Manufacturing method of sand mold for casting
A foundry sand mold composition with sodium silicate and metasilicate enhances mold filling and produces strong, thermally stable molds with reduced environmental impact.
Patent Information
- Application Number
- JP2020100085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-06-09
AI Technical Summary
Conventional foundry sand mold manufacturing compositions have low fluidity, making it difficult to fill molds effectively.
A composition comprising 100 parts by mass of foundry sand, 2 to 10 parts by mass of sodium silicate, and 3.5 to 10 parts by mass of sodium metasilicate, which provides high fluidity and can be easily filled into molds, and is hardened using hydration or heating.
The composition allows for easy mold filling and results in foundry sand molds with high strength and good thermal disintegration properties, reducing environmental impact.
Smart Images

Figure 0007577296000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to compositions for making sand molds for foundries and methods for making sand molds for foundries. [Background technology]
[0002] Compositions for manufacturing sand molds for foundries are disclosed in Patent Documents 1 to 3. The compositions for manufacturing sand molds for foundries are used to manufacture sand molds for foundries. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 53-43032 [Patent Document 2] Japanese Patent Application Publication No. 53-81430 [Patent Document 3] Japanese Unexamined Patent Publication No. 54-103734 Summary of the Invention [Problem to be solved by the invention]
[0004] When manufacturing a sand mold for casting, a composition for manufacturing a sand mold for casting is filled into the mold and cured. Conventional compositions for manufacturing a sand mold for casting have low fluidity. Therefore, it is difficult to fill the composition for manufacturing a sand mold for casting into the mold. In one aspect of the present disclosure, it is preferable to provide a composition for manufacturing a sand mold for casting that is easy to fill into the mold, and a method for manufacturing a sand mold for casting. [Means for solving the problem]
[0005] (1) One aspect of the present disclosure is a composition for manufacturing sand molds for foundry, comprising 100 parts by weight of foundry sand, 2 parts by weight or more and 10 parts by weight or less of sodium silicate, and 3.5 parts by weight or more and 10 parts by weight or less of sodium metasilicate.
[0006] The composition for producing a sand mold for foundry according to one aspect of the present disclosure has high fluidity, which makes it easy to fill a mold with the composition for producing a sand mold for foundry according to one aspect of the present disclosure. (2) Another aspect of the present disclosure is a method for producing a sand mold for foundry, which comprises filling a mold with a composition for producing a sand mold for foundry and hardening the composition for producing a sand mold for foundry, the composition for producing a sand mold for foundry containing 100 parts by mass of foundry sand, 2 to 10 parts by mass of sodium silicate, and 3.5 to 10 parts by mass of sodium metasilicate.
[0007] In the method for producing a sand mold for foundry according to another aspect of the present disclosure, the composition for producing a sand mold for foundry has high fluidity, so that the composition for producing a sand mold for foundry has high fluidity and can be easily filled into a mold. (3) Another aspect of the present disclosure is a method for producing a sand mold for foundry, which comprises filling a mold with a composition for producing a sand mold for foundry and hardening the composition for producing a sand mold for foundry. The composition for producing a sand mold for foundry contains 100 parts by mass of foundry sand and 2 to 10 parts by mass of sodium silicate. After filling the mold with the composition for producing a sand mold for foundry and before hardening, water is added to the composition for producing a sand mold for foundry.
[0008] In the method for producing a sand mold for foundry according to another aspect of the present disclosure, the composition for producing a sand mold for foundry has high fluidity at least at the time when the composition for producing a sand mold for foundry is filled into the mold, so that the composition for producing a sand mold for foundry can be easily filled into the mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Exemplary embodiments of the present disclosure will now be described with reference to the drawings. 1. First composition for manufacturing sand mold for casting The first composition for producing sand molds for foundry can be used to produce sand molds for foundry. The first composition for producing sand molds for foundry contains 100 parts by mass of foundry sand, 2 parts by mass to 10 parts by mass of sodium silicate, and 3.5 parts by mass to 10 parts by mass of sodium metasilicate.
[0010] Examples of the foundry sand include natural sand and artificial sand. Examples of the natural sand include flattery sand. The form of sodium silicate is, for example, powder. The sodium silicate functions as a binder. When the first composition for manufacturing a sand mold for foundry is filled into a mold and heated, the hydrated water of sodium metasilicate reacts with the sodium silicate, and the first composition for manufacturing a sand mold for foundry is thermally cured to become a sand mold for foundry.
[0011] The method for producing the first composition for producing sand molds for casting is, for example, a method for stirring raw materials including casting sand, sodium silicate, and sodium metasilicate. The stirring time is, for example, 1 minute. The produced first composition for producing sand molds for casting is preferably stored in a container such as a plastic bag in a sealed state.
[0012] The first composition for manufacturing sand molds for foundry does not contain an organic binder or has a low content of an organic binder, for example. When the first composition for manufacturing sand molds for foundry does not contain an organic binder or has a low content of an organic binder, adverse effects on the environment and workers can be suppressed.
[0013] The first composition for manufacturing sand molds for foundry has high fluidity. Due to the high fluidity, it is easy to fill the first composition for manufacturing sand molds for foundry into a mold. The first composition for manufacturing sand molds for foundry does not contain water, except for water of hydration, for example. When the first composition for manufacturing sand molds for foundry does not contain water, except for water of hydration, the first composition for manufacturing sand molds for foundry has even higher fluidity.
[0014] The sand mold for foundry produced using the first composition for producing sand molds for foundry has high strength and flexural strength and good thermal collapse properties. The first composition for producing sand molds for foundry can be stored for a long period of time. 2. Composition of the second composition for manufacturing sand molds for casting The second composition for producing a sand mold for foundry can be used for producing a sand mold for foundry. The second composition for producing a sand mold for foundry contains 100 parts by mass of foundry sand and 2 parts by mass or more and 10 parts by mass or less of sodium silicate.
[0015] Examples of the foundry sand include natural sand and artificial sand. Examples of the natural sand include flattery sand. The form of sodium silicate is, for example, powder. The sodium silicate functions as a binder. When the second composition for manufacturing a sand mold for foundry is filled into a mold, water is added, and the mixture is heated, the added water reacts with the sodium silicate, and the second composition for manufacturing a sand mold for foundry is thermally cured to form a sand mold for foundry.
[0016] The method for producing the second composition for producing sand molds for casting is, for example, a method of stirring raw materials including casting sand and sodium silicate. The stirring time is, for example, 1 minute. The produced second composition for producing sand molds for casting is preferably stored in a container such as a plastic bag in a sealed state.
[0017] The second composition for manufacturing sand molds for foundry does not contain an organic binder or has a low content of an organic binder, for example. When the second composition for manufacturing sand molds for foundry does not contain an organic binder or has a low content of an organic binder, the adverse effects on the environment and workers can be suppressed.
[0018] The second composition for manufacturing sand molds for foundry has high fluidity at least when it is filled into the mold. Due to its high fluidity, it is easy to fill the mold with the second composition for manufacturing sand molds for foundry. For example, the second composition for manufacturing sand molds for foundry does not contain water when it is filled into the mold. If the second composition for manufacturing sand molds for foundry does not contain water when it is filled into the mold, the second composition for manufacturing sand molds for foundry has even higher fluidity.
[0019] The sand mold for foundry produced using the second composition for producing sand molds for foundry has high strength and flexural strength and good thermal collapse properties. The second composition for producing sand molds for foundry can be stored for a long period of time. 3. First method for manufacturing sand molds for casting In the first method for producing a sand mold for casting, the first composition for producing a sand mold for casting is filled into a mold, and the first composition for producing a sand mold for casting is hardened. The hardened first composition for producing a sand mold for casting is a sand mold for casting. Finally, the sand mold for casting is removed from the mold.
[0020] As a method for filling the first composition for manufacturing sand molds for casting into a mold, for example, there is a method in which the first composition for manufacturing sand molds for casting is filled into the mold while lightly vibrating the mold by hitting it with a mallet or the like. Furthermore, as a method for filling the first composition for manufacturing sand molds for casting into a mold, there is, for example, a blowing method. The blowing method is, for example, the following method. The first composition for manufacturing sand molds for casting is charged into a blowing device and sealed. Next, air pressure is applied by a compressor, and the first composition for manufacturing sand molds for casting is blown into the mold under a blowing pressure of 1.0 MPa. Next, the mold is vibrated by a vibration table. Since the first composition for manufacturing sand molds for casting has high fluidity, it is easy to fill the mold with the first composition for manufacturing sand molds for casting.
[0021] As a method for hardening the first composition for manufacturing sand molds for casting, for example, there is a method of heating the first composition for manufacturing sand molds for casting. As a method for heating the first composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a dryer. As a method for heating the first composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a microwave oven. As a method for heating the first composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a dryer, and then heating to 80°C or higher using a microwave oven.
[0022] The sand mold for foundry produced by the first method for producing a sand mold for foundry has high strength and flexural strength, and has good thermal collapsibility. 4. Manufacturing method of second sand mold for casting In the method for producing the second sand mold for foundry, after the second composition for producing a sand mold for foundry is filled into a mold, water is added to the second composition for producing a sand mold for foundry before hardening. After the water is added, the second composition for producing a sand mold for foundry is hardened. The hardened second composition for producing a sand mold for foundry is the sand mold for foundry. Finally, the sand mold for foundry is removed from the mold.
[0023] The method for filling the second composition for manufacturing a sand mold for casting into a mold is, for example, the same as the method for filling the first composition for manufacturing a sand mold for casting into a mold in the first method for manufacturing a sand mold for casting. Since the second composition for manufacturing a sand mold for casting has high fluidity at least at the time of filling the mold, it is easy to fill the second composition for manufacturing a sand mold for casting into a mold.
[0024] As a method for hardening the second composition for manufacturing sand molds for casting, for example, there is a method of heating the second composition for manufacturing sand molds for casting. As a method for heating the second composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a dryer. As a method for heating the second composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a microwave oven. As a method for heating the second composition for manufacturing sand molds for casting, for example, there is a method of heating to 80°C or higher using a dryer, and then heating to 80°C or higher using a microwave oven.
[0025] The sand mold for foundry produced by the second method for producing a sand mold for foundry has high strength and flexural strength and good thermal collapsibility. 5. Working Example (5-1) Manufacture of composition for manufacturing sand molds for casting Compositions S1 to S16 for manufacturing sand molds for foundry containing the components shown in Table 1 were produced.
[0026] [Table 1]
[0027] The manufacturing method for S1 to S16 was to mix the respective ingredients and stir for 1 minute. "Lunamos" and "Espearl" in Table 1 were artificial sands. "Sodium silicate" in Table 1 was No. 3 powdered sodium silicate. "Sodium metasilicate" in Table 1 was a nonahydrate salt. "Sodium metasilicate" in Table 1 had been ground in advance to reduce particle size.
[0028] S10 to S16 correspond to the first composition for manufacturing sand molds for foundry, and S3 to S6 correspond to the second composition for manufacturing sand molds for foundry. (5-2) Manufacturing of sand molds for casting using S1-S2, S7-S16 For each of S1 to S2 and S7 to S16, a sand mold for casting was manufactured using the composition for manufacturing a sand mold for casting. The manufacturing method was as follows. First, the composition for manufacturing a sand mold for casting was filled into the mold while lightly vibrating the mold by hitting it with a mallet or the like. Next, the composition for manufacturing a sand mold for casting was heated and cured. The cured composition for manufacturing a sand mold for casting is the sand mold for casting. When S10 to S16 are used, this manufacturing method corresponds to the first manufacturing method of a sand mold for casting.
[0029] The heating method was as shown in Table 1. When S1 to S2 and S7 were used, heating was performed for 1.5 minutes using a microwave oven. The rated high frequency output of the microwave oven was 500W. When S8 to S9 and S13 were used, heating was performed using a dryer at the "heating temperature" and for the "heating time" shown in Table 1. When S10 to S12 and S14 to S16 were used, heating was first performed using a dryer at the "heating temperature" and for the "heating time" shown in Table 1, and then heating was performed for 3 minutes using a microwave oven. The rated high frequency output of the microwave oven was 500W.
[0030] (5-3) Manufacturing of sand molds for casting using S3 to S6 For each of S3 to S6, a sand mold for casting was manufactured using the composition for manufacturing a sand mold for casting. The manufacturing method was as follows. First, the composition for manufacturing a sand mold for casting was filled into the mold while lightly vibrating the mold by hitting it with a mallet or the like. Next, water was added to the filled composition for manufacturing a sand mold for casting in the amount of mass shown in the column "amount of water added after filling" in Table 1. When the water was added, the composition for manufacturing a sand mold for casting had not yet hardened. Next, the composition for manufacturing a sand mold for casting was heated and hardened. The hardened composition for manufacturing a sand mold for casting is a sand mold for casting. The heating method was a method of heating for 1.5 minutes using a microwave oven as shown in Table 1. The rated high-frequency output of the microwave oven was 500W. This manufacturing method corresponds to the second method for manufacturing a sand mold for casting.
[0031] (5-4) Composition for manufacturing sand molds for casting and method for evaluating sand molds for casting For each of S1 to S16, the initial strength, strength after heating, thermal collapse rate, and spread diameter were measured. The measurement methods were as follows.
[0032] (i) Initial strength Cylindrical JIS test specimens with a diameter of 50 mm and a height of 50 mm were prepared from the sand casting mold. The unconfined compressive strength of the test specimens was measured using a compression tester ABM-100SIV manufactured by Tokyo Test Instruments Co., Ltd. The measured unconfined compressive strength was regarded as the initial strength.
[0033] (ii) Strength after heating A test specimen similar to that used for measuring the early strength was prepared. The test specimen was placed in an electric furnace heated to 700°C and heated for 10 minutes. The unconfined compressive strength of the test specimen removed from the electric furnace was measured in the same manner as for measuring the early strength. The measured unconfined compressive strength was taken as the strength after heating.
[0034] (iii) Thermal decay rate When the initial strength is Y1 and the strength after heating is Y2, the thermal collapse rate R was calculated by the following formula (1). The unit of the thermal collapse rate R is %, and the thermal collapse rate is an index showing the thermal collapse property. The larger the thermal collapse rate, the better the thermal collapse property.
[0035] Formula (1) R = ((Y1-Y2) / Y1)) x 100 (iv) Spread diameter A slump cone test was carried out for each of S1 to S16. The inner diameter of the upper end of the slump cone used was 50 mm, the inner diameter of the lower end was 70 mm, and the height was 80 mm. This slump cone was placed on a horizontal table. Next, the unhardened composition for manufacturing a sand mold for casting was filled into the slump cone. Next, the slump cone was moved upward and pulled out from the composition for manufacturing a sand mold for casting. After the slump cone was pulled out, the diameter in the horizontal direction of the composition for manufacturing a sand mold for casting that had spread on the table was measured. The measured diameter was taken as the spread diameter. In the case of S3 to S6, the spread diameter was measured in a state where water was not added to the composition for manufacturing a sand mold for casting.
[0036] The spread diameter is an index reflecting the fluidity of a composition for manufacturing sand molds for foundries. The higher the fluidity of a composition for manufacturing sand molds for foundries, the larger the spread diameter. (5-5) Evaluation results of compositions for manufacturing sand molds for casting and sand molds for casting The evaluation results are shown in Table 1. The spread diameter was large in S3 to S6 and S10 to S16. Therefore, the compositions for manufacturing sand molds for foundry S3 to S6 and S10 to S16 have high fluidity and are easy to fill into a mold.
[0037] The initial strength was high in S3 to S6 and S10 to S16. Therefore, the sand molds for casting manufactured using the compositions for manufacturing sand molds for casting of S3 to S6 and S10 to S16 had high strength. The thermal collapse rate was high in S3 to S6 and S10 to S16. Therefore, the sand molds for casting manufactured using the compositions for manufacturing sand molds for casting of S3 to S6 and S10 to S16 had good thermal collapse properties.
[0038] 6. Other embodiments Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments and can be implemented in various modified forms.
[0039] (6-1) The composition for manufacturing a sand mold for foundry may further contain other components in addition to the foundry sand, sodium silicate, and sodium metasilicate. (6-2) The function of one component in each of the above embodiments may be shared by multiple components, or the functions of multiple components may be performed by one component. Also, part of the configuration of each of the above embodiments may be omitted. Also, at least part of the configuration of each of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.
[0040] (6-3) In addition to the above-mentioned composition for manufacturing sand molds for foundry, the present disclosure can also be realized in various forms, such as a system including the composition for manufacturing sand molds for foundry as a component, a method for manufacturing a composition for manufacturing sand molds for foundry, and a method for manufacturing sand molds for foundry.
Claims
[Claim 1] A method for producing a sand mold for foundry, comprising filling a mold with a composition for producing a sand mold for foundry and hardening the composition for producing a sand mold for foundry, The composition for manufacturing a sand mold for casting is produced by mixing and stirring components including 100 parts by mass of casting sand, 2 parts by mass or more and 10 parts by mass or less of sodium silicate, and 3.5 parts by mass or more and 10 parts by mass or less of sodium metasilicate. A method for manufacturing sand molds for casting.
Citation Information
Patent Citations
JP1973053929A
JP1975026498A
Additives to low circumferential contamination overrlay sand for shellmoulding its manufacturing method and usage
JP1978043032A
Mold molding method
JP1978072726A
Mold molding method
JP1978081430A