Thermosetting sheets and dicing die bond films
A thermosetting sheet with a controlled thickness change and optional conductive particles addresses peeling issues, enhancing adhesion and conductivity in semiconductor manufacturing.
Patent Information
- Application Number
- JP2021060074
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-03-31
AI Technical Summary
Thermosetting sheets used in semiconductor manufacturing often peel off from the substrate after bonding, leading to insufficient electrical and thermal conduction due to inadequate adhesion reliability.
A thermosetting sheet containing a thermosetting resin and a thermoplastic resin, with a controlled thickness change rate of 0% to 10% when temperature changes from 25°C to 200°C, to suppress shrinkage and peeling, and optionally including conductive particles and a volatile component for enhanced conductivity and heat conduction.
The solution effectively reduces peeling from the substrate, maintaining adhesion and ensuring high electrical and thermal conductivity in semiconductor devices.
Smart Images

Figure 0007577594000007 
Figure 0007577594000008 
Figure 0007577594000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting sheet and a dicing die bond film. [Background technology]
[0002] It has been known in the past to use a thermosetting sheet by adhering it to an adherend.
[0003] The thermosetting sheet is used, for example, to adhere (adhere) a semiconductor element to a substrate having a mounting area for the semiconductor element (for die bonding) (for example, Patent Document 1 below). That is, the thermosetting sheet is used, for example, in the manufacture of semiconductor devices. Patent Document 1 discloses such a thermosetting sheet that contains conductive particles and a thermosetting resin.
[0004] In the manufacture of the above-described semiconductor device, for example, a thermosetting sheet is attached to one side of a semiconductor wafer (the side opposite to the circuit-forming surface), and the semiconductor wafer and the thermosetting sheet are diced to obtain a plurality of thermosetting sheets each having a semiconductor element attached to one side. The thermosetting sheet with the semiconductor element attached on one side is temporarily attached on the other side to the region of the substrate where the semiconductor element is to be attached at a predetermined temperature (e.g., 70°C), and then is thermally cured at a higher temperature (e.g., 200°C) to be bonded (mainly bonded) to the substrate. In other words, the semiconductor element is bonded to the substrate with the thermosetting sheet interposed therebetween. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-21813 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, after the other side of the thermosetting sheet is fully adhered to the substrate (e.g., after adhesion at 200°C), a portion of the other side of the thermosetting sheet may peel off from the substrate, which is the adherend. The occurrence of such peeling is undesirable from the standpoint of the adhesive reliability of the thermosetting sheet to the adherend. Furthermore, in the semiconductor device described above, if such peeling occurs, electrical conduction and thermal conduction via the conductive particles become insufficient, which is undesirable. However, it cannot be said that sufficient research has been conducted yet on preventing the peeling of the thermosetting sheet from the substrate, which is the adherend.
[0007] The above-mentioned problem of peeling of the thermosetting sheet can occur in the same way even when the adherend is something other than a substrate having a mounting area for a semiconductor element.
[0008] Therefore, an object of the present invention is to provide a thermosetting sheet that can relatively suppress peeling from an adherend after thermal curing, and a dicing die bond film including the thermosetting sheet. [Means for solving the problem]
[0009] After extensive research, the inventors discovered that by making the thermosetting sheet contain a thermosetting resin and a thermoplastic resin, and by making the rate of change in thickness when the temperature is changed from 25°C to 200°C to be between 0% and 10%, peeling of the thermosetting sheet from the adherend after thermal curing can be relatively suppressed, which led to the invention.
[0010] That is, the thermosetting sheet according to the present invention is A thermosetting sheet comprising a thermosetting resin and a thermoplastic resin, The rate of change in thickness when the temperature is changed from 25°C to 200°C is between 0% and 10%.
[0011] According to this configuration, the sheet contains a thermosetting resin and a thermoplastic resin, and the rate of change in thickness when the temperature is changed from 25°C to 200°C is between 0% and 10%. Therefore, when the thermosetting sheet is thermally cured and finally adhered to the adherend, shrinkage of the thermosetting sheet can be suppressed. Furthermore, by preventing the thermosetting sheet from shrinking, the internal stresses (cure shrinkage stress and heat shrinkage stress) generated in the thermosetting sheet during heat curing can be made relatively small, so that peeling of the thermosetting sheet from the adherend can be relatively prevented. Furthermore, since the thermosetting sheet contains the thermoplastic resin, the thermosetting sheet can have a relatively low elasticity even after being thermally cured. This ensures adhesion between the thermosetting sheet and the adherend even after thermal curing.
[0012] In the thermosetting sheet, It is preferable that the thermoplastic resin is contained in an amount of 60 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the thermosetting resin.
[0013] According to this configuration, peeling of the thermosetting sheet from the adherend can be further suppressed.
[0014] In the thermosetting sheet, It is preferable that the conductive particles are further included.
[0015] According to this configuration, in addition to being able to suppress peeling of the thermosetting sheet from the adherend, the thermosetting sheet can be made to exhibit electrical conductivity and thermal conductivity via the conductive particles.
[0016] In the thermosetting sheet, It is preferable that the composition further contains a volatile component.
[0017] According to this configuration, since the thermosetting sheet further contains a volatile component, the volume of the thermosetting sheet can be reduced by volatilizing the volatile component during thermal curing of the thermosetting sheet. Furthermore, since the volume of the thermosetting sheet is reduced, the conductive particles are positioned closer to each other in the thermosetting sheet, making it easier for the conductive particles to form thermal conduction paths within the thermosetting sheet. This allows the thermosetting sheet to have a relatively high thermal conductivity after curing. The volumetric shrinkage caused by the evaporation of the volatile components (i.e., volumetric shrinkage due to evaporation) has a smaller effect on the peeling of the thermosetting sheet from the adherend than the volumetric shrinkage caused by the thermal curing of the thermosetting resin (i.e., volumetric shrinkage due to thermal curing). Therefore, even if volume shrinkage occurs due to volatilization, peeling of the thermosetting sheet from the adherend is relatively suppressed.
[0018] In the thermosetting sheet, It is preferable that the composition further contains 10 parts by mass or more and 300 parts by mass or less of a volatile component relative to 100 parts by mass of the thermosetting resin.
[0019] With this configuration, it becomes easier for the conductive particles to form heat conductive paths in the thermosetting sheet. This can further increase the thermal conductivity of the thermosetting sheet after curing.
[0020] The dicing die bond film according to the present invention is A base layer; a dicing tape having a pressure-sensitive adhesive layer laminated on the base layer; a thermosetting sheet laminated on the pressure-sensitive adhesive layer of the dicing tape; The thermosetting sheet is any one of the thermosetting sheets described above.
[0021] According to such a configuration, the dicing die bond film is one in which peeling of the thermosetting sheet from the adherend (a substrate having a mounting area for a semiconductor element) is suppressed. Effect of the Invention
[0022] According to the present invention, it is possible to provide a thermosetting sheet that can be relatively prevented from peeling off from an adherend, and a dicing-die-bonding film including the thermosetting sheet. [Brief description of the drawings]
[0023] [Figure 1] 1 is a cross-sectional view showing a configuration of a dicing die bond film according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a configuration of a semiconductor device according to an embodiment of the present invention; [Diagram 3] Graphs showing the change rate of thickness Rc over time obtained by performing thermomechanical analysis on the thermosetting sheets of each example. (a) Graph showing the change rate of thickness Rc over time for the thermosetting sheets of Examples 1 and 2 and Comparative Example 1. (b) Graph showing the change rate of thickness Rc over time for the thermosetting sheets of Examples 3 to 5 and Comparative Example 2. [Figure 4] Examples of SAT images of a thermosetting sheet taken before and after curing. (a) is an SAT image of a thermosetting sheet according to Example 5 taken before curing. (b) is an SAT image of a thermosetting sheet according to Example 5 taken after curing. (c) is an SAT image of a thermosetting sheet according to Comparative Example 2 taken before curing. (d) is an SAT image of a thermosetting sheet according to Comparative Example 2 taken after curing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, one embodiment of the present invention will be described.
[0025] [Thermosetting sheet] The thermosetting sheet according to this embodiment contains a thermosetting resin and a thermoplastic resin. Moreover, the thermosetting sheet according to this embodiment has a thickness change rate of 0% or more and 10% or less when the temperature is changed from 25°C to 200°C. In the following description, the rate of change in thickness when the temperature is changed from 25°C to 200°C may be given the reference symbol Rc.
[0026] As described above, since the sheet contains a thermosetting resin and a thermoplastic resin and has a thickness change rate Rc of 0% or more and 10% or less when the temperature is changed from 25°C to 200°C, shrinkage of the thermosetting sheet can be relatively suppressed when the thermosetting sheet is thermally cured and finally adhered to the adherend. Furthermore, because shrinkage of the thermosetting sheet can be relatively suppressed, the internal stress (cure shrinkage stress and heat shrinkage stress) generated in the thermosetting sheet during heat curing can be relatively small, and therefore peeling of the thermosetting sheet from the adherend due to the internal stress can be suppressed. Furthermore, since the thermosetting sheet contains the thermoplastic resin, the thermosetting sheet can have a relatively low elasticity even after being thermally cured. This ensures adhesion between the thermosetting sheet and the adherend even after thermal curing.
[0027] The rate of change in thickness Rc when the temperature is changed from 25° C. to 200° C. is preferably 1% or more, and more preferably 3% or more. As described above, the upper limit of the rate of change Rc of thickness when the temperature is changed from 25° C. to 200° C. is 10%.
[0028] The rate of change in thickness Rc when the temperature is changed from 25° C. to 200° C. can be calculated as follows. Specifically, in thermomechanical analysis (TMA), when the temperature is changed from 25°C to 200°C, the thickness T1 of the thermosetting sheet at 25°C is measured, and the thickness T2 of the thermosetting sheet immediately after the temperature is raised to 200°C is measured, and the thickness can be calculated using the measured values T1 and T2 according to the following formula. Rc = (T2 - T1) / T1 × 100 In addition, when the thermosetting sheet expands immediately after being heated from 25°C to 200°C, Rc will be a positive value, and when the thermosetting sheet contracts immediately after being heated from 25°C to 200°C, Rc will be a negative value. Also, if the thermosetting sheet does not expand or contract immediately after being heated from 25°C to 200°C, the value of Rc will be 0.
[0029] The thermomechanical analysis can be carried out under the following conditions. Thermomechanical analysis conditions Thermomechanical analyzer: TA Instruments Japan, model Q400 Probe: Macro expansion probe Measurement mode: Compression / Expansion Heating conditions: Heat from 25℃ to 200℃ in 60 minutes, hold at 200℃ for 1 hour, then cool to 25℃ in 30 minutes. Measurement atmosphere: Nitrogen (N 2 ) Load: 0.012N (constant load) Specimen: A first thermosetting sheet laminate, consisting of multiple thermosetting sheets, is pressed for 60 seconds at a temperature of 70°C and a pressure of 6kN to obtain a second thermosetting sheet laminate with a thickness of 3mm. This second thermosetting sheet laminate is then punched out with a 4mmφ punch to obtain a specimen with a thickness of 3mm x 4mmφ. The measurements using the thermomechanical analyzer were performed by placing the test specimen, which had an aluminum plate (circular when viewed from above, 0.1 mm thick, and 5 mmφ flat surface dimensions) on both sides, on the stage of the thermomechanical analyzer so that one of the aluminum plates was in contact with the other aluminum plate (the upper aluminum plate) and then applying a load using the probe from the other aluminum plate side. In addition, Rc can be calculated by taking the arithmetic average of the values obtained for two test specimens.
[0030] The thermosetting sheet according to this embodiment preferably contains 60 parts by mass or more and 500 parts by mass or less of the thermoplastic resin per 100 parts by mass of the thermosetting resin. When the content of the thermoplastic resin is within the above range, peeling of the thermosetting sheet from the adherend can be further suppressed.
[0031] The thermosetting sheet according to this embodiment more preferably contains 90 parts by mass or more of the thermoplastic resin per 100 parts by mass of the thermosetting resin. Moreover, the thermosetting sheet according to this embodiment more preferably contains 400 parts by mass or less, and even more preferably 300 parts by mass or less, of the thermoplastic resin per 100 parts by mass of the thermosetting resin.
[0032] Examples of the thermosetting resin include epoxy resin, phenol resin, amino resin, unsaturated polyester resin, polyurethane resin, silicone resin, and thermosetting polyimide resin, etc. Among these, it is preferable to use epoxy resin.
[0033] Examples of epoxy resins include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, cresol novolac type, orthocresol novolac type, trishydroxyphenylmethane type, tetraphenylolethane type, hydantoin type, trisglycidyl isocyanurate type, and glycidylamine type epoxy resins. Among these, it is preferable to use at least one of bisphenol A type epoxy resin and cresol novolac type epoxy resin, and it is more preferable to use a combination of bisphenol A type epoxy resin and cresol novolac type epoxy resin. The bisphenol A type epoxy resin includes an aliphatic modified bisphenol A type epoxy resin.
[0034] Examples of phenolic resins as a curing agent for epoxy resins include novolac-type phenolic resins, resol-type phenolic resins, biphenyl-type phenolic resins, and polyoxystyrenes such as polyparaoxystyrene. Among the above phenolic resins, it is preferable to use biphenyl-type phenolic resins.
[0035] In addition, as the thermosetting resin, a thermoplastic resin having a thermosetting functional group can also be used. As the thermoplastic resin having a thermosetting functional group, for example, a thermosetting functional group-containing acrylic resin can be mentioned. As the acrylic resin in the thermosetting functional group-containing acrylic resin, a monomer unit derived from a (meth)acrylic acid ester can be mentioned. In the case of a thermoplastic resin having a thermosetting functional group, a curing agent is selected depending on the type of the thermosetting functional group.
[0036] Examples of the thermoplastic resin include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resin such as polyamide 6 and polyamide 6,6, phenoxy resin, acrylic resin, saturated polyester resin such as PET and PBT, polyamideimide resin, fluororesin, etc. Only one type of the thermoplastic resin may be used, or two or more types may be used in combination. As the thermoplastic resin, acrylic resin is preferable from the viewpoint that it has a small amount of ionic impurities and has high heat resistance, making it easier to ensure connection reliability by a thermosetting sheet.
[0037] The acrylic resin is preferably a polymer containing a monomer unit derived from a (meth)acrylic acid ester as the monomer unit having the largest mass ratio. Examples of the (meth)acrylic acid ester include an alkyl (meth)acrylic acid ester, a cycloalkyl (meth)acrylic acid ester, and an aryl (meth)acrylic acid ester. The acrylic resin may contain a monomer unit derived from another component copolymerizable with the (meth)acrylic acid ester. Examples of the other component include a functional group-containing monomer such as a carboxyl group-containing monomer, an acid anhydride monomer, a hydroxyl group-containing monomer, a glycidyl group-containing monomer, a sulfonic acid group-containing monomer, a phosphoric acid group-containing monomer, an acrylamide, and an acrylonitrile, and various polyfunctional monomers. The acrylic resin is preferably a carboxyl group-containing acrylic polymer.
[0038] As described above, the thermosetting sheet of this embodiment contains the thermosetting resin and the thermoplastic resin, and has a thickness change rate of 0% or more and 10% or less when the temperature is changed from 25°C to 200°C. Therefore, after the thermosetting sheet is thermally cured to adhere to the adherend, peeling of a portion of the thermosetting sheet from the adherend can be relatively suppressed. It is not necessarily clear why this is the case, but the inventors speculate as follows about the reason.
[0039] The thermosetting sheet has the property of being thermosetting, and generally contains a thermosetting resin. Furthermore, since a thermosetting resin is usually cured by heat while being crosslinked at a relatively high crosslink density, a thermosetting sheet containing a thermosetting resin undergoes volumetric shrinkage when it is thermally cured and adhered to an adherend, and it is believed that this volumetric shrinkage causes part of the thermosetting sheet to peel off from the adherend. In contrast, the thermosetting sheet according to the present embodiment contains a thermoplastic resin in addition to a thermosetting resin, and it is believed that the thermoplastic resin can mitigate the thermosetting resin from being crosslinked at a relatively high crosslink density, i.e., a relatively gentle crosslinking structure can be formed in the thermosetting sheet. Furthermore, in the thermosetting sheet of this embodiment, the rate of change in thickness Rc when the temperature is changed from 25°C to 200°C (the rate of change in thickness T2 of the thermosetting sheet immediately after heating to 200°C relative to the thickness T1 of the thermosetting sheet at 25°C) is not a negative value and is adjusted to be within the above-mentioned numerical range (0% or more and 10% or less). Therefore, it is believed that the rate of change in thickness Rc becoming excessively large (the thermosetting sheet expanding too much) and causing a part of the thermosetting sheet to peel off from the adherend is suppressed. The inventors surmise that these features prevent the thermosetting sheet of this embodiment from peeling off in part from the adherend even after it has been thermally cured and adhered to the adherend.
[0040] The thermosetting sheet according to this embodiment can be obtained by appropriately adjusting the thickness change rate Rc by appropriately adjusting the content ratio of the thermosetting resin and the content ratio of the thermoplastic resin in the thermosetting sheet. More specifically, the value of the rate of change in thickness Rc can be appropriately adjusted by increasing the content ratio of the thermoplastic resin in the thermosetting sheet (by relatively decreasing the content ratio of the thermosetting resin in the thermosetting sheet). However, if the content ratio of the thermoplastic resin is too high, the thermosetting sheet may not be thermally cured easily, or the thickness change rate Rc may become excessively large (excessive expansion), which may result in the thermosetting sheet having poor adhesive reliability to the adherend. Therefore, it is necessary to appropriately adjust the content ratio of the thermoplastic resin so that the thickness change rate Rc is within the above-mentioned numerical range (0% or more and 10% or less). Furthermore, as described below, when the thermosetting sheet according to this embodiment contains conductive particles, the higher the content of the conductive particles in the thermosetting sheet, the lower the content of organic components, such as the thermosetting resin and the thermoplastic resin, in the thermosetting sheet, and the lower the degree of volumetric shrinkage of the thermosetting sheet due to the thermosetting resin. Therefore, when the thermosetting sheet according to this embodiment contains the conductive particles in addition to the thermosetting resin and the thermoplastic resin, the thickness change rate Rc can be appropriately adjusted so as to be within the above-mentioned numerical range (0% or more and 10% or less) by appropriately adjusting the content ratio of these.
[0041] When the thermosetting sheet of this embodiment is used by adhering it to a substrate having a mounting area for a semiconductor element (when used in the manufacture of a semiconductor device), it is preferable that the thermosetting sheet further contains conductive particles in addition to the thermosetting resin and the thermoplastic resin. When used in the manufacture of semiconductor devices, the thermosetting sheet according to this embodiment preferably further contains a volatile component in addition to the conductive particles. In this specification, the term "conductive particles" refers to particles having an electrical conductivity of 100 μS / cm or less as measured in accordance with JIS K 0130 (2008).
[0042] Since the thermosetting sheet according to this embodiment further contains conductive particles, peeling of the thermosetting sheet from an adherend can be suppressed, and the conductive particles can be used to provide the thermosetting sheet with electrical conductivity and thermal conductivity. Furthermore, since the thermosetting sheet according to this embodiment further contains a volatile component in addition to the conductive particles, the volume of the thermosetting sheet can be reduced by volatilizing the volatile component during thermal curing of the thermosetting sheet. Furthermore, since the volume of the thermosetting sheet is reduced, the conductive particles are positioned closer to each other in the thermosetting sheet, making it easier for the conductive particles to form thermal conduction paths within the thermosetting sheet. This allows the thermosetting sheet to have a relatively high thermal conductivity after curing.
[0043] The thermosetting sheet according to this embodiment preferably contains 700 parts by mass or more of the conductive particles per 100 parts by mass of the thermosetting resin, more preferably 1000 parts by mass or more, and even more preferably 2000 parts by mass or more. Furthermore, the thermosetting sheet according to this embodiment preferably contains 45,000 parts by mass or less of the conductive particles per 100 parts by mass of the thermosetting resin, more preferably 16,000 parts by mass or less, even more preferably 10,000 parts by mass or less, and particularly preferably 8,000 parts by mass or less. In particular, when the conductive particles are contained in an amount of 16,000 parts by mass or less relative to the parts by mass of the thermosetting resin, the thermosetting sheet maintains its sheet shape to a greater extent.
[0044] The thermosetting sheet according to the present embodiment preferably contains 10 parts by mass or more and 300 parts by mass or less of the volatile component per 100 parts by mass of the thermosetting resin. When the content of the volatile component is within the above range, it becomes easier for the conductive particles to form heat conductive paths among each other in the thermosetting sheet. This can further increase the thermal conductivity of the thermosetting sheet after curing. The thermosetting sheet according to this embodiment more preferably contains 20 parts by mass or more of the volatile component per 100 parts by mass of the thermosetting resin. Furthermore, the thermosetting sheet according to this embodiment preferably contains 250 parts by mass or less of the volatile components per 100 parts by mass of the thermosetting resin, more preferably 200 parts by mass or less, and particularly preferably 100 parts by mass or less.
[0045] The conductive particles preferably include silver particles. The silver particles may be in the form of, for example, flakes, needles, filaments, spheres, or flat (including scales). Of these, it is preferable to use spherical particles. By using spherical silver particles, the dispersibility of the silver particles in the thermosetting sheet can be improved.
[0046] The silver particles may be silver particles composed of silver element and other elements (metal elements, etc.) contained as unavoidable impurity elements, or may be silver particles that have been subjected to a surface treatment (for example, silane coupling treatment). Examples of surface treatment agents for silver particles include fatty acid-based, amine-based, and epoxy-based coating agents. Examples of commercially available silver particles surface-treated with a fatty acid-based coating agent include AG-2-8F manufactured by DOWA Electronics Co., Ltd., and examples of commercially available silver particles surface-treated with an epoxy-based coating agent include HP02 manufactured by Mitsui Mining & Smelting Co., Ltd. In the following, silver particles that have been surface-treated with a coating agent such as a fatty acid-based, amine-based, or epoxy-based coating agent may be referred to as coating agent-treated silver particles. In the thermosetting sheet according to the present embodiment, it is preferable to use coated silver particles as the silver particles. By using coated silver particles as the silver particles, it is possible to increase the affinity with the resin components (thermosetting resin and thermoplastic resin) contained in the thermosetting sheet, so that the silver particles are easily dispersed in the thermosetting sheet.
[0047] The conductive particles may include, in addition to silver particles, nickel particles, copper particles, aluminum particles, carbon black, carbon nanotubes, particles in which the surface of a metal particle serving as a core (nucleus) is plated with a metal such as gold or silver (hereinafter also referred to as plated metal particles), and particles in which the surface of a resin particle serving as a core (nucleus) is coated with a metal (hereinafter also referred to as metal-coated resin particles), etc. Only one of these conductive particles may be used, or two or more types may be used in combination.
[0048] As the plated metal particles, for example, particles having a nickel particle or copper particle as a core, the surface of which is plated with a noble metal such as gold or silver, can be used. As the metal-coated resin particles, for example, particles having a resin particle as a core, the surface of which is coated with a metal such as nickel or gold, can be used. When the thermosetting sheet according to the present embodiment contains conductive particles other than silver particles, it is preferable to use plated metal particles as the conductive particles, and it is preferable to use particles (silver-coated copper particles) in which copper particles are used as the core and the surface of the core is plated with silver as the plated metal particles. Commercially available silver-coated copper particles include 1200Y (copper particles) manufactured by Mitsui Mining & Smelting Co., Ltd., coated with 20% by mass of silver particles, MA-C03K (copper particles) manufactured by Mitsui Mining & Smelting Co., Ltd., coated with 20% by mass of silver particles, and AOP-TCY-2 (EN) manufactured by DOWA Electronics Co., Ltd. When the thermosetting sheet according to this embodiment contains conductive particles other than silver particles, the mass parts of silver particles per 100 mass parts of the conductive particles is preferably 10 parts by mass or more and 95 parts by mass or less, and more preferably 20 parts by mass or more and 90 parts by mass or less.
[0049] The conductive particles other than silver particles may be, for example, flake-shaped, needle-shaped, filament-shaped, spherical, or flat (including scale-shaped) particles, with spherical particles being preferred among these. By using spherical conductive particles other than silver particles, the dispersibility of the conductive particles other than silver particles in the thermosetting sheet can be improved. Here, since spherical particles have a smaller specific surface area than flat particles, if spherical particles are used as conductive particles other than silver particles, the contact area between the conductive particles other than silver particles and the silver particles will be small, which is thought to be disadvantageous in terms of electrical conductivity and thermal conductivity. However, since the thermosetting sheet according to this embodiment contains a volatile component, the volatile component evaporates during the thermal curing of the thermosetting sheet, thereby reducing the volume of the thermosetting sheet after curing (the thermosetting sheet shrinks in volume), and the conductive particles other than the silver particles are positioned close to the silver particles. Therefore, even when spherical particles are used as conductive particles other than silver particles, a sufficient contact area between the conductive particles other than silver particles and the silver particles can be ensured, thereby ensuring sufficient electrical conductivity and thermal conductivity. The above-mentioned 1200Y (trade name) manufactured by Mitsui Metals and Smelting Co., Ltd., coated with 20% by mass of silver particles, MA-C03K (trade name) manufactured by Mitsui Metals and Smelting Co., Ltd., coated with 20% by mass of silver particles, and AOP-TCY-2(EN) (trade name) manufactured by Dowa Electronics Co., Ltd. are all classified as spherical.
[0050] The volatile component may be an organic compound having one or more hydroxyl groups and a boiling point of 250°C or higher. The boiling point of the organic compound is preferably 350°C or lower. Such an organic compound may be a terpene compound. Among terpene compounds, the volatile component is preferably isobornylcyclohexanol represented by the following formula (1). Isobornylcyclohexanol is an organic compound having a boiling point of 308 to 318°C. When heated from room temperature (23±2°C) to 600°C under a nitrogen gas flow of 200mL / min and at a temperature increase rate of 10°C / min, it has the property of undergoing a large weight loss from 100°C or higher and volatilizing and disappearing at 245°C (no further weight loss is observed). It also has the property of exhibiting an extremely high viscosity of 1,000,000 mPa·s at 25°C, but a relatively low viscosity of 1,000 mPa·s or lower at 60°C. The weight loss is a value when the weight loss rate at the measurement start temperature (room temperature) is set to 0%. Thus, isobornylcyclohexanol exhibits extremely high viscosity at 25° C. as described above, and is therefore capable of maintaining a sheet shape at room temperature, but exhibits relatively low viscosity at 60° C. as described above, and thus becomes tacky. In other words, a thermosetting sheet containing isobornylcyclohexanol exhibits excellent sheet shape retention at room temperature, and becomes tacky at temperatures of 60° C. or higher. Here, when mounting a semiconductor element attached to one side of a thermosetting sheet on a metal lead frame or the like, the semiconductor element is usually temporarily attached (temporarily fixed) to an adherend such as a metal lead frame via the thermosetting sheet at a temperature of 60 to 80° C., but since isobornylcyclohexanol has tackiness at 60° C. or higher as described above, when the thermosetting sheet according to this embodiment contains isobornylcyclohexanol as a volatile component, the thermosetting sheet has improved temporary adhesion to an adherend such as a metal lead frame. In other words, in the temporarily attached state, the mounting position of the semiconductor element is not shifted and the thermosetting sheet is prevented from lifting off the adherend. Therefore, when the thermosetting sheet is thermally cured to bond the semiconductor element to the adherend, the semiconductor element can be bonded to the adherend with high reliability.
[0051] [ka]
[0052] The thermosetting sheet according to the present embodiment may contain a thermosetting catalyst in order to sufficiently advance the curing reaction of the resin component and to increase the curing reaction rate. Examples of the thermosetting catalyst include imidazole-based compounds, triphenylphosphine-based compounds, amine-based compounds, and trihalogen borane-based compounds.
[0053] The thermosetting sheet according to this embodiment has a particle filling rate P 1 is preferably 30% by volume or more, more preferably 40% by volume or more, and even more preferably 50% by volume or more. The particle packing ratio P 1 is preferably 70% by volume or less, and more preferably 60% by volume or less.
[0054] In addition, the thermosetting sheet according to this embodiment has a particle filling rate P 2is preferably 40% by volume or more, more preferably 50% by volume or more, and even more preferably 60% by volume or more. The particle packing ratio P 2 is preferably 80% by volume or less, and more preferably 75% by volume or less. The particle packing ratio P 2 When the value of the cured thermosetting sheet satisfies the above range, the heat dissipation property of the cured thermosetting sheet can be further improved. The particle filling rate refers to the proportion of conductive particles per unit volume, and can be determined by, as described below, mechanically polishing a thermosetting sheet to expose a cross section, taking an SEM image of an arbitrary cross-sectional region using a field emission electron microscope to obtain a reflected electron image as image data, and then performing image analysis on the image data.
[0055] The particle packing ratio P 1 can be obtained according to the following procedure. (1) The thermosetting sheet before curing is mechanically polished to expose the cross section, and the exposed cross section is subjected to ion polishing using an ion polishing device (for example, product name: Cross Section Polisher SM-09010, manufactured by JEOL Ltd.). (2) An SEM image (scanning electron microscope image) of an arbitrary cross-sectional area of the exposed cross-section that has been ion-polished is taken using a field emission scanning electron microscope (e.g., Hitachi High-Technologies Corporation, product name SU8020), and a backscattered electron image is obtained as image data. The imaging conditions can be an acceleration voltage of 5 kV and a magnification of 5000 times. (3) The obtained image data is subjected to an automatic binarization process using image analysis software (e.g., ImageJ) to binarize the metal parts and the resin parts. (4) The total area of the conductive particle parts and the total area (conductive particle part + resin part) are calculated from the binarized image, and the total area of the conductive particle parts is divided by the total area to obtain the particle packing ratio P of the conductive particles for the cured thermosetting sheet. 1 Request. The particle packing ratio P 1 is preferably determined by arithmetically averaging the filling rates determined for five cross-sectional regions on the exposed cross-section that has been ion-polished. In addition, the particle packing ratio P 2 The hardness of the thermosetting sheet after curing can be determined in the same manner as above.
[0056] The thickness of the thermosetting sheet according to this embodiment is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. When the thickness of the thermosetting sheet is 150 μm or less, the thermal conductivity can be further improved. The thickness of the thermosetting sheet can be determined, for example, by measuring the thickness at five randomly selected points using a dial gauge (manufactured by PEACOCK, model R-205) and calculating the arithmetic average of these thicknesses.
[0057] The thermosetting sheet according to this embodiment preferably has a thermal conductivity of 3 W / m·K or more after curing. When the thermal conductivity after curing is within the above range, the electrical conductivity of the thermosetting sheet after curing can be further increased. In the thermosetting sheet according to this embodiment, the upper limit of the thermal conductivity after curing is usually 100 W / m·K. The thermal conductivity after curing can be calculated by subjecting the thermosetting sheet according to this embodiment to heat curing at 200°C for 1 hour in a pressure cooker while applying a pressure of 0.5 MPa, and using the following formula for the heat-cured thermosetting sheet.
[0058]
number
[0059] In the above formula, thermal diffusivity (m 2 / s) can be measured by a TWA method (temperature wave thermal analysis, measuring device: iPhase Mobile, manufactured by iPhase Corporation). The specific heat (J / g°C) in the above formula can be measured by the DSC method. Specific heat measurement is performed using a DSC6220 manufactured by SII Nanotechnology, Inc., at a heating rate of 10°C / min and in the temperature range of 20 to 300°C. Based on the obtained data, the specific heat can be calculated using the method described in the JIS Handbook (specific heat capacity measurement method K-7123). Furthermore, the specific gravity in the above formula can be measured by Archimedes' method.
[0060] The thermosetting sheet according to the present embodiment may contain one or more other components as required, such as a filler dispersant, a flame retardant, a silane coupling agent, and an ion trapping agent.
[0061] [Dicing die bond film] Next, the dicing die bond film 20 will be described with reference to Fig. 1. In the following description, the description of the parts that overlap with the thermosetting sheet will not be repeated.
[0062] As shown in FIG. 1, the dicing die bond film 20 of this embodiment comprises a base layer 1, a dicing tape 10 having an adhesive layer 2 laminated on the base layer 1, and a thermosetting sheet 3 laminated on the adhesive layer 2 of the dicing tape 10. In the dicing die bond film 20, a semiconductor element is attached onto a thermosetting sheet 3. The semiconductor element may be a bare wafer. The bare wafer attached to the dicing die bond film 20 according to this embodiment is cleaved into a plurality of bare chips by blade dicing, DBG (Dicing Before Grinding), SDBG (Stealth Dicing Before Grinding), or the like. During the cleaving process, the thermosetting sheet 3 is also cleaved together with the bare wafer. The thermosetting sheet 3 is cleaved into pieces of a size corresponding to the size of the individual bare chips. This allows a plurality of bare chips with the thermosetting sheet 3 to be obtained.
[0063] As described above, the thermosetting sheet 3 of the dicing die bond film 20 contains a thermosetting resin and a thermoplastic resin, and the rate of change in thickness when the temperature is changed from 25°C to 200°C is greater than or equal to 0% and less than or equal to 10%.
[0064] The base layer 1 supports the adhesive layer 2 and the thermosetting sheet 3 laminated on the adhesive layer 2. The base layer 1 contains a resin. Examples of the resin include olefin-based resins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers; copolymers containing ethylene as a monomer component, such as ethylene-vinyl acetate copolymers (EVA), ionomer resins, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester (random, alternating) copolymers; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); acrylic resins; polyvinyl chloride (PVC); polyurethane; polycarbonate; polyphenylene sulfide (PPS); amide-based resins such as polyamide and fully aromatic polyamide (aramid); polyether ether ketone (PEEK); polyimide; polyetherimide; polyvinylidene chloride; ABS (acrylonitrile-butadiene-styrene copolymer); cellulose-based resins; silicone resins; and fluororesins. Among these, it is preferable to use polyethylene terephthalate.
[0065] The substrate layer 1 may contain one type of the above-mentioned resin, or may contain two or more types of the above-mentioned resin.
[0066] Materials for the base layer 1 include polymers such as crosslinked bodies of the resins (e.g., plastic films). The plastic films may be used without stretching, or may be uniaxially or biaxially stretched as necessary. When a resin sheet is provided with heat shrinkability by stretching or the like, the base layer 1 is heat-shrunk after dicing to reduce the adhesion area between the pressure-sensitive adhesive layer 2 and the thermosetting sheet 3, facilitating the recovery of the semiconductor chips (semiconductor elements).
[0067] The surface of the base layer 1 may be subjected to a general surface treatment in order to improve adhesion to adjacent layers, retention, etc. Examples of such surface treatments include chemical or physical treatments such as chromate treatment, ozone exposure, flame exposure, high-voltage shock exposure, and ionizing radiation treatment, as well as coating treatment with a primer.
[0068] The thickness of the base layer 1 is preferably from 1 μm to 1000 μm, more preferably from 10 μm to 500 μm, further preferably from 20 μm to 300 μm, and particularly preferably from 30 μm to 200 μm. The thickness of the base layer 1 can be determined using a dial gauge (Model R-205, manufactured by PEACOCK) in the same manner as the thickness of the thermosetting sheet 3 described above.
[0069] The base layer 1 may contain various additives, such as colorants, fillers, plasticizers, antioxidants, antioxidants, surfactants, and flame retardants.
[0070] The adhesive used to form the adhesive layer 2 is not particularly limited, and may be, for example, a general pressure-sensitive adhesive such as an acrylic adhesive or a rubber-based adhesive. As the pressure-sensitive adhesive, an acrylic adhesive having an acrylic polymer as a base polymer is preferred from the viewpoint of cleaning and washing properties with ultrapure water or organic solvents such as alcohol for electronic components that are sensitive to contamination, such as semiconductor wafers and glass.
[0071] Examples of the acrylic polymer include acrylic polymers using one or more of (meth)acrylic acid alkyl esters and (meth)acrylic acid cycloalkyl esters as monomer components. Examples of the (meth)acrylic acid alkyl esters include methyl esters, ethyl esters, propyl esters, isopropyl esters, butyl esters, isobutyl esters, s-butyl esters, t-butyl esters, pentyl esters, isopentyl esters, hexyl esters, heptyl esters, octyl esters, 2-ethylhexyl esters, isooctyl esters, nonyl esters, decyl esters, isodecyl esters, undecyl esters, dodecyl esters, tridecyl esters, tetradecyl esters, hexadecyl esters, octadecyl esters, and eicosyl esters, and the like, which are linear or branched alkyl esters having 1 to 30 carbon atoms, particularly 4 to 18 carbon atoms. Examples of the (meth)acrylic acid cycloalkyl esters include cyclopentyl esters and cyclohexyl esters. The (meth)acrylic acid ester means at least one of an acrylic acid ester and a methacrylic acid ester, and all (meth) in the present invention have the same meanings as those described above.
[0072] The acrylic polymer may contain units corresponding to other monomer components copolymerizable with the (meth)acrylic acid alkyl ester or (meth)acrylic acid cycloalkyl ester, if necessary, for the purpose of modifying the cohesive strength, heat resistance, etc. Examples of such monomer components include carboxyl-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and 10-hydroxydecyl (meth)acrylate. , 12-hydroxylauryl (meth)acrylate, (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, and other hydroxyl group-containing monomers; styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acryloyloxynaphthalenesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, and other sulfonic acid-containing monomers; 2-hydroxyethylacryloylphosphate, and other phosphoric acid-containing monomers; acrylamide, acrylonitrile, and the like. These copolymerizable monomer components can be used alone or in combination. The amount of these copolymerizable monomers used is preferably 40% by mass or less of the total monomer components.
[0073] Furthermore, the acrylic polymer may contain a polyfunctional monomer as a copolymerization monomer component for crosslinking, if necessary. Examples of such polyfunctional monomers include hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy(meth)acrylate, polyester(meth)acrylate, and urethane(meth)acrylate. These polyfunctional monomers may be used alone or in combination. The amount of the polyfunctional monomer used is preferably 30% by mass or less of the total monomer components in terms of adhesion properties, etc.
[0074] The acrylic polymer can be obtained by polymerizing a single monomer or a mixture of two or more monomers. The polymerization may be carried out by any method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, etc. From the viewpoint of preventing contamination of clean adherends, it is preferable that the content of low molecular weight substances is small. From this viewpoint, the number average molecular weight of the acrylic polymer is preferably 300,000 or more, and more preferably about 400,000 to 3,000,000.
[0075] In addition, an external crosslinking agent can be appropriately added to the adhesive in order to increase the number average molecular weight of the base polymer, such as an acrylic polymer. Specific means for the external crosslinking method include a method of adding a crosslinking agent such as a polyisocyanate compound, an epoxy compound, an aziridine compound, or a melamine crosslinking agent and reacting it. When using an external crosslinking agent, the amount of the agent is appropriately determined in consideration of the balance with the base polymer to be crosslinked and the intended use as an adhesive. In general, the external crosslinking agent is preferably blended in an amount of about 5 parts by mass or less, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the base polymer.
[0076] In addition to the above components, the pressure-sensitive adhesive may contain various known additives such as a tackifier and an antiaging agent, if necessary.
[0077] The adhesive layer 2 can be formed from a radiation-curable adhesive. The degree of crosslinking of a radiation-curable adhesive can be increased by irradiation with radiation such as ultraviolet light, and the adhesive strength can be easily reduced. That is, by forming the adhesive layer 2 from a radiation-curable adhesive, the adhesive layer 2 can be sufficiently adhered to the thermosetting sheet 3 without being irradiated with radiation before dicing, and after dicing, the adhesive layer 2 can be irradiated with radiation to reduce the adhesive strength of the adhesive layer 2, allowing the semiconductor chip (semiconductor element) to be easily picked up (recovered).
[0078] The radiation curable adhesive can be used without any particular limitation as long as it has a radiation curable functional group such as a carbon-carbon double bond and exhibits adhesive properties. Examples of the radiation curable adhesive include additive-type radiation curable adhesives in which a radiation curable monomer component or oligomer component is blended with a general pressure-sensitive adhesive such as an acrylic adhesive or a rubber adhesive.
[0079] Examples of the radiation-curable monomer component include urethane (meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 1,4-butanediol di(meth)acrylate. Examples of the radiation-curable oligomer component include various oligomers such as urethane-based, polyether-based, polyester-based, polycarbonate-based, and polybutadiene-based oligomers, and those having a molecular weight in the range of about 100 to 30,000 are preferred. The amount of the radiation-curable monomer component or the radiation-curable oligomer component is preferably an amount that can suitably reduce the adhesive strength of the adhesive layer 2 after radiation irradiation. In general, the amount of the radiation-curable monomer component or the radiation-curable oligomer component is, for example, preferably 5 to 500 parts by mass, and more preferably 40 to 150 parts by mass, per 100 parts by mass of the base polymer, such as an acrylic polymer, that constitutes the pressure-sensitive adhesive.
[0080] In addition to the above-mentioned additive-type radiation-curable adhesives, examples of the radiation-curable adhesive include internal-type radiation-curable adhesives using a base polymer having a carbon-carbon double bond in the polymer side chain, in the main chain, or at the end of the main chain. The internal-type radiation-curable adhesive does not need to contain low molecular weight oligomer components or the like, or the content of the oligomer components or the like is relatively small. Therefore, when the internal-type radiation-curable adhesive is used, the oligomer components or the like are prevented from moving over time in the adhesive layer 2. As a result, the adhesive layer 2 can have a relatively stable layer structure.
[0081] The base polymer having a carbon-carbon double bond can be used without any particular limitation as long as it has a carbon-carbon double bond and has adhesiveness. As such a base polymer, it is preferable that the base polymer has an acrylic polymer as a basic skeleton. As the basic skeleton of the acrylic polymer, the above-mentioned acrylic polymer can be mentioned.
[0082] The method of introducing a carbon-carbon double bond into the acrylic polymer is not particularly limited, and various methods can be adopted, but the adoption of a method of introducing a carbon-carbon double bond into a polymer side chain makes molecular design easier. For example, a method of copolymerizing a monomer having a functional group with an acrylic polymer in advance, and then carrying out a condensation reaction or addition reaction with a compound having a functional group and a carbon-carbon double bond that can react with the functional group while maintaining the radiation curability of the carbon-carbon double bond can be mentioned.
[0083] Examples of combinations of these functional groups include a carboxyl group and an epoxy group, a carboxyl group and an aziridyl group, and a hydroxyl group and an isocyanate group. Among these combinations of functional groups, a combination of a hydroxyl group and an isocyanate group is preferred from the viewpoint of ease of reaction tracking. In addition, as long as the combination of these functional groups produces an acrylic polymer having a carbon-carbon double bond, either of the functional groups may be on the acrylic polymer side or on the compound having a carbon-carbon double bond side. In the case of the above preferred combination, it is preferred that the acrylic polymer has a hydroxyl group and the compound having a carbon-carbon double bond has an isocyanate group. In this case, examples of the isocyanate compound having a carbon-carbon bond include methacryloyl isocyanate, 2-methacryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, and the like. As the acrylic polymer, a copolymer of the above-mentioned hydroxyl group-containing monomers or ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether can be used.
[0084] The inherent type radiation-curable adhesive can use the base polymer having a carbon-carbon double bond (particularly, an acrylic polymer) alone, but can also contain the radiation-curable monomer component or the radiation-curable oligomer component to the extent that the properties are not deteriorated. The radiation-curable oligomer component is usually contained in an amount of 30 parts by mass or less, and preferably 1 to 10 parts by mass, per 100 parts by mass of the base polymer.
[0085] The radiation-curable adhesive contains a photopolymerization initiator when curing with ultraviolet light or the like. Examples of the photopolymerization initiator include α-ketol-based compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-hydroxypropiophenone, and 1-hydroxycyclohexylphenylketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether-based compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; and ketal-based compounds such as benzyl dimethyl ketal. Examples of the photopolymerization initiator include aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates. The amount of the photopolymerization initiator is, for example, 0.05 to 20 parts by mass relative to 100 parts by mass of the base polymer such as an acrylic polymer constituting the adhesive.
[0086] Examples of radiation-curable adhesives include rubber-based adhesives and acrylic-based adhesives that contain a photopolymerizable compound, such as an addition-polymerizable compound having two or more unsaturated bonds or an alkoxysilane having an epoxy group, and a photopolymerization initiator, such as a carbonyl compound, an organic sulfur compound, a peroxide, an amine, or an onium salt compound, as disclosed in JP-A-60-196956.
[0087] In cases where curing is inhibited by oxygen during radiation irradiation, it is desirable to use some method to block oxygen (air) from the surface of the radiation-curable pressure-sensitive adhesive layer 2. Examples of such methods include a method of covering the surface of the pressure-sensitive adhesive layer 2 with a separator, and a method of irradiating the pressure-sensitive adhesive layer 2 with radiation such as ultraviolet light in a nitrogen gas atmosphere.
[0088] The thickness of the adhesive layer 2 is not particularly limited, but from the viewpoint of preventing chipping of the cut surface of the chip and at the same time maintaining the fixing and retention of the thermosetting sheet 3, it is preferably 1 to 50 μm, more preferably 2 to 30 μm, and even more preferably 5 to 25 μm.
[0089] [Semiconductor Devices] The semiconductor device of this embodiment comprises a substrate having a mounting area for a semiconductor element, and a semiconductor element mounted in the mounting area for the semiconductor element, the semiconductor element being mounted in the mounting area for the semiconductor element of the substrate via a thermosetting sheet. In the semiconductor device according to this embodiment, the semiconductor element is mounted in the semiconductor element mounting region of the substrate by thermally curing the thermosetting sheet.
[0090] In the semiconductor device of this embodiment, before the thermosetting sheet is thermally cured, the bonding rate JR1 of the thermosetting sheet to the substrate (hereinafter also referred to as the pre-thermal curing bonding rate JR1) is preferably 85% or more, and more preferably 90% or more. In the semiconductor device of this embodiment, after the thermosetting sheet is thermally cured, the bonding rate JR2 of the thermosetting sheet to the substrate (hereinafter also referred to as the bonding rate JR2 after thermal curing) is preferably 80% or more, and more preferably 90% or more. In the semiconductor device according to this embodiment, the ratio of the post-thermal curing bonding rate JR2 to the pre-thermal curing bonding rate JR1 is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. In the semiconductor device of this embodiment, it is preferable that the pre-thermosetting bonding rate JR1 is 85% or more, the post-thermosetting bonding rate JR2 is 80% or more, and the ratio of the post-thermosetting bonding rate JR2 to the pre-thermosetting bonding rate JR1 is 80% or more, it is more preferable that the pre-thermosetting bonding rate JR1 is 90% or more, the post-thermosetting bonding rate JR2 is 90% or more, and the ratio of the post-thermosetting bonding rate JR2 to the pre-thermosetting bonding rate JR1 is 90% or more, it is even more preferable that the pre-thermosetting bonding rate JR1 is 95% or more, the post-thermosetting bonding rate JR2 is 90% or more, and the ratio of the post-thermosetting bonding rate JR2 to the pre-thermosetting bonding rate JR1 is 95% or more.
[0091] In this specification, the bonding rate of a thermosetting sheet to a substrate means the ratio of the area of the thermosetting sheet actually attached to the mounting area of the semiconductor element to the total area of the thermosetting sheet that will be attached to the mounting area of the semiconductor element.
[0092] An example of the semiconductor device according to this embodiment is configured as shown in FIG. As shown in FIG. 2, the semiconductor device 30 includes a lead frame substrate 31 having a die pad 31a which is partitioned into an approximately rectangular shape when viewed from above, and a pair of lead portions 31b, 31b extending from both ends of the die pad 31a, a semiconductor element 32 which is attached to the die pad 31a of the lead frame substrate 31 while being laminated on a thermosetting sheet 3, a pair of wires 33, 33 which electrically connect the semiconductor element 32 to the pair of lead portions 31b, 31b, and a hollow package 34 which accommodates inside the entire die pad 31a, part of the pair of lead portions 31b, 31b, the entire semiconductor element 32 laminated on the thermosetting sheet 3, and the entire pair of wires 33, 33, and the gap between the semiconductor element 32 etc. and the package 34 is filled with molded resin 35. That is, in the semiconductor device 30 shown in FIG. 2, the lead frame substrate 31 is a substrate having a mounting area for a semiconductor element, and the die pad 31a is the mounting area for the semiconductor element.
[0093] In addition, in the semiconductor device 30, one end of a pair of lead portions 31b, 31b is arranged on the upper surface side of both ends of the die pad 31a, extends in a direction parallel to the upper surface of the die pad 31a (hereinafter also referred to as the horizontal direction), and then extends downward in a direction perpendicular to the upper surface of the die pad 31a (hereinafter also referred to simply as the vertical downward direction), and the horizontally extending portions of the pair of lead portions 31b, 31b penetrate the package 34. That is, in the semiconductor device 30, a portion of the horizontally extending portion of a pair of lead portions 31b, 31b is accommodated inside the package 34, and the remainder of the horizontally extending portion and the entire portion extending vertically downward are exposed to the outside of the package 34.
[0094] As shown in FIG. 2, the semiconductor device 30 is mounted on a wiring board 40 having a pair of electrodes 41, 41 spaced apart from each other on its surface. More specifically, the semiconductor device 30 is attached to a wiring board 40 by joining a portion of the vertically downward extending portions of a pair of lead portions 31b, 31b to a pair of electrodes 41, 41, respectively, using solder or the like.
[0095] In the semiconductor device according to this embodiment, as described above, the thermosetting sheet is a thermosetting sheet that contains a thermosetting resin and a thermoplastic resin, and has a thickness change rate of 0% or more and 10% or less when the temperature is changed from 25°C to 200°C.
[0096] The bonding ratio of the thermosetting sheet to the substrate can be determined according to the following procedure. (1) A test specimen for evaluating the bonding rate is obtained by attaching one surface of a thermosetting sheet (or a laminate of multiple thermosetting sheets) having a silicon chip (bare chip) attached to the other surface of the sheet to a semiconductor element mounting area of a substrate having the semiconductor element mounting area. (2) Using an ultrasonic imaging device (manufactured by Hitachi Construction Machinery Finetech Co., Ltd., model: FineSAT FS200II, hereinafter also referred to as SAT), the specimen for evaluation of the bonding rate is imaged by a reflection method to obtain an SAT image. The imaging is performed by adjusting the gate so as to match the echo of the bonding portion between the substrate and the thermosetting sheet displayed on the waveform monitor of the ultrasonic imaging device, setting the pixel to 1, the gain to 25 dB, and the Z-axis height to 11.34 mm. (3) Using the image analysis software ImageJ, the obtained SAT image is subjected to an automatic binarization process to binarize the bonded portion between the substrate and the thermosetting sheet (hereinafter also referred to as the bonded portion) and the non-bonded portion between the substrate and the thermosetting sheet (hereinafter also referred to as the non-bonded portion). The threshold value is set to 82. (4) From the binarized image, the area of the bonded parts and the area of the non-bonded parts are calculated, the value of the area of the bonded parts is divided by the sum of the area of the bonded parts and the area of the non-bonded parts, and then multiplied by the number 100 to calculate the bonding rate of the thermosetting sheet to the substrate. In the binarized image, the joints are shown in black, and the non-joints are shown in white.
[0097] The thermosetting sheet and dicing die bond film according to the present invention are not limited to the above-mentioned embodiment. The thermosetting sheet and dicing die bond film according to the present invention are not limited by the above-mentioned action and effect. The thermosetting sheet and dicing die bond film according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0098] The present invention will now be described in more detail with reference to examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.
[0099] [Example 1] A mixture containing each material in the mass ratio shown in the Example 1 section of Table 1 below was stirred and mixed in “stirring mode” using a hybrid mixer (manufactured by Keyence Corporation, product name: HM-500) to prepare a varnish. The stirring and mixing using the hybrid mixer was performed in three stages. Specifically, first, a primary mixture containing a thermosetting resin and a thermoplastic resin was stirred and mixed for 3 minutes (primary stirring), then, a secondary mixture obtained by adding conductive particles and a volatile material to the primary mixture was stirred and mixed for 6 minutes (secondary stirring), and further, a tertiary mixture obtained by adding a catalyst and a solvent to the secondary mixture was stirred and mixed for 3 minutes (tertiary stirring). This varnish was applied to one side of a release-treated film (manufactured by Mitsubishi Chemical Corporation, product name: MRA38, thickness 38 μm) and then dried at a temperature of 100° C. for 2 minutes to obtain a thermosetting sheet with a thickness of 30 μm. The materials used in the following Table 1 are as follows: Phenolic resin MEHC-7851S (biphenyl-type phenolic resin, phenol equivalent: 209 g / eq) manufactured by Meiwa Kasei Co., Ltd. Solid epoxy resin Nippon Steel & Sumikin Chemical's KI-3000-4 (cresol novolac type multifunctional epoxy resin, epoxy equivalent 200g / eq) Liquid epoxy resin Mitsubishi Chemical's YL980 (bisphenol A type epoxy resin, epoxy equivalent 180-190g / eq) ·Silver (Ag) coated copper (Cu) particles DOWA Electronics' product name: AOP-TCY-2(EN) (Spherical copper particles coated with 20% by mass of silver particles. The particle shape is spherical.) ·Silver (Ag) particles AG-2-8F manufactured by DOWA Electronics (silver particles surface-treated with a fatty acid-based coating agent. The particles are spherical.) · Volatile material (isobornylcyclohexanol (MTPH)) MTPH manufactured by Nippon Terpene Chemical Acrylic resin solution Nagase Chemitec's Teisan Resin SG-70L (contains MEK and toluene as solvents, solids content 12.5%, glass transition temperature -13°C, mass average molecular weight 900,000, acid value 5mg / KOH, carboxyl group-containing acrylic copolymer) Coupling Agent Shin-Etsu Chemical Co., Ltd.'s KBE-846 (bis(triethoxysilylpropyl)tetrasulfide) ·catalyst TPP-MK (Tetraphenylphosphonium tetra-p-tolylborate) manufactured by Hokko Chemical Industry Co., Ltd. ·solvent Methyl ethyl ketone (MEK) Table 2 below shows the mass ratio (parts by mass) of thermoplastic resin (acrylic resin, hereinafter also referred to as TMR) per 100 parts by mass of thermosetting resin (epoxy resin (solid and liquid) and phenolic resin, hereinafter also referred to as TSR), the mass ratio (parts by mass) of volatile material (isobornylcyclohexanol) per 100 parts by mass of thermosetting resin, and the mass ratio (parts by mass) of conductive particles per 100 parts by mass of thermosetting resin. Furthermore, the mass proportions of silver-coated copper particles and silver particles in 100 parts by mass of the conductive particles (silver-coated copper particles and silver particles) are shown in Table 3 below.
[0100] [Example 2] A thermosetting sheet according to Example 2 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 2 in Table 1 below was obtained.
[0101] [Example 3] A thermosetting sheet according to Example 3 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 3 in Table 1 below was obtained.
[0102] [Example 4] A thermosetting sheet according to Example 4 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 4 in Table 1 below was obtained.
[0103] [Example 5] A thermosetting sheet according to Example 5 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the section for Example 5 in Table 1 below was obtained.
[0104] [Comparative Example 1] A thermosetting sheet according to Comparative Example 1 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the column for Comparative Example 1 in Table 1 below was obtained.
[0105] [Comparative Example 2] A thermosetting sheet according to Comparative Example 2 was obtained in the same manner as in Example 1, except that a mixture containing each material in the mass ratio shown in the column for Comparative Example 2 in Table 1 below was obtained.
[0106] [Table 1]
[0107] [Table 2]
[0108] <Conductive particle filling rate> According to the following procedure, the particle packing ratio P of the conductive particles of the thermosetting sheet according to each example before curing was measured. 1 asked for. (1) The thermosetting sheet before curing is mechanically polished to expose the cross section, and the exposed cross section is subjected to ion polishing using an ion polishing device (manufactured by JEOL Ltd., product name: Cross Section Polisher SM-09010). (2) An SEM image (image taken by a scanning electron microscope) of an arbitrary cross-sectional area of the exposed cross-section that has been ion-polished is taken using a field emission scanning electron microscope SU8020 (manufactured by Hitachi High-Technologies Corporation), and a backscattered electron image is obtained as image data. The imaging conditions are an acceleration voltage of 5 kV and a magnification of 5000 times. (3) The obtained image data is subjected to automatic binarization processing using the image analysis software ImageJ to binarize the metal parts and the resin parts. (4) The total area of the metal parts and the total area (metal parts + resin parts) are calculated from the binarized image, and the total area of the metal parts is divided by the total area to obtain the particle packing ratio P of the conductive particles for the cured thermosetting sheet. 1 Request. The particle packing ratio P 1 was calculated by arithmetically averaging the particle packing ratios determined for five cross-sectional areas on the exposed cross-section that had been ion-polished. For the thermosetting sheets according to each example before curing, the particle filling rate P 1 The results are shown in Table 3 below. In addition, for the thermosetting sheets according to each example after curing, the particle packing ratio P 2 was determined in the same manner as above. For the thermosetting sheets according to each example after curing, the particle filling rate P 2 The results are shown in Table 3 below.
[0109] <Thermal conductivity of thermosetting sheets> The thermosetting sheet according to each example was heat-cured in a pressure cooker at 200° C. for 1 hour while applying a pressure of 0.5 MPa. The thermal conductivity of the heat-cured thermosetting sheet according to each example was calculated according to the following formula.
[0110]
number
[0111] Thermal diffusivity α(m 2 / s) was measured by the TWA method (temperature wave thermal analysis, measuring device: iPhase Mobile, manufactured by iPhase Corporation). Specific heat C pThe specific heat capacity (J / g·°C) was measured by the DSC method. Specific heat measurements were performed using a DSC6220 manufactured by SII Nanotechnology, Inc., at a heating rate of 10°C / min and in the temperature range of 20 to 300°C. Based on the data obtained, the specific heat was calculated using the method described in the JIS Handbook (specific heat capacity measurement method K-7123). The specific gravity was measured by the Archimedes method. The thermal conductivity of the cured thermosetting sheets of each example was calculated and the results are shown in Table 3 below.
[0112] <Joining rate> For each of the thermosetting sheets according to the examples, the bonding rate to the substrate was measured. When measuring the bonding rate, the thermosetting sheet of each example was cut into a 5 cm square, 10 of the 5 cm square thermosetting sheets were stacked together, and then pressed under vacuum (pressure of 3.3 kPa) to obtain a sheet laminate with a thickness of 300 μm. A bare chip diced into a 5 cm square was attached to one side of the sheet laminate to produce a sheet laminate with bare chips. The bonding rate to the substrate was measured according to the following procedure. (1) A sheet laminate having a bare chip attached to one surface thereof is attached to the other surface thereof on a die pad of a lead frame substrate (Cu lead frame substrate) to obtain a test specimen for evaluating a bonding rate. (2) Using an ultrasonic imaging device (manufactured by Hitachi Construction Machinery Finetech Co., Ltd., model: FineSAT FS200II, hereinafter also referred to as SAT), the test specimen for evaluating the bonding rate is imaged by a reflection method to obtain an SAT image. The imaging is performed by adjusting the gate so as to match the echo of the bonding portion between the thermosetting sheet and the test specimen displayed on the waveform monitor of the ultrasonic imaging device, setting the pixel to 1, the gain to 25 dB, and the Z-axis height to 11.34 mm. (3) Using image analysis software ImageJ, the obtained SAT image is subjected to automatic binarization processing to binarize the joint portion between the lead frame substrate and the sheet laminate (hereinafter also simply referred to as the joint portion) and the non-joint portion between the lead frame substrate and the sheet laminate (hereinafter also simply referred to as the non-joint portion). The threshold value is set to 82. (4) From the binarized image, the area of the bonded portions and the area of the non-bonded portions are calculated, and the area of the bonded portions is divided by the sum of the area of the bonded portions and the area of the non-bonded portions. Then, the resulting area is multiplied by the number 100 to calculate the bonding rate of the sheet laminate (the thermosetting sheet abutting against the lead frame substrate) to the lead frame substrate. In the binarized image, the joints are shown in black, and the non-joints are shown in white.
[0113] The bonding rate of the thermosetting sheet according to each example to the substrate (lead frame substrate) was measured, and the results are shown in Table 3 below.
[0114] <Rate of change in thickness Rc> For the thermosetting sheets according to each example, the rate of change in thickness Rc when the temperature was changed from 25° C. to 200° C. was determined as follows. Specifically, in thermomechanical analysis (TMA), the temperature was changed from 25°C to 200°C, and the thickness T1 of the thermosetting sheet at 25°C was measured, and the thickness T2 of the thermosetting sheet immediately after heating to 200°C was also measured. The thickness was calculated using the measured values T1 and T2 according to the following formula. Rc = (T2 - T1) / T1 × 100
[0115] The thermomechanical analysis was carried out under the following conditions. Thermomechanical analysis conditions Thermomechanical analyzer: TA Instruments Japan, model Q400 Probe: Macro expansion probe Measurement mode: compression / expansion Heating conditions: Heat from 25℃ to 200℃ in 60 minutes, hold at 200℃ for 1 hour, then cool to 25℃ in 30 minutes. Measurement atmosphere: Nitrogen (N 2 ) Load: 0.012N (constant load) Specimen: A first thermosetting sheet laminate, consisting of multiple thermosetting sheets, is pressed for 60 seconds at a temperature of 70°C and a pressure of 6kN to obtain a second thermosetting sheet laminate with a thickness of 3mm. This second thermosetting sheet laminate is then punched out with a 4mmφ punch to obtain a specimen with a thickness of 3mm x 4mmφ. The measurements using the thermomechanical analyzer were performed by placing the test specimen, which had an aluminum plate (circular in plan view, 0.1 mm thick, 5 mmφ plan dimension) on each side, on the stage of the thermomechanical analyzer so that one of the aluminum plates was in contact with the other aluminum plate (the upper aluminum plate) and then applying a load using the probe from the other aluminum plate side. In addition, Rc was calculated by taking the arithmetic average of the values obtained for two test pieces.
[0116] The thickness change rate Rc of each thermosetting sheet according to the examples was measured, and the results are shown in Table 3 below. FIG. 3 is a graph showing the change in thickness Rc over time as measured by thermomechanical analysis of the thermosetting sheets according to the respective examples.
[0117] [Table 3]
[0118] From Table 3, it can be seen that in the thermosetting sheets of each Example, the bonding rate JR1 before curing was high, at 85% or more, and the bonding rate JR2 after curing was high, at 85% or more, and the ratio of the bonding rate JR2 after curing to the bonding rate JR1 before curing was also high, at 90% or more. In contrast, in the thermosetting sheet of Comparative Example 1, the bonding rate JR1 before curing was high at 98.70%, but the bonding rate JR2 after curing was low at 76.8%, and it can also be seen that the ratio of the bonding rate JR2 after curing to the bonding rate JR1 before curing was also significantly reduced to 77.8%. In addition, in the thermosetting sheet of Comparative Example 2, the bonding rate JR1 before curing was high at 92.6%, but the bonding rate JR2 after curing was significantly low at 20.6%, and the ratio of the bonding rate JR2 after curing to the bonding rate JR1 before curing was also significantly low at 22.2%. Furthermore, examples of SAT images (taken using an ultrasonic imaging device) of the thermosetting sheet before and after curing are shown in Figure 4 (Example 5 and Comparative Example 2). For the thermosetting sheet of Example 5 (Figures 4(a) and (b)), no peeling was observed at all on the edge side after curing. In contrast, for the thermosetting sheet of Comparative Example 2 (FIGS. 4(c) and (d)), significant peeling was observed from the edges after curing, and only the center area was found to be bonded. Thus, it can be seen from the SAT images that there is a significant difference in peelability from an adherend between the thermosetting sheets according to the examples and the thermosetting sheets according to the comparative examples. Looking at the values of the rate of change in thickness Rc, the thermosetting sheet of Example 1 was 5.0%, the thermosetting sheet of Example 2 was 7.1%, the thermosetting sheet of Example 3 was 5.8%, the thermosetting sheet of Example 4 was 2.8%, and the thermosetting sheet of Example 5 was 4.5%, all of which were within the range of 0% or more and 10% or less. In contrast, the rates of change in thickness Rc of the thermosetting sheets of Comparative Examples 1 and 2 were -4.4% and -1.8%, respectively, which were outside the range of 0% or more and 10% or less. From these results, it can be seen that by making the thermosetting sheet contain a thermosetting resin and a thermoplastic resin, and further making the thickness change rate Rc in the range of 0% or more and 10% or less, the peeling of the thermosetting sheet from the adherend after thermal curing is relatively suppressed.
[0119] In addition, from Table 3, in the thermosetting sheets according to Examples 1 to 5, the particle packing ratio P 2It can be seen that by having a volume percentage of 50% or more, sufficient thermal conductivity exceeding 4 W / m K is obtained.
[0120] Furthermore, from FIGS. 3(a) and (b), it can be seen that in the thermosetting sheets according to Comparative Examples 1 and 2, the thickness change rate Rc continues to decrease, generally taking negative values, as the heating temperature increases. Furthermore, in the thermosetting sheets of Comparative Examples 1 and 2, the thickness change rate Rc tends to decrease further while the temperature is maintained at 200°C to further advance the thermosetting reaction, and it can be seen that during this temperature maintenance, the thermosetting sheet of Comparative Example 1 shows a minimum value of -6.7%, and the thermosetting sheet of Comparative Example 2 shows a minimum value of -5.6%. Furthermore, it can be seen that in the thermosetting sheets of Comparative Examples 1 and 2, the rate of change in thickness Rc becomes even larger negative values (a minimum of -7.9% in the thermosetting sheet of Comparative Example 1, and a minimum of -7.3% in the thermosetting sheet of Comparative Example 2) due to the volumetric shrinkage of the resin component caused by cooling after maintaining the temperature at 200°C.
[0121] In contrast, looking at Figures 3(a) and (b), in the thermosetting sheets according to Examples 1 to 5, the rate of change in thickness Rc tends to increase with increasing heating temperature, all of which show generally positive values (more specifically, in the thermosetting sheet according to Example 1, the rate of change in thickness Rc shows positive values from 50°C or higher, in the thermosetting sheets according to Examples 2 and 4, the rate of change in thickness Rc shows positive values immediately after heating, and in the thermosetting sheets according to Examples 3 and 5, the rate of change in thickness Rc shows positive values from 30°C or higher), and shows maximum values in the temperature range of 100°C or higher and 200°C or lower (a maximum of 3.9% in the thermosetting sheet according to Example 1, a maximum of 8% in the thermosetting sheet according to Example 2, a maximum of 5.8% in the thermosetting sheet according to Example 3, a maximum of 3% in the thermosetting sheet according to Example 4, and a maximum of 4.5% in the thermosetting sheet according to Example 5). Furthermore, in the thermosetting sheets of Examples 1 to 3, the thickness change rate Rc tends to decrease while the temperature is maintained at 200°C to further advance the thermosetting reaction, but it can be seen that all of them continue to show positive values. Furthermore, in the thermosetting sheets of Examples 1 and 2, the rate of change in thickness Rc becomes even smaller due to the volumetric shrinkage of the resin component upon cooling after maintaining the temperature at 200°C, but still remains a positive value, whereas in the thermosetting sheet of Example 3, the rate of change in thickness Rc becomes negative (minimum -2.3%) upon cooling after maintaining the temperature at 200°C, but still remains a higher value than the rates of change in thickness Rc of the thermosetting sheets of Comparative Examples 1 and 2. Furthermore, in the thermosetting sheets of Examples 4 and 5, the thickness change rate Rc tends to decrease to a negative value while the temperature is maintained at 200°C in order to further advance the thermosetting reaction, and furthermore, it becomes a smaller negative value upon cooling after maintaining the temperature at 200°C (a minimum of -5.3% in the thermosetting sheet of Example 4 and a minimum of -4.9% in the thermosetting sheet of Example 5), but it can be seen that it shows a higher value than the thickness change rate Rc of the thermosetting sheets of Comparative Examples 1 and 2.
[0122] Taking the above results into consideration, it can be seen that it is preferable for the thermosetting sheet of this embodiment to have a thickness change rate Rc of greater than 0% (a positive value) within the temperature range of 50°C or higher and 200°C or lower when the temperature is changed from 25°C to 200°C. Furthermore, in the case of the thermosetting sheet according to this embodiment, it is understood that when the temperature is changed from 25°C to 200°C, it is preferable that the maximum value is shown in the temperature range of 100°C or more and 200°C or less, and that the maximum value is preferably 3% or more. In addition, since solid epoxy resins usually begin to soften at 80 to 100°C, when the thermosetting sheet exhibits a positive thickness change rate Rc at temperatures of 80 to 100°C as described above, the thermosetting reaction proceeds in a state in which the thermosetting sheet has improved adhesion to the adherend, and therefore the adhesion to the adherend is further improved; in other words, it is believed that peeling from the adherend after thermal curing is further suppressed. [Explanation of symbols]
[0123] 1 Base material layer 2 Adhesive layer 3 Thermosetting Sheet 10 Dicing tape 20 Dicing die bond film 30 Semiconductor Devices 31 Lead frame substrate 32 Semiconductor elements 33 Wire 34 Packages 35 Molding resin 40 Wiring board 41 electrode 31a Die pad 31b Lead section.
Claims
1. A thermosetting sheet containing a thermosetting resin and a thermoplastic resin, the thermosetting sheet being adhered to a substrate having a mounting area for a semiconductor element, The thermosetting resin includes an epoxy resin and a phenolic resin, and the thermoplastic resin includes an acrylic resin; The thermoplastic resin is contained in an amount of 60 parts by mass or more and 500 parts by mass or less relative to 100 parts by mass of the thermosetting resin, The rate of change in thickness when the temperature is changed from 25°C to 200°C is 0% or more and 10% or less. Thermosetting sheet.
2. Further containing conductive particles The thermosetting sheet according to claim 1 .
3. Contains additional volatile components The thermosetting sheet according to claim 2 .
4. The volatile component is contained in an amount of 10 parts by mass or more and 300 parts by mass or less per 100 parts by mass of the thermosetting resin. The thermosetting sheet according to claim 3 .
5. Base layer and a dicing tape having a pressure-sensitive adhesive layer laminated on the base layer; a thermosetting sheet laminated on the adhesive layer of the dicing tape; The thermosetting sheet is the thermosetting sheet according to any one of claims 1 to 4. Dicing die bond film.
Citation Information
Patent Citations
Adhesive for semiconductor device
JP2004018720A
Resin composition and semiconductor device
JP2010084008A
Rear-surface film for flip-chip semiconductor, dicing tape integrated rear-surface film for semiconductor, manufacturing method of semiconductor device, and flip-chip semiconductor device
JP2011228499A
Thermosetting resin composition and method for manufacturing semiconductor device
JP2014210880A
Resin composition for die attachment
JP2015012069A