Method for preparing spherical silica fine powder with ultra-low dielectric loss

The method addresses the challenge of reducing dielectric loss in silica fillers by high-temperature treatment and inert gas processing, achieving significant dielectric loss reduction and stable quality for high-filling applications.

JP7577764B2Active Publication Date: 2024-11-05JIANGSU NOVORAY NEW MATERIAL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022574483
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2022-08-29
Publication Date
2024-11-05
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

Existing methods for preparing silica fillers for printed circuit boards fail to adequately reduce dielectric loss tangent (Df) while maintaining stability and suitability for high-filling applications, often leading to moisture reabsorption and unstable quality.

Method used

A method involving high-temperature treatment in an oxidizing atmosphere to remove impurities, followed by cooling in a non-polar gas atmosphere and packaging with inert gas to produce ultra-low dielectric loss spherical silica fine powder.

Benefits of technology

The method achieves a dielectric loss reduction of over 30% to 67%, ensuring stable product quality and suitability for high-filling applications by effectively removing inorganic carbon, metals, and polar molecules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577764000001
    Figure 0007577764000001
Patent Text Reader

Abstract

To provide a method for preparing spherical silica fine powder with ultra-low dielectric loss. [Solution] Spherical silica fine powder is treated at high temperature in an oxidizing agent atmosphere to remove impurities such as moisture, carbon, metal, etc., then directly put into a non-polar gas atmosphere to cool to room temperature, and finally filled with inert gas and packaged. The method of the present invention can effectively reduce the dielectric loss of spherical silica fine powder, the dielectric loss reduction rate can reach more than 30%, the highest can reach 67%, and the product quality can be stably controlled.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application filed with the China Patent Office on April 25, 2022, bearing application number CN202210442307.1 and entitled "Method for preparing ultra-low dielectric loss spherical silica micropowder", the entire contents of which are incorporated herein by reference.

[0002] The present invention belongs to the technical field of preparing high-performance fillers, and relates to a method for preparing spherical silica fine powder with ultra-low dielectric loss. [Background technology]

[0003] The fifth generation mobile communication system (5G), an extension technology of 4G, will greatly improve the experience of mobile Internet services, fully support IoT business, and realize large-scale intelligent interconnection between people and people, people and things, and things and things. This requires higher data transfer speeds, lower data transfer delays, and better high-speed communication capabilities. The lower the tangent value of the loss angle of a material (hereinafter referred to as dielectric loss, Df), the lower the power loss. Therefore, only low-dielectric-loss Df printed circuit boards can meet the smaller signal loss during 5G transmission. Silicon oxide, an important filler in printed circuit boards, needs to meet two requirements: high filling of fillers and reduction of the Df value of silicon oxide itself. The Df value of silicon oxide itself is affected by its purity, for example, the content of impurity elements such as Fe / C, and also by polar molecules / functional groups such as water / hydroxyl groups. How to further reduce the Df value of silicon oxide is the focus of current research.

[0004] Patent Document 1: In Chinese Patent Application CN113614036A, spherical silica powder is heated at 500-1100°C, the circularity is controlled to 0.85 or more, the surface is treated, and the powder is stored in a moisture-proof bag, thereby reducing the dielectric tangent of the spherical silica powder. Patent Document 2: In Chinese Patent Application CN1123996A, a polyorganosiloxane compound is used to treat the surface of a metal oxide particle material, thereby reducing its Df value. Patent Document 3: In Chinese Patent Application CN110938238A, a silica particle material is used to remove moisture at 200°C, and then the surface is treated with a silane compound to reduce its Df value. All of the above methods first remove the moisture in the material, and then use a silane compound to perform surface treatment to reduce the dielectric tangent value of the material, but they still have the following shortcomings: if the type of surface modifier is not properly selected and the process is not properly processed, it will cause the material to reabsorb moisture during subsequent storage and use; or, if some moisture is adsorbed during the surface treatment process, the dielectric loss reduction will vary greatly, the quality will be unstable, and the expected effect will not be achieved.

[0005] Patent Document 4: In Chinese patent application CN113666380A, a blocking agent is added to a mixed solution of an aqueous nanosilica sol solution and crystal seeds to obtain silica powder with a blocking agent attached thereto by a hydrothermal reaction method, and then a spherical silica powder is prepared by a calcination process, effectively increasing the yield while ensuring the spheroidization rate, and the spherical silica produced has low dielectric loss and narrow particle size distribution. Patent Document 5: Chinese patent application CN112745529A also adopts a method of improving dielectric properties by controlling the specific surface area in a narrow range. The above method mainly reduces the dielectric tangent value by controlling the narrow particle size distribution of the powder, but has the following disadvantages: the reduction of the dielectric tangent value is limited, and the narrow particle size distribution is disadvantageous for high-filling applications, making grading during application difficult, and limiting the application in the field of electronic packaging. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Chinese Patent Application No. 113614036A [Patent Document 2] Chinese Patent Application 1123996A [Patent Document 3] Chinese patent application 110938238A [Patent Document 4] Chinese patent application 113666380A [Patent Document 5] Chinese patent application 112745529A Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above problems, the present invention provides a method for preparing spherical silica fine powder with ultra-low dielectric loss, which involves treating spherical silica fine powder at high temperature in an oxidizing agent atmosphere to remove impurities such as moisture, carbon and metal, then directly entering a non-polar gas atmosphere to cool to room temperature, and finally filling with inert gas and packaging, thereby effectively reducing the dielectric loss, and the product quality is stable and controllable. [Means for solving the problem]

[0008] The technical solutions of the present invention are as follows: A method for preparing ultra-low dielectric loss spherical silica fine powder, comprising the steps of: Step 1, in which a spherical silica fine powder is first treated at 150-300°C for 3-24 hours and then at 800-1200°C for 24-90 hours in a dry oxidizing agent atmosphere, the oxidizing agent being selected from oxygen, oxygen-enriched air, or ozone; Step 2 is to cool the spherical silica fine powder treated in step 1 to room temperature under a non-polar gas atmosphere; Step 3 includes packaging the cooled fine silica powder in an inert gas filled package.

[0009] In step 1, the median particle size D50 of the spherical silica fine powder is 0.1 to 150 μm, and the sphericity is >0.99.

[0010] In step 1, the spherical silica micropowder is prepared by an existing method, and the existing method includes spheronization by a flame method. The specific steps for preparing the spherical silica micropowder by spheronization by a flame method are as follows: silica powder or silica sol with a purity of 99.9% or more and a total content of metal oxides of 100 ppm or less is used as raw material, oxygen is used as carrier gas, 1-5 carbon alkane or H2 is used as combustible gas, and oxygen is used as combustion accelerator, which are respectively introduced into a reaction vessel and ignited, and under the high temperature of 2400-3200°C of the flame, the powder or silica sol is melted at high temperature, and then cooled to form a spherical silica micropowder.

[0011] Preferably, in step 1, the spherical silica fine powder is first treated at 250 to 300° C. for 10 to 24 hours, and then treated at 1100 to 1200° C. for 48 to 90 hours.

[0012] In step 2, the non-polar gas is selected from argon, helium, neon, nitrogen, oxygen or carbon dioxide.

[0013] In step 2, the room temperature is 10 to 30°C.

[0014] In step 3, the inert gas is selected from nitrogen, argon, helium or neon.

[0015] The present invention realizes ultra-low dielectric loss of silica micropowder from two perspectives. The first is to remove inorganic carbon and metal in the micropowder. Both inorganic carbon and metal affect the Df of silica micropowder. Therefore, the present invention first removes inorganic carbon of conductive material by reacting with carbon under high temperature conditions in an oxidizing agent atmosphere; at the same time, it reacts with metal (such as Fe) introduced by the micropowder to form metal oxide and remove some metal. The second is to remove polar molecules such as bound water in the micropowder. A step heating method is adopted to first remove the bound water in the micropowder at a relatively low temperature, and avoid the aggregation of the micropowder caused by directly heating to a high temperature. Effect of the Invention

[0016] Compared with the prior art, the present invention has the following advantages: The present invention selects ultra-high purity raw materials, prepares spherical silica fine powder with a relatively small specific surface area and high sphericity by flame method, removes moisture, metal and inorganic carbon by high temperature treatment in an oxidizing agent atmosphere, directly puts into a non-polar gas atmosphere, cools to room temperature, fills with inert gas and packs, and carries out related processes under the protection of inert gas. The quality of the product produced by the present invention is stable, and the reduction rate of dielectric loss is more than 30%, and can reach up to 67%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention is described in further detail below with reference to specific embodiments. All raw materials or reagents used in the following examples are commercially available. EXAMPLES

[0018] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion accelerator. Each was placed in a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0019] In a dry oxygen atmosphere 1, spherical silica fine powder A was successively treated at 200°C for 3 hours and at 1100°C for 48 hours to obtain spherical silica fine powder B. It was then cooled to room temperature for 10 hours in a non-polar gas argon atmosphere 2. It was then filled with nitrogen, sealed and packaged to obtain a spherical silica fine powder B with an average particle size of 2.5 μm and a specific surface area of ​​3.6 m. 2 Thus, spherical fine silica powder C having a particle size of 0.993 / g and a spherical degree of 0.993 was obtained. EXAMPLES

[0020] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion promoter. Each was introduced into a reaction vessel, ignited, and melted into a spherical shape at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0021] In a dry oxygen atmosphere 1, spherical silica fine powder A was successively treated at 150°C for 10 hours and at 800°C for 60 hours to obtain spherical silica fine powder B. It was then cooled to room temperature in a non-polar nitrogen gas atmosphere 2 for 10 hours, filled with nitrogen, sealed and packaged to obtain a spherical silica fine powder B with an average particle size of 2.2 μm and a specific surface area of ​​3.8 m. 2 Thus, spherical fine silica powder C having a particle size of 0.995 / g and a sphericity of 0.995 was obtained. EXAMPLES

[0022] Using angular silica fine powder with an average particle size of 8 μm and a purity of 99.95% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion accelerator. Each was placed in a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0023] In a dry oxygen atmosphere 1, spherical silica fine powder A was successively treated at 300°C for 24 hours and at 1200°C for 90 hours to obtain spherical silica fine powder B. It was then cooled to room temperature in a non-polar gas argon atmosphere 2 for 10 hours, filled with nitrogen, sealed and packaged to obtain a spherical silica fine powder B with an average particle size of 9.2 μm and a specific surface area of ​​0.86 m. 2 Thus, spherical fine silica powder C having a particle size of 0.991 / g and a sphericity of 0.991 was obtained. EXAMPLES

[0024] Using angular silica fine powder with an average particle size of 35 μm and a purity of 99.90% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion promoter. Each was introduced into a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C to obtain spherical silica fine powder A.

[0025] Under a dry oxygen-enriched air atmosphere 1, spherical silica fine powder A was successively treated at 250°C for 24 hours and then at 900°C for 24 hours to obtain spherical silica fine powder B. It was then cooled to room temperature for 10 hours in a non-polar gas nitrogen atmosphere 2, filled with nitrogen, sealed and packaged to obtain spherical silica fine powder B with an average particle size of 39 μm and a specific surface area of ​​0.36 m. 2 Thus, spherical fine silica powder C having a particle size of 0.992 was obtained. Comparative Example 1

[0026] Using angular silica fine powder with an average particle size of 2μm and purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion promoter, and each was introduced into a reaction vessel, ignited, and melted into a spherical shape at high temperatures of 2400-3200℃ to obtain spherical silica fine powder A. Spherical silica fine powder A was not treated, and was directly cured with polyethylene resin to test the dielectric loss. Comparative Example 2

[0027] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion accelerator. Each was placed in a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0028] Under open conditions, spherical silica fine powder A was successively treated at 200°C for 3 hours and at 1100°C for 48 hours to obtain spherical silica fine powder B. Under open conditions, it was cooled to room temperature for 10 hours, filled with nitrogen, sealed and packaged to obtain spherical silica fine powder B with an average particle size of 2.4 μm and a specific surface area of ​​3.7 m. 2 Thus, spherical fine silica powder C having a particle size of 0.994 / g and a sphericity of 0.994 was obtained. Comparative Example 3

[0029] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion promoter. Each was introduced into a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C to obtain spherical silica fine powder A.

[0030] In a dry oxygen atmosphere 1, spherical silica fine powder A was successively treated at 200°C for 3 hours and at 400°C for 48 hours to obtain spherical silica fine powder B. In a non-polar argon atmosphere 2, it was cooled to room temperature for 10 hours, filled with nitrogen, sealed and packaged to obtain spherical silica fine powder B having an average particle size of 2.4 μm and a specific surface area of ​​3.8 m. 2 Thus, spherical fine silica powder C having a particle size of 0.75 / g and a sphericity of 0.993 was obtained. Comparative Example 4

[0031] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion accelerator. Each was placed in a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0032] In a dry oxygen atmosphere 1, spherical silica fine powder A is successively treated at 200°C for 3 hours and at 1500°C for 96 hours to obtain spherical silica fine powder B, in which the powder aggregates and forms lumps. Because the temperature in the high-temperature stage is too high, the temperature exceeds the melting point of the powder, and the powder melts and forms lumps. Comparative Example 5

[0033] Using angular silica fine powder with an average particle size of 8 μm and a purity of 99.95% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion promoter. Each was introduced into a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C to obtain spherical silica fine powder A.

[0034] In a dry oxygen atmosphere 1, spherical silica fine powder A was directly treated at 1200°C for 90 hours to obtain spherical silica fine powder B. In a non-polar argon atmosphere 2, it was cooled to room temperature for 10 hours, filled with nitrogen, and sealed in a package to obtain spherical silica fine powder C, which has an average particle size of 15.6 μm and a tail in the particle size distribution, indicating that aggregation between fine powders is likely to occur when directly heated to a high temperature. Comparative Example 6

[0035] Using angular silica fine powder with an average particle size of 2 μm and a purity of 99.92% as the raw material, oxygen was used as the carrier gas, H2 as the combustible gas, and oxygen as the combustion accelerator. Each was placed in a reaction vessel, ignited, and melted into spherical shapes at high temperatures of 2400 to 3200°C, to obtain spherical silica fine powder A.

[0036] Under a dry argon atmosphere 1, spherical silica fine powder A was successively treated at 200°C for 3 hours, then at 1100°C for 48 hours to obtain spherical silica fine powder B. The powder was cooled to room temperature for 10 hours under a non-polar argon gas atmosphere 2, filled with nitrogen, sealed and packaged, and the average particle size was 2.6 μm and the specific surface area was 3.5 m. 2 Thus, spherical fine silica powder C having a particle size of 0.993 / g and a spherical degree of 0.993 was obtained.

[0037] According to Table 1, it can be seen that, compared to Comparative Example 1 (untreated), Examples 1 to 4 each have a two-stage heat treatment, different particle sizes, and different atmospheres, which reduces polar molecules and foreign matter (C, Fe, etc.) in the spherical silica fine powder, thereby lowering Df. When the temperature of heat treatment 2 is high (1200°C) and the treatment time is long, under the premise that atmosphere 1 is oxygen, the metal foreign matter and carbon content are the lowest, and the corresponding Df is also the lowest, with a reduction of 67%. Comparative Example 2 is a direct heat treatment under open conditions without the need for atmosphere protection, and the number of metals is too high and moisture is adsorbed during the cooling process, so the reduction in Df is only 22%. In Comparative Examples 3 and 6, the temperature of heat treatment 2 is too low and atmosphere 1 is adjusted to argon gas, so the reduction in foreign matter is insufficient and the reduction in Df is not noticeable. In Comparative Examples 4 and 5, the temperature of heat treatment 2 was controlled too high (1500°C) and heat treatment 1 was not performed and the powder was directly heated to a high temperature, causing the powder to aggregate into large particles or lumps.

[0038] [Table 1]

[0039] The above description of the embodiments is only intended to help understand the method of the present invention and its core idea. For those skilled in the art, some improvements and modifications to the present invention are possible without departing from the principles of the present invention, which are also included in the scope of protection of the claims of the present invention. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not intended to be limited to the embodiments shown in this specification, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing ultra-low dielectric loss spherical silica fine powder, comprising the steps of: Step 1, in a dry oxidizing agent atmosphere, first treating the spherical silica fine powder at 150-300°C for 3-24 hours, and then treating it at 800-1200°C for 24-90 hours, the oxidizing agent being selected from oxygen, oxygen-enriched air, or ozone; Step 2 of cooling the spherical silica fine powder treated in step 1 to room temperature under a non-polar gas atmosphere; Step 3 includes packaging the cooled silica fine powder in an inert gas. A preparation method comprising the steps of:

2. In step 1, the median particle diameter D50 of the spherical silica fine powder is 0.1 to 150 μm and the sphericity is >0.

99.

2. The method of claim 1.

3. In step 1, spherical silica fine powder is prepared by flame spheronization; The raw material is silica powder or silica sol with a purity of 99.9% or more and a total metal oxide content of 100 ppm or less. Oxygen is used as the carrier gas, and 1 to 5 carbon alkanes or H 2 is used as a combustible gas and oxygen is used as a combustion promoter. They are introduced into a reaction vessel and ignited. Under the high temperature of the flame at 2400 to 3200°C, the powder or silica sol is melted at high temperature and cooled into a spherical shape to form spherical silica fine powder.

2. The method of claim 1.

4. In step 1, the spherical silica fine powder is first treated at 250-300°C for 10-24 hours, and then treated at 1100-1200°C for 48-90 hours.

2. The method of claim 1.

5. In step 2, the non-polar gas is selected from argon, helium, neon, nitrogen, oxygen, or carbon dioxide.

2. The method of claim 1.

6. In step 2, the room temperature is 10 to 30°C.

2. The method of claim 1.

7. In step 3, the inert gas is selected from nitrogen, argon, helium, or neon.

2. The method of claim 1.

Citation Information

Patent Citations

  • Filler for electronic materials and method for manufacturing the same, method for manufacturing resin composition, substrate for high frequency, and paste for electronic materials

    CN110938238A

  • Ultralow dielectric constant hollow silicon dioxide material for 5G high-frequency and preparation method thereof

    CN111232993A

  • Method and apparatus for dynamic radio communication menu

    CN1123996A

  • Hollow glass microspheres as well as preparation method and application thereof

    CN112479595A

  • Silica particle, resin composition, resin film, and metal-clad laminate

    CN112745529A