Decorative fiber sheet

The decorative fiber sheet addresses poor appearance quality by ensuring uniform print distribution through a specific color difference calculation and the use of cellulose nanofibers, achieving minimal color variation and enhanced abrasion resistance.

JP7576942B2Active Publication Date: 2024-11-01JAPAN VILENE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020140057
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-26
Filing Date
2020-08-21
Publication Date
2024-11-01
Estimated Expiration
2040-08-21

AI Technical Summary

Technical Problem

Decorative fiber sheets for automobile interiors often suffer from poor appearance quality due to bleeding or chipping of prints, leading to uneven color distribution and thickness variations.

Method used

A decorative fiber sheet with a print on one main surface, where the color difference ΔE of measurement samples is calculated using a specific method, ensuring a ratio of less than 0.2 for 50% of samples, and incorporating cellulose nanofibers with a mass ratio of 0.5 to 5.0% and an average fiber diameter of 8 nm or less to enhance uniformity and dispersibility of printing components.

Benefits of technology

The solution results in a decorative fiber sheet with minimal color variation and excellent appearance quality, featuring clear prints and improved abrasion resistance due to the uniform dispersion of printing components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576942000008
    Figure 0007576942000008
  • Figure 0007576942000009
    Figure 0007576942000009
  • Figure 0007576942000010
    Figure 0007576942000010
Patent Text Reader

Abstract

To provide a decorative fiber sheet excellent in appearance quality.SOLUTION: A decorative fiber sheet has a print resin on one of principal planes of a fiber sheet. The decorative fiber sheet has small variations in the print resin of the decorative fiber sheet and thus the decorative fiber sheet has small variations in color and is excellent in appearance quality. It has been found that, when a cellulose nanofiber is included in the print resin, a decorative fiber sheet having small variations in color of the print included in the decorative fiber sheet and excellent in appearance quality can be achieved.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative fiber sheet. [Background technology]

[0002] Conventionally, decorative fiber sheets having a print on the surface of a fiber sheet, such as the decorative fiber sheet for automobiles disclosed in JP 2012-179985 A (Patent Document 1), have been used as skin materials for automobile interior materials such as ceiling materials. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-179985 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the applicant of the present application produced a decorative fiber sheet having a print on the surface of the fiber sheet, the appearance quality of the decorative fiber sheet was sometimes deteriorated.

[0005] The applicant of the present application observed the surface of a decorative fiber sheet to investigate the cause of the poor appearance quality of the decorative fiber sheet. As a result, it was found that the cause of the poor appearance quality of the decorative fiber sheet was the printing on the surface of the decorative fiber sheet bleeding in some places and the printing lines becoming thicker in some places, and the printing on the surface of the decorative fiber sheet being chipped in some places.

[0006] The present invention has been made under these circumstances, and has an object to provide a decorative fiber sheet that has excellent appearance quality. [Means for solving the problem]

[0007] The invention according to claim 1 of the present invention is a decorative fiber sheet having a print on one of its main surfaces, the color difference ΔE of 50 or more measurement samples being calculated by the following [color difference variation measurement method], and the ratio of the number of measurement samples having a color difference ΔE of less than 0.2 to the total number of measurement samples being 50% or more. [Color difference variation measurement method] (1) Cut out 50 or more measurement samples into rectangles of 5 cm x 15 cm from the decorative fiber sheet. (2) Using a spectrophotometer, measure the lightness L of the main surface having the print of the measurement samples in (1). * and chromaticity a * ,b * (CIE1976L * a * b * (3) The individual average value L of the lightness of the three points on one sample measured in (2) is calculated by measuring the lightness of the three points on one sample in the measurement range of 2.5 cm in diameter. * 1 and the individual average value of chromaticity a * 1,b * (4) Calculate the individual average lightness L of all the measurement samples obtained in (3). * 1 and the individual average value of chromaticity a * 1,b * Take the average value of 1 and calculate the overall average value L of the brightness of the entire measured sample. * 2 and overall average color value a * 2,b * (5) Using the following formula, calculate the overall average value of the brightness obtained in (4) L * 2 and overall average color value a * 2,b * Calculate the color difference ΔE of the measurement sample (1) relative to 2 for each of the measurement samples (1). The file is "TIFF0007576942000001.tif14150".

[0008] The invention of claim 2 of the present invention is "a decorative fiber sheet as described in claim 1, in which the color difference ΔE of the measurement samples is calculated using the above-mentioned [color difference variation measurement method], and the ratio of the number of measurement samples having a color difference ΔE of less than 0.5 to the total number of measurement samples is 90% or more."

[0009] The invention according to claim 3 of the present invention is "the decorative fiber sheet according to claim 1 or 2, one of the main surfaces of which is bonded with a fiber bonding binder resin."

[0010] The invention according to claim 4 of the present invention is "the decorative fiber sheet according to any one of claims 1 to 3, wherein the print contains cellulose nanofibers."

[0011] The invention according to claim 5 of the present invention is "the decorative fiber sheet according to claim 4, wherein the mass ratio of the cellulose nanofibers contained in the print is 0.5 to 5.0 mass % of the print mass."

[0012] The invention according to claim 6 of the present invention is "the decorative fiber sheet according to claim 4 or 5, wherein the average fiber diameter of the cellulose nanofibers is 8 nm or less." Effect of the Invention

[0013] The decorative fiber sheet according to claim 1 of the present invention is a decorative fiber sheet with little variation in the amount of printing on the decorative fiber sheet, and therefore with little variation in the color of the decorative fiber sheet, resulting in a decorative fiber sheet with excellent appearance quality.

[0014] The decorative fiber sheet according to claim 2 of the present invention has very few points where there is a large variation in color difference in the decorative fiber sheet, and therefore has little color variation in the decorative fiber sheet and is a decorative fiber sheet with excellent appearance quality.

[0015] The decorative fiber sheet according to claim 3 of the present invention has one main surface bonded with a fiber bonding binder resin, so that the decorative fiber sheet tends to be smooth, and therefore the print on the decorative fiber sheet is clear, resulting in a decorative fiber sheet with excellent appearance quality.

[0016] The decorative fiber sheet according to claim 4 of the present invention contains cellulose nanofibers in the print, which reduces color variation in the print contained in the decorative fiber sheet, making it possible to provide a decorative fiber sheet with excellent appearance quality. The reason for this is not completely clear, but it is thought that the fine fiber diameter of the cellulose nanofiber makes it easier and more effective to uniformly disperse the components of the printing liquid, resulting in less variation in the amount of print on the decorative fiber sheet.

[0017] The decorative fiber sheet according to claim 5 of the present invention has a mass ratio of cellulose nanofibers contained in the print of 0.5 to 5.0 mass% of the print mass, so that the color of the print contained in the decorative fiber sheet is less varied, and a decorative fiber sheet with excellent appearance quality can be provided. The reason for this is not completely clear, but when the mass ratio of cellulose nanofibers contained in the print is 0.5 mass% or more, the components of the print liquid are easily dispersed uniformly, and when the mass ratio of cellulose nanofibers contained in the print is 5.0 mass% or less, the cellulose nanofibers are less likely to aggregate, and in addition, the cellulose nanofibers are contained in the print liquid, so that the print liquid is more likely to behave uniformly against stress during printing. This is thought to be because, as a result, there is less variation in the amount of print liquid applied on the decorative fiber sheet, and therefore less variation in the amount of print on the decorative fiber sheet.

[0018] The decorative fiber sheet according to claim 6 of the present invention has an average fiber diameter of cellulose nanofibers contained in the print of 8 nm or less, which reduces color variation in the print contained in the decorative fiber sheet, thereby providing a decorative fiber sheet with excellent appearance quality. The reason for this is not completely clear, but it is thought that the fine fiber diameter of the cellulose nanofibers makes it easier to effectively and uniformly disperse the components of the printing liquid, resulting in less variation in the amount of print on the decorative fiber sheet. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a plan view showing the arrangement of one main surface of the decorative fiber sheets of Example 1 and Comparative Example 1 after only the print PA has been applied. [Diagram 2] FIG. 2 is a plan view showing the arrangement of one main surface of the decorative fiber sheets of Examples 2 and 3 and Comparative Example 2 after only the print PB has been applied. [Diagram 3] FIG. 2 is a plan view showing the arrangement of prints PA and PB on one main surface of the decorative fiber sheets of Examples 2 and 3 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In the present invention, various configurations can be appropriately selected, for example, the following configurations.

[0021] The decorative fiber sheet of the present invention has a print on one of its main surfaces, and the color difference ΔE of 50 or more measurement samples is calculated using a color difference variation measurement method described in detail below, and the ratio of the number of measurement samples with a color difference ΔE of less than 0.2 to the total number of measurement samples is 50% or more. Note that in the present invention, the "main surface" refers to the surface with the widest area.

[0022] Examples of fiber sheets that can be used to form the decorative fiber sheet of the present invention include nonwoven fabrics, woven fabrics, and knitted fabrics, but it is preferable for the fiber sheet to be composed of nonwoven fabric, as this can provide a decorative fiber sheet that is flexible and has a soft texture and excellent appearance.

[0023] Examples of the resin constituting the fibers of the fiber sheet include polyolefin resins (e.g., polyethylene, polypropylene, polymethylpentene, polyolefin resins having a structure in which a portion of a hydrocarbon is substituted with a cyano group or a halogen such as fluorine or chlorine), styrene resins, polyvinyl alcohol resins, polyether resins (e.g., polyether ether ketone, polyacetal, modified polyphenylene ether, aromatic polyether ketone, etc.), polyester resins (e.g., polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polycarbonate, polyarylate, wholly aromatic polyester resins, etc.), polyimide resins (e.g., ethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polycarbonate, polyarylate, wholly aromatic polyester resins, etc.), and the like. The insulating layer can be made of known organic resins such as polyacrylonitrile resins, polyamide-imide resins, polyamide-based resins (e.g., aromatic polyamide resins, aromatic polyetheramide resins, nylon resins, etc.), resins having nitrile groups (e.g., polyacrylonitrile), urethane-based resins, epoxy-based resins, polysulfone-based resins (e.g., polysulfone, polyethersulfone, etc.), fluorine-based resins (e.g., polytetrafluoroethylene, polyvinylidene fluoride, etc.), cellulose-based resins, polybenzimidazole resins, and acrylic-based resins (e.g., polyacrylonitrile-based resins copolymerized with acrylic acid esters or methacrylic acid esters, modacrylic-based resins copolymerized with acrylonitrile and vinyl chloride or vinylidene chloride, etc.).

[0024] These organic resins may be either linear or branched polymers, may be block or random copolymers, may have any three-dimensional structure, may have any crystallinity, or may be a mixture of multiple organic resins.

[0025] In addition, when flame retardancy is required for the decorative fiber sheet, it is preferable that the constituent fibers of the fiber sheet contain a flame retardant organic resin. Examples of such flame retardant organic resins include modacrylic resins, vinylidene resins, polyvinyl chloride resins, polyvinylidene fluoride resins, novoloid resins, polychlar resins, polyester resins copolymerized with phosphorus compounds, acrylic resins copolymerized with halogen-containing monomers, aramid resins, and resins kneaded with halogen-based, phosphorus-based, or metal compound-based flame retardants.

[0026] The constituent fibers can be obtained by known methods such as melt spinning, dry spinning, wet spinning, direct spinning (melt blowing, spunbonding, electrostatic spinning, etc.), a method of extracting fibers having a small fiber diameter by removing one or more resin components from composite fibers, and a method of beating fibers to obtain split fibers.

[0027] The constituent fibers may be made of one type of organic resin or may be made of multiple types of organic resins. Fibers made of multiple types of organic resins may be generally called composite fibers, such as core-sheath type, sea-island type, side-by-side type, orange type, bimetal type, and the like. The constituent fibers may also include irregular cross-sectional fibers other than fibers having a substantially circular or elliptical cross-sectional shape. The irregular cross-sectional fibers may be fibers having a fiber cross-section such as a hollow shape, a polygonal shape such as a triangular shape, an alphabet character shape such as a Y-shape, an indefinite shape, a multi-leaf shape, a symbol shape such as an asterisk shape, or a shape in which multiple of these shapes are combined. When the constituent fibers include heat-fusible fibers, the strength and shape stability of the decorative fiber sheet are excellent due to the heat fusion of the fibers, and further, the decorative fiber sheet has excellent appearance quality with less fluffing and less scattering of fibers. This is preferable. Such a heat-fusible fiber may be a fully fusible type heat-fusible fiber, or may be a partially fusible type heat-fusible fiber such as the above-mentioned composite fiber. The type of component that exhibits the heat-fusible property of the heat-fusible fiber is appropriately selected, and for example, a low-melting point polyolefin resin or a low-melting point polyester resin can be used.

[0028] When the fiber sheet contains a crimpable fiber, the fiber sheet has increased elasticity, excellent conformity to a mold, and excellent appearance quality, which is preferable. As such a crimpable fiber, for example, a crimpable fiber in which crimping of a latent crimpable fiber is expressed can be used.

[0029] The fineness of the constituent fibers of the fiber sheet is not particularly limited, but may be 0.01 dtex or more, 1 dtex or more, or 2 dtex or more so that the decorative fiber sheet is less prone to pilling and has excellent appearance quality. On the other hand, it may be 3 dtex or less so that the decorative fiber sheet has a homogeneous texture and therefore has excellent appearance quality. The "fineness" refers to a value measured according to the A method specified in JIS L 1015 (2010), 8.5.1.

[0030] The average fiber length of the fibers constituting the fiber sheet is not particularly limited, but can be 20 mm or more, 30 mm or more, or 35 mm or more, so that the decorative fiber sheet has a homogeneous texture and excellent appearance quality. On the other hand, if the average fiber length exceeds 110 mm, fiber clumps tend to form during the preparation of the fiber sheet, making the texture non-homogeneous, and there is a risk that a decorative fiber sheet with excellent appearance quality cannot be provided, so the average fiber length can be 110 mm or less. The "average fiber length" refers to a value measured according to the C method specified in JIS L 1015 (2010), 8.4.1.

[0031] The decorative fiber sheet of the present invention can be composed of, for example, the fibers described above, but if one main surface of the decorative fiber sheet is bonded with a fiber bonding binder resin, the decorative fiber sheet tends to be smooth, making the print on the decorative fiber sheet clearer and resulting in excellent appearance quality, which is preferable.

[0032] The type of fiber bonding binder resin that can be used in the decorative fiber sheet is appropriately selected, but examples of the binder resin that can be used include polyolefins (such as modified polyolefins), ethylene-vinyl alcohol copolymers, ethylene-acrylate copolymers such as ethylene-ethyl acrylate copolymers, various rubbers and their derivatives [styrene-butadiene rubber (SBR), fluororubber, urethane rubber, ethylene-propylene-diene rubber (EPDM), etc.], cellulose derivatives [carboxymethyl cellulose (CMC), hydroxyethyl cellulose, hydroxypropyl cellulose, etc.], polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinyl pyrrolidone (PVP), polyurethane, epoxy resins, polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), acrylic resins, etc. In particular, if the binder resin for fiber bonding contains an acrylic resin, it is preferable because it is moderately softened during heat molding such as heat pressing using a mold, and therefore a molded body with excellent moldability and excellent appearance quality can be formed.

[0033] The amount of fiber bonding binder resin contained in the decorative fiber sheet is appropriately selected, but the greater the amount of fiber bonding binder resin, the smoother the main surface of the decorative fiber sheet tends to be, and as a result, the decorative fiber sheet has excellent appearance quality, which is preferable. Therefore, the amount of fiber bonding binder resin contained in the fiber sheet is preferably 2 g / m 2 On the other hand, if the amount of the binder resin for bonding fibers is excessively large, the flexibility of the decorative fiber sheet may be deteriorated, and the decorative fiber sheet may not conform to the mold when molded. Therefore, the amount of the binder resin for bonding fibers is preferably 20 g / m or more. 2 It is preferable that the thickness is less than 10 g / m 2 It is preferable that:

[0034] The fiber adhesive binder resin may be present on only one or both of the main surfaces of the decorative fiber sheet. Since the main surface of a decorative fiber sheet having a fiber adhesive binder resin tends to be smooth, it is preferable that the fiber adhesive binder resin is present at least on the main surface having the print.

[0035] Furthermore, in addition to the above-mentioned resins, the binder resin for fiber adhesion may contain additives such as flame retardants, fragrances, pigments (inorganic pigments and / or organic pigments), antibacterial agents, antifungal agents, photocatalyst particles, emulsifiers, dispersants, thickeners, defoamers, and cellulose-derived materials. The various configurations of the fiber sheet, such as the thickness and basis weight, are not particularly limited and may be appropriately selected, but for example, the thickness of the fiber sheet may be 0.5 to 4.0 mm, 0.7 to 3.0 mm, or 1.0 to 2.0 mm. In addition, the basis weight of the fiber sheet is preferably 80 to 400 g / m2, because if the basis weight is too low, the sheet may break during molding, whereas if the basis weight is too high, the sheet may be poorly molded. 2 and 100 to 300 g / m 2 and 120 to 250 g / m 2 It can be.

[0036] In the present invention, the thickness is defined as a thickness of 20 g / cm in a direction perpendicular to the main surface of the object to be measured. 2 The vertical length of the object being measured when a compressive load of 1 m is applied. 2 This refers to the mass per unit.

[0037] The decorative fiber sheet of the present invention has a print on one of the main surfaces of the decorative fiber sheet. The resin that can be contained in the print can be any of the resins described above as usable as binder resins for bonding fibers.

[0038] Furthermore, if the print contains a cellulose-derived material in addition to the above-mentioned resin, the print in the decorative fiber sheet has less color variation and a decorative fiber sheet with excellent appearance quality can be provided, which is preferable. The reason for this is not completely clear, but it is thought that the cellulose-derived material makes it easier for the constituent components between the prints to be uniform. Note that the "cellulose-derived material" referred to here refers to a material whose main component is cellulose or a derivative thereof. Among these, the cellulose-derived material is more preferably cellulose nanofiber because of its small fiber diameter and excellent dispersibility, and TEMPO-oxidized cellulose nanofiber is even more preferable among cellulose nanofibers because of its uniform fiber diameter and excellent dispersibility.

[0039] When the cellulose-derived material is a cellulose nanofiber, the smaller the average fiber diameter, the better the dispersibility and the better the compatibility with other materials, so the average fiber diameter is preferably 100 nm or less, more preferably 10 nm or less, even more preferably 8 nm or less, and even more preferably 5 nm or less. The lower limit of the average fiber diameter is practically 1 nm or more. The average fiber length of the cellulose nanofiber is not particularly limited, but is preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 200 nm or more. If the average fiber length is too long, the cellulose nanofibers may become entangled with each other and may not be sufficiently dispersed in the print, so the upper limit is practically 300 nm. The average fiber diameter and average fiber length can be calculated by observing the cellulose nanofiber with an electron microscope, randomly selecting 50 cellulose nanofibers from the obtained image, and averaging them.

[0040] The mass ratio of the cellulose nanofibers contained in the print is preferably 0.5 to 5.0 mass% of the print mass, since this provides a decorative fiber sheet with less color variation in the print contained in the decorative fiber sheet, excellent appearance quality, and excellent abrasion resistance. The reason for the excellent appearance quality is not completely clear, but it is believed that the mass ratio of the cellulose nanofibers is 0.5 mass% or more of the print mass, so that the components of the print liquid are easily dispersed uniformly, and the mass ratio of the cellulose nanofibers is 5.0 mass% or less of the print mass, so that the cellulose nanofibers are less likely to aggregate, resulting in less variation in the amount of the print liquid applied on the decorative fiber sheet and less variation in the amount of the print on the decorative fiber sheet. The reason for the excellent abrasion resistance is also not completely clear, but it is believed that the cellulose nanofibers make it easy to uniformly disperse the components of the print and can retain the components of the print. The mass ratio of the cellulose nanofibers contained in the print is more preferably 0.7 to 3.5 mass%, and even more preferably 1.0 to 2.5 mass%.

[0041] Furthermore, in addition to the above-mentioned resins and cellulose-derived materials, the print may contain the additives mentioned above as being contained in the binder resin for bonding fibers.

[0042] The form of the print on the main surface of the decorative fiber sheet can be selected as appropriate, and can be a form that covers the entire main surface, or a form that covers only a portion of the main surface with a pattern such as lines, dots, or an irregular shape.

[0043] The print may be of one type or of multiple types, and the types of the additives contained in the prints may be different for each print.

[0044] As long as the print is present on at least one of the main surfaces of the decorative fiber sheet, a print may also be present on the other main surface of the decorative fiber sheet.

[0045] In addition, the print may not penetrate into the fiber sheets that make up the decorative fiber sheet, but may be present only on the surface of the decorative fiber sheet, or the print may penetrate into the fiber sheets that make up the decorative fiber sheet. However, if the print penetrates into the fiber sheets that make up the decorative fiber sheet, this is preferable because the printed pattern will remain even if it is worn away by surface friction, and the design will be maintained.

[0046] The mass of the print is appropriately selected, but in order to obtain a decorative fiber sheet with excellent design, it is set to 1 g / m 2 It can be more than 1.5 g / m 2 It can be more than 2 g / m 2 If the mass of the print is too large, the moldability of the decorative fiber sheet may be deteriorated during molding, so the mass of the print should be 20 g / m or more. 2 and can be 15 g / m or less. 2 It can be the following:

[0047] The decorative fiber sheet of the present invention has a color difference ΔE calculated for 50 or more measurement samples using the following [Color Difference Variation Measurement Method], and the ratio of the number of measurement samples with a color difference ΔE of less than 0.2 to the total number of measurement samples is 50% or more. The color difference ΔE can be used to numerically express the difference in color of one measurement sample from the average color of the measurement samples, making it possible to confirm the degree of color variation in the decorative fiber sheet. [Color difference variation measurement method] (1) Cut the decorative fiber sheet into 50 or more rectangular measurement samples measuring 5 cm x 15 cm. (2) Using a spectrophotometer, measure the lightness L of the main surface having the print of the measurement sample in (1). * and chromaticity a * ,b * (CIE1976L * a * b * Color space) is measured at three points per sample without overlapping within a measurement range of 2.5 cm in reflection measurement diameter. (3) The average brightness of the three points on one sample measured in (2) L * 1 and the individual average value of chromaticity a * 1,b * Calculate 1 for each measurement sample in (1). (4) The individual average lightness of all the measured samples obtained in (3) L * 1 and the individual average value of chromaticity a * 1,b * Take the average value of 1 and calculate the overall average value L of the brightness of the entire measured sample. * 2 and overall average color value a * 2,b * Find 2. (5) The overall average value of the brightness obtained in (4) is calculated using the following formula: * 2 and overall average color value a * 2,b * Calculate the color difference ΔE of the measurement sample (1) relative to 2 for each of the measurement samples (1). TIFF0007576942000002.tif14150

[0048] The greater the ratio of the number of measurement samples with a color difference ΔE of less than 0.2 calculated by the above-mentioned color difference variation measurement method to the total number of measurement samples, the more excellent the appearance quality of the decorative fiber sheet, so the ratio of the number of measurement samples with a color difference ΔE of less than 0.2 to the total number of measurement samples is preferably 55% or more, more preferably 60% or more, and even more preferably 65% ​​or more. Such a decorative fiber sheet can be manufactured, for example, by the manufacturing method described below.

[0049] Furthermore, if the number of measurement samples with a color difference ΔE of less than 0.1 calculated by the above-mentioned color difference variation measurement method is 50% or more of the total number of measurement samples, this is preferable because it results in less variation in the amount of print coating in the decorative fiber sheet, which in turn results in less variation in the color of the decorative fiber sheet and excellent appearance quality.

[0050] Furthermore, if the ratio of the number of measurement samples with a color difference ΔE of less than 0.5 calculated by the above-mentioned color difference variation measurement method to the total number of measurement samples is 90% or more, this is preferable because there are very few points in the decorative fiber sheet where the color difference varies greatly, and therefore there is less color variation in the prints contained in the decorative fiber sheet, resulting in excellent appearance quality.

[0051] The number of measurement samples used to calculate the color difference ΔE should be 50 or more, but the more samples used, the more accurately the color variation of the decorative fiber sheet can be evaluated, so it is more preferable to use 75 or more samples, and even more preferable to use 100 or more samples.

[0052] The various configurations of the decorative fiber sheet, such as its thickness and basis weight, are not particularly limited and may be selected appropriately, but for example, the thickness of the decorative fiber sheet may be 0.6 to 4.5 mm, 0.8 to 3.0 mm, or 1.3 to 1.8 mm. The basis weight of the decorative fiber sheet may be 83 to 440 g / m 2 and 120 to 340 g / m 2 and 180 to 220 g / m 2 It can be.

[0053] The decorative fiber sheet of the present invention may further comprise another component such as a porous body, film or foam on a main surface side different from the main surface on which the print is present.

[0054] Next, a method for producing the decorative fiber sheet of the present invention will be illustrated and described.

[0055] First, a fiber sheet such as a woven fabric, knitted fabric, or nonwoven fabric is prepared using the above-mentioned fibers. The method for preparing the fiber sheet is not particularly limited, but when the fiber sheet is a woven fabric or knitted fabric, it can be prepared by weaving or knitting the above-mentioned fibers. When the fiber sheet is a nonwoven fabric, it can be prepared by, for example, a dry method in which the above-mentioned fibers are fed to a carding device or an air-laying device to entangle the fibers, a wet method in which the fibers are dispersed in a solvent and woven into a sheet to entangle the fibers, or a direct spinning method, but it is preferable that the fiber sheet has a certain degree of bulk so that it has excellent moldability when molded into a decorative fiber sheet, so it is preferable to adopt a dry method in which the fibers are entangled by feeding the fibers to a carding device or an air-laying device.

[0056] The fiber sheet formed as described above is preferably entangled with a water stream or needles so as to be easy to handle. In particular, it is preferable to entangle with needles so as not to impair the thickness and, as a result, the moldability when the decorative fiber sheet is molded. There are no particular limitations on the suitable needle entanglement conditions, but a needle density of 300 to 1000 needles / cm is preferable. 2 It is preferable to intertwine the fibers at 300 to 600 strands / cm. 2 It is more preferable that the fibers are entangled with

[0057] If necessary, the fiber sheet may be thermocompressed after it is formed. The term "thermocompression bonding" does not mean that the fibers are melted or plasticized and deformed to bond, but that the fibers are densely attached to each other due to the heat and pressure that reduces the interfiber voids. Thermocompression bonding of the fiber sheet causes a slight microscopic shrinkage and a smooth surface, which allows a clear print to be formed when printing is performed, and is preferable because the fibers are less likely to get caught due to friction, resulting in excellent abrasion resistance.

[0058] If necessary, a part or all of the heat-fusible fibers constituting the fiber sheet may be melted by heat treatment to fuse the constituent fibers together. The heat treatment method can be appropriately selected, and examples of the method that can be used include a method of heating or heating and pressurizing the fiber sheet with a roll, a method of heating the fiber sheet by subjecting it to a heater such as an oven dryer, a far-infrared heater, a dry heat dryer, or a hot air dryer, and a method of irradiating infrared rays without pressure to heat the organic resin contained in the fiber sheet.

[0059] Furthermore, if necessary, the fiber sheet may be subjected to a pressure treatment step such as pressing to smooth the surface of the fiber sheet.

[0060] Furthermore, it is preferable that the fiber-bonding binder resin liquid is applied by a method such as impregnation, coating, or spraying, and then dried to bond the constituent fibers of the fiber sheet with the fiber-bonding binder resin.

[0061] Finally, a printing liquid is applied to one of the main surfaces of the fiber sheet to produce a decorative fiber sheet having a print on one of the main surfaces of the fiber sheet. If the printing liquid contains the above-mentioned cellulose-derived material, the color of the print is less varied, and a decorative fiber sheet with excellent appearance quality can be provided, which is preferable. The method of applying the printing liquid is not particularly limited, but a method can be adopted in which, for example, a cylinder with through holes on the entire surface, such as a cylindrical silk screen, is prepared, and the printing liquid is extruded from the inside of the cylindrical silk screen through the through holes of the cylinder and applied to one of the main surfaces of the fiber sheet, and the dispersion medium / solvent is removed from the applied printing liquid. Note that, when applying the printing liquid, it is preferable to allow the printing liquid to permeate into the fiber sheet, since this makes it easier to obtain a decorative fiber sheet with excellent abrasion resistance. The method of removing the dispersion medium / solvent is appropriately adjusted, but for example, the dispersion medium / solvent can be removed by heating and drying the fiber sheet to which the printing liquid has been applied with a dryer.

[0062] The viscosity of the printing liquid can be adjusted as appropriate by the printing method and the hole diameter of the cylinder, and it cannot be generalized because the viscosity of the printing liquid decreases as the stress applied to the liquid increases. However, if the viscosity of the printing liquid is too high, there is a tendency for the printing liquid to clog the through holes of the cylinder, resulting in pattern chipping, or pattern chipping due to uneven application of the printing liquid, or pattern chipping due to the printing liquid separating from the fiber sheet when the screen is separated. If the viscosity of the printing liquid is too low, there is a tendency for the liquid to leak from the screen. Therefore, the viscosity of the printing liquid should be measured at a shear rate of 3600 cm using an E-type viscometer. -1 In this case, it is preferable that the density is 50 to 100 cp.

[0063] When the printing liquid contains cellulose nanofibers, the inclusion of cellulose nanofibers in the printing liquid makes it possible to provide a decorative fiber sheet with less color variation, excellent appearance quality, and excellent abrasion resistance. However, if the printing liquid contains too much cellulose nanofibers, the viscosity of the printing liquid will become too high, and the cellulose nanofibers in the printing liquid will tend to aggregate, resulting in pattern chipping due to the printing liquid clogging the through holes in the cylinder, pattern chipping due to uneven application of the printing liquid, and pattern chipping due to the printing liquid separating from the fiber sheet when the screen is separated. Therefore, the concentration of cellulose nanofibers in the printing liquid is preferably 0.01 to 0.45 wt%, more preferably 0.05 to 0.40 wt%, and even more preferably 0.10 to 0.30 wt%.

[0064] In addition, various secondary processes such as punching out shapes according to the purpose and usage are also carried out. It may be served as a. EXAMPLES

[0065] (Preparation of hot-pressurized needle-punched nonwoven fabric) Polyester dyed fiber (fineness: 2.2 dtex, fiber length: 38 mm, brightness L * :81.0, chromaticity a * :-2.0, chromaticity b* :-2.0, color: blue-based) was used 100%, and the fibers were opened by a carding machine to form a fiber web, and then the needle density was 400 / cm from one side. 2 The needle-punched nonwoven fabric was then passed through a pair of rolls (slit: 0.6 mm) consisting of a heated roll and a non-heated roll so as to come into contact with a roll set at a temperature of 170°C, to produce a heated and pressed needle-punched nonwoven fabric (basis weight: 180 g / m 2 , thickness: 1.5 mm) was formed.

[0066] (Preparation of binder resin liquid for fiber bonding) A binder resin liquid for bonding fibers was prepared according to the following formulation. Acrylic resin binder: 6 parts by weight Surfactant: 0.2 parts by weight Water...93.8 parts by weight

[0067] (Preparation of binder-bonded nonwoven fabric) Next, the above-mentioned binder resin liquid for fiber adhesion was applied in a foamed state to the surface opposite to the surface that had been subjected to the needle punching treatment of the heated and pressurized needle punched nonwoven fabric. The fabric was then dried in a can dryer at a temperature of 160°C to obtain a binder-bonded nonwoven fabric (basis weight: 185 g / m 2 , thickness: 1.5 mm) was prepared.

[0068] (Preparation of Printing Liquid A) A printing liquid A having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight 10 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water...65 parts by weight The viscosity of printing liquid A is 94cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in printing liquid A was 0.1 wt%.

[0069] (Preparation of Printing Liquid B) A printing liquid B having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight Water...75 parts by weight The viscosity of printing liquid B is 110cp (E-type viscometer, shear rate 3600cm -1 ) was.

[0070] (Preparation of Printing Liquid C) A printing liquid C having the following composition was prepared. Acrylic resin binder: 14 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight White pigment: 1 part by weight 25% ammonia water: 1 part by weight 10 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water...72 parts by weight The viscosity of printing liquid C is 85cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in printing liquid C was 0.1 wt%.

[0071] (Preparation of Printing Fluid D) A printing liquid D having the following composition was prepared. Acrylic resin binder: 14 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight White pigment: 1 part by weight 25% ammonia water: 1 part by weight Water...82 parts by weight The viscosity of printing liquid D is 98cp (E-type viscometer, shear rate 3600cm -1 ) was.

[0072] (Preparation of Printing Liquid E) A printing liquid E having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight 20 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water...55 parts by weight The viscosity of the printing liquid E is 98cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in printing liquid E was 0.2 wt%.

[0073] (Preparation of Printing Fluid F) A printing liquid F having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight 30 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water...45 parts by weight The viscosity of the printing liquid F is 102cp (E-type viscometer, shear rate 3600cm -1) and the concentration of cellulose nanofibers contained in the printing liquid F was 0.3 wt%.

[0074] (Preparation of Printing Liquid G) A printing liquid G having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution ··· 5 parts by weight Water...70 parts by weight The viscosity of the printing liquid G is 102cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in the printing liquid G was 0.05 wt %.

[0075] (Preparation of Printing Fluid H) A printing liquid H having the following composition was prepared. Acrylic resin binder: 12.5 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight 10 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water...73.5 parts by weight The viscosity of the printing liquid H is 80cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in printing liquid H was 0.1 wt%.

[0076] (Preparation of Printing Liquid I) A printing liquid I having the following composition was prepared. Acrylic resin binder: 7.3 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight White pigment: 1 part by weight 25% ammonia water: 1 part by weight 10 parts by weight of 1% TEMPO-oxidized cellulose nanofiber (average fiber diameter: 4 nm, average fiber length: 200 nm, product name: Cellenpia TC-01A (manufactured by Nippon Paper Industries Co., Ltd.)) aqueous solution Water: 78.7 parts The viscosity of printing liquid I is 95cp (E-type viscometer, shear rate 3600cm -1 ) and the concentration of cellulose nanofibers contained in printing liquid I was 0.1 wt%.

[0077] (Preparation of Printing Fluid J) A printing liquid J having the following composition was prepared. Acrylic resin binder: 21 parts by weight Acrylic thickener: 1 part by weight Silicone defoaming agent: 1 part by weight Black pigment: 1 part by weight 25% ammonia water: 1 part by weight Carboxymethylated cellulose nanofiber powder (average fiber diameter: 20 nm, continuous fiber with a mesh structure, manufactured by Nippon Paper Industries Co., Ltd.) ··· 0.1 part by weight Water...74.9 parts by weight The viscosity of the printing liquid J is 110cp (E-type viscometer, shear rate 3600cm -1 The concentration of cellulose nanofibers in the printing liquid J was 0.1 wt%.

[0078] Example 1 Next, the surface of the binder-bonded nonwoven fabric on which the binder resin liquid for fiber bonding was applied was printed with the printing liquid A in a "L" shape using a cylinder. After that, it was dried with a dryer at a temperature of 160°C, and the "L"-shaped print P was obtained as shown in FIG. ADecorative fiber sheet (basis weight: 195g / m 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 The mass ratio of the TEMPO oxidized cellulose nanofiber contained in the print: 1.0 mass% was produced. When the main surface of the decorative fiber sheet having the print was observed, 2 In addition, when the cross section of the decorative fiber sheet was observed, the print P A had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0079] Example 2 On the surface of the binder-bonded nonwoven fabric described above that had been coated with the fiber-bonding binder resin liquid, multiple "L"-shaped prints were made with printing liquid A using a cylinder. Before the prints dried, multiple straight lines were printed again with printing liquid C using a cylinder diagonally upward to the right as shown in Figure 2 (line width 0.24 mm, line spacing 0.56 mm, angle: 45°). After that, it was dried with a dryer at a temperature of 160°C, and the "L"-shaped print P was left as shown in Figure 3. A and a straight line going diagonally upwards to the right B Decorative fiber sheet (weight: 200g / m 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P A Mass ratio of TEMPO oxidized cellulose nanofiber contained in: 1.0 mass%, Print P B The mass ratio of TEMPO oxidized cellulose nanofibers contained in the sheet was 2.0 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0080] Example 3 A decorative fiber sheet (basis weight: 200 g / m) was prepared in the same manner as in Example 2, except that printing liquid D was used instead of printing liquid C. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P A The mass ratio of TEMPO oxidized cellulose nanofiber contained in the sheet was 1.0 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0081] Example 4 A decorative fiber sheet (basis weight: 200 g / m2) was produced in the same manner as in Example 3, except that printing liquid E was used instead of printing liquid A. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P A The mass ratio of TEMPO oxidized cellulose nanofibers contained in the sheet was 2.0 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0082] Example 5 A decorative fiber sheet (basis weight: 200 g / m) was prepared in the same manner as in Example 3, except that printing liquid F was used instead of printing liquid A. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P A The mass ratio of TEMPO oxidized cellulose nanofibers contained in the sheet was 3.0 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print PA and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0083] Example 6 A decorative fiber sheet (basis weight: 200 g / m) was prepared in the same manner as in Example 3, except that printing liquid G was used instead of printing liquid A. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P A The mass ratio of TEMPO oxidized cellulose nanofiber contained in the sheet was 0.5 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0084] Example 7 On the surface of the binder-bonded nonwoven fabric described above that had been coated with the fiber-bonding binder resin liquid, multiple "L"-shaped prints were made with printing liquid H using a cylinder. Before the prints dried, multiple straight lines were printed again with printing liquid I using a cylinder diagonally upward to the right as shown in Figure 2 (line width 0.24 mm, line spacing 0.56 mm, angle: 45°). After that, it was dried with a dryer at a temperature of 160°C, and the "L"-shaped print P was left as shown in Figure 3. A and a straight line going diagonally upwards to the right B Decorative fiber sheet (weight: 200g / m 2 , Thickness: 1.5mm, Print P A Mass: 6g / m 2 , Print P B Mass: 3g / m 2 , Print P A Mass ratio of TEMPO oxidized cellulose nanofiber contained in: 1.7 mass%, Print P BThe mass ratio of TEMPO oxidized cellulose nanofibers contained in the sheet was 3.3 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0085] Comparative Example 1 A decorative fiber sheet (basis weight: 195 g / m) was produced in the same manner as in Example 1, except that printing liquid B was used instead of printing liquid A. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 In addition, when the cross section of the decorative fiber sheet was observed, it was found that the printed P A had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0086] Comparative Example 2 A decorative fiber sheet (basis weight: 200 g / m2, thickness: 1.5 mm, printed P) was prepared in the same manner as in Example 3, except that printing liquid B was used instead of printing liquid A. A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 In addition, when the cross section of the decorative fiber sheet was observed, it was found that the printed P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0087] Comparative Example 3 A decorative fiber sheet (basis weight: 200 g / m) was produced in the same manner as in Example 3, except that printing liquid J was used instead of printing liquid A. 2 , Thickness: 1.5mm, Print P A Mass: 10g / m 2 , Print P B Mass: 5g / m 2 , Print P AThe mass ratio of carboxymethylated cellulose nanofibers contained in the sheet was 1.0 mass%. In addition, when the cross section of the decorative fiber sheet was observed, the print P A and P B had penetrated into the binder-bonded nonwoven fabric that constituted the decorative fiber sheet.

[0088] (Reference example 1) The binder-bonded nonwoven fabric (basis weight: 185 g / m2) described above has no print on one main surface of the fiber sheet. 2 , thickness: 1.5 mm) was prepared.

[0089] In addition, the color difference ΔE of the measurement samples cut from the decorative fiber sheets of Example 1, Comparative Example 1, and Reference Example 1 was measured by subjecting them to the above-mentioned [Color Difference Variation Measurement Method]. The measurement samples used in the color difference variation measurement method were prepared by first preparing rectangular decorative fiber sheets of Example 1, Comparative Example 1, and Reference Example 1, each having a length of 125 cm in the longitudinal direction and 60 cm in the transverse direction, cutting the decorative fiber sheet into four pieces with a length of 15 cm in the transverse direction of the decorative fiber sheet, and then cutting each of the cut decorative fiber sheets into 25 rows with a length of 5 cm in the longitudinal direction to prepare 100 rectangular measurement samples having a size of 5 cm x 15 cm. In addition, an integrating sphere spectrophotometer (Color i5, manufactured by X-Rite Inc.) was used as the spectrophotometer for the measurement.

[0090] The measurement results of ΔE for 100 sheets of measurement samples in Example 1, Comparative Example 1, and Reference Example 1 are summarized by ΔE value. Table 1 below shows the Examples, and Table 2 shows the Comparative Examples and Reference Examples.

[0091] [Table 1]

[0092] [Table 2]

[0093] Furthermore, the decorative fiber sheets of the Examples and Comparative Examples were subjected to the following sensory test to evaluate the appearance quality. The evaluation results are shown in Table 3 below. Furthermore, the decorative fiber sheets of the Examples and Comparative Examples were subjected to the following abrasion resistance measurement to evaluate the abrasion resistance. The evaluation results are shown in Table 4 below.

[0094] [Sensory test] When visually inspecting the main surface bearing the print of the decorative fiber sheets of the Examples and Comparative Examples, 10 panelists (A to J) evaluated the appearance quality, i.e., whether or not there was any variation in the color of the print, on a three-point scale (1: noticeable to 3: not noticeable), and the arithmetic mean value of the evaluation was calculated.

[0095] [Table 3]

[0096] [Wear resistance measurement] A Taber rotary abrasive was used to apply a load of 2.45 N to an abrasive wheel CS-10 on the main surface carrying the print of the decorative fiber sheets of the Examples and Comparative Examples, bringing the abrasive wheel into contact with the main surface, and the abrasive wheel was rotated 50, 100, and 200 times at a speed of 60 rpm. The surface condition of the main surface was then examined and evaluated based on the following evaluation criteria. 5: There is absolutely no change in the surface of the abrasive wheel compared to before and after it was rotated. 4: There is some fuzziness on the surface. 3: Fuzz can be seen over the entire surface, but the length of the fluff is short, less than 1 mm. 2: Fuzz can be seen over the entire surface, the length of the fluff is longer than 1 mm, and the fluff is partially tangled on the surface, forming pills. 1: Fuzz can be seen all over the surface, the length of the fluff is more than 1mm, and the fluff is tangled all over the surface, forming pills.

[0097] [Table 4]

[0098] From the results of the color difference variation measurement method in Example 1, Comparative Example 1, and Reference Example 1, it was found that the color difference variation occurs due to the print on the decorative fiber sheet, not the fiber sheet itself. Also, from the results of the color difference variation measurement method in the Examples and Comparative Examples, it was found that by using a print containing TEMPO oxidized cellulose nanofiber, a decorative fiber sheet with small color difference variation can be realized. Furthermore, from the results of the sensory test, it was found that the decorative fiber sheet of the present invention can realize a decorative fiber sheet with excellent appearance quality, since the color difference ΔE of 100 measurement samples was calculated using the color difference variation measurement method, and the number of measurement samples with a color difference ΔE of less than 0.2 was 50% or more of the total number of measurement samples. Furthermore, A and Print P B Print P A Examples 3 to 5 containing 1.0 mass% or more of cellulose nanofibers only, and Print P A and Print P B From the results of the abrasion resistance measurement of Comparative Example 2, which did not contain cellulose nanofibers, it was found that prints containing 1.0 mass % or more of cellulose nanofibers with small fiber diameters had excellent abrasion resistance. [Industrial Applicability]

[0099] The decorative fiber sheet of the present invention can be used as a surface material for various interior materials, particularly as a surface material for interior materials for vehicles such as ceilings, door sides, pillar garnishes, and rear packages. [Explanation of symbols]

[0100] P A Print P B Print

Claims

1. A needle-punched nonwoven fabric made of dyed polyester fibers and heated and pressed has one main surface bonded with a fiber-bonding binder resin containing an acrylic resin, the needle-punched nonwoven fabric has a print on one main surface, and the fiber-bonding binder resin is present on at least the main surface having the print, the print comprises TEMPO oxidized cellulose nanofibers; The decorative fiber sheet has an average fiber length of the TEMPO oxidized cellulose nanofibers of 50 nm or more and 300 nm or less, A decorative fiber sheet in which the color difference ΔE of 50 or more measurement samples is calculated using the following [Color Difference Variation Measurement Method], and the ratio of the number of measurement samples with a color difference ΔE of less than 0.2 to the total number of measurement samples is 50% or more. [Color difference variation measurement method] (1) Cut the decorative fiber sheet into 50 or more rectangular measurement samples measuring 5 cm x 15 cm. (2) Using a spectrophotometer, the lightness L of the main surface having the print of the measurement sample in (1) is measured. * and chromaticity a * , b * (CIE 1976L * a * b * The color space) is measured at three points per sample without overlapping within a measurement range of 2.5 cm in reflection measurement diameter. (3) (2) The average brightness L of the three points on one sample measured * 1 and the individual average chromaticity a * 1 , b * 1 is calculated for each measurement sample in (1). (4) The individual average value L of the brightness of all the measurement samples obtained in (3) * 1 and the individual average chromaticity a * 1 , b * 1 The average value of the brightness of the entire measured sample is taken as L * 2 and the overall average chromaticity a * 2 , b * 2 Request. (5) The overall average value L of the brightness obtained in (4) is calculated using the following formula: * 2 and the overall average chromaticity a * 2 , b * 2 The color difference ΔE of the measurement sample (1) with respect to the above is calculated for each of the measurement samples (1).

2. A decorative fiber sheet as described in claim 1, wherein the color difference ΔE of the measurement samples is calculated using the above-mentioned [Color Difference Variation Measurement Method], and the ratio of the number of measurement samples having a color difference ΔE of less than 0.5 to the total number of measurement samples is 90% or more.

3. The decorative fiber sheet according to claim 1, wherein the mass ratio of the cellulose nanofiber contained in the print is 0.5 to 5.0 mass% of the print mass.

4. The decorative fiber sheet according to claim 1 or 3, wherein the average fiber diameter of the cellulose nanofibers is 8 nm or less.

Citation Information

Patent Citations

  • Decoration fiber sheet for automobile

    JP2012179985A

  • Print nonwoven fabric

    JP2014214395A

  • Aqueous pigment dispersion and aqueous ink

    JP2016148044A

  • Aqueous ink composition and aqueous ink composition for inkjet