Polyurethane adhesive and preparation method thereof

By using substances such as cellulose and functional resins containing polar groups in polyurethane adhesives to increase hydrogen bonds and adding metal powders, the problem of hydrolysis of polyurethane adhesives in high temperature and high humidity environments is solved, and the bonding is improved Performance and stability achieve excellent weather resistance and sealing.

CN118879260APending Publication Date: 2024-11-01CHANGCHUN UNIV OF TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410949823.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing polyurethane adhesives are prone to break when hydrolyzed in high temperature and high humidity environments, resulting in a degradation of adhesive properties and poor wetting of the surface of different materials, which affects sealing and safety.

Method used

Cellulose, coupling agent and functional resin containing polar groups are used to react with prepolymers to increase the content of carbamate and urea groups, form more hydrogen bonds, improve bond strength and weather resistance, and add Metal powder is used to fill the surface gullies and protect the surface.

Benefits of technology

It significantly improves the film forming properties, bonding strength, weathering and hydrolysis resistance of polyurethane adhesives, enhances storage stability and service life, and is better than similar products in the industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946892740000191
    Figure BDA0004946892740000191
  • Figure BDA0004946892740000201
    Figure BDA0004946892740000201
Patent Text Reader

Abstract

The invention provides a polyurethane adhesive and a preparation method thereof, and belongs to the technical field of adhesives. The polyurethane adhesive is prepared by common modification reaction of the cellulose containing the polar group, the coupling agent, the functional resin containing the polar group and the inorganic nanoparticles. According to the invention, the adhesive property and hydrolysis resistance of the polyurethane adhesive are obviously improved through a modification reaction, and the adhesive property and hydrolysis resistance of the polyurethane adhesive are both superior to those of sika Primer-206G + P type products and Han-Gao TEROSON PU 8511 type products with optimal performance of similar products in the industry, so that the polyurethane adhesive has relatively high practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a polyurethane adhesive and a preparation method thereof. Background Art

[0002] With the development of science and technology, the requirements for lightweight, comfort and safety of transportation vehicles such as automobiles, buses and ships are getting higher and higher. The connection between dissimilar materials such as glass and metal and car bodies and hulls is generally made by elastic bonding instead of traditional rubber strip sealing. At present, people generally use the reaction injection molding process to coat the sealant on the surface of dissimilar materials, which has high strength and is easy to use. However, there are two major problems. First, the active hydrogen on the surface of dissimilar materials and the isocyanate group content in polyurethane sealant are small, and the chemical link formed is limited, making the interface bonding weak; second, the viscosity of the sealant is high, and the wettability on the surface of dissimilar materials is poor. In the process of moisture curing, the isocyanate group in the sealant reacts with the water molecules in the air to release CO2 gas, forming bubbles to destroy the bonding interface, thereby reducing the safety of use. The use of polyurethane adhesive or combined sealant has high wettability and can fill the grooves on the surface of dissimilar materials, greatly improving its sealing with car bodies, hulls and other equipment, as well as the overall safety.

[0003] Patent CN115322670A prepares a polyurethane glass primer with good wettability and high bonding strength by adding rigid nanomaterials and reduced graphene oxide to silane-modified polyurethane. However, the current use conditions of polyurethane have strict requirements on the environment. When the humidity of the external environment is too high, the polyurethane will hydrolyze, resulting in polymer chain breakage, and it cannot be in a high temperature, high humidity or water-soaked working environment for a long time. Therefore, researching and developing a polyurethane adhesive with excellent hydrolysis resistance and excellent bonding performance has important practical value and realistic significance. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a polyurethane adhesive and a preparation method thereof, wherein the adhesive has excellent hydrolysis resistance, high temperature and high humidity resistance and good bonding performance.

[0005] The present invention provides a polyurethane adhesive, which comprises the following raw materials in parts by mass:

[0006] 100 parts of prepolymer, 0.3-30 parts of graphene and its derivatives, 0.1-20 parts of inorganic nanoparticles, 10-100 parts of carbon black, 200-500 parts of solvent B, 0.5-25 parts of cellulose containing polar groups, 5-30 parts of coupling agents, 5-50 parts of functional resin containing polar groups and 0.5-20 parts of metal powder;

[0007] The prepolymer comprises the following raw materials:

[0008] 100 parts of polyol, 30-200 parts of solvent A, 15-210 parts of isocyanate, 0.01-13 parts of catalyst, 0-30 parts of chain extender, 0.1-10 parts of antioxidant, and 0.05-10 parts of ultraviolet light absorber.

[0009] Preferably, the polyol is selected from one or more of polyethylene glycol propylene glycol adipate diol, sorbitol, polybutylene glycol, polyoxypropylene triol, polycaprolactone diol, castor oil polyol, polytetramethylene ether diol, polypropylene adipate diol, polyethylene glycol, polyhexamethylene carbonate diol, polytrimethylene ether glycol, xylitol and vegetable oil polyol;

[0010] The isocyanate is selected from one or more of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, 4,4′-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate biuret, isophorone diisocyanate trimer, lysine diisocyanate, methylcyclohexyl diisocyanate, cyclohexane dimethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate trimer, toluene diisocyanate trimer, 1,5-naphthalene diisocyanate, p-phenylene diisocyanate, toluene diisocyanate dimer and diphenylmethane diisocyanate dimer.

[0011] Preferably, the solvent A is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene;

[0012] The catalyst is selected from one or more of stannous octoate, triethylamine, dibutyltin diacetate, potassium acetate, lead isooctanoate, phenylmercuric acetate, dibutyltin dilaurate, tetrabutyl titanate, tetramethyldipropylenetriamine, tetramethylpropylenediamine, tetramethylhexanediamine, N-methylimidazole, N-methylmorpholine, 1,4-dimethylpiperazine, bismuth isooctanoate and triethylenediamine;

[0013] The chain extender is selected from one or more of 1,4-butanediol, glycidyl allyl ether, trimethylolpropane, trimethylolethane, methyldiethanolamine, carbodiimide, 1,6-hexanediol, glycerol, diethylene glycol, triethylene glycol, triethanolamine, neopentyl glycol, 4,4'-methylenebis(2-chloroaniline), ethylenediamine, 1,4-cyclohexanediol, tetramethylhexanediamine and hydrogenated bisphenol A;

[0014] The antioxidant is selected from one or more of Irganox 5057, Irganox 1098, Irganox 1135, Irgastab PUR70, MIANOX1098, antioxidant 1010, antioxidant 5057, antioxidant 168, antioxidant 1076, B225 and BHT;

[0015] The ultraviolet light absorber is selected from one or more of Tinuvin B75, Tinuvin PUR866, MIASORB UV531, UV284, UV49, UV24, UV9, UV1, UV1130, B75, UV1050 and UV1180.

[0016] Preferably, the graphene and its derivatives are selected from one or more of graphene oxide, single-layer graphene with a sheet diameter of less than 50 μm, graphene with 2 to 10 layers, and graphene with more than 10 layers.

[0017] Preferably, the inorganic nanoparticles are selected from one or more of nano-silicon dioxide, nano-titanium dioxide, nano-zinc oxide and nano-aluminum oxide.

[0018] Preferably, the carbon black is selected from one or more of ordinary carbon black, high pigment carbon black with a mesh size greater than 1250, acetylene carbon black and high wear-resistant furnace black.

[0019] Preferably, the solvent B is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene;

[0020] The polar group-containing cellulose is selected from one or more of hydroxypropyl methylcellulose, methyl cellulose, hydroxyethyl cellulose, hydroxymethyl cellulose and microcrystalline cellulose.

[0021] Preferably, the coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, titanate coupling agent, γ-methacryloxypropyltrimethoxysilane, isocyanatepropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, anilinemethyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane.

[0022] Preferably, the functional resin containing polar groups is selected from one or more of polyvinyl butyral resin, polyimide resin, acrylic resin, epoxy resin, unsaturated polyester resin, phenolic resin, polycarbonate resin, polyether sulfone resin, alkyd resin and uric acid resin;

[0023] The metal powder is selected from one or more of black iron oxide, iron powder, aluminum powder, copper oxide, copper powder, nickel powder, cobalt powder and silver powder.

[0024] The present invention provides a method for preparing the polyurethane adhesive described in the above technical solution, comprising the following steps:

[0025] After the polyol is vacuum dehydrated, it is mixed with solvent A at a temperature below 60°C, and then isocyanate, catalyst, chain extender, antioxidant and ultraviolet light absorber are added, mixed, heated, and reacted under an inert atmosphere to obtain a prepolymer;

[0026] Mixing graphene and its derivatives, inorganic nanoparticles, carbon black and solvent B to obtain a filler solution 1;

[0027] Mixing polar group-containing cellulose, a coupling agent, a polar group-containing functional resin and solvent B to obtain filler solution 2;

[0028] The filler solution 1, the filler solution 2 and the prepolymer are ground and mixed, reacted for 2 to 4.5 hours under grinding, and then metal powder is added and stirred for 18 to 23 minutes to obtain a polyurethane adhesive.

[0029] Compared with the prior art, the polyurethane adhesive provided by the present invention increases the content of polar groups such as carbamate groups and urea groups in the system by adding substances such as cellulose and functional resins containing strong polar groups on the surface, forms more hydrogen bonds during the bonding process, and significantly improves the film-forming property, bonding strength, weather resistance and hydrolysis resistance of the adhesive; the addition of metal powder can not only fill the grooves on the surface of the substrate, but also protect the surface, replace the polyurethane to be oxidized, and increase the storage stability and service life of the system. DETAILED DESCRIPTION

[0030] The present invention provides a polyurethane adhesive, which comprises the following raw materials in parts by mass:

[0031] 100 parts of prepolymer, 0.3-30 parts of graphene and its derivatives, 0.1-20 parts of inorganic nanoparticles, 10-100 parts of carbon black, 200-500 parts of solvent B, 0.5-25 parts of cellulose containing polar groups, 5-30 parts of coupling agents, 5-50 parts of functional resin containing polar groups and 0.5-20 parts of metal powder;

[0032] The prepolymer comprises the following raw materials:

[0033] 100 parts of polyol, 30-200 parts of solvent A, 15-210 parts of isocyanate, 0.01-13 parts of catalyst, 0-30 parts of chain extender, 0.1-10 parts of antioxidant, and 0.05-10 parts of ultraviolet light absorber.

[0034] The polyurethane adhesive provided by the present invention is prepared by a common modification reaction of a prepolymer with cellulose containing polar groups, a coupling agent, a functional resin containing polar groups, inorganic nanoparticles, etc., so that it has excellent film-forming property, bonding strength, weather resistance and hydrolysis resistance.

[0035] The raw materials for preparing the polyurethane adhesive provided by the invention include 100 parts of prepolymer; the prepolymer includes the following raw materials: 100 parts of polyol, 30-200 parts of solvent A, 15-210 parts of isocyanate, 0.01-13 parts of catalyst, 0-30 parts of chain extender, 0.1-10 parts of antioxidant and 0.05-10 parts of ultraviolet light absorber.

[0036] In the present invention, the polyol is used in an amount of 100 parts. The polyol is selected from one or more of polyethylene adipate glycol propylene glycol ester diol, sorbitol, polybutylene glycol, polyoxypropylene triol, polycaprolactone diol, castor oil polyol, polytetramethylene ether diol, polyadipate glycol propylene glycol ester diol, polyethylene glycol, polyhexamethylene carbonate diol, polytrimethylene ether diol, xylitol and vegetable oil polyol; preferably one or more of polycaprolactone diol, polyethylene glycol, polytetramethylene ether diol, polyethylene adipate glycol propylene glycol ester diol, polybutylene glycol, polyhexamethylene carbonate diol, polycaprolactone diol, polyoxypropylene triol and polytrimethylene ether diol.

[0037] In the present invention, the amount of the solvent A is 30 to 200 parts, preferably 40 to 150 parts, and more preferably 50 to 120 parts; the solvent A is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene, preferably one or more of ethyl acetate, butyl acetate, acetone, dichloromethane, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0038] In the present invention, the amount of the isocyanate is 15 to 210 parts, preferably 30 to 180 parts, and more preferably 50 to 150 parts. The isocyanate is selected from hexamethylene diisocyanate, hexamethylene diisocyanate trimer, 4,4′-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate biuret, isophorone diisocyanate trimer, lysine diisocyanate, methylcyclohexyl diisocyanate, cyclohexane dimethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate trimer, toluene diisocyanate trimer, 1,5-naphthalene diisocyanate, p-phenylene diisocyanate , toluene diisocyanate dimer and one or more of diphenylmethane diisocyanate dimer; preferably selected from hexamethylene diisocyanate, hexamethylene diisocyanate biuret, isophorone diisocyanate trimer, diphenylmethane diisocyanate trimer, cyclohexane dimethylene diisocyanate, toluene diisocyanate trimer, methylcyclohexyl diisocyanate, hexamethylene diisocyanate trimer, hexamethylene diisocyanate and one or more of lysine diisocyanate.

[0039] In the present invention, the amount of the catalyst is 0.01 to 13 parts, preferably 0.05 to 10 parts, and more preferably 0.08 to 5 parts. The catalyst is selected from one or more of dibutyltin dilaurate, stannous octoate, triethylamine, dibutyltin diacetate, potassium acetate, lead isooctanoate, phenylmercuric acetate, tetrabutyl titanate, tetramethyldipropylenetriamine, tetramethylpropylenediamine, tetramethylhexanediamine, N-methylimidazole, N-methylmorpholine, 1,4-dimethylpiperazine, bismuth isooctanoate and triethylenediamine, preferably one or more of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, triethylenediamine, tetrabutyl titanate, tetramethylhexanediamine, potassium acetate and tetramethylpropylenediamine.

[0040] In the present invention, the amount of the chain extender is 0 to 30 parts. The chain extender is selected from one or more of 1,4-butanediol, glycidyl allyl ether, trimethylolpropane, trimethylolethane, methyldiethanolamine, carbodiimide, 1,6-hexanediol, glycerol, diethylene glycol, triethylene glycol, triethanolamine, neopentyl glycol, 4,4'-methylenebis(2-chloroaniline), ethylenediamine, 1,4-cyclohexanediol, tetramethylhexanediamine and hydrogenated bisphenol A; preferably one or more of carbodiimide, diethylene glycol, 1,4-butanediol, trimethylolpropane, ethylenediamine, 4,4'-methylenebis(2-chloroaniline), trimethylolethane, tetramethylhexanediamine and triethanolamine.

[0041] In the present invention, the amount of the antioxidant is 0.1 to 10 parts. The antioxidant is selected from one or more of Irganox5057, Irganox 1098, Irganox 1135, Irgastab PUR 70, MIANOX 1098, antioxidant 1010, antioxidant 5057, antioxidant 168, antioxidant 1076, B225 and BHT; preferably one or more of Irgastab PUR 70, Irganox5057, Irganox 1135 and MIANOX 1098.

[0042] In the present invention, the amount of the ultraviolet light absorber is 0.05 to 10 parts. The ultraviolet light absorber is selected from one or more of Tinuvin B75, Tinuvin PUR866, MIASORB UV531, UV284, UV49, UV24, UV9, UV1, UV1130, B75, UV1050 and UV1180, preferably one or more of Tinuvin B75, MIASORB UV531, UV49, UV284, UV24 and Tinuvin PUR866.

[0043] The raw materials of the prepolymer in the present invention include 100 parts of polycaprolactone diol, 70 parts of ethyl acetate, 20 parts of hexamethylene diisocyanate, 60 parts of phenylmethane diisocyanate trimer, 0.2 parts of dibutyltin dilaurate, 2 parts of carbodiimide, 1 part of Irgastab PUR 70, and 0.5 parts of UV531;

[0044] Or including 100 parts of polyethylene glycol, 80 parts of methyl ethyl ketone, 110 parts of hexamethylene diisocyanate biuret, 0.1 parts of stannous octoate, 3 parts of diethylene glycol, 1.5 parts of Irganox 5057, 1 part of UV49;

[0045] Or including 100 parts of polytetramethylene ether glycol, 100 parts of butyl acetate, 70 parts of isophorone diisocyanate trimer, 0.15 parts of stannous octoate, 1 part of 1,4-butanediol, 1 part of Irgastab PUR70, and 1 part of Tinuvin PUR866;

[0046] or including 50 parts of polyethylene glycol propylene glycol adipate diol, 50 parts of polybutylene glycol, 90 parts of acetone, 80 parts of diphenylmethane diisocyanate trimer, 0.4 parts of dibutyltin dilaurate, 6 parts of trimethylolpropane, 3 parts of Irganox 1135, 1.5 parts of UV284;

[0047] Or including 100 parts of polyhexamethylene carbonate diol, 80 parts of N,N-dimethylformamide, 40 parts of acetone, 60 parts of cyclohexane dimethylene diisocyanate, 0.25 parts of dibutyltin diacetate, 1.5 parts of antioxidant MIANOX 1098, and 1 part of Tinuvin B75;

[0048] Or including 100 parts of polybutylene glycol, 80 parts of ethyl acetate, 90 parts of toluene diisocyanate trimer, 0.15 parts of stannous octoate, 3 parts of ethylenediamine, 1 part of Irgastab PUR 70, and 1 part of UV284;

[0049] Or including 100 parts of polyethylene glycol, 70 parts of dichloromethane, 70 parts of methylcyclohexyl diisocyanate, 0.1 parts of triethylenediamine, 1 part of 4,4'-methylenebis(2-chloroaniline), 0.5 parts of Irganox 1135, and 1.5 parts of UV531;

[0050] Or including 100 parts of polycaprolactone diol, 100 parts of dimethyl sulfoxide, 80 parts of isophorone diisocyanate trimer, 0.2 parts of tetrabutyl titanate, 2 parts of trimethylolethane, 2 parts of Irganox 5057, and 0.5 parts of Tinuvin PUR866;

[0051] Or including 100 parts of polyhexamethylene carbonate diol, 80 parts of N,N-dimethylacetamide, 100 parts of hexamethylene diisocyanate trimer, 0.15 parts of dibutyltin diacetate, 1 part of 1,4-butanediol, 0.5 parts of Irgastab PUR 70, and 1 part of UV284;

[0052] Or including 100 parts of polybutylene glycol, 50 parts of toluene, 50 parts of ethyl acetate, 110 parts of hexamethylene diisocyanate, 0.2 parts of tetramethylhexamethylenediamine, 3 parts of diethylene glycol, 1 part of antioxidant 1098, and 1 part of UV24;

[0053] Or including 20 parts of polyhexamethylene carbonate diol, 80 parts of polycaprolactone diol, 100 parts of methyl ethyl ketone, 90 parts of lysine diisocyanate, 0.1 parts of tetrabutyl titanate, 1 part of 1,4-butanediol, 0.5 parts of Irgastab PUR70, and 1 part of Tinuvin B75;

[0054] Or including 100 parts of polytetramethylene glycol, 100 parts of N,N-dimethylacetamide, 85 parts of diphenylmethane diisocyanate trimer, 0.1 parts of potassium acetate, 0.2 parts of tetramethylhexamethylenediamine, 3 parts of carbodiimide, 1 part of Irganox 1098, and 1 part of UV49;

[0055] Or including 100 parts of polyoxypropylene triol, 85 parts of N,N-dimethylformamide, 70 parts of isophorone diisocyanate trimer, 0.15 parts of triethylenediamine, 2 parts of triethanolamine, 1.5 parts of Irganox 1135, and 0.5 parts of Tinuvin PUR866;

[0056] Or include 100 parts of polytrimethylene ether glycol, 80 parts of dimethyl sulfoxide, 90 parts of hexamethylene diisocyanate, 0.2 parts of tetramethylpropylenediamine, 5 parts of ethylenediamine, 0.7 parts of Irganox 5057, and 1 part of UV531.

[0057] The raw materials for preparing the polyurethane adhesive provided by the present invention include 0.3 to 30 parts of graphene, preferably 5 to 30 parts; in a specific embodiment, the amount of graphene used is 10 parts, 13 parts, 15 parts, 18 parts, 20 parts, 25 parts, and 30 parts. The graphene in the present invention is selected from one or more of graphene oxide, single-layer graphene with a sheet diameter of less than 50 μm, graphene with 2 to 10 layers, and graphene with more than 10 layers.

[0058] The raw materials for preparing the polyurethane adhesive provided by the present invention include 0.1 to 20 parts of inorganic nanoparticles, preferably 0.5 to 5 parts; in a specific embodiment, the specific amount of the inorganic nanoparticles is 0.5 parts, 2 parts, 3 parts, 1.5 parts, 5 parts, 1 part, or 4 parts. The inorganic nanoparticles are selected from one or more of nano-silicon dioxide, nano-titanium dioxide, nano-zinc oxide and nano-aluminum oxide.

[0059] The raw materials for preparing the polyurethane adhesive provided by the present invention include 10 to 100 parts of carbon black, preferably 10 to 90 parts; in a specific embodiment, the amount of the carbon black is 40 parts, 10 parts, 50 parts, 25 parts, 48 ​​parts, 70 parts, 90 parts, 80 parts, or 35 parts. The carbon black in the present invention is selected from one or more of ordinary carbon black, high-pigment carbon black greater than 1250 mesh, acetylene carbon black and high-wear-resistant furnace black.

[0060] The raw materials for preparing the polyurethane adhesive provided by the present invention include 200 to 500 parts of solvent B, preferably 300 to 500 parts; in a specific embodiment, the amount of solvent B is 400 parts, 420 parts, 500 parts, 480 parts, 450 parts, 300 parts or 420 parts. The solvent B in the present invention is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene.

[0061] The raw materials for preparing the polyurethane adhesive provided by the present invention include 0.5 to 25 parts of cellulose containing polar groups, preferably 0.3 to 20 parts, and more preferably 0.5 to 5 parts; in a specific embodiment, the amount of the cellulose containing polar groups is 1 part, 3 parts, 2 parts, 5 parts, 0.5 parts, 1.5 parts, 1.2 parts or 0.7 parts. The cellulose containing polar groups is selected from one or more of hydroxypropyl methylcellulose, methylcellulose, hydroxyethyl cellulose, hydroxymethyl cellulose and microcrystalline cellulose.

[0062] The raw materials for preparing the polyurethane adhesive provided by the present invention include 5 to 30 parts of coupling agent, preferably; in a specific embodiment, the amount of the silane coupling agent is 40 parts, 20 parts, 30 parts, 15 parts, 10 parts, 28 parts or 25 parts. The silane coupling agent is selected from one or more of γ-aminopropyl triethoxysilane, γ-glycidyloxypropyl trimethoxysilane, titanate coupling agent, γ-methacryloxypropyl trimethoxysilane, isocyanate propyl triethoxysilane, γ-mercaptopropyl trimethoxysilane, isocyanate propyl trimethoxysilane, γ-(2,3-epoxypropyloxy)propyl trimethoxysilane, aniline methyl trimethoxysilane and γ-aminoethylaminopropyl trimethoxysilane.

[0063] The raw materials for preparing the polyurethane adhesive provided by the present invention include 5 to 50 parts of a functional resin containing a polar group, preferably 10 to 50 parts; in a specific embodiment, the amount of the functional resin containing a polar group is 15 parts, 20 parts, 10 parts, 40 parts, 50 parts, 18 parts, 28 parts or 25 parts. The functional resin containing a polar group is selected from one or more of polyvinyl butyral resin, polyimide resin, acrylic resin, epoxy resin, unsaturated polyester resin, phenolic resin, polycarbonate resin, polyether sulfone resin, alkyd resin and uric acid resin.

[0064] The inorganic nanoparticles, cellulose containing polar groups, coupling agents, and functional resins containing polar groups form covalent bonds or hydrogen bonds with NCO groups in polyurethane prepolymers and are grafted onto the prepolymers. The present invention uses polyols and isocyanates in the above raw materials to react to obtain carbamate groups; part of the carbamate groups continue to react with isocyanates to generate urea groups, and isocyanates react with amino groups in the coupling agent to also generate urea groups. Carbamate groups and urea groups are polar groups, and more hydrogen bonds are formed during the bonding process, which significantly improves the film-forming property, bonding strength, weather resistance, and hydrolysis resistance of the adhesive.

[0065] The raw materials for preparing the polyurethane adhesive provided by the present invention include 0.5 to 20 parts of metal powder, preferably 0.5 to 5 parts; in a specific embodiment, the amount of the metal powder is 0.5 parts, 0.6 parts, 1 parts, 1.5 parts or 3 parts. The metal powder is selected from one or more of black iron oxide, iron powder, aluminum powder, copper oxide, copper powder, nickel powder, cobalt powder and silver powder. The metal powder exists in the adhesive in a powder state. The metal powder in the present invention plays the role of filling the surface grooves of the substrate and protecting the surface, replacing the polyurethane to be oxidized, and increasing the storage stability and service life of the system.

[0066] In a specific embodiment of the present invention, the raw materials for preparing the polyurethane adhesive include 10 parts of graphene oxide, 2 parts of nano-silicon dioxide, 40 parts of high-color carbon black, 500 parts of butyl acetate, 1 part of microcrystalline cellulose, 15 parts of γ-aminopropyltriethoxysilane, 15 parts of acrylic resin, 100 parts of prepolymer and 1 part of iron oxide black;

[0067] Or comprising 30 parts of few-layer graphene, 3 parts of nano-alumina, 10 parts of acetylene carbon black, 500 parts of butyl acetate, 3 parts of hydroxyethyl cellulose, 28 parts of γ-methacryloxypropyltrimethoxysilane, 20 parts of polyvinyl butyral resin, 100 parts of prepolymer and 1 part of copper powder;

[0068] Or including 20 parts of monolayer graphene, 1.5 parts of nano-silicon dioxide, 50 parts of ordinary carbon black, 500 parts of ethyl acetate, 2 parts of hydroxypropyl methylcellulose, 25 parts of γ-glycidyloxypropyltrimethoxysilane, 10 parts of polyvinyl butyral resin, 100 parts of prepolymer and 0.6 parts of copper powder;

[0069] Or including 25 parts of graphene oxide, 5 parts of nano titanium dioxide, 25 parts of acetylene carbon black, 500 parts of acetone, 5 parts of hydroxyethyl cellulose, 20 parts of γ-methacryloxypropyltrimethoxysilane, 40 parts of phenolic resin, 100 parts of prepolymer and 3 parts of cobalt powder;

[0070] or comprising 30 parts of few-layer graphene, 2 parts of nano titanium dioxide, 10 parts of high-color carbon black and 450 parts of methyl ethyl ketone, 3 parts of microcrystalline cellulose, 28 parts of γ-aminoethylaminopropyltrimethoxysilane, 50 parts of epoxy resin, 100 parts of prepolymer and 1 part of iron oxide black;

[0071] Or including 20 parts of graphene oxide, 2 parts of nano-silicon dioxide, 50 parts of ordinary carbon black, 500 parts of N,N-dimethylformamide, 2 parts of hydroxyethyl cellulose, 30 parts of γ-glycidyloxypropyltrimethoxysilane, 15 parts of phenolic resin, 100 parts of prepolymer and 1 part of copper oxide;

[0072] Or including 15 parts of monolayer graphene, 1 part of nano zinc oxide, 50 parts of high-color carbon black, 500 parts of N,N-dimethylacetamide, 0.5 parts of methyl cellulose, 20 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 20 parts of phenolic resin, 100 parts of prepolymer and 0.5 parts of iron powder;

[0073] Or including 18 parts of monolayer graphene, 4 parts of nano titanium dioxide, 48 parts of high wear-resistant furnace black, 480 parts of N,N-dimethylacetamide, 1 part of hydroxypropyl methylcellulose, 20 parts of γ-mercaptopropyltrimethoxysilane and 10 parts of γ-aminopropyltriethoxysilane, 28 parts of polyethersulfone resin, 100 parts of prepolymer and 1.5 parts of copper oxide;

[0074] Or including 10 parts of few-layer graphene, 1.5 parts of nano zinc oxide, 70 parts of ordinary carbon black, 500 parts of ethyl acetate, 1.5 parts of microcrystalline cellulose, 30 parts of γ-mercaptopropyltrimethoxysilane, 25 parts of polyimide resin, 100 parts of prepolymer and 0.5 parts of copper powder;

[0075] Or including 13 parts of multilayer graphene, 2 parts of nano titanium dioxide, 90 parts of high wear-resistant furnace black, 500 parts of toluene, 1 part of hydroxyethyl cellulose, 10 parts of isocyanate propyl trimethoxy silane, 20 parts of γ-glycidyloxypropyl trimethoxy silane, 30 parts of polyimide resin, 100 parts of prepolymer and 1 part of iron powder;

[0076] Or including 30 parts of few-layer graphene, 1 part of nano-alumina, 40 parts of acetylene carbon black, 500 parts of ethyl acetate, 0.5 parts of hydroxypropyl methylcellulose, 30 parts of γ-methacryloxypropyltrimethoxysilane, 20 parts of epoxy resin, 100 parts of prepolymer and 1 part of iron powder;

[0077] Or including 10 parts of monolayer graphene, 1 part of nano titanium dioxide and 2 parts of nano silicon dioxide, 80 parts of ordinary carbon black, 420 parts of dichloromethane, 1.2 parts of methyl cellulose, 30 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 15 parts of acrylic resin, 100 parts of prepolymer and 0.5 parts of iron oxide black;

[0078] or comprising 20 parts of multilayer graphene, 0.5 parts of nano-alumina, 2 parts of nano-titanium dioxide, 35 parts of high-color carbon black, 400 parts of butyl acetate, 0.5 parts of methyl cellulose, 20 parts of aniline methyl trimethoxy silane, 28 parts of phenolic resin, 100 parts of prepolymer and 1 part of copper oxide;

[0079] Or include 15 parts of multilayer graphene, 3 parts of nano alumina, 50 parts of high wear-resistant furnace black, 400 parts of acetone, 0.7 parts of microcrystalline cellulose, 40 parts of aniline methyl trimethoxy silane, 18 parts of polyvinyl butyral resin, 100 parts of prepolymer and 0.5 parts of cobalt powder.

[0080] The present invention also provides a method for preparing the polyurethane adhesive described in the above technical solution, comprising the following steps:

[0081] After the polyol is vacuum dehydrated, it is mixed with solvent A at a temperature below 60°C, and then isocyanate, catalyst, chain extender, antioxidant and ultraviolet light absorber are added, mixed, heated, and reacted under an inert atmosphere to obtain a prepolymer;

[0082] Mixing graphene and its derivatives, inorganic nanoparticles, carbon black and solvent B to obtain a filler solution 1;

[0083] Mixing polar group-containing cellulose, a coupling agent, a polar group-containing functional resin and solvent B to obtain filler solution 2;

[0084] The filler solution 1, the filler solution 2 and the prepolymer are ground and mixed, reacted for 2 to 4.5 hours under grinding, and then metal powder is added and stirred for 18 to 23 minutes to obtain a polyurethane adhesive.

[0085] In the present invention, the polyol is vacuum dehydrated, mixed with solvent A at a temperature below 60°C, and then isocyanate, catalyst, chain extender, antioxidant and ultraviolet light absorber are added, mixed, and the temperature is raised to about 75°C for reaction. In the present invention, the polyol is preferably vacuum dehydrated for at least 2 hours. The reaction time under an inert atmosphere is 30 to 50 minutes, preferably 35 to 45 minutes.

[0086] In the present invention, the inert atmosphere is preferably nitrogen.

[0087] In the present invention, the solvent B mixed with the cellulose containing polar groups, the coupling agent and the functional resin containing polar groups accounts for 20 to 70% of the total solvent B by mass.

[0088] In the present invention, the filler solution 1, the filler solution 2 and the prepolymer are preferably mixed, preferably in a sand mill; reacted under grinding conditions for 2 to 4.5 hours, more preferably 3 to 4 hours, and most preferably 4 hours. The temperature of the reaction under grinding is 20 to 90°C; specifically, the temperature of the reaction under grinding is 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C.

[0089] The filler solution 1 prepared by the present invention can increase mechanical properties, absorb ultraviolet rays, and protect the surface; the filler solution 2 has the functions of increasing viscosity, increasing mechanical strength, preventing cracks, protecting the surface, increasing service life, and improving glossiness.

[0090] In order to further illustrate the present invention, a polyurethane adhesive and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0091] Example 1

[0092] a. Preparation of prepolymer

[0093] Pour 100 parts of polycaprolactone diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 70 parts of ethyl acetate, stir evenly, add 20 parts of hexamethylene diisocyanate and 60 parts of diphenylmethane diisocyanate trimer into a three-necked flask, add 0.2 parts of dibutyltin dilaurate, 2 parts of carbodiimide, 1 part of Irgastab PUR70, 0.5 parts of UV531, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0094] b. Preparation of adhesive

[0095] In a container, 10 parts of graphene oxide, 2 parts of nano-silicon dioxide, 40 parts of high-color carbon black and 200 parts of butyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 1 part of microcrystalline cellulose, 15 parts of γ-aminopropyltriethoxysilane, 15 parts of acrylic resin and 300 parts of ethyl acetate are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and react at 35° C. for 4 hours, and add 1 part of iron oxide black; discharge the material at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0096] Example 2

[0097] a. Preparation of prepolymer

[0098] Pour 100 parts of polyethylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 80 parts of ethyl acetate, stir evenly, add 110 parts of hexamethylene diisocyanate biuret into a three-necked flask, add 0.1 parts of stannous octoate, 3 parts of diethylene glycol, 1.5 parts of Irganox 5057, 1 part of UV49, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0099] b. Preparation of adhesive

[0100] In a container, 30 parts of few-layer graphene, 3 parts of nano-alumina, 10 parts of acetylene carbon black and 300 parts of butyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 3 parts of hydroxyethyl cellulose, 28 parts of γ-methacryloxypropyltrimethoxysilane, 20 parts of polyvinyl butyral resin and 200 parts of butyl acetate are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and stir at 40° C. for reaction for 4 hours, add 1 part of copper powder and stir for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0101] Example 3

[0102] a. Preparation of prepolymer

[0103] Pour 100 parts of polytetramethylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 100 parts of butyl acetate, stir evenly, add 70 parts of isophorone diisocyanate trimer into a three-necked flask, add 0.15 parts of stannous octoate, 1 part of 1,4-butanediol, 1 part of Irgastab PUR 70, 1 part of Tinuvin PUR866, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0104] b. Preparation of adhesive

[0105] In a container, 20 parts of single-layer graphene, 1.5 parts of nano-silicon dioxide, 50 parts of ordinary carbon black and 250 parts of ethyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 2 parts of hydroxypropyl methylcellulose, 25 parts of γ-glycidyloxypropyl trimethoxysilane, 10 parts of polyvinyl butyral resin and 250 parts of ethyl acetate are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and stir at 60° C. for reaction for 2 hours, add 0.6 parts of copper powder and stir for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0106] Example 4

[0107] a. Preparation of prepolymer

[0108] Pour 50 parts of polyethylene glycol adipate diol and 50 parts of polybutylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 90 parts of acetone, stir evenly, add 80 parts of diphenylmethane diisocyanate trimer into a three-necked flask, add 0.4 parts of dibutyltin dilaurate, 6 parts of trimethylolpropane, 3 parts of Irganox 1135, 1.5 parts of UV284, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0109] b. Preparation of adhesive

[0110] In a container, 25 parts of graphene oxide, 5 parts of nano-titanium dioxide, 25 parts of acetylene carbon black and 300 parts of acetone are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 5 parts of hydroxyethyl cellulose, 20 parts of γ-methacryloxypropyltrimethoxysilane, 40 parts of phenolic resin and 200 parts of acetone are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, ground and reacted at 30° C. for 4 hours, and 3 parts of cobalt powder are added and stirred for 20 minutes; the material is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0111] Example 5

[0112] a. Preparation of prepolymer

[0113] Pour 100 parts of polyhexamethylene carbonate diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 80 parts of N,N-dimethylformamide and 40 parts of acetone, stir evenly, add 60 parts of cyclohexane dimethylene diisocyanate into a three-necked flask, add 0.25 parts of dibutyltin diacetate, 1.5 parts of antioxidant 1098, 1 part of Tinuvin B75, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0114] b. Preparation of adhesive

[0115] In a container, 30 parts of few-layer graphene, 2 parts of nano titanium dioxide, 10 parts of high-color carbon black and 200 parts of methyl ethyl ketone are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 3 parts of microcrystalline cellulose, 28 parts of γ-aminoethylaminopropyltrimethoxysilane, 50 parts of epoxy resin and 250 parts of methyl ethyl ketone are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and stir at 40° C. for reaction for 3 hours, add 1 part of black iron oxide and stir for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0116] Example 6

[0117] a. Preparation of prepolymer

[0118] Pour 100 parts of polybutylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 80 parts of ethyl acetate, stir evenly, add 90 parts of toluene diisocyanate trimer into a three-necked flask, add 0.15 parts of stannous octoate, 3 parts of ethylenediamine, 1 part of Irgastab PUR 70, 1 part of UV284, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0119] b. Preparation of adhesive

[0120] In a container, 20 parts of graphene oxide, 2 parts of nano-silicon dioxide, 50 parts of ordinary carbon black and 300 parts of N,N-dimethylformamide are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 2 parts of hydroxyethyl cellulose, 30 parts of γ-glycidyloxypropyltrimethoxysilane, 15 parts of phenolic resin and 200 parts of N,N-dimethylformamide are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, and the mixture is ground and stirred at 60° C. for 4 hours, and 1 part of copper oxide is added and stirred for 20 minutes; the mixture is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use;

[0121] Example 7

[0122] a. Preparation of prepolymer

[0123] Pour 100 parts of polyethylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 70 parts of dichloromethane, stir evenly, add 70 parts of methylcyclohexyl diisocyanate into a three-necked flask, add 0.1 parts of triethylenediamine, 1 part of 4,4'-methylenebis(2-chloroaniline), 0.5 parts of Irganox 1135, 1.5 parts of UV531, etc., mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere, and obtain a prepolymer;

[0124] b. Preparation of adhesive

[0125] In a container, 15 parts of single-layer graphene, 1 part of nano zinc oxide, 50 parts of high-color carbon black and 250 parts of N,N-dimethylacetamide are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 0.5 parts of methyl cellulose, 20 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 250 parts of N,N-dimethylacetamide and 20 parts of phenolic resin are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, ground and stirred at 40°C for 4 hours, and 0.5 parts of iron powder are added; the material is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0126] Example 8

[0127] a. Preparation of prepolymer

[0128] Pour 100 parts of polycaprolactone diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 100 parts of dimethyl sulfoxide, stir evenly, add 80 parts of isophorone diisocyanate trimer into a three-necked flask, add 0.2 parts of tetrabutyl titanate, 2 parts of trimethylolethane, 2 parts of Irganox5057, 0.5 parts of Tinuvin PUR866, etc., mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0129] b. Preparation of adhesive

[0130] In a container, 18 parts of single-layer graphene, 4 parts of nano-titanium dioxide, 48 parts of high-wear-resistant furnace black and 200 parts of N,N-dimethylacetamide are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 1 part of hydroxypropyl methylcellulose, 20 parts of γ-mercaptopropyltrimethoxysilane and 10 parts of γ-aminopropyltriethoxysilane, 28 parts of polyethersulfone resin and 280 parts of N,N-dimethylacetamide are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, ground and stirred at 90° C. for reaction for 4 hours, 1.5 parts of copper oxide are added and stirred for 20 minutes; the material is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0131] Example 9

[0132] a. Preparation of prepolymer

[0133] Pour 100 parts of polyhexamethylene carbonate diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 80 parts of N,N-dimethylacetamide, stir evenly, add 100 parts of hexamethylene diisocyanate trimer into a three-necked flask, add 0.15 parts of dibutyltin diacetate, 1 part of 1,4-butanediol, 0.5 parts of Irgastab PUR 70, 1 part of UV284, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0134] b. Preparation of adhesive

[0135] In a container, 10 parts of few-layer graphene, 1.5 parts of nano zinc oxide, 70 parts of ordinary carbon black and 250 parts of ethyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 1.5 parts of microcrystalline cellulose, 30 parts of γ-mercaptopropyltrimethoxysilane, 25 parts of polyimide resin and 250 parts of ethyl acetate are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and stir at 60° C. for reaction for 4 hours, add 0.5 parts of copper powder and stir for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0136] Example 10

[0137] a. Preparation of prepolymer

[0138] Pour 100 parts of polybutylene glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, then add 50 parts of toluene and 50 parts of ethyl acetate, stir evenly, add 110 parts of hexamethylene diisocyanate into a three-necked flask, then add 0.2 parts of tetramethylhexamethylenediamine, 3 parts of diethylene glycol, 1 part of antioxidant 1098, 1 part of UV24, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0139] b. Preparation of adhesive

[0140] In a container, 13 parts of multilayer graphene, 2 parts of nano titanium dioxide, 90 parts of high wear-resistant furnace black and 300 parts of toluene are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 1 part of hydroxyethyl cellulose, 10 parts of isocyanate propyl trimethoxy silane and 20 parts of γ-glycidyloxypropyl trimethoxy silane, 30 parts of polyimide resin and 200 parts of toluene are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and react at 20° C. for 4 hours, add 1 part of iron powder and stir to react for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0141] Embodiment 11

[0142] a. Preparation of prepolymer

[0143] Pour 20 parts of polyhexamethylene carbonate diol and 80 parts of polycaprolactone diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 100 parts of methyl ethyl ketone, stir evenly, add 90 parts of lysine diisocyanate into a three-necked flask, add 0.1 parts of tetrabutyl titanate, 1 part of 1,4-butanediol, 0.5 parts of Irgastab PUR 70, 1 part of Tinuvin B75, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0144] b. Preparation of adhesive

[0145] In a container, 30 parts of few-layer graphene, 1 part of nano-alumina, 40 parts of acetylene carbon black and 300 parts of ethyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse the mixture uniformly to obtain filler solution 1; in another container, 0.5 parts of hydroxypropyl methylcellulose, 30 parts of γ-methacryloxypropyltrimethoxysilane, 20 parts of epoxy resin and 200 parts of ethyl acetate are mixed, and the mixture is stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, and the mixture is ground and reacted at 30° C. for 4 hours, and 1 part of iron powder is added and stirred for 20 minutes; the mixture is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0146] Example 12

[0147] a. Preparation of prepolymer

[0148] Pour 100 parts of polytetrahydrofuran ether diol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, then add 100 parts of N,N-dimethylacetamide, stir evenly, add 85 parts of diphenylmethane diisocyanate trimer into a three-necked flask, then add 0.1 parts of potassium acetate and 0.2 parts of tetramethylhexamethylenediamine, 3 parts of carbodiimide, 1 part of Irganox 1098, 1 part of UV49, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0149] b. Preparation of adhesive

[0150] In a container, 10 parts of single-layer graphene, 1 part of nano-titanium dioxide and 2 parts of nano-silicon dioxide, 80 parts of ordinary carbon black and 200 parts of dichloromethane are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 1.2 parts of methyl cellulose, 30 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 15 parts of acrylic resin and 220 parts of dichloromethane are mixed, and stirred to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, grind and stir at 50° C. for reaction for 4 hours, add 0.5 parts of iron oxide black and stir for 20 minutes; discharge the material at room temperature to obtain a polymer adhesive, and put it into an aluminum bottle for standby use.

[0151] Embodiment 13

[0152] a. Preparation of prepolymer

[0153] Pour 100 parts of polyoxypropylene triol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 85 parts of N,N-dimethylformamide, stir evenly, add 70 parts of isophorone diisocyanate trimer into a three-necked flask, add 0.15 parts of triethylenediamine, 2 parts of triethanolamine, 1.5 parts of Irganox 1135, 0.5 parts of Tinuvin PUR866, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0154] b. Preparation of adhesive

[0155] In a container, 20 parts of multilayer graphene, 0.5 parts of nano-alumina, 2 parts of nano-titanium dioxide, 35 parts of high-color carbon black and 200 parts of butyl acetate are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 0.5 parts of methyl cellulose, 20 parts of aniline methyl trimethoxy silane, 28 parts of phenolic resin and 200 parts of butyl acetate are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, ground and reacted at 50° C. for 4 hours, and 1 part of copper oxide is added and stirred for 20 minutes; the material is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0156] Embodiment 14

[0157] a. Preparation of prepolymer

[0158] Pour 100 parts of polytrimethylene ether glycol into a reaction bottle and vacuum dehydrate for more than 2 hours, cool to below 60°C, add 80 parts of dimethyl sulfoxide, stir evenly, add 90 parts of hexamethylene diisocyanate into a three-necked flask, add 0.2 parts of tetramethylpropylenediamine, 5 parts of ethylenediamine, 0.7 parts of Irganox 5057, 1 part of UV531, etc. and mix evenly, heat to about 75°C, react for 40 minutes under N2 atmosphere to obtain a prepolymer;

[0159] b. Preparation of adhesive

[0160] In a container, 15 parts of multilayer graphene, 3 parts of nano-alumina, 50 parts of high-wear-resistant furnace black and 200 parts of acetone are mixed, and ultrasonic mechanical stirring is used to disperse them uniformly to obtain filler solution 1; in another container, 0.7 parts of microcrystalline cellulose, 40 parts of aniline methyl trimethoxysilane, 18 parts of polyvinyl butyral resin and 200 parts of acetone are mixed, and stirred uniformly to obtain filler solution 2; filler solution 1 and filler solution 2 are added to 100 parts of prepolymer prepared in step a, ground and reacted at 40° C. for 4 hours, 0.5 parts of cobalt powder are added and stirred for 20 minutes; the material is discharged at room temperature to obtain a polymer adhesive, which is put into an aluminum bottle for standby use.

[0161] Comparative Example 1

[0162] This comparative example uses Swiss sika Primer-206G+P adhesive with excellent performance in the industry;

[0163] Comparative Example 2

[0164] This comparative example uses German Henkel TEROSON PU 8511 adhesive with excellent performance in the same field;

[0165] (II) Performance test of adhesive

[0166] 1) Shear strength: According to the GB / T7124-2008 test method, 100mm×25mm glass is selected as the bonded substrate. The adhesive surface needs to be cleaned of oil and dust with solvents such as ethyl acetate and acetone, and then dried. Then, wipe the substrate surface with ethanol using an absorbent cotton ball. After standing for 5 minutes, use a brush to dip the shaken adhesive and evenly apply it on the substrate surface. The thickness is about 0.5mm. After standing for 5-10 minutes, use a glue gun to apply the sealant. The parallel overlap length of the two glass plates is 12.5mm, and the thickness of the sealant is about 3-4mm. Use a scraper to quickly wipe off the residual glue remaining around the sample. During the gluing process, ensure that there are no bubbles inside the glue. Place it under standard conditions (23℃, 50%RH), test the shear strength and failure form after curing for 7 days, and compare it with the blank sample without adhesive.

[0167] 2) Determination of surface drying time: According to GB / T1728-2020 standard, the finger touch method is used. Touch the surface of the adhesive lightly with your finger. If there is no adhesive sticking to your hand, the surface is considered dry.

[0168] 3) Hydrolysis resistance: After the prepared polyurethane adhesive bonding sample is cured, it is placed in a 40°C environment and soaked in water for 72 hours to test its shear strength and failure form.

[0169] 4) High temperature and high humidity performance: After the polyurethane adhesive bonding sample is cured, it is placed in an environment of 70±2°C, 90%-100% RH for 300 hours to test its shear strength and failure form.

[0170] The polyurethane adhesives prepared in the above Examples 1 to 14 and Comparative Examples 1 to 2 were subjected to shear strength tests. The results are shown in Table 1 below, where the blank examples are samples without adhesive.

[0171] Table 1

[0172]

[0173]

[0174] In summary, the adhesive of the present invention is prepared by the joint modification reaction of the cellulose containing polar groups, the coupling agent, the functional resin containing polar groups, and the inorganic nanoparticles, and has excellent hydrolysis resistance, high temperature and high humidity resistance, and good bonding performance, which are superior to the best-performing sika Primer-206G+P model and Henkel TEROSON PU 8511 model products in the industry, and have great practical application value.

[0175] It can be seen from the above embodiments that the present invention provides a polyurethane adhesive, which comprises the following raw materials, in parts by mass: 100 parts of prepolymer, 0.3-30 parts of graphene and its derivatives, 0.1-20 parts of inorganic nanoparticles, 10-100 parts of carbon black, 200-500 parts of solvent B, 0.5-25 parts of cellulose containing polar groups, 5-30 parts of coupling agents, 5-50 parts of functional resins containing polar groups and 0.5-20 parts of metal powder; the prepolymer comprises the following raw materials: 100 parts of polyol, 30-200 parts of solvent A, 15-210 parts of isocyanate, 0.01-13 parts of catalyst, 0-30 parts of chain extender, 0.1-10 parts of antioxidant and 0.05-10 parts of ultraviolet light absorber. Compared with the prior art, the polyurethane adhesive provided by the present invention increases the content of polar groups such as carbamate groups and urea groups in the system by adding substances such as cellulose and functional resins with strong polar groups on the surface, forms more hydrogen bonds during the bonding process, and significantly improves the film-forming property, bonding strength, weather resistance and hydrolysis resistance of the adhesive; the addition of metal powder can not only fill the grooves on the surface of the substrate, but also protect the surface, replace the polyurethane to be oxidized, and increase the storage stability and service life of the system. The experimental results show that the surface drying time of the polyurethane adhesive is 2 to 3 minutes; the shear strength under standard conditions is 4.0 to 4.8 MPa, in the form of cohesive failure; after soaking in water for 72 hours at 40°C, the shear strength is 4.0 to 4.8 MPa, in the form of cohesive failure; after being treated for 300 hours at 70±2°C and 90% to 100% RH, the shear strength is 3.9 to 4.6 MPa, in the form of cohesive failure.

[0176] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A polyurethane adhesive comprising the following raw materials in parts by mass: 100 parts of prepolymer, 0.3-30 parts of graphene and its derivatives, 0.1-20 parts of inorganic nanoparticles, 10-100 parts of carbon black, 200-500 parts of solvent B, 0.5-25 parts of cellulose containing polar groups, 5-30 parts of coupling agents, 5-50 parts of functional resin containing polar groups and 0.5-20 parts of metal powder; The prepolymer comprises the following raw materials: 100 parts of polyol, 30-200 parts of solvent A, 15-210 parts of isocyanate, 0.01-13 parts of catalyst, 0-30 parts of chain extender, 0.1-10 parts of antioxidant, and 0.05-10 parts of ultraviolet light absorber.

2. The polyurethane adhesive according to claim 1, It is characterized in that The polyol is selected from one or more of polyethylene glycol propylene glycol adipate diol, sorbitol, polybutylene glycol, polyoxypropylene triol, polycaprolactone diol, castor oil polyol, polytetramethylene ether diol, polypropylene adipate diol, polyethylene glycol, polyhexamethylene carbonate diol, polytrimethylene ether glycol, xylitol and vegetable oil polyol; The isocyanate is selected from one or more of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, 4,4′-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate biuret, isophorone diisocyanate trimer, lysine diisocyanate, methylcyclohexyl diisocyanate, cyclohexane dimethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate trimer, toluene diisocyanate trimer, 1,5-naphthalene diisocyanate, p-phenylene diisocyanate, toluene diisocyanate dimer and diphenylmethane diisocyanate dimer.

3. The polyurethane adhesive according to claim 1, It is characterized in that The solvent A is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene; The catalyst is selected from one or more of stannous octoate, triethylamine, dibutyltin diacetate, potassium acetate, lead isooctanoate, phenylmercuric acetate, dibutyltin dilaurate, tetrabutyl titanate, tetramethyldipropylenetriamine, tetramethylpropylenediamine, tetramethylhexanediamine, N-methylimidazole, N-methylmorpholine, 1,4-dimethylpiperazine, bismuth isooctanoate and triethylenediamine; The chain extender is selected from one or more of 1,4-butanediol, glycidyl allyl ether, trimethylolpropane, trimethylolethane, methyldiethanolamine, carbodiimide, 1,6-hexanediol, glycerol, diethylene glycol, triethylene glycol, triethanolamine, neopentyl glycol, 4,4'-methylenebis(2-chloroaniline), ethylenediamine, 1,4-cyclohexanediol, tetramethylhexanediamine and hydrogenated bisphenol A; The antioxidant is selected from one or more of Irganox 5057, Irganox 1098, Irganox 1135, Irgastab PUR70, MIANOX1098, antioxidant 1010, antioxidant 5057, antioxidant 168, antioxidant 1076, B225 and BHT; The ultraviolet light absorber is selected from one or more of Tinuvin B75, Tinuvin PUR866, MIASORB UV531, UV284, UV49, UV24, UV9, UV1, UV1130, B75, UV1050 and UV1180.

4. The polyurethane adhesive according to claim 1, It is characterized in that The graphene and its derivatives are selected from one or more of graphene oxide, single-layer graphene with a sheet diameter less than 50 μm, graphene with 2 to 10 layers, and graphene with more than 10 layers.

5. The polyurethane adhesive according to claim 1, It is characterized in that The inorganic nanoparticles are selected from one or more of nano-silicon dioxide, nano-titanium dioxide, nano-zinc oxide and nano-aluminum oxide.

6. The polyurethane adhesive according to claim 1, It is characterized in that The carbon black is selected from one or more of ordinary carbon black, high-pigment carbon black with a mesh size greater than 1250, acetylene carbon black and high-wear-resistant furnace black.

7. The polyurethane adhesive according to claim 1, It is characterized in that The solvent B is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, toluene, ethyl acetate, methyl ethyl ketone, butyl acetate, dichloromethane, ethanol, methanol, acetone and xylene; The polar group-containing cellulose is selected from one or more of hydroxypropyl methylcellulose, methylcellulose, hydroxyethyl cellulose, hydroxymethyl cellulose and microcrystalline cellulose.

8. The polyurethane adhesive according to claim 1, It is characterized in that The coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, titanate coupling agent, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, isocyanatepropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, anilinemethyltrimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane.

9. The polyurethane adhesive according to claim 1, It is characterized in that The functional resin containing polar groups is selected from one or more of polyvinyl butyral resin, polyimide resin, acrylic resin, epoxy resin, unsaturated polyester resin, phenolic resin, polycarbonate resin, polyether sulfone resin, alkyd resin and uric acid resin; The metal powder is selected from one or more of black iron oxide, iron powder, aluminum powder, copper oxide, copper powder, nickel powder, cobalt powder and silver powder.

10. A method for preparing the polyurethane adhesive according to any one of claims 1 to 9, It is characterized in that The following steps are involved: After the polyol is vacuum dehydrated, it is mixed with solvent A at a temperature below 60°C, and then isocyanate, catalyst, chain extender, antioxidant and ultraviolet light absorber are added, mixed, heated, and reacted under an inert atmosphere to obtain a prepolymer; Mixing graphene and its derivatives, inorganic nanoparticles, carbon black and part of solvent B to obtain filler solution 1; Mixing polar group-containing cellulose, a coupling agent, a polar group-containing functional resin and the remaining portion of solvent B to obtain a filler solution 2; The filler solution 1, the filler solution 2 and the prepolymer are ground and mixed, reacted for 2 to 4.5 hours under grinding, and then metal powder is added and stirred for 18 to 23 minutes to obtain a polyurethane adhesive.

Citation Information

Cited By

  • Polymer primer and preparation method thereof

    CN119350939A

  • Laminating composite equipment and cross composite film production process

    CN119928200A

  • A film laminating composite device and a cross composite film production process

    CN119928200B

  • High and low temperature resistant polyurethane primer as well as preparation method and application thereof

    CN121851875A