Slide member and piston ring

The DLC coating on piston rings with specific Raman spectrum and hardness properties, combined with intermediate layers, addresses wear issues in boundary lubrication environments, achieving reduced wear and cost-effective durability.

JP7577245B1Active Publication Date: 2024-11-01RIKEN CO LTD

Patent Information

Application Number
JP2024517584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-02
Publication Date
2024-11-01
Estimated Expiration
2043-10-02

AI Technical Summary

Technical Problem

Piston rings with hard DLC coatings wear rapidly in boundary lubrication environments due to direct metal-to-metal contact, and increasing DLC thickness for durability increases manufacturing costs.

Method used

A DLC coating on piston rings with a central wave number of 1585 cm⁻¹ in the Raman spectrum, hardness of 15-35 GPa, and an elastic modulus ratio of 0.095 or more, combined with an intermediate layer of Cr, Ti, Co, V, Mo, Si, or W carbides/nitrides/carbonitrides, enhances wear resistance.

Benefits of technology

The DLC coating reduces wear by half compared to conventional methods, allowing thinner films and improved adhesion, thus maintaining durability without increasing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577245000003
    Figure 0007577245000003
  • Figure 0007577245000004
    Figure 0007577245000004
  • Figure 0007577245000005
    Figure 0007577245000005
Patent Text Reader

Abstract

The present invention provides a sliding member and a piston ring having a DLC coating that has excellent wear resistance even when used in a boundary lubrication environment. The sliding member according to the present invention is a sliding member having a substrate and a DLC coating that is substantially free of hydrogen and is formed on the surface of the substrate, and the central wave number of the G band in the Raman spectrum of the DLC coating obtained by Raman spectroscopy using a visible laser as excitation light is 1585 cm. -1 The hardness H of the DLC coating obtained by the nanoindentation method, expressed in gigapascals, IT is greater than 15 GPa and less than 35 GPa.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sliding member and a piston ring. [Background technology]

[0002] Piston rings are a type of sliding component that are attached to the pistons of internal combustion engines to maintain airtightness between the piston and the cylinder. Two or three piston rings are attached near the head of the piston, and act as a seal to prevent the combustion gases generated in the cylinder from leaking out to the crankshaft. They also have the function of controlling the thickness of the engine oil film formed on the inner wall of the cylinder. They also have the function of releasing the combustion heat received by the piston back to the cylinder.

[0003] In addition to these basic functions, piston rings are also required to be durable. In particular, the outer circumferential surface of the piston ring is required to be wear-resistant because it rubs against the inner wall of the cylinder as the piston reciprocates. In order to reduce the sliding friction between the piston ring and the inner wall of the cylinder, the formation of a hard carbon coating on the surface of the piston ring substrate has been studied.

[0004] For example, Patent Document 1 describes an invention of a member in which a hard carbon layer made of diamond-like carbon (hereinafter sometimes referred to as "DLC") is formed on the surface of a substrate, and when the hard carbon layer is measured by Raman spectroscopy, ID / IG, which is the area intensity ratio of the peaks of the D band and the G band in the Raman spectroscopy spectrum, is 1 to 6. Patent Document 2 describes an invention of a member in which hard carbon layers made of two types of DLC with different properties are alternately laminated on the surface of a substrate. All of these hard carbon layers according to the prior art are formed while applying a bias voltage to the substrate and heating the substrate with a heater at the same time. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-123431 A [Patent Document 2] International Publication No. 2017 / 104822 Summary of the Invention [Problem to be solved by the invention]

[0006] In the prior art, a method for increasing the durability of piston rings has been to form a DLC coating with as high a hardness as possible on the surface of the piston ring base material. By having a DLC coating with high hardness on the surface of the piston ring, wear of the DLC coating on the outer circumferential surface of the piston ring that rubs against the inner wall of the cylinder can be effectively prevented. This would extend the product life of the piston ring, and it was thought that the frequency of replacing the piston ring could be reduced.

[0007] In recent automobile engines, there is a trend to increase the combustion temperature of gasoline in the cylinder, use engine oil with lower viscosity than before, and reduce the amount of engine oil used in order to meet the demands for higher power output and stricter exhaust gas regulations. With these new technological trends, the lubrication between the outer circumferential surface of the piston ring and the inner wall of the cylinder is changing from a fluid lubrication environment in which a continuous oil film made of engine oil is formed as in the past, to a boundary lubrication environment in which direct metal-to-metal contact occurs locally in areas where the oil film is thin.

[0008] According to the research of the inventors, it was found that when a piston ring having a hard DLC film on its surface is used in a boundary lubrication environment, the wear of the DLC film on the outer peripheral surface of the piston ring is more likely to progress than in a hydrodynamic lubrication environment. This suggests that for piston rings used in a boundary lubrication environment, it is difficult to ensure the necessary wear resistance for the piston ring by simply increasing the hardness of the DLC film as in the past.

[0009] In addition, in the conventional technology, when trying to improve the durability of a piston ring by using a DLC coating with high hardness, the thickness of the DLC coating must be made thick to a certain extent, which poses a problem that the manufacturing cost of the piston ring increases because it takes time to form the DLC coating.

[0010] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a sliding member and a piston ring provided with a DLC coating that has excellent wear resistance even when used in a boundary lubrication environment. [Means for solving the problem]

[0011] The gist and configuration of the present invention are as follows.

[0012] [1] A slide member having a substrate and a DLC coating that is substantially free of hydrogen and is formed on a surface of the substrate, The central wave number of the G band in the Raman spectrum of the DLC film obtained by Raman spectroscopy using a visible laser as excitation light is 1585 cm -1 That's all. The hardness H of the DLC coating measured by nanoindentation, expressed in gigapascals IT is between 15GPa and 35GPa A sliding member characterized by: [2] The elastic modulus of the DLC film obtained by the nanoindentation method, expressed in gigapascals, is E IT When IT Elastic modulus E IT Ratio to H IT / E IT is 0.095 or more The sliding member described in [1]. [3] An intermediate layer is provided between the substrate and the DLC coating, the intermediate layer being made of one or more elements selected from the group consisting of Cr, Ti, Co, V, Mo, Si and W, or a carbide, nitride or carbonitride thereof. The sliding member according to [1] or [2]. [4] A piston ring comprising a sliding member according to any one of [1] to [3]. Effect of the Invention

[0013] According to the present invention, the amount of sliding wear of the DLC film when a sliding member having a DLC film slides against a counter material is suppressed compared to the conventional technology. This improves the wear resistance of the sliding member. In addition, the thickness of the DLC film can be made thinner than in the past. [Brief description of the drawings]

[0014] [Figure 1] 3A to 3C are schematic diagrams showing examples of cross-sectional shapes of sliding members. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a cross-sectional shape of a base material of a piston ring. [Diagram 3] FIG. 2 is a schematic diagram showing the structure of a sliding wear tester. [Figure 4] 1 is a graph showing the relationship between the central wave number of the G band in the Raman spectrum of a DLC film obtained by Raman spectroscopy and the sliding friction amount ratio. [Diagram 5] 1 is a graph showing the relationship between the hardness of a DLC film obtained by a nanoindentation method and the sliding friction ratio. [Figure 6] 1 is a graph showing the relationship between the ratio of hardness to elastic modulus of a DLC film and the sliding friction amount ratio. [Figure 7] 1 is a graph showing the relationship between the peak area intensity ratio ID / IG of the D band and the G band in the Raman spectrum of a DLC coating obtained by Raman spectroscopy and the sliding friction amount ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described in detail.

[0016] [Sliding parts] In one embodiment, the present invention is an invention of a sliding member. FIG. 1 is a schematic diagram showing an example of a cross-sectional shape of a sliding member according to the present invention. The sliding member 100 has a substrate 10 and a DLC coating 12 that is formed on the surface of the substrate 10 and does not substantially contain hydrogen. The sliding member 100 according to the present invention has excellent wear resistance, and can be applied to various products, such as piston rings, pistons, piston pins, tappets, valve lifters, shims, rocker arms, cams, camshafts, timing gears, timing chains, etc. used in sliding parts of internal combustion engines in which lubricating oil such as engine oil is present, and vanes, injectors, plungers, cylinders, etc. used in fuel supply systems.

[0017] [Base material] The slide member according to the present invention has a substrate and a DLC coating that is substantially free of hydrogen and formed on the surface of the substrate. The substrate is a member that becomes the main body of the slide member. The material and shape of the substrate constituting the slide member according to the present invention may be any material and shape as long as the material and shape allow the formation of a DLC coating on the surface.

[0018] [DLC coating] The sliding member according to the present invention has a DLC coating formed on the surface of a substrate. The DLC coating is a coating made of diamond-like carbon, which is amorphous carbon that exhibits properties similar to those of diamond. The DLC coating of the sliding member according to the present invention may be formed directly on the surface of the substrate, or may be formed on the surface of one or more intermediate layers formed on the surface of the substrate.

[0019] The DLC film of the sliding member according to the present invention is substantially free of hydrogen. In this specification, the term "DLC film substantially free of hydrogen" refers to a DLC film having a diamond-like carbon content of 2.0% or less in atomic percentage. The DLC film is softened by containing hydrogen. In the present invention, the DLC film of the sliding member is a DLC film having substantially no hydrogen, thereby ensuring the hardness required for the DLC film defined in the present invention, which will be described later. The amount of hydrogen contained in the DLC film is preferably 1.0% or less in atomic percentage, and more preferably 0.5% or less.

[0020] [Method for measuring the amount of hydrogen contained in DLC film] The hydrogen content of the DLC film can be measured by Rutherford Backscattering Spectrometry (RBS) / Hydrogen Forward Scattering Spectrometry (HFS) for DLC films formed on flat sliding surfaces or surfaces with a sufficiently large curvature. RBS / HFS is a known method for analyzing film composition, but cannot be applied to the analysis of non-flat surfaces. For this reason, the hydrogen content of DLC films formed on non-flat sliding surfaces such as the outer peripheral surface of a piston ring can be measured by combining RBS / HFS and Secondary Ion Mass Spectrometry (SIMS). The procedure is described below.

[0021] First, a DLC film to be measured as a reference value is formed on a mirror-polished flat test piece (hardened SKH51 disk, φ25 × thickness 5 mm, hardness HRC60-63) as a reference sample with a flat surface. The film is formed on the reference sample using a reactive sputtering method, with C2H2, Ar, and H2 introduced as atmospheric gases. The amount of hydrogen contained in the DLC film is adjusted by changing the flow rate of H2 and / or C2H2 introduced. In this way, DLC films composed of hydrogen and carbon and with different hydrogen contents are formed, and the hydrogen and carbon contents are evaluated by RBS / HFS.

[0022] Next, the above sample is analyzed by SIMS to measure the secondary ion intensity of hydrogen and carbon. Here, SIMS analysis can also be performed on a non-flat surface, such as a DLC film formed on the outer peripheral surface of a piston ring. Therefore, for the same film of a reference sample with a DLC film, an empirical formula (metric curve) is obtained that shows the relationship between the hydrogen content and carbon content (unit: atomic %) obtained by RBS / HFS and the ratio of the secondary ion intensity of hydrogen and carbon obtained by SIMS. In this way, the hydrogen content and carbon content can be calculated from the secondary ion intensity of hydrogen and carbon measured by SIMS on the outer peripheral surface of an actual piston ring. The value of the secondary ion intensity by SIMS is the average value of the secondary ion intensity of each element observed at least at a depth of 20 nm or more from the surface of the DLC film and within a range of 50 nm square.

[0023] [DLC film formation method] In the present invention, in order to form a DLC film that is substantially free of hydrogen on the surface of the substrate of the sliding member, the DLC film may be formed by using a PVD method such as an ion plating method by vacuum arc discharge using a carbon target. The PVD method can form a DLC film that is almost free of hydrogen, has high hardness, and is excellent in wear resistance. It is preferable to use a filtered cathodic vacuum arc method (FCVA method) that is equipped with a filter that removes carbon microparticles. However, the method for forming a DLC film that is substantially free of hydrogen is not limited to these methods.

[0024] The DLC coating may be formed on at least a part of the surface of the substrate, and may be formed over the entire surface of the substrate. When the DLC coating is formed on a part of the surface of the substrate, it is preferable to form the DLC coating on a part of the surface of the sliding member that is particularly required to have wear resistance. In this case, the surface of the formed DLC coating constitutes the sliding surface of the sliding member.

[0025] [G band central wave number] The DLC coating of the sliding member according to the present invention has a central wave number of the G band of 1585 cm in the Raman spectrum of the DLC coating obtained by Raman spectroscopy using a visible laser as excitation light. -1 That is all. The Raman spectrum of a DLC film can be obtained by measuring a sliding member having a DLC film formed on its surface using Raman spectroscopy. A visible laser beam is used as the excitation light when measuring the Raman spectrum. When it is desired to measure the Raman spectrum for each part of the sliding member, a Raman microscope can be used.

[0026] The G band in the Raman spectrum of the DLC film is due to the sp 2 It is believed that the central wave number of the G band is related to the bonding component and changes according to the change in the crystal structure of graphite. The central wave number of the G band in the present invention was determined by the following procedure. First, the central wave number of the G band was determined by the following procedure. -1 After subtracting the background in the range of 1350 cm -1 The peak near 1550 cm is the D band. -1 The peak near the center of the spectrum was assumed to be the G band, and fitting was performed with two Gaussian functions. Next, the wavenumber of the peak position of the separated G band spectrum was calculated, and this wavenumber was set as the central wavenumber of the G band.

[0027] In the present invention, the central wave number of the G band in the Raman spectrum of the DLC film is 1585 cm -1When the DLC coating of a sliding member satisfies this condition, the amount of wear when sliding friction occurs between the sliding member and a mating material is reduced, compared to a sliding member having a DLC coating according to the conventional technology, which serves as the standard for comparison.

[0028] The amount of wear of the DLC film on the sliding member when sliding friction occurs between the sliding member and the counter member is measured when the central wave number of the G band in the Raman spectrum of the DLC film is 1585 cm -1 Although it is not clear why it decreases when the value is above this level, the following is thought to be the most likely reason. As mentioned above, it is thought that the central wavenumber of the G band changes according to changes in the crystal structure of the graphite contained in the DLC film. It is speculated that the load and heat caused by the sliding make it easier for a protective film called a tribofilm to form on the surface of the DLC film, and that the wear phenomenon known as abrasive wear, in which the surface is scraped away by foreign matter present between the frictional surfaces, is suppressed.

[0029] The central wave number of the G band is 1585 cm -1 There is no particular upper limit as long as it is equal to or greater than this. However, it is believed that there is a limit to the amount of shift in the G band caused by changes in the crystal structure of graphite. For this reason, the central wave number of the G band is essentially 1610 cm -1 Limited to the following:

[0030] [DLC film hardness] The sliding member according to the present invention has a hardness H of the DLC film obtained by the nanoindentation method, which is expressed in gigapascals. ITThe hardness is 15 GPa or more and 35 GPa or less. In this specification, the term "nanoindentation method" refers to a measurement method based on the nanoindentation hardness test method specified in the international standard ISO14577. In this method, a tiny diamond indenter with a regular triangular pyramid (Berkovich type) tip shape is pressed into the surface of the sample, and the hardness and elastic modulus of a micro-area can be measured by measuring the load-displacement curve at that time. In order to avoid the influence of the base material that is the base of the DLC film, the indentation load is set so that the maximum indentation depth of the diamond indenter is 1 / 10 or less of the film thickness. In addition, as a pretreatment for the test, the test area is mirror-polished to reduce the variation in the test value.

[0031] Hardness H of DLC film measured by nanoindentation method IT It is known that the hardness H of the DLC film varies greatly depending on the conditions for forming the DLC film. For example, the hardness of graphite is about 4 GPa, and the hardness of diamond is 90 to 100 GPa. The hardness H of the DLC film of the sliding member according to the present invention is IT lies between these values.

[0032] DLC film hardness H IT If the hardness H of the DLC film is less than 15 GPa, the amount of wear of the DLC film increases when sliding friction occurs with a sliding member. IT If the hardness H of the DLC film is greater than 35 GPa, abrasive wear is likely to occur due to the generation of wear debris, and the amount of wear of the DLC film will also increase. IT If is too small or too large, the amount of wear of the DLC film increases. IT When the compressive strength is within the range of 15 GPa or more and 35 GPa or less as specified in the present invention, the wear amount of the DLC film is reduced to less than half that of the DLC film according to the conventional technology, which is used as the standard for comparison.

[0033] [DLC film thickness] In a preferred embodiment, the thickness of the DLC coating of the sliding member according to the present invention is not particularly limited, but is preferably 1.0 μm or more and 30 μm or less. If it is 1.0 μm or more, the durability of the DLC coating is sufficient, and if it is 30 μm or less, the adhesion to the base material is insufficient and peeling does not occur. More preferably, the thickness of the DLC coating is 5.0 μm or more and 20.0 μm or less. The thickness of the DLC coating can be measured by Calotest or by observing the cross section of the coating embedded in resin.

[0034] [Ratio of DLC film hardness to elastic modulus] In a preferred embodiment, the elastic modulus of the DLC film obtained by nanoindentation, expressed in gigapascals, is defined as E IT When IT Elastic modulus E IT Ratio to H IT / E IT The elastic modulus E of the DLC film is 0.095 or more. IT is an index that indicates the resistance of the DLC film to elastic deformation when a load is applied. The elastic modulus E of the DLC film IT The smaller the hardness H, the more flexibly the DLC film deforms when the sliding component with the DLC film is pressed against the counter material. IT When comparing when the values ​​are the same, the ratio H IT / E IT It is considered that the larger the value, the more flexibly the DLC film deforms, and therefore the progression of abrasive wear of the DLC film is suppressed.

[0035] In a preferred embodiment, the ratio H of the hardness to the elastic modulus of the DLC coating is IT / E IT The ratio of the elastic modulus to the hardness of a material is generally correlated to a certain extent, and the ratio H of the elastic modulus to the hardness expressed in the same units for a DLC film that does not substantially contain hydrogen is IT / E IT is substantially limited to 0.120 or less.

[0036] [Middle layer] In a preferred embodiment, the sliding member according to the present invention further has an intermediate layer between the substrate and the DLC coating, the intermediate layer being made of one or more elements selected from the group consisting of Cr, Ti, Co, V, Mo, Si, and W, or carbides, nitrides, or carbonitrides thereof. The intermediate layer is provided on at least a portion of the surface of the substrate. The presence of the intermediate layer on the surface of the substrate relieves stress between the substrate and the DLC coating, improving the adhesion of the DLC coating.

[0037] The intermediate layer may cover at least a part of the surface of the substrate, or may cover the entire surface. When a piston ring is selected as the substrate of the sliding member, for example, the outer peripheral surface of the piston ring may be covered. This is preferable because it improves the adhesion of the DLC coating on the outer peripheral surface. When the entire surface of the substrate is covered, the intermediate layer may be left covering the entire surface of the substrate, or the substrate may be exposed by removing unnecessary portions of the intermediate layer by polishing or the like after forming the intermediate layer.

[0038] The thickness of the intermediate layer is preferably 0.1 μm or more and 0.6 μm or less, and more preferably 0.2 μm or more and 0.5 μm or less. If the thickness is 0.1 μm or more, the adhesion of the DLC film can be increased, and if the thickness is 0.6 μm or less, the intermediate layer is less likely to undergo plastic flow during sliding, and the DLC film is less likely to peel off. The intermediate layer can be formed on the substrate by, for example, suitably using a known PVD (physical vapor deposition) method.

[0039] [Piston rings] In another embodiment, the present invention is an invention of a piston ring. The piston ring according to the present invention is a piston ring made of the sliding member according to the present invention. The base material of the piston ring according to the present invention is made of steel having a ring shape. The steel used for the base material is not particularly limited as long as it has properties such as strength, elastic modulus, and thermal conductivity required for a piston ring. As the steel, it is preferable to use carbon steel, spring steel, martensitic stainless steel, etc. The piston ring according to the present invention has a ring shape, and a gap is provided in a part of the ring shape. The piston ring is mounted in a groove provided on the outer peripheral surface of the piston in a state in which the gap is closed and the diameter is reduced. In the cylinder, the outer peripheral surface of the piston ring slides while being pressed against the inner wall of the cylinder by tension.

[0040] Fig. 2 is a schematic diagram showing an example of a cross-sectional shape of a substrate of a piston ring according to the present invention. In Fig. 2, a DLC coating, which will be described later, is omitted. As shown in Fig. 2, a piston ring 200 includes a substrate 20 whose cross section approximates a rectangle. However, there are many variations in the cross-sectional shape of the substrate 20 constituting the piston ring, and it does not necessarily have to be rectangular.

[0041] The outer peripheral surface 22 is a surface that is located outside the outer peripheral surface of the piston when the piston ring 200 is attached to a groove of the piston (not shown) and slides in contact with the inner wall of the cylinder. The shape of the outer peripheral surface 22 may be a flat shape as shown in FIG. 2, a barrel shape with a central portion bulging outward, or a tapered shape with a diameter that changes continuously depending on the position. As described above, the outer peripheral surface 22 is required to have wear resistance that makes it difficult to wear due to sliding against the inner wall surface of the cylinder. In the piston ring according to the present invention, a DLC coating (not shown) is formed on the outer peripheral surface 22.

[0042] The side surfaces 24a, 24b are surfaces where the piston ring 200 comes into contact with a groove of a piston (not shown). An upper side surface 24a and a lower side surface 24b are shown in FIG. 2. An inner peripheral surface 28 is located on the opposite side of the outer peripheral surface 22. Outer peripheral edges 26a, 26b are located at the boundaries between the outer peripheral surface 22 and the side surfaces 24a, 24b. Generally, the outer peripheral edges 26a, 26b are chamfered (not shown) to prevent chipping of the base material 20.

[0043] [Slip fatigue test] A method for evaluating the wear amount of the DLC film on a sliding member when sliding friction is caused between the sliding member and a counter member according to the present invention will be described. FIG. 3 is a schematic diagram showing an outline of a method for performing a sliding fatigue test for this evaluation. A sliding fatigue tester 300 used in the sliding fatigue test has a rotating drum 30. The sliding fatigue tester 300 repeatedly applies a load while pressing the surface of a test piece 32 against the outer circumferential surface of the drum 30 by a drive mechanism (not shown). The wear amount of the DLC film formed on the surface of the test piece 32 is obtained by measuring the change in the dimensions of the test piece 32 before and after the test. This is divided by the wear amount of a standard sample obtained under the same conditions to obtain a sliding wear amount ratio.

[0044] The test conditions for carrying out the sliding fatigue test are exemplified below. The drum 30, which is the mating material against which the test piece 32 slides, is a cylindrical member with a diameter of 80 mm. The material constituting the drum 30 is preferably a steel with high wear resistance, for example, a bearing steel of steel type number SUJ2 specified in the Japanese Industrial Standard JIS G 4805 "High Carbon Chromium Bearing Steel Material". The speed of the circumferential surface of the drum 30 rotating relative to the fixed test piece 32 is 10.0 m / s. The rotation of the drum 30 is accelerated from a stationary state to a speed of 10.0 m / s in 30 seconds, held at the speed of 10.0 m / s for 20 seconds, and then decelerated to zero speed in 30 seconds. Next, the rotation direction is reversed, and acceleration, holding, and deceleration are repeated, forming one cycle, and 10 cycles are repeated.

[0045] A load is repeatedly applied to the test piece 32 by a drive mechanism (not shown), and the test piece 32 is pressed perpendicularly against the outer circumferential surface of the drum 30. The magnitude of the load is set to a maximum load of 50 N and a minimum load of 20 N, and the load is changed over time between the maximum load and the minimum load in a sine wave shape with a frequency of 50 Hz. The surface temperature of the drum 30 is maintained at 80°C by a heater (not shown). Additive-free motor oil is supplied from the tip of the oil supply pipe 34 at a rate of 0.1 cm per minute. 3 The oil is supplied to the surface of the drum 30 at a rate of 1000 to 15000 rpm. This oil supply rate is insufficient for fluid lubrication, creating a boundary lubrication environment. EXAMPLES

[0046] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0047] As the substrate for the piston ring, a substrate made of silicon chrome steel was prepared, having a ring shape with a cross section approximating a rectangle. The size of the substrate was a nominal diameter of 78 mm, a thickness of 2.5 mm, and a width of 1.2 mm. The shape of the outer peripheral surface was a barrel face with a slight bulge in the center. The outer peripheral edge of the substrate was chamfered with a width of 0.15 mm. Using a cathodic arc ion plating device (M720, manufactured by Nippon ITF Co., Ltd.), the outer peripheral surface of the substrate was coated with an intermediate layer made of chrome with a thickness of 0.5 μm.

[0048] Next, the substrate was degreased and washed, and then set in a cathodic arc ion plating device with the sides in contact with each other. The surface was cleaned by ion bombardment treatment, and the outer peripheral surface of the substrate was coated with a DLC film using an ion plating method by vacuum arc discharge. After the DLC film was formed, the DLC film that had spread around to the side was removed using a honing device and a lapping device, and a plurality of piston rings of Examples 1 to 5 and Comparative Examples 1 to 9 shown in Table 1 were obtained. The film formation conditions for the DLC film are shown in Table 1.

[0049] [Table 1]

[0050] The set bias in Table 1 is the bias voltage of the substrate set on the equipment during film formation. Regardless of the set bias value, the bias voltage holding circuit of the equipment functions to hold the bias voltage at the set bias value. The measured bias in Table 1 is the bias voltage of the substrate actually monitored during film formation. Even if the set bias is set to zero, the substrate is charged by the charge of the carbon ions, and a non-zero bias voltage is measured. This is sometimes called the self-bias voltage. When a self-bias voltage occurs, the carbon ions are accelerated and their energy increases, making it easier for the substrate temperature to rise even when not heated by a heater.

[0051] As shown in Examples 1 to 4, when the absolute value of the self-bias voltage is greater than the absolute value of the set bias, the measured bias voltage is dominated by the self-bias voltage and is not affected by the set bias. Also, when the set bias is the same, the measured bias changes depending on the magnitude of the arc current.

[0052] The term "floating potential" in Example 5 means that the bias voltage holding circuit of the device is cut off and the bias voltage is not controlled. In this case, too, the substrate is charged by the charge of the carbon ions.

[0053] Regarding the deposition rates shown in Table 1, "fast" indicates that the deposition rate is faster than the conditions of Comparative Example 1 used as a reference, "same" indicates that the deposition rate is the same, and "slow" indicates that the deposition rate is slower.

[0054] The piston ring samples thus obtained were subjected to the following evaluations. First, the Raman spectrum of the DLC coating on the outer peripheral surface of the piston ring was measured using a Raman spectrometer (Renishaw, inViaReflex). Measurements were performed under the following conditions: Ar ion excitation laser wavelength 532.0 nm, laser output 50 mW, objective lens 100x, and light passed through a light attenuator. From the obtained Raman spectrum data, the central wave number of the G band and ID / IG, which is the area intensity ratio of the D band and G band peaks, were calculated.

[0055] Next, the hardness H of the DLC film was measured by the nanoindentation method conforming to the international standard ISO14577 using a nanoindenter (Elionix, model number ENT-1100a). IT and the elastic modulus E IT The ratio of hardness to elastic modulus H was calculated from the measured values. IT / E IT was calculated.

[0056] Next, using a sliding fatigue tester shown in Figure 3, the sliding wear amount of the DLC coating of the piston ring was measured under the above-mentioned test conditions. For the measurement, a test piece with a length of about 20 mm including the outer peripheral surface cut from the piston ring sample was used. In the sliding wear test, the wear amount after 10 cycles of one-hour tests was measured, and the ratio of the wear amount to the wear amount of Comparative Example 1, which served as a benchmark, was calculated and used as the sliding wear amount ratio. These evaluation results are shown in Table 2. The central wave number of the G band and the hardness H IT , ratio H IT / E IT The relationship between the ratio ID / IG and the sliding wear ratio is shown in Figures 4 to 7, respectively.

[0057] [Table 2]

[0058] According to Table 2 and Figure 4, the central wave number of the G band is 1585 cm -1 Among the piston rings having the above values, those of Examples 1 to 5 had significantly less sliding wear than those of Comparative Example 1 having a DLC coating according to the conventional technology, which was used as the standard for comparison. -1 The sliding wear amounts of the piston rings of Comparative Examples 2 to 7, which did not exceed 100 mm, were larger than that of Comparative Example 1, or slightly smaller, but no significant improvement was observed. In Comparative Examples 8 and 9, the hardness of the DLC coating, which will be described later, was insufficient, and the sliding wear amounts increased compared to Comparative Example 1.

[0059] According to Table 2 and Figure 5, the hardness H IT Among the piston rings having a pressure of 15 GPa or more and 35 GPa or less, the piston rings of Examples 1 to 5 had significantly less sliding wear than Comparative Example 1. As described above, Comparative Examples 3, 4, and 6 have a central wave number of the G band of 1585 cm -1 Therefore, the amount of sliding wear was not significantly smaller than that of Comparative Example 1. From the above results, it is understood that the sliding member according to the present invention has superior wear resistance compared to the prior art, and that the film formation speed can be increased by appropriately adjusting the film formation conditions.

[0060] Next, according to Figure 6, the ratio of hardness to elastic modulus H IT / E IT A good correlation was observed between the hardness and the sliding wear ratio, except for Comparative Example 5, which had an extremely high hardness. IT / E IT The amount of sliding wear was smaller than that of Comparative Example 1 when the modulus of elasticity E was in the range of 0.095 or more. This is because, when comparing DLC ​​films having the same hardness, IT This suggests that the smaller the value, the more flexible the DLC film is against repeated loads, thereby reducing the amount of sliding wear.

[0061] On the other hand, according to Table 2 and FIG. 7, no clear correlation was found between ID / IG, which is the area intensity ratio of the peaks of the D band and the G band described in Patent Document 1, and the sliding wear amount ratio.

[0062] As described above, the DLC coatings of Examples 1 to 5, which showed good abrasion resistance, were all formed without heating the substrate with a heater under conditions where the set bias was 0 V or a floating potential and the self-bias voltage was about 0 V to -35 V. In contrast, the DLC coating of Comparative Example 4, in which the set bias was set to a non-zero value similar to the conventional film formation conditions, had a central wavenumber of the G band of 1585 cm -1 The slip wear ratio did not improve, and the DLC coating deposited with a non-zero bias had a hard sp 3 This is thought to be because there is a tendency for clusters to increase.

[0063] As for heater heating, it is preferable to adjust the temperature of the substrate only by heating with arc current, without using heater heating. This is because heater heating tends to increase the adhesion of foreign matter such as macroparticles from the coating formed on places other than the substrate during film formation, leading to an increase in the amount of wear. Thus, in the sliding member according to the present invention, the central wave number of the G band and the hardness H IT By adjusting the DLC film formation conditions shown in Table 1 so that the above properties fall within the specified ranges, excellent sliding friction properties can be obtained. [Explanation of symbols]

[0064] 100 Sliding member 10 Base material 12 DLC coating 200 Piston rings 20 Base material 22 Outer surface 24a, 24b side 26a, 26b Outer edge 28 Inner surface 300 Slip fatigue testing machine 30 Dram 32 Test specimen 34 Fuel Pipe

Claims

1. A slide member having a substrate and a DLC coating that is substantially free of hydrogen and is formed on a surface of the substrate, The central wave number of the G band in the Raman spectrum of the DLC coating obtained by Raman spectroscopy using a visible laser as excitation light is 1589.5 cm -1 That's all. The hardness H of the DLC coating measured by nanoindentation, expressed in gigapascals IT is 17.0 GPa or more and 33.4 GPa or less A sliding member characterized by:

2. The elastic modulus of the DLC film obtained by the nanoindentation method, expressed in gigapascals, is E IT When IT Elastic modulus E IT Ratio to H IT / E IT is 0.095 or more The sliding member according to claim 1 .

3. The DLC coating further includes an intermediate layer between the substrate and the DLC coating, the intermediate layer being made of one or more elements selected from the group consisting of Cr, Ti, Co, V, Mo, Si, and W, or a carbide, nitride, or carbonitride thereof. The sliding member according to claim 1 .

4. A piston ring comprising the sliding member according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • High abrasion resistance and high seizure resistance slide member, and method for manufacturing the same

    JP2003336542A

  • Friction coefficient estimation device and method of DLC film

    JP2009031064A

  • DLC film and DLC coating die

    JP2013136511A

  • Piston ring

    JP2020200803A

  • Piston ring and coating

    JP2021116870A

Cited By

  • Combination of sliding members, and gas compressor

    WO2026182232A1

  • Combination of sliding members, and gas compressor

    WO2026182233A1