Method for producing phosphor particles

By using LiF as a flux and employing specific processing steps, the method addresses the issue of foreign phases in phosphor particle production, resulting in improved internal quantum efficiency and luminous efficiency for phosphor particles.

JP7577660B2Active Publication Date: 2024-11-05DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021533942
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-22
Filing Date
2020-07-10
Publication Date
2024-11-05
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Existing methods for producing phosphor particles, such as those described in Patent Document 1, suffer from degraded internal quantum efficiency due to foreign phases generated during the manufacturing process.

Method used

A method involving the selection of LiF as a flux, followed by a series of processing steps including mixing, firing, pulverizing, acid treatment, hydrofluoric acid treatment, and heat treatment, to produce phosphor particles with improved internal quantum efficiency by removing foreign phases and enhancing optical properties.

Benefits of technology

The method results in phosphor particles with enhanced internal quantum efficiency, improved emission characteristics, and increased luminous efficiency, suitable for use in LEDs and other light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577660000001
    Figure 0007577660000001
Patent Text Reader

Abstract

This method is for producing fluorescent particles having a composition comprising a group consisting of N, Al, at least one element M1 selected from the group consisting of Sr, Mg, Ca, and Ba, at least one element M2 selected from the group consisting of Li and Na, and at least one element M3 selected from the group consisting of Eu and Ce, the method comprising: a mixing step for obtaining a mixture by mixing LiF and a raw material mixture containing the respective elements constituting said composition; a sintering step for sintering the mixture; a grinding step for obtaining a ground product by grinding the mixture; an acid treatment step for performing an acid treatment on the ground product by using a liquid mixture containing an acid and an alcohol; a fluoric acid treatment step for performing a fluoric acid treatment on the ground product; and a heating step for heating the ground product in the atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing phosphor particles. [Background technology]

[0002] Various developments have been made on phosphors up to now. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a method for producing SrLiAl3N4:Eu (SLAN phosphor) (see claim 1, paragraph 0113, etc. of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2013 / 175336 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations conducted by the present inventors, it was found that the method for producing phosphor particles described in Patent Document 1 above leaves room for improvement in terms of internal quantum efficiency. [Means for solving the problem]

[0005] The present inventors have conducted research and found that a different phase that occurs during the manufacturing process of phosphor particles can cause a decrease in the luminescence characteristics of the phosphor, such as the internal quantum efficiency. Based on this knowledge, the inventors conducted further intensive research and discovered that by appropriately selecting the type of flux to be mixed into the raw material mixture of the phosphor particles and performing acid treatment using a mixed liquid containing an acid and an alcohol during the manufacturing process, phosphor particles with excellent internal quantum efficiency can be realized, which led to the completion of the present invention.

[0006] Although the detailed mechanism is unclear, it is believed that LiF functions as an appropriate flux, promoting grain growth and improving the optical properties of the phosphor particles, and that the acid treatment makes it possible to remove foreign phases that occur when LiF is used.

[0007] On the other hand, when SrF2 is used as the flux, the amount of foreign phase remaining after the reaction is greater than that of LiF, and even if acid treatment is performed, it becomes difficult to remove the foreign phase, resulting in a decrease in the internal quantum efficiency.

[0008] According to the present invention, At least one element M selected from the group consisting of Sr, Mg, Ca and Ba 1 At least one element M selected from the group consisting of Li, Na, and 2 At least one element M selected from the group consisting of Eu and Ce 3 , Al, and N A method for producing phosphor particles having the following structure: a mixing step of mixing a raw material mixture containing each element constituting the composition with LiF to obtain a mixture; A calcination step of calcining the mixture; A grinding step of grinding the mixture after the firing step to obtain a ground product; an acid treatment step of subjecting the pulverized material to an acid treatment using a mixed liquid containing an acid and an alcohol; a hydrofluoric acid treatment step of subjecting the pulverized material after the acid treatment step to a hydrofluoric acid treatment; a heat treatment step of heating the pulverized material after the hydrofluoric acid treatment step in the atmosphere; A method for producing phosphor particles having the following structure is provided. Effect of the Invention

[0009] According to the present invention, there is provided a method for producing phosphor particles having excellent internal quantum efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] A method for producing phosphor particles according to this embodiment will be described.

[0011] The method for producing phosphor particles includes the steps of: adding at least one element M selected from the group consisting of Sr, Mg, Ca, and Ba; 1 At least one element M selected from the group consisting of Li and Na 2 At least one element M selected from the group consisting of Eu and Ce 3 The present invention relates to the manufacture of phosphor particles having a composition including the group consisting of Al and N.

[0012] The method for producing phosphor particles can include a mixing step, a firing step, a pulverizing step, an acid treatment step, a hydrofluoric acid treatment step, and a heat treatment step. Each step will be described in detail.

[0013] (Mixing process) In the mixing step, a raw material mixture containing each element constituting the composition of the phosphor is mixed with LiF as a flux to obtain a mixture. For example, each raw material may be weighed so as to obtain the desired phosphor particles and mixed to obtain a powdery mixture.

[0014] The method for mixing the raw materials is not particularly limited, but examples include a method in which the raw materials are thoroughly mixed using a mixing device such as a mortar, a ball mill, a V-type mixer, or a planetary mill. Strontium nitride, lithium nitride, and the like, which react violently with moisture and oxygen in the air, should be handled appropriately in a glove box whose interior is replaced with an inert atmosphere, or using a mixing device.

[0015] In the mixing process, when the molar ratio of Al is 3, M 1 The amount of M is preferably 1.10 or more in terms of molar ratio. 1 By setting the molar ratio of M to 1.10 or more, 1 The M in the phosphor is removed by volatilization, etc. 1 The shortage of M 1This makes it difficult for defects to occur in the crystals, and maintains good crystallinity. As a result, it is assumed that a narrow band fluorescence spectrum can be obtained and the emission intensity can be increased. In addition, in the mixing process, when the molar ratio of Al is 3, 1 The amount of M charged is preferably 1.20 or less in terms of molar ratio. 1 By setting the molar ratio of M to 1.20 or less, 1 The increase of the heterogeneous phase including ZnO is suppressed, and the heterogeneous phase is easily removed by the acid treatment step, so that the luminescence intensity can be increased.

[0016] Each raw material used in the mixing step may contain at least one selected from the group consisting of simple metals of the metal elements contained in the composition of the phosphor and metal compounds containing the metal elements. Examples of the metal compounds include nitrides, hydrides, fluorides, oxides, carbonates, chlorides, etc. Among these, from the viewpoint of improving the luminous intensity of the phosphor, M 1 and M. 2 As the metal compound containing M, a nitride is preferably used. 1 Examples of metal compounds containing M include Sr3N2, SrN2, and SrN. 2 Examples of metal compounds containing Li3N and LiN3 include M 3 Examples of metal compounds containing Eu include Eu2O3, EuN, and EuF3. Examples of metal compounds containing Al include AlN, AlH3, AlF3, and LiAlH4.

[0017] In the mixing step, the lower limit of the amount of LiF added is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 4% by mass or more, based on 100% by mass of the total of LiF and the raw material mixture. This allows phosphor particles with excellent internal quantum efficiency to be realized. On the other hand, the upper limit of the amount of LiF added may be, for example, 10% by mass or less, preferably 5% by mass or less, based on 100% by mass of the total of LiF and the raw material mixture. As the flux, LiF may be used alone, or may be used in combination with other fluxes. The content of LiF in the flux used in the mixing step is, for example, 50 mass % or more, preferably 80 mass % or more, and more preferably 100 mass %.

[0018] (Firing process) In the firing step, the mixture is fired. For example, the mixture may be fired while being filled in a firing vessel.

[0019] The firing container preferably has a structure that can enhance airtightness. The firing container is preferably made of a material that is stable under a high-temperature atmospheric gas and does not easily react with the mixture of raw materials and its reaction products. For example, it is preferable to use a container made of boron nitride or carbon, or a container made of a high-melting point metal such as molybdenum, tantalum, or tungsten.

[0020] The inside of the firing vessel is preferably filled with an atmospheric gas of a non-oxidizing gas such as argon, helium, hydrogen, or nitrogen.

[0021] [Firing temperature] The lower limit of the firing temperature in the firing step is preferably 900° C. or higher, more preferably 1000° C. or higher, and even more preferably 1100° C. or higher. On the other hand, the upper limit of the firing temperature is preferably 1500° C. or lower, more preferably 1400° C. or lower, and even more preferably 1300° C. or lower. By setting the firing temperature within the above range, it is possible to reduce the amount of unreacted raw materials after the firing step is completed, and also to suppress decomposition of the main crystal phase.

[0022] [Type of firing atmosphere gas] As the type of the firing atmosphere gas in the firing step, for example, a gas containing nitrogen as an element can be preferably used. Specifically, nitrogen and / or ammonia can be mentioned, and nitrogen is particularly preferable. Similarly, inert gases such as argon and helium can also be preferably used. The firing atmosphere gas may be composed of one type of gas or may be a mixed gas of multiple types of gases.

[0023] [Firing atmosphere gas pressure] The pressure of the firing atmosphere gas is selected according to the firing temperature, but is usually in a pressurized state in the range of 0.1 MPa·G to 10 MPa·G. The higher the firing atmosphere gas pressure, the higher the decomposition temperature of the phosphor, but considering industrial productivity, it is preferable to keep the pressure in the range of 0.5 MPa·G to 1 MPa·G.

[0024] [Baking time] The firing time in the firing step is selected within a time range that does not cause problems such as the presence of a large amount of unreacted material, insufficient growth of phosphor particles, or reduced productivity. The lower limit of the firing time is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 2 hours or more. The upper limit of the firing time is preferably 48 hours or less, more preferably 36 hours or less, and even more preferably 24 hours or less.

[0025] (Crushing process) In the pulverization step, the raw material mixture (calcined product) after the calcination step is pulverized to obtain a pulverized product.

[0026] The state of the fired product obtained from the firing process varies depending on the raw material composition and firing conditions, from powder to lumps. The fired product can be made into powder of a specified size by the crushing / grinding process and / or classification process.

[0027] In the above-mentioned crushing and pulverizing step, in order to prevent the inclusion of impurities resulting from the process, it is preferable that the components of the equipment that come into contact with the fired product are made of ceramics such as silicon nitride, alumina, and sialon.

[0028] The average particle size of the pulverized material may be adjusted so that the average particle size of the phosphor particles is 5 μm or more and 30 μm or less. This makes the phosphor particles excellent in excitation light absorption efficiency and light emission efficiency, and therefore suitable for use in LEDs, etc.

[0029] (Acid treatment process) In the acid treatment step, the pulverized material is treated with an acid mixture containing an acid and an alcohol. The acid treatment may be carried out by adding the ground material to a mixed solution containing an acid and an alcohol, or by adding an acid to the ground material in the alcohol. During the acid treatment, the mixed solution may be left to stand, or may be stirred under appropriate conditions. After the acid treatment, decantation (solid-liquid separation) may be carried out using alcohol, if necessary. Decantation may be carried out once or twice or more. This allows the acid to be washed and removed from the pulverized material. Thereafter, the ground product is filtered and dried.

[0030] The acid may be, for example, an inorganic acid, specifically, nitric acid, hydrochloric acid, acetic acid, sulfuric acid, formic acid, phosphoric acid, etc. Among inorganic acids, it is preferable to include at least one of nitric acid and hydrochloric acid. These may be used alone or in combination of two or more kinds.

[0031] The mixture may include a water solvent.

[0032] As the alcohol, for example, an aliphatic alcohol, specifically, MeOH, EtOH, IPA, etc., is used.

[0033] The alcohol and the acid may be mixed so that the concentration of the acid in the mixed solution is, for example, 0.1% by mass to 5% by mass, and preferably 0.5% by mass to 3% by mass.

[0034] The acid treatment can dissolve and remove impurity elements contained in the raw materials, impurity elements originating from the firing vessel, foreign phases generated during the firing process, and impurity elements mixed in during the pulverization process. In other words, the acid treatment can wash away foreign matter, etc. This can improve the internal quantum efficiency of the phosphor.

[0035] As an example of the acid treatment, the pulverized material may be dispersed and immersed in a mixed liquid containing an acid and an alcohol for, for example, about 0.5 to 5 hours.

[0036] (Hydrofluoric acid treatment process) In the hydrofluoric acid treatment, the pulverized material after the acid treatment step is subjected to hydrofluoric acid treatment.

[0037] For the hydrofluoric acid treatment, an aqueous solution containing hydrogen fluoride as a compound containing elemental fluorine, that is, so-called hydrofluoric acid, is preferably used. The hydrofluoric acid treatment may be carried out by adding the pulverized material to hydrofluoric acid, for example. The lower limit of the concentration of hydrogen fluoride (HF) in hydrofluoric acid is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. On the other hand, the upper limit of the concentration of hydrogen fluoride in hydrofluoric acid is preferably 40% by mass or less, more preferably 38% by mass or less, and even more preferably 35% by mass or less. By setting the hydrogen fluoride concentration to the above lower limit or more, a coating containing (NH4)3AlF6 can be formed on at least a part of the outermost surface of the phosphor-containing particle. On the other hand, by setting the hydrogen fluoride concentration to the above upper limit or less, the reaction between the particle and hydrofluoric acid can be prevented from becoming too vigorous.

[0038] The pulverized material and hydrofluoric acid can be mixed by a stirring means such as a stirrer. The lower limit of the mixing time of the pulverized material and hydrofluoric acid is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 15 minutes or more, while the upper limit of the mixing time of the sintered material and hydrofluoric acid is preferably 30 minutes or less, more preferably 25 minutes or less, and even more preferably 20 minutes or less. By setting the mixing time of the pulverized material and hydrofluoric acid within the above range, a coating portion containing (NH4)3AlF6 can be stably formed on at least a part of the outermost surface of the particle containing the phosphor.

[0039] In this embodiment, by appropriately adjusting the types of acid and solvent in the acid treatment step, the acid concentration, the hydrofluoric acid concentration in the hydrofluoric acid treatment step, the hydrofluoric acid treatment time, the heating temperature and heating time in the heat treatment step performed after the hydrofluoric acid treatment, etc., a coating portion that covers the surface of the particles containing the phosphor can be formed.

[0040] (Heat treatment process) In the heat treatment, the pulverized material after the hydrofluoric acid treatment is heated in the atmosphere.

[0041] When the resultant product obtained by the hydrofluoric acid treatment contains (NH4)3AlF6 as a coating portion, a heat treatment process can be carried out to change a part or all of the (NH4)3AlF6 to AlF3.

[0042] The lower limit of the heating temperature in the heat treatment step is preferably 220° C. or higher, more preferably 250° C. or higher, while the upper limit of the heating temperature is preferably 380° C. or lower, more preferably 350° C. or lower, and even more preferably 330° C. or lower.

[0043] By setting the heating temperature to the above lower limit or higher, the following reaction formula (1) proceeds, whereby (NH4)3AlF6 can be converted to AlF3. (NH4)3AlF6→AlF3+3NH3+3HF...(1)

[0044] On the other hand, by setting the heating temperature to the above upper limit or less, the crystal structure of the phosphor can be well maintained and the emission intensity can be increased.

[0045] The lower limit of the heating time is preferably 1 hour or more, more preferably 1.5 hours or more, and even more preferably 2 hours or more. On the other hand, the upper limit of the heating time is preferably 6 hours or less, more preferably 5.5 hours or less, and even more preferably 5 hours or less. By setting the heating time within the above range, (NH4)3AlF6 can be reliably converted into AlF3, which has higher moisture resistance.

[0046] The heat treatment step is preferably carried out in air or a nitrogen atmosphere, so that the substance in the heating atmosphere itself does not inhibit the above reaction formula (1) and the target substance can be produced.

[0047] The phosphor particles of this embodiment will be described.

[0048] The phosphor particles of this embodiment may be composed of surface-coated phosphor particles that include a particle containing a phosphor and a coating portion that coats the surface of the particle.

[0049] The phosphor contained in the phosphor particles has the general formula M 1 a M 2 b M 3 c Al3N 4-d O d In the general formula, M 1 is one or more elements selected from Sr, Mg, Ca and Ba, M 2 is one or more elements selected from Li and Na, and M 3 is one or more elements selected from Eu and Ce. In the general formula, a, b, c, 4-d, and d represent the molar ratios of each element.

[0050] In the general formula, a, b, c, and d satisfy the following formulas. 0.850≦a≦1.150 0.850≦b≦1.150 0.001≦c≦0.015 0≦d≦0.40 0≦d / (a+d)<0.30

[0051] M 1 is one or more elements selected from Sr, Mg, Ca and Ba, and preferably contains at least Sr. 1 The lower limit of the molar ratio a is preferably 0.850 or more, more preferably 0.950 or more. 1 The upper limit of the molar ratio a is preferably 1.150 or less, more preferably 1.100 or less, and even more preferably 1.050 or less. 1 By setting the molar ratio a within the above range, the stability of the crystal structure can be improved.

[0052] M 2 is one or more elements selected from Li and Na, and preferably contains at least Li. 2 The lower limit of the molar ratio b of M is preferably 0.850 or more, more preferably 0.950 or more. 2 The upper limit of the molar ratio b is preferably 1.150 or less, more preferably 1.100 or less, and even more preferably 1.050 or less.2 By setting the molar ratio a within the above range, the stability of the crystal structure can be improved.

[0053] M 3 is an activator added to the host crystal, i.e., an element constituting the luminescent center ion of the phosphor, and is one or more elements selected from Eu and Ce. 3 can be selected depending on the desired emission wavelength, and preferably contains at least Eu. M 3 The lower limit of the molar ratio c of M is preferably 0.001 or more, more preferably 0.005 or more. 3 The upper limit of the molar ratio c is preferably 0.015 or less, more preferably 0.010 or less. 3 By setting the lower limit of the molar ratio c in the above range, sufficient emission intensity can be obtained. 3 By setting the upper limit of the molar ratio c within the above range, concentration quenching can be suppressed and the luminescence intensity can be maintained at a sufficient value.

[0054] The lower limit of the molar ratio d of oxygen (O) is preferably 0 or more, and more preferably 0.05 or more. On the other hand, the upper limit of the molar ratio d of oxygen is preferably 0.40 or less, and more preferably 0.35 or less. By setting the molar ratio d of oxygen in the above range, the crystal state of the phosphor can be stabilized and the emission intensity can be maintained at a sufficient value. The content of oxygen element in the phosphor is preferably less than 2 mass%, more preferably 1.8 mass% or less. By keeping the content of oxygen element less than 2 mass%, the crystal state of the phosphor can be stabilized and the emission intensity can be maintained at a sufficient value.

[0055] M 1 The lower limit of the value of d / (a+d) calculated from the molar ratio of a and oxygen, i.e., a and d, is preferably 0 or more, and more preferably 0.05 or more. On the other hand, the upper limit of the value of d / (a+d) is preferably less than 0.30, and more preferably 0.25 or less. By setting d / (a+d) in the above range, the crystal state of the phosphor can be stabilized, and the emission intensity can be maintained at a sufficient value.

[0056] The coating portion constitutes at least a part of the outermost surface of the particle containing the phosphor. The coating portion contains a fluorine-containing compound that contains elemental fluorine and elemental aluminum.

[0057] In the fluorine-containing compound, it is preferable that the fluorine element and the aluminum element are directly covalently bonded, and more specifically, it is preferable that the fluorine-containing compound contains either one or both of (NH4)3AlF6 and AlF3. Note that the fluorine-containing compound may be composed of a single compound containing the fluorine element and the aluminum element.

[0058] The coating portion containing a fluorine-containing compound constitutes at least a part of the outermost surface of the phosphor-containing particle, so that the moisture resistance of the phosphor constituting the particle can be improved. From the viewpoint of further improving the moisture resistance of the phosphor, it is more preferable that the coating portion contains AlF3.

[0059] The form of the coating part is not particularly limited. For example, the coating part may be a form in which a large number of particulate fluorine-containing compounds are distributed on the surface of the particle containing the phosphor, or a form in which the fluorine-containing compound continuously coats the surface of the particle containing the phosphor. The coating part may be configured to cover a part or the whole of the particle surface.

[0060] The characteristics of the phosphor particles will be described below.

[0061] The phosphor particles have a diffuse reflectance with respect to light irradiation with a wavelength of 300 nm of, for example, 56% or more, preferably 65% ​​or more, and more preferably 70% or more. Furthermore, the phosphor particles have a diffuse reflectance with respect to light irradiation at the peak wavelength of the fluorescence spectrum of, for example, 80% or more, preferably 83% or more, and more preferably 85% or more. By providing such a diffuse reflectance, the luminous efficiency is further increased, and the luminous intensity is improved.

[0062] When excited with blue light having a wavelength of 455 nm, the phosphor particles may be configured so that the peak wavelength is, for example, in the range of 640 nm to 670 nm, and the half width is, for example, in the range of 45 nm to 60 nm. By providing such characteristics, excellent color rendering properties and color reproducibility can be expected.

[0063] When excited with blue light having a wavelength of 455 nm, the phosphor particles may be configured so that the x value in the CIE-xy chromaticity diagram satisfies, for example, 0.680≦x<0.735. With these characteristics, excellent color rendering and color reproducibility can be expected. If the x value is 0.680 or more, red light emission with good color purity can be expected, and if the x value is 0.735 or more, it exceeds the maximum value in the CIE-xy chromaticity diagram, so it is preferable to satisfy the above range.

[0064] The light emitting device according to this embodiment will be described below. The light emitting device according to this embodiment includes phosphor particles and a light emitting element.

[0065] The light-emitting element may be an ultraviolet LED, a blue LED, a fluorescent lamp, or a combination of these. The light-emitting element is preferably one that emits light with a wavelength of 250 nm or more and 550 nm or less, and among these, a blue LED light-emitting element with a wavelength of 420 nm or more and 500 nm or less is preferable.

[0066] As the phosphor particles, in addition to the phosphor particles, phosphor particles emitting other luminescent colors may be used in combination. Phosphor particles of other luminescent colors include blue-emitting phosphor particles, green-emitting phosphor particles, yellow-emitting phosphor particles, orange-emitting phosphor particles, and red phosphors, for example, Ca3Sc2Si3O 12 :Ce, CaSc2O4:Ce, β-SiAlON:Eu, Y3Al5O 12 : Ce, Tb3Al5O 12 :Ce, (Sr, Ca, Ba)2SiO4:Eu, La3Si6N 11 :Ce, α-SiAlON:Eu, Sr2Si5N8:Eu, etc.

[0067] The other phosphor particles are not particularly limited and can be appropriately selected depending on the brightness, color rendering, etc. required for the light emitting device. By mixing the phosphor particles with phosphor particles of other luminescent colors, it is possible to realize white light of various color temperatures, such as daylight white and warm white.

[0068] Specific examples of the light-emitting device include a lighting device, a backlight device, an image display device, and a signal device.

[0069] By including phosphor particles, the light emitting device can achieve high luminous intensity and high reliability.

[0070] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0071] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the description of these examples.

[0072] <Preparation of phosphor particles> Comparative Example 1 [Mixing process] AlN (Tokuyama Corp.), Eu2O3 (Shin-Etsu Chemical Co., Ltd.), and LiF (Wako Pure Chemical Industries, Ltd.) were weighed and mixed in air, and the agglomerates were broken down using a nylon sieve with 150 μm openings to obtain a pre-mixture. The premix was moved into a glove box that maintained a nitrogen atmosphere with moisture of 1 ppm or less and oxygen of 1 ppm or less. Sr3N2 (manufactured by Taiheiyo Cement Corporation) and Li3N (manufactured by Materion Corporation) were then weighed out and added so that the stoichiometric ratio (a=1, b=1) was such that the value of a was 15% in excess and the value of b was 20% in excess, and then mixed. The phosphor raw material mixture was obtained by breaking down the agglomerates using a nylon sieve with 150 μm openings. Sr and Li are easily dispersed during firing, so they were mixed in larger amounts than the theoretical values. Here, the amount of Sr charged was 1.15 in molar ratio when the molar ratio of Al was 3, and the amount of Eu charged was 0.01 in molar ratio. 5 mass% of LiF was added as a flux to the total amount of the raw material mixture and flux, which was 100 mass%. As described above, the amount of Eu charged was 0.01 in molar ratio when the molar ratio of Al was 3.

[0073] [Firing process] Next, the raw material mixture was filled into a cylindrical BN container with a lid (manufactured by Denka Co., Ltd.). Next, the container filled with the mixture of phosphor raw materials was taken out of the glove box, and then placed in an electric furnace (manufactured by Fuji Dempa Kogyo Co., Ltd.) equipped with a graphite heat insulator and a carbon heater, where the firing step was carried out. At the start of the firing process, the electric furnace was degassed to a vacuum state, and then firing was started from room temperature under a pressurized nitrogen atmosphere of 0.8 MPa·G. After the temperature inside the electric furnace reached 1100°C, firing was continued for 8 hours while maintaining that temperature, and then the material was cooled to room temperature.

[0074] [Crushing process] The obtained fired product was pulverized in a mortar and then classified using a nylon sieve with 75 μm openings, to obtain a phosphor powder of Comparative Example 1.

[0075] Example 1 5 g of phosphor powder obtained in the same manner as in Comparative Example 1 was added to a mixed solution of 500 ml of MeOH (purity 99%) (manufactured by Kokusan Chemical Co., Ltd.) and 10 ml of nitric acid (HNO3 concentration 60%) (manufactured by Wako Pure Chemical Industries, Ltd.), and the mixture was stirred for 3 hours. The mixture was then neutralized by decantation with MeOH, filtered, and dried to obtain phosphor powder. [Hydrofluoric acid treatment process] The obtained phosphor powder was added to hydrofluoric acid with a hydrogen fluoride concentration of 30% and stirred for 15 minutes to carry out a hydrofluoric acid treatment process. After the hydrofluoric acid treatment process, the powder was passed through a sieve with 45 μm openings to break up agglomerates. [Heat treatment] The phosphor powder from which the agglomerations had been deflocculated was subjected to a heat treatment at 300° C. for 4 hours in an air atmosphere, thereby obtaining the phosphor powder of Example 1.

[0076] Example 2 The phosphor powder of Example 2 was obtained using the same amounts of raw materials and following the same procedures as in Example 1, except that the phosphor powder obtained in the same manner as in Comparative Example 1 was added to a mixed solution of EtOH and nitric acid (HNO3 concentration 60%) (manufactured by Wako Pure Chemical Industries, Ltd.) and stirred for 3 hours.

[0077] Example 3 The phosphor powder of Example 3 was obtained using the same amounts of raw materials and following the same procedures as in Example 1, except that the phosphor powder obtained in the same manner as in Comparative Example 1 was added to a mixed solution of IPA and nitric acid (HNO3 concentration 60%) (manufactured by Wako Pure Chemical Industries, Ltd.) and stirred for 3 hours.

[0078] Comparative Example 2 A phosphor powder of Comparative Example 2 was obtained using the same amounts of raw materials and in the same procedure as in Example 1, except that SrF2 was used as the flux instead of LiF.

[0079] The crystal phases of the phosphor powders obtained in Examples 1 to 3 and Comparative Example 1 were examined by powder X-ray diffraction measurement (XRD measurement) using Cu-Kα radiation. a Li b EU c Al3N 4-d O d It was confirmed that the phosphor had the composition represented by the formula:

[0080] The obtained phosphor particles were a Li b EU c Al3N 4-d O d The subscripts a to d of each element were obtained. Specifically, the subscripts a to d were calculated using the analysis results of Sr, Li, Al, and Eu using an ICP optical emission spectrometer (SPECTRO, CIROS-120) and O and N using an oxygen / nitrogen analyzer (HORIBA, EMGA-920). Table 1 shows the numerical values ​​a to d of each phosphor particle.

[0081] [Table 1]

[0082] The obtained phosphor particles were evaluated based on the following evaluation items.

[0083] (Internal quantum efficiency, peak wavelength, half-width, chromaticity x) A standard reflector (Spectralon, manufactured by Labsphere) with a reflectance of 99% was set at the side opening (φ10 mm) of an integrating sphere (φ60 mm). Monochromatic light, which was split into 455 nm wavelengths from a Xe lamp as a light source, was introduced into this integrating sphere through an optical fiber, and the spectrum of the reflected light was measured with a spectrophotometer (MCPD-7000, manufactured by Otsuka Electronics). At that time, the number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 to 465 nm. Next, a concave cell filled with phosphor so that the surface was smooth was set at the opening of the integrating sphere, and monochromatic light with a wavelength of 455 nm was irradiated, and the spectrum of the reflected light and fluorescence of the excitation was measured with a spectrophotometer. The number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) were calculated from the obtained spectral data. The number of excitation reflected light photons was calculated in the same wavelength range as the number of excitation light photons, and the number of fluorescence photons was calculated in the range of 465 to 800 nm. The internal quantum efficiency was calculated from the obtained numbers of the three types of photons: Qem / (Qex-Qref) x 100. From the fluorescence spectrum obtained by this measurement, the peak wavelength, half width, and chromaticity x value were obtained. The chromaticity was calculated according to JIS Z 8724 (Method of measuring color - Light source color) and the chromaticity coordinates (x, y) were calculated by the calculation method in the XYZ color system specified in JIS Z 8701. The wavelength range used for calculating the chromaticity coordinates was 550 to 780 nm.

[0084] (Absorption rate at 700 nm) The same measurements were performed as above, except that monochromatic light with a wavelength of 700 nm was used as the light source from a Xe lamp. For the reflection spectra of the standard reflector and the phosphor, Qex and Qref were calculated from the spectra in the wavelength range of 695 to 710 nm, respectively, and the absorptance = (Qex-Qref) / Qex x 100 was calculated.

[0085] (Diffuse reflectance) The diffuse reflectance was measured using an integrating sphere (ISV-469) attached to a UV-Vis spectrophotometer (JASCO Corporation, V-550). Baseline correction was performed using a standard reflector (Spectralon), and a solid sample holder filled with the obtained phosphor particles was attached to measure the diffuse reflectance for light at 300 nm and the peak wavelength.

[0086] The results showed that the powdered phosphor particles of Examples 1 to 3 had improved internal quantum efficiency compared to Comparative Examples 1 and 2.

[0087] This application claims priority based on Japanese Patent Application No. 2019-134712, filed on July 22, 2019, the disclosure of which is incorporated herein in its entirety.

Claims

1. At least one element M selected from the group consisting of Sr, Mg, Ca and Ba 1 At least one element M selected from the group consisting of Li, Na, and 2 At least one element M selected from the group consisting of Eu and Ce 3 , Al, and N A method for producing phosphor particles having the following structure: The phosphor contained in the phosphor particles has a composition represented by the general formula M 1 a M 2 b M 3 c Al 3 N 4-d O d (wherein M 1 is one or more elements selected from Sr, Mg, Ca, and Ba, M 2 is one or more elements selected from Li and Na, and M 3 is one or more elements selected from Eu and Ce), and the a, b, c, and d satisfy the following formulas: 0.850≦a≦1.150 0.850≦b≦1.150 0.001≦c≦0.015 0≦d≦0.40 0≦d / (a+d)<0.30 a mixing step of mixing a raw material mixture containing each element constituting the composition with LiF to obtain a mixture; A calcination step of calcining the mixture; A grinding step of grinding the mixture after the firing step to obtain a ground product; an acid treatment step of subjecting the pulverized material to an acid treatment using a mixed liquid containing an acid and an alcohol; a hydrofluoric acid treatment step of subjecting the pulverized material after the acid treatment step to a hydrofluoric acid treatment; a heat treatment step of heating the pulverized material after the hydrofluoric acid treatment step in the atmosphere; A method for producing phosphor particles having the above structure.

2. A method for producing phosphor particles according to claim 1, comprising the steps of: The method for producing phosphor particles, wherein in the mixing step, an amount of the LiF added is 1 mass % or more with respect to a total of 100 mass % of the LiF and the raw material mixture.

3. A method for producing phosphor particles according to claim 1 or 2, comprising the steps of: The method for producing phosphor particles, wherein the alcohol includes at least one selected from the group consisting of MeOH, EtOH, and IPA.

4. A method for producing phosphor particles according to any one of claims 1 to 3, comprising the steps of: The method for producing phosphor particles, wherein in the acid treatment step, the acid includes an inorganic acid.

5. A method for producing phosphor particles according to claim 4, comprising the steps of: The method for producing phosphor particles, wherein the inorganic acid includes nitric acid.

6. A method for producing phosphor particles according to any one of claims 1 to 5, comprising the steps of: In the acid treatment step, the pulverized material is placed in the mixed solution for 0.5 hours or more and 5 hours or less.

7. A method for producing phosphor particles according to any one of claims 1 to 6, comprising the steps of: In the hydrofluoric acid treatment step, the pulverized material is treated with hydrofluoric acid having a hydrogen fluoride concentration of 20% by mass or more and 40% by mass or less.

8. A method for producing phosphor particles according to any one of claims 1 to 7, comprising the steps of: Said M 1 contains at least Sr, and the M 2 contains at least Li, and the M 3 A method for producing phosphor particles containing at least Eu.

9. A method for producing phosphor particles according to any one of claims 1 to 8, comprising the steps of: In the firing step, the heating time is kept at a constant temperature in the range of 900° C. to 1300° C. for 1 hour to 10 hours.

10. A method for producing phosphor particles according to any one of claims 1 to 9, comprising the steps of: The method for producing phosphor particles, wherein the heating temperature in the heat treatment step is 220° C. or higher and 380° C. or lower.

Citation Information

Patent Citations

  • Display screen

    JP1996236035A

  • Phosphor, method for producing the same, phosphor-containing composition, light-emitting device, image display device, and illuminating device

    JP2008274254A

  • Method for manufacturing high temperature-fired phosphor, and phosphor

    JP2012082269A

  • Method for producing complex fluoride phosphor

    JP2015193857A

  • Phosphor, production method thereof, and light emitting device

    JP2015224339A