resin, polyurethane resin, phenol resin, melamine resin, polyacetal resin, chlorinated polyolefin resin, polyolefin resin, polyamide resin, polyether ether ketone, etc. Examples of the material include substrates molded from materials such as olefin resins, such as polyethylene resin, polyphenylene sulfide resin, NBR resin, chloroprene resin, SBR resin, SEBS resin, polyethylene, and polypropylene; organic fibers containing at least one type of main component selected from polyethylene terephthalate resin, polytrimethylene terephthalate resin, polybutylene terephthalate resin, polyethylene resin, polypropylene resin, polystyrene resin, 6-nylon resin, 6,6-nylon resin, acrylic resin, polyvinyl alcohol resin, cellulose, polylactic acid, cotton, and wool; inorganic fibers, such as glass wool; and carbon fibers.
[0064] In order to improve the adhesiveness of these substrates, the surfaces of the substrates may be previously subjected to treatments such as corona discharge treatment, frame treatment, ultraviolet irradiation treatment, and ozone treatment. EXAMPLES
[0065] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0066] [Synthesis of polyurethane urea resin composition] [Example 1] In a 2-liter four-neck flask equipped with a stirrer, thermometer, heater, and distillation column, 159 g of polycarbonate diol 1 (1,6-hexanediol-based polycarbonate polyol, number average molecular weight 3,000) and 700 g of N,N-dimethylformamide (hereinafter referred to as DMF) were charged, and these were uniformly stirred at 45°C while bubbling with nitrogen gas to prepare a polymer polyol solution. 14 g of isophorone diisocyanate (hereinafter referred to as IPDI) and 49 g of hydrogenated diphenylmethane diisocyanate (hereinafter referred to as hydrogenated MDI) were charged into this polymer polyol solution, and a urethane reaction was carried out at 75°C for 2 hours under a nitrogen gas flow to obtain an isocyanate group-terminated urethane prepolymer (P) solution. The NCO content of this prepolymer solution was 1.1% by mass.
[0067] To the resulting isocyanate-terminated urethane prepolymer (P) solution was added an amine solution in which 20 g of isophorone diamine (hereinafter referred to as IPDA) and 2 g of monoethanolamine (hereinafter referred to as MEA) were mixed in advance, and a chain extension reaction was carried out at 40°C for 2 hours to obtain a polyurethane urea resin composition. The resulting polyurethane urea resin composition had a number average molecular weight of 75,000 by GPC and a viscosity of 20,000 mPa s at 25°C.
[0068] [GPC: Molecular weight measurement conditions] (1) Measuring instrument: HLC-8220 (manufactured by Tosoh Corporation) (2) Column: TSKgel (Tosoh Corporation) G3000H-XL G2500H-XL G2000H-XL G1000H-XL (3) Carrier: THF (tetrahydrofuran) (4) Detector: RI (refractive index) detector (5) Temperature: 40℃ (6)Flow rate: 1.000ml / min (7) Calibration curve: Standard polystyrene (Tosoh Corporation) ·F-80 (molecular weight: 7.06×10 5 , molecular weight distribution: 1.05) ·F-20 (molecular weight: 1.90×10 5 , molecular weight distribution: 1.05) ·F-10 (molecular weight: 9.64×10 4 , molecular weight distribution: 1.01) ·F-2 (molecular weight: 1.81×10 4 , molecular weight distribution: 1.01) ·F-1 (molecular weight: 1.02×10 4 , molecular weight distribution: 1.02) ·A-5000 (molecular weight: 5.97×10 3 , molecular weight distribution: 1.02) ·A-2500 (molecular weight: 2.63×10 3 , molecular weight distribution: 1.05) ·A-500 (molecular weight: 5.0×10 2 , molecular weight distribution: 1.14) (8) Sample solution concentration: 0.5% THF solution.
[0069] [Synthesis of other polyurethane urea resin compositions] The polyurethane urea resins of Examples 2 to 5 and Comparative Examples 1 to 3 were synthesized in the same manner as in the production of the polyurethane urea resin composition of Example 1, with the charging composition of each raw material (amount blended by mass) being as shown in Table 1.
[0070] [Film production using polyurethane urea resin composition] The obtained polyurethane urea resin composition was applied onto a release paper so that the dry thickness was 60 μm, and after standing at room temperature for 20 minutes, it was heat-treated in a dryer at 60° C. for 20 minutes and then at 120° C. for 20 minutes, and then aged at 40° C. for 24 hours to obtain a film. The physical properties of this film were evaluated.
[0071] [Evaluation test 1] [Tensile properties] The tensile properties of the obtained film were measured in accordance with JIS K6251. The results are shown in Tables 1 and 2. Test equipment: Tensilon UTA-500 (manufactured by A&D) Measurement conditions: 25℃×50%RH Head speed: 200mm / min ·Dumbbell No. 4.
[0072] [Evaluation test 2] [Softening temperature] A test piece was obtained from the obtained film using a dumbbell, a 2 cm mark was drawn on the test piece, and the thickness at the center of the mark was measured. A weight of a specified weight was attached to one grip of the test piece, and the other grip was clamped with a double clip, and the test piece was hung in a dryer with the clip on the upper side. The temperature in the dryer was then increased and the distance between the gauge lines was observed. The temperature at which the distance between the gauge lines reached 4 cm was read as the softening temperature. If this softening temperature was 150°C or higher, it could be said to be evaluated as good. The results are shown in Tables 1 and 2. Processing equipment: constant temperature blower dryer DRK633DA (manufactured by Advantec) Weight: thickness of center of gauge line (μm) x 0.05g Dumbbell No. 2 (JIS K6251 compliant) Heating rate: 5℃ / min.
[0073] [Evaluation test 3] [Handling] The handleability is considered good if the viscosity at 25°C is 80,000 mPa·s or less.
[0074] [Evaluation test 4] [Weather resistance] The obtained film was subjected to a weather resistance treatment under the following conditions, and the color number was measured. <Weather resistance test> Processing equipment: QUV (manufactured by Q-LAB) Lamp: EL-313 ·Illuminance: 0.59w / m 2 λmax:313nm 1 cycle: 12 hours (UV irradiation: 8 hours (temperature 70°C), condensation: 4 hours (temperature 50°C)) Processing time: 300 hours <Color measurement> The weather-resistant film was measured for b* using a color difference meter (CR-310, manufactured by Konica Minolta). A b* value of 1.0 or less was considered to be good.
[0075] [Evaluation test 5] [Wear resistance] In accordance with JIS L1096, the abrasion resistance was measured using a Taber abrasion tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) with a load of 1 kg, a disk rotation speed of 60 rpm x 500 rotations, and an abrasion wheel H-22. <Evaluation criteria> The coating film has peeled off or most of it has worn away (rating: ×) · Part of the coating film has worn away (Rating: △) No change in appearance was observed (rating: ○)
[0076] [Table 1]
[0077] [Table 2]
[0078] The raw materials used in Tables 1 and 2 are as follows. (1) IPDI: Isophorone diisocyanate (manufactured by Evonik) (2) Hydrogenated MDI: Hydrogenated diphenylmethane diisocyanate (manufactured by Sumika Covestro Urethane Co., Ltd.) (3)MDI-1:2,2'-MDI+2,4'-MDI=1.8 mass%, 4,4'-MDI=98.2 mass% (4)MDI-2: 2,2'-MDI+2,4'-MDI=93.0 mass%, 4,4'-MDI=7.0 mass% *MDI: Diphenylmethane diisocyanate (manufactured by Tosoh Corporation) (5) Polyol-1: 1,6 hexanediol-based polycarbonate polyol, number average molecular weight 3,000 (6) Polyol-2: 1,6 hexanediol-based polycarbonate polyol (number average molecular weight 3,000) / polycaprolactone polyol (number average molecular weight 3,000) = copolymer polyol with a mass ratio of 7 / 3, number average molecular weight 3,000 (7) Polyol-3: 1,6 hexanediol-based polycarbonate polyol, number average molecular weight 2,500 (8) Polyol-4: 1,6 hexanediol-based polycarbonate polyol, number average molecular weight 2,000 (9) 1,4-BG: 1,4-butanediol (manufactured by Mitsubishi Chemical Corporation) (10) 1,6-HG: 1,6-hexanediol (manufactured by Ube Industries, Ltd.) (11) IPDA: Isophoronediamine (manufactured by Evonik) (12) DMF: N,N-dimethylformamide (manufactured by Mitsubishi Gas Chemical Co., Ltd.) (13) MEK: Methyl ethyl ketone (Maruzen Oil Co., Ltd.)
Claims
1. A polyurethane urea resin composition obtained from a polyol (A), a polyisocyanate (B), a diamine (C), and a monoamine (M), The polyol (A) contains a polycarbonate diol (a1) having a number average molecular weight of 2,200 to 6,000; The polyisocyanate (B) contains an alicyclic diisocyanate (b1), The alicyclic diisocyanate (b1) includes dicyclohexylmethane-4,4'-diisocyanate and isophorone diisocyanate; The polyurethane urea resin composition has a number average molecular weight of 30,000 to 90,000.
2. The ratio of dicyclohexylmethane-4,4'-diisocyanate to isophorone diisocyanate is Isophorone diisocyanate:dicyclohexylmethane-4,4'-diisocyanate=22.03:77.97-70.59:29.41 The polyurethane urea resin composition according to claim 1,
3. The polyol (A) contains the polycarbonate diol (a1) and a chain extender (a2), 3. The polyurethane urea resin composition according to claim 1, wherein the chain extender (a2) is 1,4-butanediol or 1,6-hexanediol.
4. The polyurethane urea resin composition according to claim 1 , which has a softening temperature of 170° C. or higher.
5. 4. The polyurethane urea resin composition according to claim 1, which has a softening temperature of 180° C. or higher.
6. A coating agent comprising the polyurethane urea resin composition according to any one of claims 1 to 5.
7. The coating agent according to claim 6, wherein the polyurethane urea resin composition is used as a one-component system.
8. A coating film obtained from the coating agent according to claim 6 or 7.
9. A molded product using the coating agent according to claim 6 or 7.
10. A method for producing a polyurethane urea resin composition obtained by reacting an isocyanate-terminated prepolymer (P) obtained from a polyol (A) and a polyisocyanate (B), with a diamine (C) and a monoamine (M), comprising the steps of: The polyol (A) contains a polycarbonate diol (a1) having a number average molecular weight of 2,200 to 6,000; The polyisocyanate (B) contains an alicyclic diisocyanate (b1), The alicyclic diisocyanate (b1) includes dicyclohexylmethane-4,4'-diisocyanate and isophorone diisocyanate; The polyurethane urea resin composition has a number average molecular weight of 30,000 to 90,000.
Citation Information
Patent Citations
Multiple stage sheet feeding and transferring device
JP1992080141A
Production of highly durable synthetic leather with thermoplastic polyurethane resin having excellent solubility
JP1998008383A
Ultraviolet absorber resistant polyurethane urea resin composition, and molded body and coating material using the composition
JP2017122169A
Moisture-permeable polyurethane urea resin composition, molded body using the same, and coating material
JP2017128642A
Polyurethane urea resin composition exhibiting UV-absorption-agent resistance, moulded body using said composition, and coating material
WO2016006566A1