Pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, laminate, and display including said laminate
The adhesive composition, featuring a specific acrylic polymer and curing agent, addresses the challenges of automotive adhesive requirements by enhancing adhesive strength, heat resistance, and other properties, particularly when using biologically derived materials.
Patent Information
- Application Number
- JP2022209352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing adhesives for optical displays, particularly those used in automotive applications, face challenges in achieving high adhesive strength, heat resistance, moist heat whitening resistance, outgassing resistance, light resistance, low dielectric constant, and metal corrosion resistance, especially when using biological materials.
An adhesive composition comprising an acrylic polymer with specific monomer ratios and a curing agent, including a silane coupling agent, to enhance properties such as adhesive strength, heat resistance, and low dielectric constant, while using biologically derived materials.
The adhesive composition demonstrates excellent adhesive strength, heat resistance, moist heat whitening resistance, outgassing resistance, light resistance, low dielectric constant, and metal corrosion resistance, making it suitable for demanding applications like automotive displays.
Smart Images

Figure 0007577253000007 
Figure 0007577253000008 
Figure 0007577253000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, a pressure-sensitive adhesive sheet, a laminate, and a display including the laminate. [Background technology]
[0002] Adhesive sheets having an adhesive layer formed from an adhesive are easy to handle and are therefore used in a wide range of fields such as label applications, medical applications, etc. Among them, adhesives used in applications where long-term use is expected, such as marking films, window films, automotive parts, optical displays, etc., require durability such as heat resistance, moist heat resistance, weather resistance, and light resistance, and in recent years, active research has been conducted to improve the durability of adhesives.
[0003] Various optical displays, such as liquid crystal displays (LCDs) and organic electroluminescence displays (OLEDs), are widely used as display devices. In addition to being used as display devices, optical displays are also used as input devices such as touch panels. A cover panel is installed on the touch panel to protect the surface. Usually, the components that make up these optical displays are bonded together via an adhesive layer.
[0004] As mentioned above, adhesives for optical displays, which are expected to be used for a long time, are required to have high durability, such as not floating or peeling from the adherend in high temperature / high humidity environments (peel resistance), not discoloring the adhesive layer itself to white (humid heat whitening resistance), and not discoloring the adhesive layer itself to yellow (yellowing resistance). In addition to the above durability, adhesives used to fix cover panels made of transparent plastic materials such as polycarbonate (PC) and polymethyl methacrylate (PMMA) are required to not cause appearance defects due to gases generated from the transparent plastic (outgassing resistance). Furthermore, if the dielectric constant of the adhesive used around the capacitive touch panel is high, it tends to cause malfunctions when touching the display, so adhesives that can form adhesive layers with low dielectric constants are required, and they are also required to have properties that do not corrode such metal materials, assuming that they will be used for transparent electrodes.
[0005] In terms of durability, displays, especially those for in-vehicle use, require high durability. In particular, due to the recent revolutionary advances in information technology such as the 5th generation mobile communication system (5G), Internet of Things (IoT), and artificial intelligence (AI), the development of automobiles equipped with electrical equipment and external displays is progressing, and the required performance is becoming even stricter, requiring heat resistance at higher temperatures such as 120°C (previously around 85-105°C). Therefore, it has been a major challenge to develop an adhesive that satisfies all of the requirements, such as heat resistance at higher temperatures and the continued resistance to moist heat whitening and outgassing, which have been required up until now.
[0006] Up until now, many studies have been conducted to satisfy the durability required for adhesives for optical displays. For example, the adhesive described in Patent Document 1 uses an acrylic adhesive obtained by copolymerizing a hydroxyl-containing acrylic ester and a nitrogen-containing acrylic ester in order to impart resistance to moist heat whitening and outgassing, but the heat resistance and light resistance at 120°C are insufficient. In addition, the adhesive described in Patent Document 2 uses an acrylic adhesive obtained by copolymerizing an acrylic acid alkyl ester having 4 to 8 carbon atoms and N-(2-hydroxyethyl)acrylamide as monomers in order to suppress display unevenness, but the heat resistance, moist heat whitening resistance, outgassing resistance, and adhesion at 120°C are insufficient.
[0007] In addition to the increasing performance requirements, the depletion of petroleum resources and carbon dioxide emissions from the combustion of petroleum-derived products are becoming issues in the industries in which PSA sheets are used. Therefore, attempts are being made to conserve petroleum resources by using bio-derived materials instead of petroleum-derived materials in various industries, starting with the packaging materials field, as well as the optical and semiconductor fields.
[0008] In a pressure-sensitive adhesive mainly composed of an acrylic polymer, a method for increasing the ratio of biologically derived materials includes a method for obtaining an acrylic polymer by copolymerizing a monomer mixture containing a linear alkyl alcohol produced from a living organism and a (meth)acrylic acid alkyl ester monomer obtained by esterifying (meth)acrylic acid. Since linear alcohols derived from living organisms are currently distributed at a relatively low cost and in stable quantities, they can be used industrially. For example, Patent Document 3 discloses a pressure-sensitive adhesive obtained by copolymerizing a monomer mixture containing a biomass-derived acrylate having an alkyl group with 12 to 24 carbon atoms, but the conditions for the heat resistance retention test are low temperature and short time, and even if it is cleared, it is insufficient in reality. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2017-106000 A [Patent Document 2] JP 2007-264092 A [Patent Document 3] JP 2020-105308 A Summary of the Invention [Problem to be solved by the invention]
[0010] The problem that the present invention aims to solve is to provide an adhesive and adhesive sheet that have adhesive strength, heat resistance, resistance to moist heat whitening, resistance to outgassing, light resistance, low dielectric constant, and resistance to metal corrosion, even when using biological materials. [Means for solving the problem]
[0011] As a result of extensive investigations, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have thus completed the present invention. That is, the present invention provides a pressure-sensitive adhesive composition comprising an acrylic polymer (A) and a curing agent (B), wherein the acrylic polymer (A) is a copolymer of a monomer mixture comprising the following (a1), (a2) and (a3): The present invention relates to a pressure-sensitive adhesive composition comprising, based on 100 mass% of a monomer mixture, 2.5 to 20 mass% of (a1), 30 to 80 mass% of (a2), and 0.1 to 20 mass% of (a3). (a1) (meth)acrylic acid ester monomer having an alicyclic structure (excluding (a3)) (a2) (Meth)acrylic acid alkyl ester monomer having a linear alkyl group having 8 to 18 carbon atoms (a3) (meth)acrylic acid ester monomer having a carboxy group and / or (meth)acrylic acid ester monomer having a hydroxy group
[0012] The present invention also relates to the above pressure-sensitive adhesive composition, wherein (a3) contains a (meth)acrylic acid ester monomer having a hydroxy group.
[0013] The present invention also relates to the above pressure-sensitive adhesive composition, wherein the monomer mixture further contains (a4) a (meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 4 carbon atoms.
[0014] The present invention also relates to the above pressure-sensitive adhesive composition, further comprising a silane coupling agent (C).
[0015] The present invention also relates to the above pressure-sensitive adhesive composition, wherein the curing agent (B) contains an isocyanate-based curing agent or a blocked product thereof.
[0016] The present invention also relates to a pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition.
[0017] The present invention also relates to a laminate comprising the above pressure-sensitive adhesive sheet and a light-transmitting substrate.
[0018] The present invention also relates to a display comprising the above laminate, a polarizing plate, and an optical element. Effect of the Invention
[0019] The present invention aims to provide an adhesive and adhesive sheet that have adhesive strength, heat resistance, resistance to moist heat whitening, resistance to outgassing, light resistance, low dielectric constant, and resistance to metal corrosion, even when a biologically derived material is used. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic cross-sectional view partially showing a laminate of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view partially illustrating a display, which is an example of the use of the laminate of the present invention. [Diagram 3] Schematic cross-sectional view of a dielectric constant measurement sample DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The pressure-sensitive adhesive, pressure-sensitive adhesive sheet, laminate and display of the present invention will be described below, but the present invention is not limited thereto. In this specification, the term "(meth)acrylic acid ester" includes acrylic acid ester and methacrylic acid ester. The term "monomer" refers to a monomer having an ethylenically unsaturated group. In addition, in this specification, a numerical range specified by "~" includes the numerical values written before and after "~" as the range of the lower and upper limits. Furthermore, "film" and "sheet" are not distinguished by thickness. In other words, in this specification, a "sheet" includes a thin film-like material, and a "film" includes a thick sheet-like material. Furthermore, the adherend refers to a counterpart to which the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is attached. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types.
[0022] <<Adhesive composition>> The pressure-sensitive adhesive composition of the present invention contains an acrylic polymer (A) and a curing agent (B).
[0023] <Acrylic polymer (A)> The acrylic polymer (A) is a copolymer of a monomer mixture containing the monomers (a1), (a2), and (a3) described below, and is characterized in that it contains 2.5 to 20 mass% of (a1), 30 to 80 mass% of (a2), and 0.1 to 20 mass% of (a3) based on 100 mass% of the monomer mixture.
[0024] [Monomer (a1)] (a1) is a (meth)acrylic acid ester monomer having an alicyclic structure. However, in this specification, a (meth)acrylic acid ester monomer having a carboxy group or a hydroxy group is considered to be monomer (a3) even if it has an alicyclic structure. Examples of the alicyclic structure include a cycloalkane structure, a cycloalkene structure, and an alicyclic ether structure. From the viewpoint of yellowing resistance, a cycloalkane structure or an alicyclic ether structure having no unsaturated bond in the ring is preferred.
[0025] Examples of the monomer (a1) include isobornyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, (5-ethyl-1,3-dioxane-5-yl)methyl (meth)acrylate, etc. Among them, from the viewpoint of outgas resistance and increasing the ratio of biologically derived materials, isobornyl (meth)acrylate and tetrahydrofurfuryl (meth)acrylate, which can be produced from alcohol available as a biomass raw material, are more preferable.
[0026] The content of (a1) is 2.5 to 20% by mass, preferably 5 to 15% by mass, and more preferably 7 to 13% by mass, based on 100% by mass of the monomer mixture. If the content of (a1) is less than 2.5% by mass, the cohesive strength of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance. If the content of (a1) is more than 20% by mass, the tack of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance.
[0027] [Monomer (a2)] (a2) is a (meth)acrylic acid alkyl ester monomer having a linear alkyl group with 8 to 18 carbon atoms. Since (meth)acrylic acid alkyl ester monomers with such a carbon number are available as biologically derived materials, the ratio of biologically derived materials can be increased by using these. In addition, the polarity of the entire adhesive layer can be reduced, thereby reducing the dielectric constant. In addition, since the alkyl group is linear, it can be partially crystallized in the adhesive layer, thereby increasing heat resistance.
[0028] Examples of monomer (a2) include normal octyl (meth)acrylate, normal nonyl (meth)acrylate, normal decyl (meth)acrylate, normal undecyl (meth)acrylate, normal dodecyl (meth)acrylate, normal tridecyl (meth)acrylate, normal tetradecyl (meth)acrylate, normal pentadecyl (meth)acrylate, normal hexadecyl (meth)acrylate, normal heptadecyl (meth)acrylate, and normal octadecyl (meth)acrylate.
[0029] The content of (a2) is 30-80% by mass, preferably 40-70% by mass, and more preferably 50-60% by mass, based on 100% by mass of the monomer mixture. If the content of (a2) is less than 30% by mass, sufficient biological material cannot be used in the adhesive and adhesive layer, and the dielectric constant becomes too high to be used in electronic devices with high-frequency signal transmission functions. If the content of (a2) is more than 80% by mass, the cohesive strength of the adhesive layer decreases, resulting in insufficient adhesive strength, heat resistance, and light resistance.
[0030] In 100% by mass of (a2), the content of (meth)acrylic acid alkyl ester monomers having a linear alkyl group with 8 to 14 carbon atoms is preferably 70% by mass or more. By setting the content at such a ratio, higher adhesive strength is easily obtained.
[0031] (a2) 100% by mass of acrylate And Metak The ratio of the relate is preferably 70:30 to 100:0. By setting the ratio in this manner, higher adhesive strength is easily obtained.
[0032] [Monomer (a3)] (a3) is a (meth)acrylic acid ester monomer having a carboxy group and / or a (meth)acrylic acid ester monomer having a hydroxy group.
[0033] The content of (a3) is 0.1 to 20 mass% in 100 mass% of the monomer mixture, preferably 0.1 to 15 mass%, more preferably 0.5 to 10 mass%, and most preferably 1 to 5 mass%. By making it 0.1 mass% or more, it is possible to ensure resistance to moist heat, and by making it 20 mass% or less, it is possible to reduce outgassing and the dielectric constant.
[0034] The (meth)acrylic acid ester monomer having a carboxy group is not limited as long as it is a monomer having a carboxy group in the molecule, and specific examples thereof include (meth)acrylic acid, p-carboxybenzyl acrylate, β-carboxyethyl acrylate, maleic acid, monoethyl maleic acid, itaconic acid, citraconic acid, and fumaric acid. Of these, (meth)acrylic acid is preferred from the viewpoint of adhesive strength.
[0035] The content of the (meth)acrylic acid ester monomer having a carboxy group is preferably 0 to 5 mass %, more preferably 0 to 2 mass %, and most preferably 0 to 1 mass % in 100 mass % of the monomer mixture. By setting the content within this range, metal corrosiveness can be reduced in a configuration in which the adhesive layer is in contact with metal such as a transparent conductive layer, and the dielectric constant can be reduced.
[0036] The (meth)acrylic acid ester monomer having a hydroxy group is not limited as long as it is a monomer having a hydroxy group in the molecule, and specific examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Of these, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred from the viewpoints of adhesive strength and resistance to moist heat.
[0037] The content of the (meth)acrylic acid ester monomer having a hydroxyl group is 0.1 to 20 mass% in 100 mass% of the monomer mixture, preferably 0.1 to 15 mass%, more preferably 0.5 to 10 mass%, and most preferably 1 to 5 mass%. By making it 0.1 mass% or more, it is possible to ensure resistance to moist heat, and by making it 20 mass% or less, it is possible to reduce outgassing and lower the dielectric constant.
[0038] [Monomer (a4)] The monomer mixture serving as the raw material of the acrylic polymer (A) preferably further contains a (meth)acrylic acid alkyl ester monomer (a4) having an alkyl group having 1 to 4 carbon atoms. By containing (a4), it becomes easier to achieve both adhesive strength, heat resistance, and moist heat resistance.
[0039] Examples of the monomer (a4) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, and tert-butyl (meth)acrylate. Among these, acrylic acid alkyl ester monomers are preferred from the viewpoint of ease of molecular weight control.
[0040] The content of (a4) is preferably 10 to 40% by mass, and more preferably 20 to 40% by mass, in 100% by mass of the monomer mixture. By making it 10% by mass or more, it becomes easier to achieve both adhesive strength, heat resistance, and moist heat resistance, and by making it 40% by mass or less, the dielectric constant can be reduced. In order to ensure tackiness, the ratio of acrylate to (meth)acrylate in 100% by mass of (a4) is preferably 80:20 to 100:0.
[0041] [Other monomers] The monomer mixture used as the raw material for the acrylic polymer (A) may contain other monomers other than the above (a1) to (a4) as optional components. Examples of other monomers include (meth)acrylic acid alkyl ester monomers having a branched alkyl group, nitrogen-containing (meth)acrylic acid esters such as acrylamide, alkoxy-based (meth)acrylic acid esters such as methoxyethyl acrylate, vinyl-based monomers such as vinyl acetate and styrene, and monomers having a glycidyl group such as glycidyl (meth)acrylate. The content of other monomers in 100% by mass of the monomer mixture is preferably 35% by mass or less, more preferably 25% by mass or less, even more preferably 15% by mass or less, and most preferably 5% by mass or less.
[0042] (Production of acrylic polymer (A)) The acrylic polymer (A) can be produced by polymerizing the above-mentioned monomer mixture. The polymerization can be carried out by known polymerization methods such as solution polymerization, bulk polymerization, emulsion polymerization, and suspension polymerization, but solution polymerization is preferred. The solvent used in the solution polymerization is preferably, for example, acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, cyclohexanone, etc. The polymerization temperature is preferably a boiling point reaction at 60 to 120°C. The polymerization time is preferably about 5 to 12 hours.
[0043] The polymerization initiator used in the polymerization is preferably a radical polymerization initiator, and the radical polymerization initiator is generally a peroxide or an azo compound. Examples of the peroxide include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; Peroxyesters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; Peroxyketals such as 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; Hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; Diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; Examples include peroxydicarbonates such as bis(t-butylcyclohexyl) peroxydicarbonate.
[0044] Examples of the azo compound include 2,2'-azobisbutyronitrile such as 2,2'-azobisisobutyronitrile (abbreviation: AIBN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitrile such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitriles such as 2,2'-azobis(2-hydroxymethylpropionitrile); Examples include 1,1'-azobis-1-alkanenitriles such as 1,1'-azobis(cyclohexane-1-carbonitrile).
[0045] The polymerization initiator is preferably used in an amount of 0.01 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, based on 100 parts by mass of the monomer mixture.
[0046] (Weight average molecular weight (Mw)) The weight average molecular weight of the acrylic polymer (A) is preferably 500,000 to 1,500,000, more preferably 600,000 to 1,200,000. By setting the weight average molecular weight within the above range, peel resistance, outgas resistance, and light resistance in high temperature / high humidity environments are further improved. The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0047] <Hardening agent (B)> The adhesive composition of the present invention contains a curing agent (B). The curing agent to be blended into the adhesive is preferably one that reacts with the carboxyl group and hydroxyl group of the monomer (a3) by heat or the like to form bonds. The blending of the curing agent improves the cohesive strength of the adhesive layer, and improves the adhesive strength, heat resistance, and light resistance.
[0048] The curing agent can be selected from known crosslinking agents such as isocyanate-based curing agents, epoxy-based curing agents, oxazoline-based curing agents, aziridine-based curing agents, carbodiimide-based curing agents, metal chelate-based curing agents, and melamine-based curing agents, taking into consideration the reactivity with the functional groups of the polymer in the adhesive. From the viewpoints of adhesive strength, heat resistance, and light resistance, it is preferable to use an isocyanate-based curing agent or a block thereof.
[0049] The isocyanate-based curing agent is an isocyanate having two or more isocyanate groups or a block thereof. As the isocyanate, for example, aromatic isocyanate, aliphatic isocyanate, araliphatic isocyanate, alicyclic isocyanate, and their biuret, nurate, and adduct are preferable, and from the viewpoint of yellowing resistance, aliphatic isocyanate, alicyclic isocyanate, and their biuret, nurate, and adduct are more preferable.
[0050] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HMDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.
[0051] Examples of alicyclic polyisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane.
[0052] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, and 4,4',4"-triphenylmethane triisocyanate.
[0053] Examples of the aromatic aliphatic polyisocyanate include ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.
[0054] The biuret form is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, for example, a biuret form of hexamethylene diisocyanate.
[0055] The nurate form is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.
[0056] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.
[0057] The isocyanate compound is preferably a trifunctional isocyanate compound from the viewpoint of forming a sufficient crosslinked structure. The isocyanate compound is more preferably an adduct or nurate, which is a reaction product between an isocyanate monomer and a trifunctional low molecular weight active hydrogen-containing compound. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.
[0058] Examples of epoxy compounds include glycerin diglycidyl ether, 1,6-hexanediol diglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidylaminophenylmethane.
[0059] Examples of the aziridine compound include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxite), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.
[0060] The carbodiimide compound is preferably a high molecular weight polycarbodiimide produced by decarboxylation condensation of a diisocyanate compound in the presence of a carbodiimide catalyst. The commercially available high molecular weight polycarbodiimide is preferably the Carbodilite series from Nisshinbo Industries, Ltd. Among them, Carbodilite V-03, 07, and 09 are preferred because of their excellent compatibility with organic solvents.
[0061] The metal chelate is preferably a coordination compound of a polyvalent metal such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, or zirconium with acetylacetone or ethyl acetoacetate. Examples of the metal chelate include aluminum ethyl acetoacetate diisopropylate, aluminum trisacetylacetonate, aluminum bisethyl acetoacetate monoacetylacetonate, and aluminum alkyl acetoacetate diisopropylate.
[0062] The oxazoline-based curing agent has two or more oxazoline groups in the molecule, and may be a low molecular weight compound or a polymer. Examples of the low molecular weight compound oxazoline-based curing agent include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2,2'-bis-(2-oxazoline), 2,2'-methylene-bis-(2-oxazoline), 2,2'-ethylene-bis-(2-oxazoline), 2,2'-trimethylene-bis-(2-oxazoline), and 2,2'-tetramethylene-bis-(2-oxazoline). , 2,2'-hexamethylene-bis-(2-oxazoline), 2,2'-octamethylene-bis-(2-oxazoline), 2,2'-ethylene-bis-(4,4'-dimethyl-2-oxazoline), 2,2'-p-phenylene-bis-(2-oxazoline), 2,2'-m-phenylene-bis-(2-oxazoline), 2,2'-m-phenylene-bis-(4,4'-dimethyl-2-oxazoline), 2,2'-(1,3-phenylene)-bis-(2-oxazoline), bis-(2-oxazolinylcyclohexane)sulfide, bis-(2-oxazolinylnorbornane)sulfide, etc. Examples of oxazoline-based curing agents for polymers include polymers that contain addition-polymerizable oxazoline as an essential component. Examples of the addition-polymerizable oxazoline include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline.
[0063] Representative examples of the melamine-based hardener include fully alkyl-etherified melamine resins, methylol group-type melamine resins, and imino group-type melamine resins partially containing imino groups.
[0064] The curing agent (B) is preferably contained in an amount of 0.02 to 4 parts by mass, and more preferably 0.04 to 1 part by mass, per 100 parts by mass of the acrylic polymer (A) in the pressure-sensitive adhesive composition. When the content is 0.02 parts by mass or more, the cohesive strength is further improved, and when the content is 4 parts by mass or less, it becomes easier to achieve both cohesive strength and flexibility, and therefore it is easy to obtain sufficient adhesive strength, heat resistance, and light resistance.
[0065] <Silane coupling agent (C)> The pressure-sensitive adhesive composition of the present invention preferably contains a silane coupling agent (C). By containing the silane coupling agent (C), the adhesive strength, heat resistance, wet heat whitening resistance, and light resistance can be improved. The silane coupling agent (C) is preferably contained in an amount of 0.05 to 0.2 parts by mass per 100 parts by mass of the acrylic polymer (A). By making it 0.05 to 0.2 parts by mass, it becomes easy to achieve both heat resistance, outgassing resistance, and light resistance.
[0066] Examples of the silane coupling agent (C) include an alkoxysilane compound having a (meth)acryloxy group, an alkoxysilane compound having a vinyl group, an alkoxysilane compound having an amino group, an alkoxysilane compound having a mercapto group, and an alkoxysilane compound having an epoxy group. Specific examples of commercially available products include KBM-403 (3-glycidoxypropyltrimethoxysilane), KBE-403 (3-glycidoxypropyltriethoxysilane), KBM-303 (2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane) (all manufactured by Shin-Etsu Chemical Co., Ltd.), BYK-325N (polyether-modified polymethylalkylsiloxane) (manufactured by BYK Japan KK), and the like.
[0067] The pressure-sensitive adhesive composition of the present invention may contain, as optional components, various resins, chlorinated polyolefins described below, oils, softeners, dyes, pigments, antioxidants, ultraviolet absorbers, etc., as long as the problem can be solved.
[0068] Examples of chlorinated polyolefins include chlorinated polypropylene, acid-modified chlorinated polypropylene, acrylic-modified chlorinated polypropylene, chlorinated polyethylene, and chlorinated ethylene-vinyl acetate copolymer. From the viewpoints of good compatibility with acrylic polymers and the like and effective reduction in polarity, chlorinated polypropylene and chlorinated ethylene-vinyl acetate copolymer are preferred. Specific examples of commercially available products include Superchlorine 390S (chlorinated polypropylene, chlorine content 36%) and Superchlorine BX (chlorinated EVA, chlorine content 18%) (both manufactured by Nippon Paper Industries Co., Ltd.).
[0069] Adhesive sheet The pressure-sensitive adhesive sheet comprises a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition of the present invention.
[0070] The pressure-sensitive adhesive sheet of the present invention has a configuration in which a release film is formed on both sides of a pressure-sensitive adhesive layer, or a release film is formed on one side of the pressure-sensitive adhesive layer and a light-transmitting substrate is provided on the other side of the pressure-sensitive adhesive, and the pressure-sensitive adhesive layer is an adhesive layer formed from the pressure-sensitive adhesive composition of the present invention.
[0071] <Release film> The release film is not particularly limited, but a transparent plastic substrate can be suitably used. Examples of the material of the transparent plastic substrate include polyester such as polyethylene terephthalate (PET), acrylic resin such as polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose, polysulfone, polyarylate, polycycloolefin, and other plastic materials. The plastic materials can be used alone or in combination of two or more kinds.
[0072] As the release film, among the above-mentioned transparent plastic substrates, a transparent plastic substrate having excellent heat resistance, i.e., a transparent plastic substrate in which deformation is suppressed or prevented under severe conditions such as high temperature, high temperature and high humidity, etc. As the transparent plastic substrate, a PET film or sheet is particularly suitable.
[0073] <Light transparent base material> A transparent plastic substrate is used as the light-transmitting substrate. Examples of the material of such a light-transmitting substrate include acrylic resins such as polyethylene terephthalate (PET), polyethylene naphthalate, and polymethyl methacrylate (PMMA), and plastic materials such as polycarbonate (PC), polycycloolefin, polyimide, polyphenylene ether, polysulfone, polyethersulfone, polystyrene, and polypropylene. In particular, PET film or PC is preferable, and PC is more preferable in terms of durability. The plastic materials can be used alone or in combination of two or more kinds. The light-transmitting substrate may be subjected to an appropriate surface treatment, for example, a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as an undercoat treatment.
[0074] The pressure-sensitive adhesive sheet of the present invention has excellent adhesion, heat resistance, wet heat whitening resistance, outgas resistance, light resistance, low dielectric constant, and metal corrosion resistance, and is therefore suitable as a pressure-sensitive adhesive for forming optical display members such as display devices such as LCDs and OLEDs and input devices such as touch panels, and for bonding these members together. The optical members are not particularly limited, and include PET films, polarizing plates, retardation plates, elliptical polarizing plates, optical compensation films, brightness improvement films, infrared / electromagnetic wave cut films, front anti-reflection films, surface protection films, films having an ITO (indium tin oxide) layer, films having a zinc oxide (ZnO) layer, films obtained by coating or printing metal nanoparticles, films obtained by coating or printing a dispersion containing carbon nanotubes, films obtained by coating or printing a dispersion containing graphene, films obtained by coating or printing a dispersion containing a conductive polymer, metal plates formed of SUS, metal meshes, and further laminates thereof.
[0075] The thickness of the transparent plastic substrate is not particularly limited, and is, for example, preferably from 10 to 200 μm, and more preferably from 25 to 150 μm.
[0076] In coating the adhesive composition, a suitable liquid medium can be added to adjust the viscosity.Specific examples of the solvent include hydrocarbon solvents such as toluene, xylene, hexane, and heptane; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone and methyl ethyl ketone; halogenated hydrocarbon solvents such as dichloromethane and chloroform; ether solvents such as diethyl ether, methoxytoluene, and dioxane, and other hydrocarbon solvents.However, water and alcohol should be used with caution because they may cause reaction inhibition between the acrylic polymer (A) and the isocyanate curing agent (B).
[0077] The coating method is not particularly limited, and various coating methods can be used, such as a Mayer bar, applicator, brush, spray, roller, gravure coater, die coater, lip coater, comma coater, knife coater, reverse coater, spin coater, etc. In addition, the drying and curing method is not particularly limited, and examples thereof include hot air drying, infrared rays, reduced pressure methods, and active energy rays, but hot air or steam heating at 60 to 180°C is preferred from the viewpoint of outgassing resistance.
[0078] The thickness of the pressure-sensitive adhesive layer is preferably from 2 to 1000 μm, more preferably from 5 to 500 μm. The pressure-sensitive adhesive layer may be in the form of either a single layer or a laminate of two or more layers.
[0079] <Laminate> The laminate includes a light-transmitting substrate and a pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is formed using the pressure-sensitive adhesive sheet of the present invention. Specifically, for example, the release film is peeled off from the pressure-sensitive adhesive sheet of the present invention, and the pressure-sensitive adhesive layer is attached to the light-transmitting substrate to form the laminate. The laminate of the present invention has a structure of, for example, a light-transmitting substrate / a pressure-sensitive adhesive layer / a polarizing plate. In this case, it is preferable to provide the light-transmitting substrate, the pressure-sensitive adhesive layer, and the polarizing plate in this order. This makes it possible to obtain a laminate with excellent transparency.
[0080] An example of a schematic cross-sectional view partially showing the laminate of the present invention is shown in Fig. 1. In Fig. 1, 3 is a light-transmitting substrate (cover panel), 1 is a pressure-sensitive adhesive layer, and 4 is a polarizing plate.
[0081] In the laminate shown in FIG. 1, a light-transmitting substrate (cover panel) is attached to a polarizing plate via a pressure-sensitive adhesive layer.
[0082] <Production of Laminate for Display> The laminate can be produced, for example, by peeling off the release film from a pressure-sensitive adhesive sheet having release films on both sides of the pressure-sensitive adhesive layer, and attaching the pressure-sensitive adhesive layer to an adherend such as a light-transmitting flexible substrate or a polarizing plate, etc. Alternatively, the pressure-sensitive adhesive layer can be directly formed on a light-transmitting flexible substrate, and then an adherend or a pressure-sensitive adhesive layer provided on another pressure-sensitive adhesive sheet can be attached to the pressure-sensitive adhesive layer to form a laminate.
[0083] "display" A display preferably comprises the laminate of the present invention, a polarizing plate, and an optical element, thereby providing the display of the present invention with excellent flexibility and visibility. The optical element is not particularly limited, and examples thereof include a liquid crystal element and an organic EL element.
[0084] Fig. 2 shows an example of a schematic cross-sectional view partially illustrating a display, which is an example of the use of the pressure-sensitive adhesive sheet of the present invention. In Fig. 2, 3 is a light-transmitting substrate (cover panel), 1 is a pressure-sensitive adhesive layer 1, 4 is a polarizing plate, 5 is a pressure-sensitive adhesive layer 2, 6 is a barrier layer such as silicon nitride, 7 is an organic EL layer, 8 is a support such as polyimide, and 9 is an organic EL cell. Note that the configuration of the display is not limited to that shown in Fig. 2.
[0085] In the display shown in Fig. 2, a light-transmitting substrate (cover panel) is attached to a polarizing plate via the pressure-sensitive adhesive layer (pressure-sensitive adhesive layer 1) of the present invention, and is further attached to an organic EL cell via a pressure-sensitive adhesive layer for polarizing plate (pressure-sensitive adhesive layer 2). Thus, the pressure-sensitive adhesive sheet of the present invention can be used in a form in which a transparent pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive is attached to a light-transmitting substrate (cover panel) and a polarizing plate, and the laminate is further attached to an organic EL cell via a pressure-sensitive adhesive layer for polarizing plate. For example, in FIG. 2, the pressure-sensitive adhesive layer of the present invention can be used as either pressure-sensitive adhesive layer 1 or pressure-sensitive adhesive layer 2. In general, when comparing pressure-sensitive adhesive layer 1 and pressure-sensitive adhesive layer 2, the pressure-sensitive adhesive layer 1 has higher quality requirements, and since the pressure-sensitive adhesive of the present invention has good adhesion and bonding properties to the substrate, it is preferably used for pressure-sensitive adhesive layer 1. In this case, the pressure-sensitive adhesive for forming pressure-sensitive adhesive layer 2 may be the pressure-sensitive adhesive of the present invention or a conventionally known pressure-sensitive adhesive.
[0086] There are no particular limitations on the uses of the displays, but examples include OLED televisions, OLED smartphones, OLED tablets, and OLED smartwatches. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". The blending amounts in the tables are parts by mass, and the amounts other than the solvent are calculated as non-volatile contents. The blanks in the tables indicate that no blending was performed. The method for measuring the weight average molecular weight of the acrylic polymer is as follows.
[0088] <Measurement of weight average molecular weight (Mw)> Weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC). Shimadzu Corporation's GPC device: LC-GPC system "Prominence" was used. Tosoh Corporation's TSKgel α-M was used as the column, and two columns were connected in series. N,N-dimethylformamide (DMF) was used as the eluent, and measurements were performed at 40°C. Mw was determined by conversion using polystyrene with a known Mw as the standard substance.
[0089] The materials used in the examples and comparative examples are listed below. <Hardening agent (B)> [Isocyanate-based hardener] B-1: ("NP-1200", manufactured by Mitsui Chemicals, burette form of hexamethylene diisocyanate) B-2: ("D-172N", Mitsui Chemicals, Inc., hexamethylene diisocyanate nurate) B-3: ("D-160N", Mitsui Chemicals, Inc., hexamethylene diisocyanate modified with trimethylolpropane) B-4: ("Desmodur 2565", manufactured by Covestro, nurate form of isophorone diisocyanate) B-5: ("Coronate L", Tosoh Corporation, trimethylolpropane modified tolylene diisocyanate) [Other hardeners] B-6: Zirconium tetraacetylacetonate: ("Orgatics ZC-700", Matsumoto Fine Chemical Co., Ltd.) B-7: N,N,N',N'-Tetraglycidyl-m-xylylenediamine (TETRAD-X)
[0090] <Silane coupling agent (C)> KBM-303: ([2-(3,4-epoxycyclohexyl)ethyl]trimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) KBE-403: (3-glycidoxypropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.)
[0091] <Production example of acrylic polymer> (Acrylic polymer (A-1)) Using a reaction apparatus equipped with a stirrer, reflux condenser, nitrogen inlet tube, thermometer, and dropping tube, 11 parts of isobornyl acrylate (IBXA) as monomer (a1), 56.5 parts of octyl acrylate (OA) as monomer (a2), 2 parts of 2-hydroxyethyl acrylate (HEA) and 0.5 parts of acrylic acid (AA) as monomer (a3), and 30 parts of methyl acrylate (MA) as monomer (a4) were charged in a reaction vessel in half of each monomer mixture, 0.2 parts of azobisisobutyronitrile as an initiator, and 60 parts of ethyl acetate as a solvent. The remaining half of the monomer mixture, 60 parts of ethyl acetate, and 0.2 parts of azobisisobutyronitrile were added and mixed, and the mixture was dropped from the dropping tube over about 2 hours, and polymerized for 6 hours at about 80 ° C. under a nitrogen atmosphere. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain an acrylic polymer solution with a non-volatile content of 30%. Here, the obtained acrylic polymer was designated (A-1). The weight average molecular weight (Mw) of the obtained acrylic polymer is shown in Table 1.
[0092] (Acrylic polymers (A-2 to 47, A'-1 to 10)) Acrylic polymers (A-2 to 47, A'-1 to 10) were synthesized in the same manner as for the production of acrylic polymer (A-1), except that the compositions and amounts (parts by mass) were changed to those shown in Tables 1 to 4. The weight average molecular weights of the obtained acrylic polymers are shown in Tables 1 to 4.
[0093] [Table 1]
[0094] [Table 2]
[0095] [Table 3]
[0096] [Table 4]
[0097] The abbreviations are as follows: IBXA: Isobornyl acrylate THFA: Tetrahydrofurfuryl acrylate TMCHA: 3,3,5-trimethylcyclohexyl acrylate IBXMA: Isobornyl methacrylate CTFA: (5-ethyl-1,3-dioxane-5-yl)methyl acrylate BZA: Benzyl acrylate PEA: Phenoxyethyl acrylate OA: normal octyl acrylate (alkyl group carbon number: 8) OMA: normal octyl methacrylate (alkyl group carbon number: 8) DA: normal decyl acrylate (alkyl group carbon number: 10) DMA: normal decyl methacrylate (alkyl group carbon number: 10) DDA: normal dodecyl acrylate (alkyl group carbon number: 12) DDMA: normal dodecyl methacrylate (alkyl group carbon number 12) TrDA: normal tridecyl acrylate (alkyl group carbon number: 13) TrDMA: normal tridecyl methacrylate (alkyl group carbon number: 13) TeDA: normal tetradecyl acrylate (alkyl group carbon number 14) TeDMA: normal tetradecyl acrylate (alkyl group carbon number 14) HDA: normal hexadecyl acrylate (alkyl group carbon number 16) HDMA: normal hexadecyl methacrylate (alkyl group carbon number 16) ODA: normal octadecyl acrylate (alkyl group carbon number: 18) ODMA: normal octadecyl methacrylate (alkyl group carbon number 18) 2EHA: 2-Ethylhexyl acrylate iDA: Isodecyl acrylate iDMA: Isodecyl methacrylate HEA: Hydroxyethyl 4HBA: 4-Hydroxy n-butyl AA: Acrylic acid MAA: Methacrylic acid MA: Methyl acrylate EMA: Ethyl methacrylate BA: n-butyl acrylate
[0098] <Example 1> A pressure-sensitive adhesive composition was obtained by blending 100 parts of the acrylic polymer (A-1) with 0.4 parts of "NP-1200" (manufactured by Mitsui Chemicals, Inc., biuret form of hexamethylene diisocyanate) as the isocyanate curing agent (B) and 0.1 parts of KBE-403 (3-glycidoxypropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) as the silane coupling agent (C). The obtained adhesive composition was coated using a comma coater onto a 38 μm thick release liner (SP-PET-O1-BU: manufactured by Mitsui Chemicals Tocello) as a release sheet so that the thickness after drying would be 100 μm. After drying at 110°C for 3 minutes, a 75 μm thick release liner (SP-PET-O3-B3: manufactured by Mitsui Chemicals Tocello) as a release sheet was bonded to the adhesive layer and aged in this state at 23°C for 7 days to obtain an adhesive sheet.
[0099] <Examples 2 to 59 and Comparative Examples 1 to 11> As shown in Table 5, pressure-sensitive adhesive compositions and pressure-sensitive adhesive sheets were obtained in the same manner as in Example 1, except that the types and amounts of the acrylic polymer, curing agent, and silane coupling agent were changed. However, in the embodiment 22、23、 29 to 31 are reference examples.
[0100] [Table 5]
[0101] {Physical properties and evaluation of pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet} The adhesive composition and adhesive sheet of the present invention were evaluated for adhesive strength, heat resistance (peeling, yellowing), humidity and heat whitening resistance, outgassing resistance, light resistance (peeling, yellowing), and metal corrosion resistance, and the dielectric constant was measured by the following methods. The results are shown in Table 6.
[0102] <Adhesive strength> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film substrate (Toyobo Co., Ltd., Cosmoshine A-4360, thickness 100 μm), and cut to a size of 25 mm wide x 100 mm long to prepare a test adhesive sheet. The other 75 μm release liner of this test adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate in an atmosphere of 23°C and 50% relative humidity (50% RH), and further pressed with a roll in accordance with JIS Z-0237. After 24 hours from pressing, the peel strength (peel angle 180°, peel speed 300 mm / min; unit N / 25 mm width) was measured using a tensile tester (Tensilon: Orientec Co., Ltd.). [Evaluation criteria] ◎: Peel strength is 25N / 25mm or more. Excellent. ○: Peel strength is 21N / 25mm or more and less than 25N / 25mm. Good. △: Peel strength is 18N / 25mm or more and less than 21N / 25mm. Fairly good. ▲: Peel strength is 15N / 25mm or more and less than 18N / 25mm. Practical use is possible. ×: Peel strength is less than 15N / 25mm. Not practical.
[0103] <Heat resistance (peeling)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000: manufactured by Mitsubishi Gas Chemical Co., Ltd.) using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was attached to a glass plate using a laminator as described above. The test piece was prepared by applying a pressure of 0.5 MPa and holding it for 20 minutes in an atmosphere of 50 ° C, and laminated in the order of PC plate / adhesive layer / glass plate, and was left in an environment of 120 ° C for 1000 hours. The test piece was cooled at 23 ° C-50% RH for 24 hours, and then the degree of peeling of the test piece was visually evaluated. [Evaluation Criteria] ◎: Peeling area is less than 5% of the whole. Excellent. ○: Peeling area is 5% or more and less than 15% of the whole area. Good. △: Peeling area is 15% or more and less than 30% of the total area. Fairly good. ▲: Peeling area is 30% or more and less than 50% of the total area. Practical use is possible. ×: Peeling area is 50% or more of the whole. Not practical.
[0104] <Heat resistance (yellowing)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator as described above. The test piece was prepared by applying a pressure of 0.5 MPa to the glass plate / adhesive layer / glass plate and holding it for 20 minutes in an atmosphere of 50 ° C., and was left for 1000 hours in an environment of 120 ° C. After cooling it for 1 hour at 23 ° C.-50% RH, the b value was measured, and the difference Δb from the b value before the heat resistance test was calculated. The b value was measured using a spectrophotometer SE6000 manufactured by Nippon Denshoku Kogyo Co., Ltd. under conditions of a D65 light source and a viewing angle of 2 °. [Evaluation Criteria] ◎: Δb is less than 0.8. Excellent. ○: Δb is 0.8 or more and less than 1.3. Good. △: Δb is 1.3 or more and less than 2.0. Fairly good. ▲: Δb is 2.0 or more and less than 3.0. Practical use is possible. ×: Δb is 3.0 or more. Not practical.
[0105] <Wet and heat whitening resistance (glass composition)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator in an atmosphere of 23 ° C-50% RH. Next, the other 75 μm release liner of the adhesive sheet was peeled off, and the adhesive layer was laminated to a glass plate using a laminator as described above. The test piece was prepared by laminating the glass plate / adhesive layer / glass plate in this order by applying a pressure of 0.5 MPa and holding it for 20 minutes in an atmosphere of 50 ° C, and was left in an environment of 85 ° C-85% RH for 1000 hours. The test piece was cooled at 23 ° C-50% RH for 1 hour, and then the HAZE was measured. The HAZE was measured using a Turbidimeter NDH5000W manufactured by Nippon Denshoku Kogyo Co., Ltd. [Evaluation Criteria] ◎: Haze is less than 1.0. Excellent. ○: Haze is 1.0 or more and less than 2.0. Good. △: Haze is 2.0 or more and less than 3.5. Fairly good. ▲: Haze is 3.5 or more and less than 5.0. Practical use is possible. ×: Haze is 5.0 or more. Not practical.
[0106] <Resistance to moist heat whitening (PC composition)> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film (Toyobo Co., Ltd., A-4300, thickness 100 μm), and cut to a size of 40 mm wide x 60 mm long to prepare a test adhesive sheet. Next, the other 75 μm release liner of the test adhesive sheet was peeled off, and it was attached to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000: Mitsubishi Gas Chemical Co., Ltd.). It was held for 20 minutes under a pressure of 0.5 MPa in an atmosphere of 50 ° C. to prepare a test piece in which the PET film / adhesive layer / PC plate were laminated in this order, and left in an environment of 85 ° C.-85% RH for 240 hours. It was cooled at 23 ° C.-50% RH for 1 hour, and then the HAZE was measured. The HAZE was measured using a Turbidimeter NDH5000W manufactured by Nippon Denshoku Kogyo Co., Ltd. [Evaluation Criteria] ◎: Haze is less than 1.5. Excellent. ○: Haze is 1.5 or more and less than 2.5. Good. △: Haze is 2.5 or more and less than 4.0. Fairly good. ▲: Haze is between 4.0 and 5.5. Practical use is possible. ×: Haze is 5.5 or more. Not practical.
[0107] <Outgassing resistance> Test pieces were prepared in the same manner as in the evaluation of heat and humidity whitening resistance (PC composition), and then left in an environment of 85°C and 85% RH for 72 hours. After leaving it in an atmosphere of 23°C and 50% RH for 1 hour, the appearance of the test pieces was visually observed. [Evaluation Criteria] ◎: No bubbles or floating. Excellent. ◯: There are very few air bubbles or lifted adhesive layers (1 to less than 5 air bubbles, and the lifted area is less than 3% of the total). Good. △: There are a few air bubbles or lifting of the adhesive layer (5 to less than 15 air bubbles, and 3% to less than 5% of the total lifted area). Fairly good. ▲: Air bubbles or lifted adhesive layer are found (15 to less than 30 air bubbles, and lifted area is 5 to less than 10% of the total). Practical use is possible. ×: There are many air bubbles or raised areas of the adhesive layer (30 or more air bubbles, or 10% or more of the raised area). Not suitable for practical use.
[0108] <Light resistance (peeling)> A coating liquid was prepared by mixing 100 parts of a surface protective coating agent (YL454UR, acrylic varnish, manufactured by Toyo Ink Mfg. Co., Ltd.) with 10 parts of D-172N as a curing agent, and applying the mixture to a 0.5 mm thick polycarbonate (PC) plate (Iupilon NF2000, manufactured by Mitsubishi Gas Chemical Co., Ltd.) using a bar coater. The plate was then aged at 40°C for 72 hours to prepare a PC plate having a surface protective layer. Test pieces were prepared in the same manner as in the evaluation of heat resistance (peeling), except that the PC plate having the above-mentioned surface protective layer was used instead of Iupilon NF2000, and then the test pieces were subjected to a test using a Q-Lab xenon weather resistance tester at a black panel temperature of 83°C and an illuminance of 60 W / m 2 The specimen was exposed to light for 500 hours under the above conditions. After cooling for 24 hours at 23°C and 50% RH, the degree of peeling of the specimen was visually evaluated. [Evaluation Criteria] ◎: Peeling area is less than 5% of the whole. Excellent. ○: Peeling area is 5% or more and less than 15% of the whole area. Good. △: Peeled area is 15% or more and less than 25% of the total area. Fairly good. ▲: Peeling area is between 25% and 50% of the total area. Practical use is possible. ×: Peeling area is 50% or more of the whole. Not practical.
[0109] <Light resistance (yellowing)> After preparing test pieces using the same procedure as for the evaluation of heat resistance (yellowing), they were tested using a Q-Lab xenon weathering tester at a black panel temperature of 63°C and an illuminance of 85W / m 2 The sample was exposed to light for 1000 hours under these conditions. After cooling for 1 hour at 23℃-50%RH, the b-value was measured and the difference Δb from the b-value before the lightfastness test was calculated. The b-value was measured using a Nippon Denshoku Industries Co., Ltd. SE6000 spectrophotometer under conditions of a D65 light source and a viewing angle of 2°. [Evaluation Criteria] ◎: Δb is less than 1.0. Excellent. ○: Δb is 1.0 or more and less than 2.0. Good. △: Δb is 2.0 or more and less than 3.5. Fairly good. ▲: Δb is 3.5 or more and less than 5.0. Practical use is possible. ×: Δb is 5.0 or more. Not practical.
[0110] <Metal corrosion resistance> The 38 μm release liner of the obtained adhesive sheet was peeled off, and the adhesive layer was attached to a PET film (Toyobo Co., Ltd., A-4300, thickness 100 μm), and cut to a size of 40 mm wide x 60 mm long to prepare a test adhesive sheet. Next, the other 75 μm release liner of the test adhesive sheet was peeled off, and the exposed adhesive layer was attached to a transparent conductive film of a PET film with a width of 40 mm and a length of 160 mm, on which a transparent conductive film was formed by ITO, using a laminator under a 23° C.-50% RH atmosphere to obtain a laminate, and its resistance value was measured using Loresta GP (model number MCP-T600, manufactured by Mitsubishi Chemical Corporation). The laminate was then left for 1000 hours in an environment of 85° C. and 90% RH, and the resistance was then measured again. The rate of change in resistance before and after the leaving was calculated to evaluate the corrosion resistance of the transparent conductive film. [Evaluation Criteria] ◎: The rate of change in resistance value is less than 120%. Excellent. ○: The rate of change in resistance value is 120% or more and less than 130%. Good. △: The rate of change in resistance value is 130% or more and less than 140%. Fairly good. ▲: The rate of change in resistance value is between 140% and 150%. Practical use is possible. ×: The rate of change in resistance value is 150% or more. Not practical.
[0111] <Dielectric constant> The method for measuring the dielectric constant will be described with reference to FIG. 3. The obtained adhesive sheet was prepared to a size of 100 mm wide x 100 mm long to prepare a test adhesive sheet. The 38 μm release liner of the test adhesive sheet was peeled off, and the exposed adhesive layer 4 was attached to the aluminum vapor deposition layer 3C formed on the glass plate 6. Next, the other 75 μm release liner of the test adhesive sheet was peeled off, and aluminum vapor deposition layers 3A and 3B were formed on the surface of the exposed adhesive layer 4 that was not in contact with the aluminum vapor deposition layer 3C, thereby obtaining a dielectric constant measurement sample 1. Next, the connection terminal 2A of the measurement device 7 was connected to the measurement terminal connection part 5 of the dielectric constant measurement sample 1, and the connection terminal 2B was connected to the aluminum vapor deposition layer 3A. The dielectric constant was then measured under the following conditions. The evaluation criteria are as follows.
[0112] Measurement equipment: Solartron 1260 impedance meter Amplifier: Solartron 1296 type dielectric constant measurement interface Electrode structure: 21mmΦ, 40nm thick aluminum vapor deposition layer Counter electrode: 21 mm diameter, 40 nm thick aluminum vapor deposition layer AC current: 100mV Terminal: Pin probe Frequency: 100kHz Measurement environment: 23℃-50%RH Sample thickness: 25μm
[0113] [Evaluation Criteria] ◎: Dielectric constant is 3.0 or less. Excellent. ○: The dielectric constant is greater than 3.0 and less than 3.1. Good. △: Dielectric constant is more than 3.1 and 3.3 or less. Fairly good. ▲: Dielectric constant is over 3.3 and 3.5 or less. Practical use is possible. ×: The dielectric constant is more than 3.5. Not practical.
[0114] [Table 6]
[0115] As shown in Table 6, the adhesive composition of the present invention had excellent results in adhesion, heat resistance, wet heat whitening resistance, outgassing resistance, light resistance, low dielectric constant, and metal corrosion resistance. On the other hand, the adhesive composition of the comparative example did not satisfy all of the adhesion, heat resistance, wet heat whitening resistance, outgassing resistance, light resistance, low dielectric constant, and metal corrosion resistance. From these results, it can be said that the pressure-sensitive adhesive composition of the present invention can be suitably used for bonding optical members. [Explanation of symbols]
[0116] The symbols in Figures 1 and 2 are explained below. 1 Adhesive layer 1 2 Release film 3 Film substrate (cover panel) 4. Polarizing Plate 5 Adhesive layer 2 6 Barrier Layer 7 Organic EL layer 8 Support 9 Organic EL Cell
[0117] The symbols in FIG. 3 are explained below. 1. Dielectric constant measurement sample 2A measurement terminal 2B Measurement terminal 3A Aluminum deposition layer 3B Aluminum deposition layer 3C Aluminum deposition layer 4 Adhesive layer 5 Measurement terminal joint part 6 Glass Plate 7. Measuring Equipment
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic polymer (A) and a curing agent (B), The acrylic polymer (A) is a copolymer of a monomer mixture containing the following (a1), (a2), and (a3), and the weight average molecular weight of the acrylic polymer (A) is 470,000 or more and 1,520,000 or less: The monomer mixture contains 2.5 to 20 mass% of (a1), 45 to 70 mass% of (a2), and 0.5 to 20 mass% of (a3) based on 100 mass% of the monomer mixture, and the ratio of acrylate to methacrylate in (a2) is 70:30 to 100:0, The monomer mixture contains 0.2% by mass or more of a monomer having a carboxy group in its molecule, based on 100% by mass of the monomer mixture, A pressure-sensitive adhesive composition, wherein the curing agent (B) is a curing agent that reacts with a carboxy group or a carboxy group and a hydroxy group to form a bond. (a1) (meth)acrylic acid ester monomer having an alicyclic structure (excluding (a3)) (a2) (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 8 to 18 carbon atoms (a3) (meth)acrylic acid ester monomer having a carboxy group and / or (meth)acrylic acid ester monomer having a hydroxy group
2. The pressure-sensitive adhesive composition according to claim 1, wherein (a3) contains a (meth)acrylic acid ester monomer having a hydroxy group.
3. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the monomer mixture further comprises (a4) a (meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 4 carbon atoms.
4. The pressure-sensitive adhesive composition according to claim 1, further comprising a silane coupling agent (C).
5. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the curing agent (B) comprises an isocyanate-based curing agent or a blocked product thereof.
6. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to any one of claims 1 to 5.
7. A laminate comprising the pressure-sensitive adhesive sheet according to claim 6 and a light-transmitting substrate.
8. A display comprising the laminate according to claim 7, a polarizing plate, and an optical element.
Citation Information
Patent Citations
Optical adhesive, optical film with binder and image display device
JP2007264092A
Pressure-sensitive adhesive, pressure-sensitive adhesive layer, and pressure-sensitive adhesive sheet
JP2013133440A
Pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet
JP2013173912A
Adhesive composition and adhesive sheet
JP2014012808A
Adhesive and adhesive sheet
JP2015183177A