Method for forming dense metal layer
The cold spray technique with copper particles at specific angles forms a dense, stable metal layer on power plant components, addressing film formability issues and corrosion resistance.
Patent Information
- Application Number
- JP2020182512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Existing methods for forming metal layers in environments exposed to water or steam, such as power generation plants, face challenges with film formability, erosion, and require specialized devices or nozzles, limiting their applicability and stability.
A method using a cold spray technique with copper or copper alloy particles, applied at a relative angle of 30 to 80 degrees, forms a dense metal layer on base materials without a complex structure, utilizing a standard cold spray device and gas heating to ensure adhesion and density.
The method stabilizes metal layer formation, preventing corrosion and ensuring a dense, uniform layer that withstands water or steam exposure, enhancing the reliability of power generation components.
Smart Images

Figure 0007577511000001 
Figure 0007577511000002 
Figure 0007577511000003
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention is a method for forming a dense metal layer. method Regarding. [Background technology]
[0002] Many of the pipes and equipment used for supplying steam from a boiler or the like to a steam turbine, for supplying water from a condenser to a boiler or the like, and for draining water from these systems are used in environments where they come into contact with liquids such as water or gases such as water vapor. In addition, in direct water-cooled turbine generators used in large-capacity generators, the system is cooled with water, and some of the components are in contact with cooling media such as water. Many of the components of these systems are made of metal, and there is a risk of various types of corrosion occurring when they are used in environments where they come into contact with water or steam.
[0003] Water or steam leakage caused by corrosion of system components directly leads to the shutdown of the plant, and many processes are required before recovery, such as investigating the cause, implementing countermeasures, and verifying the effectiveness of those countermeasures. Therefore, even the occurrence of corrosion in a single component or system can be a major obstacle to the stable operation of the plant. For this reason, countermeasure technologies against the deterioration of components that come into contact with water or steam environments are important for improving the reliability of not only each system component but also the entire plant system.
[0004] For example, the coil conductor, which is the conductive part of the stator coil of a direct water-cooled turbine generator, is composed of a solid wire (copper wire) and a hollow wire (hollow copper wire) with holes through which cooling water flows. Clips that are connected to cooling piping and supply cooling water are brazed to both ends of the coil conductor. The clip integrates multiple wires, and the brazing that connects the clip to the wire bundle in which the multiple wires are integrated provides an electrical connection function as well as a seal for cooling water at the end faces of the wire bundle. In the past, problems such as corrosion of this end face causing water leakage have been experienced, and various countermeasures have been taken.
[0005] Furthermore, components that have composite parts of dissimilar materials, such as joints between dissimilar materials, and are used in environments where they come into contact with liquids have degradation factors specific to joints between dissimilar materials.
[0006] For example, in the clip portion of the stator coil mentioned above, if the clip material is a metal other than copper-based, conventional measures for the joint between these different materials have been to use materials that do not contain elements that lower the pH value of the environment in order to reduce corrosion-accelerating factors, or to avoid the risk of different materials coming into contact with the same liquid by separating the parts.
[0007] As another countermeasure, development is also underway to cover the target area with thermal spraying and treat the surface with highly corrosion-resistant materials to suppress deterioration. Thermal spraying techniques include normal high-temperature thermal spraying, as well as low-temperature thermal spraying, which is carried out at relatively low temperatures of around 300°C to 700°C.
[0008] In order to stably operate large power generation equipment such as power plants, improve the reliability of the equipment, and achieve a smooth energy supply, it is necessary to have a means of avoiding the risk of damage caused by corrosion of metal parts.
[0009] In the thermal spraying method, which is a corrosion countermeasure for metal parts, the heat input to the substrate is large, and there are concerns about the thermal impact on the substrate and residual stress on the substrate to be treated, so the substrate to be used is limited. In contrast, there is a method in which a metal layer is formed on a substrate using the cold spray method, which is one of the low-temperature thermal spraying methods, as a method that is relatively low in temperature and is said to have little impact on the substrate to be treated.
[0010] The cold spray method is different from the conventional thermal spraying method in which powder particles to be collided with a substrate are sprayed in a molten state. Instead, a gas having a temperature lower than the melting point or softening temperature of the powder particles to be collided with the substrate is accelerated to a supersonic speed, the powder particles are transported by the gas, and the powder particles are collided with the substrate in a solid phase state to form a coating. Here, metals, alloys, intermetallic compounds, ceramics, etc. are selected as the material of the powder particles. The softening temperature of the powder particles is the temperature at which the strength or hardness of the powder particles is half the strength or hardness at room temperature. The cold spray method is applied to, for example, metals that are difficult to produce by melting or dissolving, or metals with a composition that is difficult to mold after production, and is also considered for application when forming a film on a substrate of a material with a higher melting point than the substrate. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Patent No. 4310251 [Patent Document 2] Patent No. 5171125 Summary of the Invention [Problem to be solved by the invention]
[0012] Various studies have been conducted on the cold spray method in recent years. For example, a technology is known that enables large-area coating by setting the dimensions of the diameter-reduced part of the nozzle inlet and the distance between the powder inlet and the throat within a predetermined range, mixing different types of metal powder particles as necessary, and plastically deforming the substrate and particles by collision energy without excessively heating the powder particles. This method accelerates the application gas using a supersonic nozzle to achieve coating with less oxide layer in order to avoid the decrease in conductivity of the formed layer due to the formation of an oxide layer, which is a common problem in thermal spraying.
[0013] In addition, in order to ensure the efficiency of low-temperature thermal spraying, a technology has been proposed in which the powder particles are heated more effectively by using a nozzle for cold spraying, the compression section of which is characterized by having a preheating area on the nozzle inlet side and a compression area.
[0014] On the other hand, there are many material systems for which it is difficult to form a film even with low-temperature spraying, and when applying the coating layer, depending on the application conditions, erosion may occur due to the sprayed particles, making it impossible to form a film. There are also many material systems for which denseness cannot be ensured.
[0015] Furthermore, for parts made of materials with low melting points, low softening points, or materials that may cause brazing, methods of plating with reduced heat input have been considered, but there are significant limitations on the shape of the base material, the plating location, and the like.
[0016] When low-temperature thermal spraying is selected as a countermeasure technology for components used in liquid-contact environments such as power plants, the prior art described above has the following two problems. First, they require specially configured devices or attachments. Secondly, it requires the use of a nozzle having a special compression section shape compared to a typical straight nozzle.
[0017] Therefore, an object of an embodiment of the present invention is to enable stable formation of a dense metal layer without using a complicated configuration. [Means for solving the problem]
[0018] The method for forming a dense metal layer according to the embodiment includes the steps of: Used in environments where it comes into contact with water or steam Made of copper (Cu) Substrate In contact with water or steam On the substrate surface The material is the same as the base material. Copper or copper alloy, zinc (Zn), tin (Sn), silver (Ag), aluminum (Al ), gold (Au), or two or more of these Metal powder particles are collided to produce metal A method for forming a dense metal layer, comprising: a metal powder particle supplying section; A cold spray apparatus having a distillation vessel, a gas heating section, and an injection section is provided. and spraying the application gas and the metal powder particles onto the substrate surface by the cold spray device. The direction of the jet including the above is determined by the angle between the center line of the jet and a straight line on the surface of the substrate. The line formed by the projection of the spray direction onto the surface of the substrate and the spray direction is The relative angle Θ of the jet flow, which is the smaller angle of the two angles, is 30 degrees or more and 80 degrees or less. An angle setting step of setting the angle to be within a predetermined angle range below; A spraying step of spraying the jet onto the substrate surface from a position. And, from the injection part The temperature of the gas injected from the gas supply is set so that the strength or hardness of the metal powder particles is equal to the strength or hardness at room temperature. or the softening temperature of the metal powder particles, which is the temperature at which the hardness is half the value. It is characterized by do. [Brief description of the drawings]
[0019] [Figure 1] 1 is a conceptual block diagram showing an example of a cold spray device used in a method for forming a dense metal layer according to an embodiment. [Diagram 2] 5 is a conceptual diagram illustrating a relative angle in the method for forming a dense metal layer according to the embodiment. FIG. [Diagram 3] 1A to 1D are conceptual diagrams showing examples of the nozzle of the injection part of a cold spray device used in a method for forming a dense metal layer according to an embodiment, the examples being other than circular, where (a) is an ellipse, (b) is a rectangle with smooth corners, (c) is a triangle, and (d) is a polygon. [Figure 4] 1 is a first conceptual diagram illustrating a state in which a relative angle between the flow direction of a jet and the surface of a substrate is a first angle, for illustrating a method of forming a dense metal layer according to an embodiment. FIG. [Diagram 5] 10 is a second conceptual diagram illustrating a state in which the relative angle between the flow direction of the jet and the surface of the substrate is a second angle, for illustrating the method of forming a dense metal layer according to the embodiment. FIG. [Figure 6] 4 is a graph showing an example of the dependency of the denseness of a substrate surface on the relative angle, for illustrating a method of forming a dense metal layer according to an embodiment. [Figure 7] 4 is a conceptual diagram for explaining the efficiency of forming a dense metal layer on a substrate surface depending on the relative angle between the substrate surface and the flow direction of a jet in a method of forming a dense metal layer according to an embodiment. FIG. [Figure 8] 11 is a graph showing an example of the dependency of the formation efficiency of a layer formed on a substrate surface on the relative angle between the substrate surface and the flow direction of a jet in a method of forming a dense metal layer according to an embodiment. [Figure 9] 11 is a graph showing an example of the dependency of a formation index of a dense metal layer on a substrate surface on a relative angle between the substrate surface and the flow direction of a jet in a method of forming a dense metal layer according to an embodiment. [Figure 10] 1 is a flow diagram showing the steps of a method for forming a dense metal layer according to an embodiment. [Figure 11] 1 is a photograph showing the appearance of the surface of a first sample in an example. [Figure 12] 1 is a photograph showing the appearance of the surface of a second sample in an example. [Figure 13] 13 is a photograph showing the appearance of the surface of a third sample in the example. [Figure 14] 1 is an evaluation table showing evaluation results based on test results in examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, with reference to the drawings, a method for forming a dense metal layer according to an embodiment of the present invention will be described. method Explain Here, the same or similar parts are denoted by the same reference numerals, and overlapping explanations are omitted. Omitted.
[0021] FIG. 1 is a conceptual block diagram showing an example of a cold spray apparatus 30 used in a method for forming a dense metal layer according to an embodiment.
[0022] The cold spray device 30 is a device for forming a formation layer 20 on a substrate surface 1a of a substrate 1 to be treated, and has a metal powder particle supply unit 31, a gas supply unit 32, a gas heating unit 33, and an injection unit .
[0023] The metal powder particle supply unit 31 has a metal powder particle storage tank 31a for storing the metal powder particles 10 and a transfer pipe 31b for transferring the metal powder particles 10 from the metal powder particle storage tank 31a to the injection unit .
[0024] Here, the metal powder particles 10 are preferably metals that have low hardness in a solid state and are relatively easy to melt. Specifically, the metal powder particles 10 contain one or more of copper (Cu), zinc (Zn), tin (Sn), silver (Ag), aluminum (Al), and gold (Au). Alternatively, in the case of a copper alloy, the metal powder particles 10 contain at least one of gold (Au), silver (Ag), zinc (Zn), tin (Sn), and phosphorus (P).
[0025] The average particle size of the metal powder particles 10 is preferably in the range of 1 μm to 20 μm. Here, the average particle size refers to the particle size of D50 measured using a particle size distribution measuring device: MT3300 (LOW-WET MT3000II Mode). If the particle size of the metal powder particles 10 is smaller than 1 μm, the formation efficiency of the forming layer 20 decreases. Also, if the particle size is larger than 20 μm, the denseness of the forming layer 20 decreases.
[0026] The gas supply unit 32 supplies a gas such as helium or air to the injection unit 34. The gas heating unit 33 heats the gas supplied from the gas supply unit 32 before it flows into the injection unit 34. The gas heating unit 33 is, for example, an electric heater or a heating device that uses high-temperature gas.
[0027] The heating temperature is lower than the melting point of the metal powder particles 10 and is effective for the cold spray method, and is appropriately selected depending on the type of metal of the metal powder particles 10. For example, copper has an embrittlement temperature range due to heat input, so it is important to select the temperature conditions for both the substrate 1 to be processed and the metal powder particles 10 to be used. In addition, zinc and tin have low melting points, so low-temperature spraying is preferable to high-temperature spraying.
[0028] Thus, the heating temperature varies depending on the type of metal powder particles 10 and also on the particle size of the metal powder particles 10, but for example, the softening temperature of the metal powder particles 10, which is the temperature at which the strength or hardness of the metal powder particles 10 is half that at room temperature, may be used, and is a heating temperature at which the temperature of the jet 14 sprayed from the spraying part 34 is 250°C to 750°C. If the temperature is too low, it will not melt even when it collides with the substrate surface 1a and will not contribute to the formation of the formation layer 20. Also, if the temperature is too high, the advantages of the cold spray method cannot be secured.
[0029] The ejection unit 34 accelerates the metal powder particles 10 supplied from the metal powder particle supply unit 31 by the gas supplied from the gas supply unit 32 and ejects them.
[0030] The flow velocity of the accelerated jet 14, that is, the flow velocity of the working gas 15 and the metal powder particles 10 sprayed together with the working gas 15, is, for example, about 500 m / sec.
[0031] The metal powder particles 10 in the jet 14 injected under the above-mentioned conditions collide with the substrate surface 1a of the substrate 1, and a layer 20 is formed in sequence.
[0032] The cold spray device 30 is not limited to the one shown in FIG. 1, and may be a device of another configuration as long as it can spray the processing gas 15 and the jet 14 containing the metal powder particles 10 sprayed together with the processing gas 15 onto the target substrate surface 1a.
[0033] 2 is a conceptual diagram for explaining the relative angle in the method for forming a dense metal layer according to the embodiment, conceptually showing the spread of the jet 14 sprayed from the circular nozzle 35 formed at the tip of the spray unit 34 of the cold spray device 30.
[0034] 1 and 2, the relative angle Θ between the flow direction of the jet 14 and the substrate surface 1a is defined as follows.
[0035] First, the center line 14a of the jet 14 is defined. In FIG. 2, a circular imaginary plane surrounded by the periphery of the jet nozzle 35 is defined as plane S1. Also, consider plane S2, which is a cross section of the jet on the way from the jet nozzle 35 to the substrate surface 1a, cut by an imaginary plane parallel to plane S1. Plane S2 is a cross section of the jet 14 that passes through the circular plane S1 and spreads uniformly, and can be considered to be circular like plane S1. The point at the center of plane S1 is defined as center point P1, and the point at the center of plane S2 is defined as center point P2. Center line 14a is defined as a straight line that starts from center point P1 and passes through center point P2.
[0036] Next, the relative angle Θ is defined. As shown in FIG. 1, the jet 14 collides with the substrate surface 1a of the target substrate 1, and the angle that the center line 14a of the jetted jet 14 makes with the substrate surface 1a is called the relative angle Θ. Here, the relative angle Θ refers to the minimum angle between the center line 14a and a straight line on the substrate surface 1a passing through the intersection point 1p of the center line 14a with the substrate surface 1a. In other words, except when the center line 14a is perpendicular to the substrate surface 1a, it is the smaller of the two angles made by the center line 14a and a straight line that is a projection of the center line 14a onto the substrate surface 1a. The relative angle Θ obtained in this way is also an angle at which the sum of the incidence angle of the center line 14a to the substrate surface 1a is 90 degrees.
[0037] 3 is a conceptual diagram showing examples of the nozzle of the nozzle part of the cold spray device used in the method for forming a dense metal layer according to the embodiment, in which (a) is an ellipse, (b) is a rectangle with smooth corners, (c) is a triangle, and (d) is a polygon. By appropriately using the nozzle of a shape other than the circle according to the shape of the substrate surface 1a of the target substrate 1, it is possible to efficiently form a dense metal layer. The center points in each case, i.e., the center point P1a of the nozzle 35a, the center point P1b of the nozzle 35b, the center point P1c of the nozzle 35c, and the center point P1d of the nozzle 35d, may be, for example, the center of gravity of each.
[0038] Next, in the method for forming a dense metal layer according to this embodiment, when a jet 14 is sprayed onto the substrate surface 1a of the target substrate 1 using the cold spray device 30, the basis for selecting the relative angle Θ between the center line 14a and the substrate surface 1a will be described.
[0039] 4 is a first conceptual diagram for explaining the method for forming a dense metal layer according to the embodiment, showing a state in which the relative angle Θ between the flow direction of the jet flow 14 and the substrate surface 1a is a first angle Θ1, where the first angle Θ1 is 90 degrees.
[0040] The jet 14 collides with the substrate surface 1a of the substrate 1, which is the target of processing. As a result, a rebound gas 16, which is a flow in the opposite direction to the flow of the processing gas 15, is generated.
[0041] In the case shown in Figure 4, the jet 14 collides with the substrate surface 1a at an angle of 90 degrees, so that the main direction of the rebound gas 16 is opposite to the jet 14, as shown by the thick arrow, i.e., in a counterflow direction to the construction gas 15.
[0042] The presence of the countercurrent flow reduces the flow rate of the working gas 15. In addition, the presence of the countercurrent flow causes a part of the rebound gas 16 itself to be entrained in the forming layer 20 and to be incorporated in the forming layer 20 in the form of bubbles, voids, holes, etc.
[0043] Furthermore, once the processing gas 15 collides with the substrate surface 1a or the forming layer 20, it becomes the rebound gas 16, and the temperature of the rebound gas 16 is reduced by providing heat to the substrate 1. Therefore, the rebound gas 16 reduces the temperature of the processing gas 15 and the metal powder particles 10 of the proceeding jet 14.
[0044] In addition, in the vicinity of the substrate surface 1a, an unnecessary flow occurs due to collision between the processing gas 15 and the rebound gas 16, which creates a risk of causing excessive heat input to the substrate 1.
[0045] As described above, when the relative angle Θ between the flow direction of the jet flow 14 and the substrate surface 1a is 90 degrees, the formation of the dense metal layer by the forming layer 20 is significantly hindered.
[0046] 5 is a second conceptual diagram for explaining the method for forming a dense metal layer according to the embodiment, showing a state in which the relative angle Θ between the flow direction of the jet flow 14 and the substrate surface 1a is a second angle Θ2, where the second angle Θ2 is an angle smaller than 90 degrees.
[0047] In this case, the main direction of the rebound gas 16 is in the direction of the reflection angle Φ3, which is approximately equal to the incidence angle Φ2 of the jet. Therefore, the extent to which the rebound gas 16 flows counter to the jet 14 is reduced compared to the first angle shown in Figure 4, reducing problems with the forming layer 20 and improving the formation of a dense metal layer by the forming layer 20.
[0048] 6 is a graph showing an example of the dependency of the denseness of the substrate surface on the relative angle to explain the method of forming a dense metal layer according to the embodiment. The horizontal axis is the relative angle Θ, and the vertical axis is the denseness of the formed layer 20 as a function F1(Θ) of the relative angle Θ.
[0049] Here, the denseness of the formation layer 20 refers to the degree to which the formation layer 20 becomes a dense metal layer. In other words, a formation layer 20 in which the metal powder particles 10 are completely welded to the substrate surface 1a to form a dense metal layer and which does not contain bubbles, voids, holes, etc. is considered to have high density.
[0050] The denseness of the formation layer 20 may be confirmed, in detail, for example, by microscopic observation using an optical microscope, an electron microscope, or the like, or by measuring the density of the formation layer 20. Alternatively, it may be confirmed visually.
[0051] Here, in the case of visual inspection, for example, there is a method of checking the surface condition after placing it in a corrosive environment such as exposing it to water or steam for a predetermined period of time, and evaluating the denseness based on the presence or absence of discoloration, oxidation, and unevenness on the surface of the formation layer 20. The judgment is made based on the level of, for example, "good" if no discoloration, oxidation, or unevenness is observed on the surface of the formation layer 20, "△ (not sufficient)" if there is any sign of discoloration, oxidation, or unevenness, and "× (not acceptable)" if there is obvious discoloration, oxidation, or unevenness.
[0052] As described above, the density of the forming layer 20 is low in the angular region where the relative angle Θ is close to 0 degrees and in the angular region where the relative angle Θ is close to 90 degrees, but sufficient density is obtained in the region less than 90 degrees, for example, in the region of 80 degrees or less.
[0053] On the other hand, the component of the flow velocity V0 of the jet 14 and the metal powder particles 10 in the jet 14 in the direction perpendicular to the substrate surface 1a is (sinΘ) of the flow velocity V0, and in the region where the relative angle Θ is small, the adhesion force of the metal powder particles 10 to the substrate surface 1a decreases, and the density of the formation layer 20 decreases as shown in Figure 6.
[0054] Therefore, the function F1(Θ) of the relative angle Θ, which represents the denseness of the formation layer 20, exhibits a characteristic of decreasing in the region where Θ is small and in the region close to 90 degrees.
[0055] FIG. 7 is a conceptual diagram for illustrating the efficiency of forming a dense metal layer on the substrate surface 1a depending on the relative angle Θ between the substrate surface 1a and the flow direction of the jet flow 14 in the method of forming a dense metal layer according to the embodiment.
[0056] The rate at which the layer 20 is formed by the metal powder particles 10 in the jet 14 is proportional to the amount of metal powder particles 10 sprayed per unit area of the substrate surface 1a of the substrate 1. In addition, in a region where the relative angle Θ is small, the velocity component in the direction perpendicular to the substrate surface 1a becomes extremely small, so that the adhesive force to the substrate surface 1a decreases and the formation rate becomes even slower than the rate proportional to the amount of metal powder particles 10.
[0057] Now, consider jet 14 being sprayed onto a portion of substrate surface 1a having a size of S0, as shown in Figure 7. When the relative angle is 90 degrees, jet 14 having an area of S0 is sprayed, whereas when the relative angle is Θ, as shown in Figure 7, a jet having an area S is sprayed onto the portion of substrate surface 1a having a size of S0. Here, S is S0·cos(90-Θ), that is, S0·sinΘ. When the formation rate of layer 20 is proportional to the amount of metal powder particles sprayed per unit area of substrate surface 1a of substrate 1, the formation rate of layer 20 is proportional to sinΘ.
[0058] 8 is a graph showing an example of the dependency of the formation efficiency of the layer 20 on the substrate surface 1a in the method for forming a dense metal layer according to the embodiment on the relative angle Θ between the substrate surface 1a and the flow direction of the jet 14. The horizontal axis represents the relative angle Θ, and the vertical axis represents the formation efficiency of the layer 20 as a function F2(Θ) of the relative angle Θ.
[0059] Since the formation efficiency is proportional to the formation speed of the formation layer 20, the formation efficiency of the formation layer 20 on the substrate surface 1a, which is a function F2(Θ) of the relative angle Θ, is proportional to the sine value of the relative angle Θ, i.e., sinΘ, as shown in Fig. 7. Therefore, the function F2(Θ) of the relative angle Θ, which represents the formation efficiency of the formation layer 20, becomes smaller as Θ becomes smaller.
[0060] For example, in order to secure 50% of the maximum efficiency as the forming efficiency, a relative angle Θ of 30 degrees or more is often required. However, for the forming layer 20 targeted in this embodiment, there are many cases where denseness is required more than the forming efficiency, so the forming efficiency may be used as a target for achievement. Alternatively, since a decrease in the forming efficiency tends to increase the proportion of formed powder generated during construction, a priority order may be set according to requirements.
[0061] Next, based on the density of the formation layer 20 shown in Figure 6 and the formation efficiency of the formation layer 20 shown in Figure 8, a comprehensive metal dense layer formation index is considered that takes into account the qualitative and quantitative aspects of the formation of a metal dense layer by the formation layer 20.
[0062] 9 is a graph showing an example of the dependency of the formation index of a dense metal layer on a substrate surface 1a in the method of forming a dense metal layer according to the embodiment on the relative angle Θ between the substrate surface 1a and the flow direction of the jet flow 14. The horizontal axis represents the relative angle Θ, and the vertical axis represents the formation index of a dense metal layer as a function G(Θ) of the relative angle Θ.
[0063] Here, the function G(Θ) indicating the formation index of the dense metal layer is given by the following formula (1). G(Θ)=F1(Θ)·F2(Θ) ···(1) The function G(Θ) is not limited to the formula (1). For example, the values of the functions F1(Θ) and F2(Θ) may be raised to a weighted power and then the product of the two may be calculated. Alternatively, the values of the functions F1(Θ) and F2(Θ) may be weighted and then the sum of the two may be calculated.
[0064] As shown in FIG. 9, the function G(Θ) indicating the formation index of the dense metal layer has small values when the relative angle Θ is near 0 degrees and near 90 degrees, and has large values in the intermediate range.
[0065] For example, the minimum level of G(Θ) taking into account both qualitative and quantitative aspects is g th In this case, as shown in FIG. 9, the relative angle Θ must be equal to or larger than Θ1 and equal to or smaller than Θ2.
[0066] Based on the above-described background, the procedure of the method for forming a dense metal layer according to this embodiment will be described.
[0067] FIG. 10 is a flow diagram showing the steps of a method for forming a dense metal layer according to an embodiment.
[0068] First, the cold spray device 30 is prepared (step S01). That is, for example, the cold spray device 30 shown in FIG.
[0069] Next, the relative angle Θ with respect to the target substrate surface 1a is set to be within a predetermined angle range (step S02). That is, based on the above-mentioned content, the relative relationship between the cold spray device 30 and the substrate surface 1a of the substrate 1 is adjusted so that the relative angle Θ of the spraying direction of the jet 14 with respect to the target substrate surface 1a is an angle of Θ1 or more and Θ2 or less.
[0070] Next, a jet 14 is sprayed from the cold spray device 30 onto the substrate surface 1a (step S03).
[0071] Next, it is checked whether there is any abnormality in the formation layer 20 formed on the substrate surface 1a (Step S04). The check can basically be performed visually.
[0072] If it is not confirmed that there is no abnormality in the formation layer 20 formed on the substrate surface 1a (NO in step S04), a cause investigation is performed (step S06).
[0073] If it is confirmed that there is no abnormality in the formation layer 20 formed on the substrate surface 1a (step S04: YES), it is determined whether the formation of the formation layer 20 has been completed to the required extent (step S05). If it is determined that the formation of the formation layer 20 has not been completed to the required extent (step S05: NO), the process returns to step S03. If it is determined that the formation of the formation layer 20 has been completed to the required extent (step S05: YES), the formation of the formation layer 20 is terminated.
[0074] As described above, in the method for forming a dense metal layer according to this embodiment, it is possible to form a stable dense metal layer using a conventional cold spray device 30, without using complex configurations such as special nozzles or devices with special configurations.
[0075] Power plant components having a dense metal layer formed as described above in a portion that comes into contact with liquids such as water or gases such as water vapor can avoid the risk of damage caused by corrosion and contribute to the stable operation of the power plant. (Evaluation of methods for forming dense metal layers)
[0076] Next, it will be described how the method for forming a dense metal layer according to this embodiment enables stable formation of a dense metal layer.
[0077] The formation of a dense metal layer was confirmed using a test piece. The material of the test piece was selected based on the assumption that it would be a clip that is connected to both ends of the coil conductor of a stator coil in a direct water-cooled turbine generator and supplies cooling water from a cooling pipe.
[0078] The substrate of the test specimen is oxygen-free copper, just like the clip.
[0079] The metal powder particles to be sprayed are of the same material as the base material, such as copper, copper alloy, zinc, tin, or aluminum, and have an average particle size (D50) of, for example, φ2.5 μm, 5 μm, 20 μm, or 20 μm. The particle size is listed as the particle size measured by a particle size distribution measuring device. The jet speed is about V Cr m / sec or less, V Cr is expressed by the following formula (Quoted from: Current status and issues of the new thermal spraying method, cold spray (Vol. 63, No. 9, 2012)). In actual coating, the speed is determined taking into consideration the physical properties, temperature, and surface condition of the substrate, and is often controlled by the temperature, pressure, and powder supply speed. V cr =667-14ρ+0.08T m +0.1σ u -0.4T i V cr :Critical speed (m / sec) ρ: Particle density (g / m 3 ) T m : Melting point of particles (℃) σ u : Tensile strength of particle (MPa) T i : Particle impact temperature (℃)
[0080] The distance between the nozzle and the surface of the test piece was approximately 0.5 mm to 30 mm, and spraying was performed when the relative angle Θ between the center line of the jet and the surface of the test piece was 90 degrees and nearby angles, 60 degrees, 45 degrees, 30 degrees, 20 degrees, and 15 degrees.
[0081] After the formation of the cambium layer, the test pieces were placed in an aerated environment for one month, and then the surface condition was observed.
[0082] Examples of the confirmation results are shown in Figures 11 to 13. Figure 11 is a photograph of the appearance of the surface of the first sample in the embodiment, Figure 12 is a photograph of the second sample, and Figure 13 is a photograph of the third sample. In each photograph, the dark parts on the left and right ends are the surface of the substrate, and the light parts excluding the ends are the formation layer.
[0083] The first sample shown in Figure 11 is when the relative angle Θ is 90 degrees. After the formation of the formation layer on the surface, there are very few areas, particularly in the range shown in part A at the center of the photo, that have a brownish copper color due to fine irregularities on the surface, and it was possible to confirm with the naked eye that the surface roughness is high. Also, although very small, air bubbles were visible in the dark area shown in part B at the upper left of the photo. This shows that the formation layer formed on the surface has not yet reached the stage of forming a sufficient dense metal layer, and the judgment level is "△ (not sufficient)".
[0084] When the relative angle Θ is 90 degrees, a good formation layer may be formed depending on the construction conditions, but a slight change in the construction conditions will result in an unsatisfactory formation layer, confirming that the method has little robustness to the construction conditions or construction conditions.
[0085] In addition, even in the angle region where the relative angle Θ is close to 90 degrees, when the angle is checked at an angle away from 90 degrees, for example, 80 degrees, the formation of the formation layer becomes rapidly stable. In other words, when the relative angle Θ is 80 degrees, no discoloration, oxidation, or unevenness is observed on the surface of the formation layer 20, and the surface condition is smooth. Therefore, the evaluation level for the denseness is "◯ (good)".
[0086] The second sample shown in Fig. 11 is a case where the relative angle Θ is 60 degrees. No discoloration, oxidation, or irregularities are observed on the surface of the formation layer 20, and the surface condition is smooth. Therefore, the denseness is judged to be "good".
[0087] The third sample shown in Fig. 12 is a case where the relative angle Θ is 45 degrees. No discoloration, oxidation, or irregularities are observed on the surface of the formation layer 20, and the surface condition is smooth. Therefore, the denseness is judged to be "good".
[0088] The observation results when the relative angle Θ is 30 degrees and 20 degrees show that, similar to the cases when the relative angle Θ is 60 degrees and 45 degrees, no discoloration, oxidation, or unevenness is observed on the surface of the formation layer 20, and the surface condition is smooth. Therefore, the denseness is judged to be "good".
[0089] The observation results when the relative angle Θ was 15 degrees showed that minute irregularities on the surface were visible to the naked eye and that the formation layer formed on the surface had not yet reached the stage of forming a sufficient dense metal layer, and the judgment level was determined to be "△ (not sufficient)."
[0090] These results show that when the formation of the forming layer forms a dense metal layer, it also has the effect of modifying the surface by reducing surface irregularities.
[0091] FIG. 14 is an evaluation table showing the evaluation results based on the test results in the examples.
[0092] The first row is the relative angle (degrees), the second row is the density based on the appearance photograph, the third row is the formation efficiency of the forming layer, and the fourth row is the formation index of the metal dense layer.
[0093] The second row shows the results of the confirmation of the denseness of the cambium layer, which is the first index of the qualitative aspect. As mentioned above, when the relative angle Θ is between 20 degrees and 80 degrees, it is ◯ (good), i.e., a good result, and when the relative angle Θ is between 15 degrees and 90 degrees, it is △ (not sufficient), i.e., the result is insufficient denseness.
[0094] The third row is the efficiency of formation of the formation layer, which is the second quantitative index. Based on the results shown in Figure 8, when the relative angle Θ is 20 degrees, it is rated as △ (insufficient), and when it is 30 degrees or more, it is rated as ◯ (good).
[0095] The fourth row is the metal dense layer formation index, which is a comprehensive index of the first qualitative index and the second quantitative index. The metal dense layer formation index is rated as ◯ (good) only when both the first and second indexes are ◯ (good), and when at least one of the first and second indexes is △ (not sufficient) or × (unacceptable), the metal dense layer formation index is rated as the lower of the first and second indexes.
[0096] As described above, it was confirmed that a dense metal layer that was generally stable could be formed at each of the relative angles Θ ranging from 30 degrees to 80 degrees. [Other embodiments]
[0097] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0098] Reference Signs List 1...substrate, 1a...substrate surface, 10...metal powder particles, 14...jet, 15...working gas, 16...rebound gas, 20...forming layer, 30...cold spray device, 31...metal powder particle supply section, 31a...metal powder particle storage tank, 31b...transfer pipe, 32...gas supply section, 33...gas heating section, 34...spray section, 35...spray nozzle
Claims
1. A copper (Cu) substrate used in an environment where it comes into contact with water or steam. The surface of the substrate that comes into contact with the steam is coated with copper, copper alloy, zinc (Zn), or Tin (Sn), silver (Ag), aluminum (Al), gold (Au), or any of these A method for forming a dense metal layer by colliding two or more metal powder particles to form a dense metal layer. There was, A coal purifier having a metal powder particle supply section, a metal powder particle storage tank, a gas heating section, and an injection section. a preparation step of preparing a spray device; The application gas and the metal powder particles are applied to the substrate surface by the cold spray device. The direction of the jet of air, including the surface of the substrate, is determined by the angle between the center line of the jet of air and a straight line on the surface of the substrate. The two lines formed by the straight line which is the projection of the spray direction onto the surface of the base material and the spray direction The relative angle Θ of the jet flow, which is the smaller angle of the angles above, is 30 degrees or more and 80 degrees or less. an angle setting step for setting the angle to be within a predetermined angle range; A spraying step of spraying the jet from the cold spray device onto the substrate surface. and, having The temperature of the gas injected from the injection unit is determined based on the strength or hardness of the metal powder particles. The softening temperature of the metal powder particles is the temperature at which the strength or hardness is half that at room temperature.
1. A method for forming a dense metal layer comprising the steps of:
2. The substrate is a stator coil in a direct water-cooled turbine generator, the stator coil having a coil conductor portion at both ends. The clip is connected to the cooling pipe and supplies cooling water, and the base material is made of copper.
2. The method for forming a dense metal layer according to claim 1.
3. The material of the metal powder particles is copper (Cu), gold (Au), silver (Ag), zinc (Zn ), tin (Sn) or phosphorus (P). The method for forming a dense metal layer according to claim 1 or 2.
4. The metal powder particles have an average particle size in the range of 1 μm to 20 μm. The method for forming a dense metal layer according to any one of claims 1 to 3.
5. The temperature of the working gas injected from the injection part is in the range of 250° C. to 750° C. The method for forming a dense metal layer according to any one of claims 1 to 4, Law.
Citation Information
Patent Citations
Kankozairyo
JP1976071125A
Hyperfine-grained material blowing film deposition method
JP2002020878A
Cold spray nozzle, cold spray film, and production method therefor
JP2005095886A
Film deposition method and film deposition apparatus
JP2008214702A
Method of forming metal film and metal film
JP2011050888A