Glass cloth, prepreg, and printed wiring boards
A glass cloth with controlled mass and filament characteristics, along with optimized resin content, addresses the challenges of achieving a 16 μm thickness in printed wiring boards, ensuring reduced waviness and improved resin impregnation, thereby enhancing dimensional stability and handling properties.
Patent Information
- Application Number
- JP2023113147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2037-12-11
AI Technical Summary
Existing glass cloths used in printed wiring boards face challenges in achieving a thickness of 16 μm or less while maintaining dimensional stability, resistance to waviness during prepreg coating, and uniform resin impregnation, leading to issues like corrugation, misalignment, and poor mechanical strength.
A glass cloth with specific textile structure, characterized by controlled mass per unit length, filament diameter, and weft/warp ratio, along with optimized resin content and layer thickness, is developed to achieve a thickness of 16 μm or less, ensuring reduced waviness and improved resin impregnation properties.
The solution results in a glass cloth with enhanced dimensional stability, reduced waviness, and uniform resin layers, facilitating the production of prepregs with improved handling and stability during the prepreg coating process.
Smart Images

Figure 0007577797000003 
Figure 0007577797000004 
Figure 0007577797000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass cloth, a prepreg, and a printed wiring board. [Background technology]
[0002] Most printed wiring boards are usually made of a base material such as glass cloth and a thermosetting resin such as epoxy resin. The prepreg is impregnated with oil and dried to form a prepreg, and one or more sheets of the prepreg are stacked together as necessary. After stacking copper foils according to the requirements, the laminate is formed by heating and pressing. Then, the laminate is photolithographed. A method for forming a circuit pattern from copper foil by roughing and etching or plating. Thus, it is manufactured. Furthermore, the above-mentioned printed wiring board is used as a core substrate, and a prepreg is laminated on the surface of the core substrate. Then, copper foil is placed on the outside of the laminate, and the laminate is heated and pressurized to form a multilayer board. A multilayer printed wiring board is manufactured by forming a circuit on the substrate.
[0003] On the other hand, in recent years, the printed wiring boards used in digital devices have become more sophisticated and smaller in size and weight. There is a demand for smaller, thinner, and more dense devices. The glass cloth used as the material is made thinner, and the number of layers in multilayer printed wiring boards is increased. By increasing the thickness of the glass cloth, the density is increased. In order to achieve high functionality and small size and light weight for cutting-edge smartphones and wearable devices, For this reason, there is a demand to thin the substrate to, for example, 16 μm or less.
[0004] Here, examples of thin glass cloth include glass fibers described in Patent Documents 1 to 6. Specifically, Patent Document 1 proposes a glass cloth having a thickness of 7 to 14 μm. Patent Document 2 describes a glass cloth having a thickness of 14 μm or less, and Patent Document 3 describes a glass cloth having a thickness of 10 μm or more and Patent Document 4 describes a glass cloth with a thickness of 10 μm to 50 μm. Patent Document 5 describes a glass cloth with a thickness of 5 to 15 μm, and Patent Document 6 describes a glass cloth with a thickness of 25 μm or less. A glass cloth of the above formula has been proposed.
[0005] The glass cloth described in Patent Document 1 has an average diameter of 3.5 to 4.4 μm for both the warp and weft. , 20 to 60 filaments, 0.5 × 10 per unit length -6 ~1.7×10 -6 kg / m of glass yarn, and the ratio of the mass of the warp yarn to the mass of the weft yarn is 1.2 By increasing the number of filaments in the weft yarn to be in the range of 6 to 1.42, The gap between the weft threads is less likely to open, and the breathability can be adjusted to a specific range. It is said that it can improve problems such as pinholes and warping when made into a prepreg.
[0006] The glass cloth described in Patent Document 2 has an average filament diameter of warp and weft of 3.0 to 4. .3μm, and the number of filaments in the weft is greater than that in the warp, with the ratio (weft / warp ratio) being 0. .9 or more, and the degree of opening is greater in the weft than in the warp, i.e., the width of the warp bundle is greater than the width of the weft bundle. The yarn bundles are wider in this glass cloth, and the number of weft filaments is increased, making it easier to open. This reduces the distance between adjacent weft threads, which reduces the occurrence of pinholes when used as a substrate. It is believed to be possible to control.
[0007] The glass cloth described in Patent Document 3 has a warp and weft of mass 1.8×10 -6 kg / m or more 14×10 -6The average filament diameter of the warp is 1.0 kg / m or less. The ratio of the average filament diameter of the weft to that of the warp is 1.01 or more and less than 1.20. The lath cloth is made of the above-mentioned material, and the lath cloth has a thickness of 40 μm or less. Even if the fabric is subjected to a tensile load, the distortion and the weft / warp ratio can be kept within a specific range, and the dimensions can be controlled. It is possible to manufacture printed wiring boards with little anisotropy in the shape change and without warping or twisting. has been disclosed.
[0008] The glass cloth described in Patent Document 4 has warp and weft yarns made of the same type of glass yarn, The width of the weft thread is close to the width of the warp thread, and the ratio (weft / warp ratio) is between 0.8 and 1.2. The elongation rate in the weft direction when a load of 25N to 100N is applied per 25mm width The ratio of elongation in the warp direction (weft / warp ratio) is in the range of 0.8 to 1.2. The loss is that the same glass yarn is used for the warp and weft, and the cross-sectional shape and waviness are the same. By doing so, the film substrate using this glass cloth is said to have excellent dimensional stability. is.
[0009] The glass cloth described in Patent Document 5 has an average filament count of at least one of the warp and weft threads. The diameter of the fiber is less than 4.5 μm, and the number of filaments on both sides is 5 to 70. It is a glass cloth made of lath yarn, and although the number of glass filaments that make it up is small, Regardless of the thickness, the fiber is opened and spread under gentle conditions to achieve a surface glass coverage rate of 50% to 100%. This is said to result in a glass cloth having excellent dimensional stability and mechanical properties.
[0010] The glass cloth disclosed in Patent Document 6 has a warp thread and / or a weft thread that are on average The filament diameter is 3 to 4 μm, and the number of filaments is 70 to 200. The glass cloth is made of adjacent warp and weft yarns. Since they are arranged with virtually no gaps, they are said to have excellent surface smoothness and excellent small hole processing properties. There are.
[0011] In addition, as glass cloth registered with ICP standards, 1000 (12μm), 1010 ( Thin glass cloth with thicknesses such as 1017 (14 μm), 1015 (15 μm) are commercially available. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Publication No. 5831665 [Patent Document 2] Publication No. 5936726 [Patent Document 3] Publication No. 5027335 [Patent Document 4] Publication No. 3897789 [Patent Document 5] Publication No. 4446754 [Patent Document 6] Publication No. 3756066 [Patent Document 7] Japanese Patent Application Publication No. 10-245743 [Patent Document 8] JP 2001-269931 A Summary of the Invention [Problem to be solved by the invention]
[0013] Patent Document 6 describes a glass cloth having a thickness of 25 μm or less, but in the examples The glass cloth specifically disclosed in 1 to 5 has a thickness of 17 to 21 μm, and The thinnest glass cloth disclosed in Patent Document 6 has a thickness of 17 μm. In order to place the yarns together without any gaps, it is necessary to use glass yarns with a large number of filaments. As a result, it is difficult to reduce the thickness of the glass cloth. In Nos. 1 to 5, specifically, the warp and weft yarns are all glass yarns with 100 filaments. A string was used.
[0014] The glass cloth disclosed in Patent Document 5 is made of glass filaments constituting the warp and weft. The average diameter of the yarn is reduced, and the number of filaments constituting the warp and weft is reduced. By doing so, we were able to reduce the thickness of the glass cloth to between 5μm and 15μm. The glass cloths in Patent Documents 1 and 2 are also thin in thickness. However, the glass cloth disclosed in Patent Document 1 has a warp and weft yarn weight of 0.5 ×10 -6 ~1.7×10 -6 The stiffness of the glass cloth is high because it uses thin glass threads of 1 kg / m. However, the adhesiveness is low, and there is an issue of waviness occurring when applying the prepreg. In Patent Document 2, the mass of both the warp and weft yarns is 1.65 × 10 -6 kg / m or more Below, specifically, BC3000, BC3750, BC5000, and BC6000 are lighter threads. Since thin glass threads are used, the rigidity of the glass cloth is low and the prepreg coating is difficult. There is a problem of rippling during construction. Furthermore, in the glass cloth disclosed in Patent Document 5, the filaments constituting the warp and weft are Since the number of filaments is reduced, waviness is likely to occur.
[0015] Here, the waviness of the glass cloth refers to the waviness that occurs when the glass cloth is impregnated with thermosetting resin and dried. During the manufacturing process of the prepreg, the prepreg is deformed into the shape shown in Figure 1. If the prepreg is significantly corrugated, wrinkles may occur due to the corrugation, and the There is a problem that the alignment of the prepreg during the molding process is difficult and misalignment occurs. In addition, when prepregs are stored in layers or rolled up, wavy patterns may occur. The protrusions of the resin come into contact with each other and rub against each other, so the resin is in the B stage, i.e., in a semi-cured state. There is also the problem of cracks appearing in the grease, causing the resin to peel off.
[0016] The waviness of the prepreg occurs due to the shrinkage of the thermosetting resin as it dries during the prepreg coating process. The tension in the line is relieved by the undulation in the weft direction, which is free from the restraining force of the line tension. For example, Patent Document 7 states that the mass per unit area is 48 g / m 2 Glass cloth is used When manufacturing a prepreg having a thickness of 70 μm, waviness occurs. In the case of prepreg manufacturing using glass cloth with a thickness of 60 μm or less, waviness occurs. It is stated that
[0017] As mentioned above, the waviness occurs when the hardening resin shrinks during hardening, causing the glass cloth to shrink. The glass cloth is unable to maintain tension and is unable to resist the force of shrinking in the weft direction. Therefore, the waviness occurs when the glass cloth is thin and has low rigidity. The smaller the diameter, the more likely it is to occur. Also, when the glass cloth becomes thinner and weaker, the warp direction The line tension applied is also smaller, so there is no back pressure on the glass cloth during the prepreg coating process. Therefore, the thinner the glass cloth, the more likely it is to become wavy. This has problems that are prone to occur.
[0018] The glass cloth described in Patent Document 4 is processed under low tension conditions to separate the warp and weft yarns. The undulation structure of the yarn can be made the same, and the elongation rate when a tensile load is applied is the same for warp and weft yarns. It is said to be equivalent and has excellent dimensional stability. However, the glass cloth described in Patent Document 4 uses the same glass yarn for the warp and weft. Therefore, it is difficult to make the undulating structure of the warp and weft yarns equal. The glass cloth in this example is one that stretches more in the weft direction than in the warp direction. However, the effect of stabilizing the dimensions in the weft direction during prepreg coating is insufficient, and there is room for improvement in preventing waviness. There is land.
[0019] The glass cloth described in Patent Document 3 has a weft made of glass filaments having a larger diameter than the warp. By adjusting the number of filaments in the yarn, the strain (elongation) when a tensile load is applied can be controlled. This glass cloth has a small strain anisotropy. The glass cloth described in has a reduced wavy structure of the weft yarn, so that the prepreg coating It is also useful for improving waviness. However, the glass cloth of Patent Document 3 has a property that reduces distortion when a tensile force is applied. Therefore, the warp and weft threads are 1.8 x 10 -6 It is necessary to use relatively thick glass thread of 1.0 kg / m or more. Therefore, as specifically disclosed in the examples of the patent document, However, the minimum thickness is 17 μm, and it is not possible to obtain a glass cloth having a thickness of 16 μm or less. In addition, the glass cloth of Patent Document 3 has a filler in the weft as shown in the examples of the patent document. By using thick yarn with a ment diameter of 4.5 μm or more and 100 filaments, This reduces distortion when tension is applied in the direction of the weft. Usually, the glass cloth is impregnated with resin and the excess resin is removed. After the removal of the resin, the resin on the front and back of the glass cloth is transferred to the non-glass part of the glass cloth. The glass cloth in Patent Document 3 does not have sufficient resin impregnation. It is difficult to make the resin layer uniform on both sides of the glass cloth.
[0020] In addition, 1000 (12 μm), 1010 (11 μm), and 1017 ( Glass cloth with a thickness of 16 μm or less, such as 1015 (14 μm) and 1015 (15 μm), is commercially available. However, any glass cloth can be used without the above-mentioned waviness during prepreg coating. There are several issues that need to be addressed. In addition, during the manufacturing process of printed wiring boards, the heat and pressure of the lamination process and the circuit patterns In the process of forming the copper foil, a part of the copper foil is etched out, so the dimensions of the copper-clad laminate are It is known that deformations, warping, and twisting may occur. Glass cloth with a thickness of 16 μm or less, such as 1015 style, has low mechanical strength and is therefore The problem is that the above-mentioned problems of dimensional change, warping, and twisting are highly likely to occur. However, dimensional changes are likely to occur in the weft direction, and the amount of dimensional change varies greatly. The higher the density, the more important stability against dimensional changes becomes. If a thin glass cloth is used for this purpose, the dimensional stability is deteriorated as described above.
[0021] The present invention has been made in view of the above problems, and is intended to provide a method for reducing waviness during coating of a prepreg. It has excellent handling properties, resin impregnation properties, and allows the resin layer to be uniform on both sides of the glass cloth. Glass cloth with a thickness of 6μm or less, prepregs and printed wiring boards using said glass cloth The present invention provides a substrate. The present invention also provides a 16 μm thick film that is excellent in stability of dimensional change during prepreg coating. A prepreg composed of the following glass cloth and matrix resin, and a The object of the present invention is to provide a substrate for a printed wiring board. [Means for solving the problem]
[0022] As a result of intensive research to solve the above problems, the inventors of the present invention have discovered a method for manufacturing a woven fabric comprising warp yarns and weft yarns. The glass cloth has a specific woven structure, which allows the thickness to be kept below 16μm. Improves the rigidity of the glass cloth, reduces waviness during prepreg coating, and provides excellent handling. We have also discovered that the glass cloth has excellent resin impregnation properties and can have a uniform resin layer on both sides. The invention has been completed. The present inventors have also developed a method for producing a film having a specific resin content, a ratio of resin layer thicknesses, and a specific waviness size. It was found that the prepreg having such a structure can improve stability against dimensional changes, and the present invention was completed. This has led to the development of
[0023] That is, the present invention is as follows. [1] A thick cloth made by weaving glass yarns consisting of a plurality of glass filaments as warp and weft yarns. A glass cloth having a thickness of 8 μm or more and 16 μm or less, The average mass per unit length of the warp thread is 1.40 x 10 -6 kg / m or more 1.80×10-6 Less than kg / m The average mass per unit length of the weft is 1.80 x 10 -6 kg / m or more 4.00×10 -6 kg / m or less, The ratio of the average mass per unit length of the weft to the average mass per unit length of the warp (weft A glass cloth having a yarn / warp ratio of greater than 1.20 and less than 1.80. [2] The average filament count of the warp and weft yarns is substantially the same; and The average filament diameter of the warp yarn is 3.7 μm or more and 4.3 μm or less, The average filament diameter of the weft yarn is 4.2 μm or more and 5.3 μm or less, The ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) is The glass cloth according to [1], wherein the modulus of elasticity is 1.07 or more and 1.40 or less. [3] The average filament diameters of the warp and weft yarns are substantially the same, and The average number of warp filaments is 45 or more and 70 or less, The average number of filaments in the weft is 55 or more and 80 or less, The ratio of the average number of filaments in the weft to the average number of filaments in the warp (weft / warp ratio) is , which is greater than 1.25 and not greater than 1.50. [4] The part where the weft exists in the longitudinal direction (MD direction) of the weft, calculated by formula (1), [1] to [3], in which the coefficient indicating the ratio (Y: weft occupancy rate) is 76% or more and 90% or less. The glass cloth according to any one of the above. Y = F / (25000 / G) × 100 (1) (In formula (1), F is the weft width (μm), and G is the weaving density of the weft (threads / 25 mm). ( [5] The gap width between adjacent weft yarns in the longitudinal direction (MD) is 40 μm or more and 80 The glass cloth according to any one of [1] to [4], wherein the glass cloth has a diameter of 1 μm or less. [6] [1]-[5], comprising the glass cloth and a matrix resin. Prepreg. [7] A thickness of a glass yarn made of a plurality of glass filaments woven as warp and weft. A pre-made sheet consisting of glass cloth with a thickness of 8 μm to 16 μm and matrix resin. A leg, 1) to 3) below); 1) Resin content is 50% or more and 76% or less by mass. 2) The thickness of the first resin layer located on one side of the glass cloth and the thickness of the other side of the glass cloth the thickness ratio of the second resin layer located on the surface side of the first resin layer to the first resin layer is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm. Prepreg meets the above requirements. [8] The glass cloth is the glass cloth according to any one of [1] to [5]. [7] The prepreg according to claim 1. [9] The gap width between adjacent weft yarns in the longitudinal direction (MD) is 40 μm or more and 80 The prepreg according to [7] or [8], wherein the thickness is equal to or less than 1 μm.
[10] A printed wiring board produced using the prepreg according to any one of [6] to [9]. Effect of the Invention
[0024] According to the present invention, the prepreg is less prone to waviness during coating and is excellent in handleability. It is possible to provide a thin glass cloth with a thickness of 16 μm or less that has excellent resin impregnation properties when Furthermore, according to the present invention, a prepreg having excellent dimensional stability can be provided. . [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a schematic diagram of a prepreg having corrugations. [Diagram 2] FIG. 1 is a diagram showing a method for measuring the height of waviness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. However, the present invention is not limited to this, and various modifications can be made without departing from the spirit and scope of the present invention. It is possible.
[0027] <Glass cloth> The glass cloth of the present embodiment is made of glass yarns each consisting of a plurality of glass filaments as warp yarns. The glass cloth is woven using the fiberglass yarn as a weft and has a thickness of 8 μm or more and 16 μm or less. The thickness of the glass cloth is 8 μm or more and 16 μm or less, so that the thickness is, for example, 1 Thin prepregs, such as those with thicknesses of 8 μm to 35 μm, can be obtained, enabling the development of high-performance electronic devices. A printed wiring board that can accommodate smaller and lighter sizes can be obtained.
[0028] In the glass cloth of this embodiment, the mass per unit length of the warp yarn is 1.40 × 10 -6 kg / m or more 1.80×10 -6 kg / m. In the glass cloth of this embodiment, the mass per unit length of the weft is 1.80 × 10 -6 kg / m or more 4.00×10 -6 kg / m or less. The average mass per unit length of the weft yarn relative to the average mass per unit length of the warp yarn The ratio of the mass of the warp yarn to the mass of the weft yarn (weft / warp ratio) is greater than 1.20 and less than 1.8. is less than or equal to 0.
[0029] Mass per unit length of warp thread, mass per unit length of weft thread, and mass of warp thread and weft thread The ratio ranges are preferably: warp; 1.45×10 -6 kg / m or more 1.75×10 -6 kg / m or less, weft: 1.90×10 -6 kg / m or more 3.50×10 -6 kg / m or less, Weft / warp ratio: 1.22 or more and 1.75 or less, more preferably warp: 1. 5×10 -6 kg / m or more 1.70×10 -6 kg / m or less, weft: 2.00 x 10 -6 kg / m or more 3.00×10 -6 kg / m or less, weft / warp ratio: 1.23 to 1.70 .
[0030] During the manufacturing process, the glass cloth is impregnated with a silane treatment agent and then coated with a silane agent. During the process of adjusting the amount of coating or during the fiber opening process, physical stress is applied. When using SCROSS to coat prepregs, the amount of resin varnish is reduced after impregnation coating. The glass cloth is subjected to physical stress during the processes of adjusting the thickness and drying. In order to transport the cloth stably and continuously without breaking it, the warp threads must have a certain level of strength. Therefore, the average mass per unit length of the warp thread is 1.40 × 10 -6 kg / On the other hand, the average mass per unit length of the warp thread must be 1.80 x 1 0 -6By using glass yarns less than kg / m, the thickness can be kept below 16μm. The weave density can be increased to, for example, 90 or more threads, which reduces the occurrence of pinholes. There is a tendency for this to happen.
[0031] As a weft thread, the average mass per unit length is 1.80 × 10 -6 kg / m or more of glass yarn By using this, the reinforcing effect against the shrinkage of thermosetting resin during prepreg coating is enhanced, This is advantageous in suppressing the occurrence of waviness. The mass per unit length of the glass yarn used for the weft is: The larger the thickness, the stronger the reinforcing effect, which is preferable. In order to keep the average mass per unit length of the weft yarn below 4.00×10 -6 kg / m or less It is necessary to do so.
[0032] In addition, the mass ratio of the warp yarn to the weft yarn is greater than 1.20, so that the stiffness of the weft yarn and the stiffness of the warp yarn are Therefore, even if the weft thread is thin and has low rigidity, the weaving process In addition, the swell of the weft yarn during the weaving process can be suppressed. Depending on the variation in the line tension, the weft thread inserted without any binding force may have a wavy shape. However, by having the mass ratio of the warp yarn to the weft yarn in the above range, the undulating structure of the weft yarn can be obtained. Therefore, the variation of the thermosetting resin in the prepreg coating process can be suppressed to a small value. It can improve the dimensional stability effect against the hardening shrinkage of the resin. On the other hand, when the mass ratio of the warp threads to the weft threads is 1.80 or less, the difference in stiffness between the warp threads and the weft threads is extremely It prevents the edge from becoming too large, and the ripple structure of the weft is moderately preserved, so that the ripples of the warp and weft are Since there is no significant difference in the structure, it prevents anisotropy in dimensional stability when used as a printed wiring board. It is possible. Mass per unit length of warp thread, mass per unit length of weft thread, and mass of warp thread and weft thread By setting the ratio within the above range, the anisotropy of the dimensional stability when the material is made into a printed wiring board can be suppressed. This prevents the yarn from being damaged while increasing the rigidity in the warp and weft directions. It has the strength to not break easily, and it is possible to reduce the waviness of the prepreg, and it is also resistant to dimensional changes. This results in a glass cloth with a thickness of 16 μm or less that has excellent stability against water. The average mass per unit length of the warp yarn and the average mass per unit length of the weft yarn are, for example, Adjusting the filament diameter of the filaments constituting the warp and weft yarns, and / or This can be controlled, for example, by adjusting the average number of filaments.
[0033] In the glass cloth of the present embodiment, the average number of filaments in the warp and weft is substantially the same. The average filament diameter of the warp yarn is 3.7 μm or more and 4.3 μm or less, and the weft yarn is The average filament diameter of the warp yarn is 4.2 μm or more and 5.3 μm or less, The ratio of the average filament diameter of the weft to the diameter (weft / warp ratio) is 1.07 to 1.40. The following glass cloth (hereinafter, also referred to as glass cloth X) is preferred. By the number of warp and weft filaments and the filament diameter being within the above range, While maintaining the thickness of the glass cloth at 16 μm or less, the dimensional stability of the printed wiring board is improved. This prevents the glass cloth from becoming unstable and gives it a high rigidity in the weft direction.
[0034] The average filament diameters of the warp and weft yarns and the weft / warp ratio are more preferably in the range are respectively: warp: 3.8μm to 4.2μm, weft: 4.3μm to 5.2μm The weft / warp ratio of the average filament diameter is preferably 1.08 or more and 1.25 or less. Or respectively, warp: 3.9μm to 4.1μm, weft: 4.4μm to 5.1μm m or less, and the weft / warp ratio of the average filament diameter is 1.09 or more and 1.20 or less.
[0035] The average filament count of the warp and weft yarns is substantially the same if the filament count of the warp yarns is equal to the average filament count of the weft yarns. The ratio of the number of filaments (weft / warp ratio) is between 0.94 and 1.06. The average filament count weft / warp ratio is between 0.94 and 1.06. This allows the effect of the large weft filament diameter to be realized, i.e., the rigidity in the weft direction to be realized. This is preferable because In addition, in this embodiment, when the average number of filaments in the warp and weft is substantially the same, The number of filaments in each of the warp and weft threads is preferably 60 or less. If the number of filaments in the yarn is 60 or less, the physical processing in the glass cloth manufacturing process Filaments are easily dispersed, and the filament distribution in the Z direction of the glass yarn bundle can be reduced. Therefore, it is easy to reduce the thickness of the glass cloth. The number of lament is preferably small, but from the viewpoint of the strength and handling of the glass cloth, the number of lament is preferably large. If the average number of filaments in the weft yarn is substantially the same, the lower limit of the average number of filaments in the warp and weft yarns is preferably 44 or more, more preferably 46 or more, and even more preferably 48 or more. be.
[0036] In addition, the glass cloth of the present embodiment has an average filament diameter of the warp yarn and the average filament diameter of the weft yarn being substantially the same. The average number of filaments in the warp is 45 or more and 70 or less, and the average number of filaments in the weft is The average number of filaments in the warp is 55 or more and 80 or less. The ratio of the average number of filaments in the weft (weft / warp ratio) is greater than 1.25 and less than or equal to 1.50. A certain glass cloth (hereinafter, also referred to as glass cloth Y) is preferable. By the number of warp and weft filaments and the filament diameter being within the above range, While maintaining the thickness of the glass cloth at 16 μm or less, the dimensional stability of the printed wiring board is not impaired. Therefore, the glass cloth can have a high rigidity in the weft direction without any trouble.
[0037] The average number of filaments in the warp and weft and the ratio thereof (weft / warp ratio) are preferably in the range or respectively, warp: 43 to 65, weft: 57 to 75, average fiber length: Weft / warp ratio of lament number: 1.27 or more and 1.45 or less, more preferably Warp: 45 to 60, Weft: 60 to 70, Average number of filaments Weft / warp ratio: 1.30 or more and 1.40 or less.
[0038] The average filament diameters of the warp and weft yarns are substantially the same as each other. The ratio of the filament diameter (weft / warp ratio) is in the range of 0.95 to 1.05. The ratio of the average filament diameter of the weft to the warp is in the range of 0.95 to 1.05. As a result, the effect of increasing the number of filaments in the weft, i.e., the weft direction This is preferable since it provides rigidity. In addition, in this embodiment, when the average filament diameters of the warp and weft yarns are substantially the same, The filament diameter of each of the warp and weft threads is preferably 3.8 μm or more. And when the average filament diameter of the weft yarn is 3.8 μm or more, the rigidity of the glass cloth is increased. In order to increase the rigidity of the glass cloth, it is preferable that the filament diameter is large. However, from the viewpoint of the thickness of the glass cloth, the average filament diameter of the warp and weft is substantially In the same case, the upper limit of the filament diameter of the warp and weft yarns is preferably 4.4 μm or less, more preferably It is preferably 4.3 μm or less, and more preferably 4.2 μm or less.
[0039] The glass cloth of the present embodiment is, among the above-mentioned glass cloth X and glass cloth Y, Among them, glass cloth X is preferred because it has superior dimensional stability.
[0040] The glass cloth of the present embodiment has a weft length (MD direction) calculated by the formula (1). The coefficient (Y: weft occupancy rate), which indicates the proportion of the area where the weft is present, is 76% or more and 90% or less. It is preferable that: Here, the weft occupancy rate Y is the value obtained by dividing the weft width by the sum of the weft width and the width of the weft gap. , the value calculated using equation (1). Y = F / (25000 / G) × 100 (1) (In formula (1), F is the weft width (μm), and G is the weaving density of the weft (threads / 25 mm). ( The weft width is measured by microscopy of a glass cloth sample measuring 100 mm x 100 mm from the surface. This is the average value of the widths of all weft threads measured by observing them in a mirror. The weft occupancy rate Y is more preferably 78% or more and less than 89%, and further preferably 79% or more. It is less than 88%.
[0041] In the glass cloth of this embodiment, the weft yarn is made of glass yarn having a larger mass than the warp yarn. Therefore, the width of the weft thread is wider than the width of the warp thread, and the gap between the warp threads makes it easier to separate the weft threads from the warp threads. The gaps between the weft threads tend to be wider than the gaps between the weft threads. By having areas where there is no glass, when the resin is impregnated and coated onto the glass cloth, , there is no glass in the glass cloth after removing excess resin to adjust the resin amount. The resin on one side and the resin on the other side penetrate each other through the part. A prepreg is obtained in which the resin thickness is the target thickness for the loss. The occupation ratio Y is preferably 90% or less. In addition, since the weft yarn occupancy rate Y is 76% or more, the glass yarns are uniformly distributed throughout the glass cloth. The basket is formed by the gaps between the warp threads and the gaps between the weft threads. This makes it possible to reduce the area where there are no glass threads, called pinholes, and thus reduce the occurrence of pinholes. You can suppress life.
[0042] Furthermore, in the glass cloth of the present embodiment, adjacent weft yarns in the longitudinal direction (MD direction) The gap width between the wefts, i.e., the distance between the wefts, is preferably 40 μm or less. The thickness is preferably from 45 to 75 μm, and more preferably from 45 to 75 μm. The average particle size is generally between 50 μm and 70 μm. By setting the spacing between the wefts at 40 μm or more and 80 μm or less, the glass cloth The balance between the distribution of fluorine and the resin impregnation is optimal, suppressing pinholes and preventing glass cloth from being damaged. It is possible to simultaneously satisfy the requirement that the resin be applied symmetrically to the surface of the substrate. The spacing between the weft threads can be adjusted, for example, by adjusting the weft width and / or the weaving density of the weft threads. This allows for greater control. In addition, the spacing between the wefts is adjusted by performing a fiber opening process, etc., to form a glass cloth. The width of the yarn can also be adjusted by flattening the yarn. The fiber-opening process can be carried out, for example, by using water pressure to open the fibers, or by using high-frequency vibrations with a liquid as a medium. Examples include opening the fibers by pressing them with a roller, processing by the pressure of a fluid having a surface pressure, and processing by applying pressure with a roll. Among these fiber-opening methods, water pressure opening and / or Alternatively, it is preferable to spread the fibers by high-frequency vibration using a liquid as a medium. In order to increase the efficiency, the tension applied to the glass cloth for transportation is reduced, and the fiber opening process is performed. In addition, the adjustment of the spacing between the weft yarns is preferably performed by adding a lubricant to the glass yarns. Weaving glass cloth with organic matter attached that shows the above characteristics, or ordinary glass cloth. The flattening process is carried out using glass cloth with binders and adhesives attached, which are used in the manufacturing process. After the fiber-opening process, the surface is treated with a silane coupling agent and then the fiber-opening process is carried out again. This can also be done by
[0043] The glass yarn constituting the glass cloth of the present embodiment is not particularly limited, and generally E-glass (alkali-free glass) used for printed wiring boards may be used. Alternatively, low dielectric constant glass such as D glass, L glass, NE glass, silica glass (Q glass) Using high strength glass such as glass, S glass, T glass, and high dielectric constant glass such as H glass, Good too.
[0044] The weaving structure of the glass cloth is not particularly limited, but may be, for example, a plain weave or a sash weave. In addition, mixed weave structures using different types of glass yarns are also available. Among these, the plain weave structure is preferred.
[0045] In addition, the glass cloth that constitutes the laminates used in printed wiring boards and the like usually contains silane. The surface may be treated with a treatment liquid containing a coupling agent. As the coupling agent, a commonly used silane coupling agent can be used. If necessary, acids, dyes, pigments, surfactants, etc. may be added.
[0046] As the silane coupling agent, for example, a silane coupling agent represented by the formula (2) It is preferred to use X(R) 3-n SiY n (2) In formula (2), X is an organic group having at least one of an amino group and an unsaturated double bond group. Each Y is independently an alkoxy group; n is an integer of 1 to 3. Each R is independently selected from the group consisting of a methyl group, an ethyl group, and a phenyl group. It is based on
[0047] X is an organic functional group having at least three of the amino groups and unsaturated double bond groups. X is preferably at least four of an amino group and an unsaturated double bond group. It is more preferable that the organic functional group has the formula: The alkoxy group may be in any form, but it is preferable to use the alkoxy group in a form suitable for stabilization of the glass cloth. From the viewpoint of chemistry, an alkoxy group having 5 or less carbon atoms is preferred.
[0048] Specific examples of silane coupling agents include N-β-(N-vinylbenzylamino) N-β-(N-vinyl)-γ-aminopropyltrimethoxysilane and its hydrochloride benzylaminoethyl)-γ-aminopropylmethyldimethoxysilane and its hydrochloride salt, N-β-(N-di(vinylbenzyl)aminoethyl)-γ-aminopropyltrimethoxy Silane and its hydrochloride, N-β-(N-di(vinylbenzyl)aminoethyl)-N-γ- (N-vinylbenzyl)-γ-aminopropyltrimethoxysilane and its hydrochloride, N- β-(N-benzylaminoethyl)-γ-aminopropyltrimethoxysilane and its salts Acid salt, N-β-(N-benzylaminoethyl)-γ-aminopropyl triisoethoxysilane and its hydrochloride, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ- (2-Aminoethyl)aminopropyltriethoxysilane, aminopropyltrimethoxy Silane, vinyltrimethoxysilane, methacryloxypropyltrimethoxysilane, acrylic Examples of the known simple substances include aryloxypropyltrimethoxysilane, and mixtures thereof. .
[0049] The molecular weight of the silane coupling agent is preferably 100 to 600, more preferably The molecular weight is preferably 150 to 500, and more preferably 200 to 450. It is preferable to use two or more different silane coupling agents. By treating the glass fiber surface with a silane coupling agent of the above class, the glass surface This increases the density of the treatment agent in the matrix resin, and the reactivity with the matrix resin tends to be further improved.
[0050] The ignition loss value of the glass cloth is preferably 0.10 mass % or more and 1.20 mass % or less. More preferably, the content is 0.11% by mass or more and 1.10% by mass or less, and further preferably, 0. .12% by mass or more and 1.00% by mass or less. Ignition loss value is 0.10% by mass or more and 1.2% by mass or less. By using a prepreg having a thickness of 0.01 to 0.1%, the prepreg can be more easily transported, i.e., handled, than conventional prepregs. In addition, the resin and the glass cloth tend to peel off at the interface. This can suppress the deterioration of the insulation reliability of the board caused by the plating, and the plating solution soaks into the glass cloth. This tends to suppress the deterioration of the insulation reliability of the board caused by the above-mentioned problems. The "ignition loss value" referred to here is the value measured according to the method described in JIS R 3420. First, the glass cloth is placed in a dryer at 110°C and dried for 6 After drying, transfer the glass cloth to a desiccator and leave it there for 20 minutes, then leave it to cool to room temperature. After cooling, weigh the glass cloth to the nearest 0.1 mg. Heat in a muffle furnace at 625°C for 20 minutes. After heating in the muffle furnace, place the glass cloth in a desiccator. Transfer the glass cloth to a container and leave it for 20 minutes to cool to room temperature. After cooling, remove the glass cloth from the container and discard the remaining 0.1 mg or less of the glass cloth. The ignition loss value obtained by the above measurement method is used to determine the silane coupling of the glass cloth. Define the amount of agent to be treated.
[0051] <Glass cloth manufacturing method> The method for producing the glass cloth of the present embodiment is not particularly limited, but may be, for example, a method using a silane cup. The ring agent concentration is 0.1 to 3.0 wt%. The surface of the cement is covered with a silane coupling agent in a coating process, and the silane coupling agent is then removed by heating and drying. The adhesive is applied to the surface of the glass filaments, and the glass threads of the glass cloth are then opened. and a fiber-opening step for fiberizing the fibers.
[0052] The solvent for dissolving or dispersing the silane coupling agent may be either water or an organic solvent. However, from the viewpoints of safety and global environmental protection, it is preferable to use water as the main solvent. As a method for obtaining a treatment liquid with water as the main solvent, a silane coupling agent is directly added to water. The method includes dissolving a silane coupling agent in a water-soluble organic solvent to prepare an organic solvent solution, and then or a method in which the organic solvent solution is poured into water. To improve water dispersibility and stability in the processing solution, surfactants can be used in combination. be.
[0053] The method of applying the treatment liquid to the glass cloth is as follows: (a) collect the treatment liquid in a bath and apply it to the glass cloth. (a) A method of immersing and passing the resin through a roll coater (hereinafter referred to as the "immersion method"); Examples of methods include applying the treatment solution directly to the glass cloth using a gravure coater or a photocoater. When applying by the immersion method (a) above, the immersion time of the glass cloth in the treatment solution is It is preferable to set the time to 0.5 seconds or more and 1 minute or less.
[0054] In addition, as a method for heating and drying the solvent after applying the treatment liquid to the glass cloth, hot air Known methods such as radiation and electromagnetic waves can be used. The heating and drying temperature is set to a suitable temperature so that the reaction between the silane coupling agent and the glass is sufficiently carried out. The heating and drying temperature is preferably 90° C. or higher, and more preferably 100° C. or higher. In order to prevent deterioration of the organic functional groups of the silane coupling agent, it is preferable to heat the silane coupling agent at a temperature of 300° C. or lower. The temperature is preferably 200° C. or lower, and more preferably 200° C. or lower.
[0055] The method for opening the glass cloth in the opening step is not particularly limited. For example, the glass cloth may be Spray water (high pressure water opening), vibro washer, ultrasonic water, mangle, etc. In order to keep the total area of the basket hole within a certain range, spraying is It is preferable to carry out the opening step using water. When using spray water to open the fibers, the water pressure can be set appropriately. In order to adjust the total area of the kethole, it is preferable to keep the water pressure constant. The pressure is kept constant by setting the maximum value between the spray water pressure set for spreading and the actual water pressure. This refers to reducing the difference between the maximum and minimum values. The method may include a step of:
[0056] <Prepreg> One of the present embodiments is composed of the glass cloth of the present embodiment and a matrix resin. The matrix resin is a prepreg (hereinafter referred to as prepreg A). It is impregnated into the scrub.
[0057] In one embodiment of the present invention, glass yarns consisting of a plurality of glass filaments are used as warp yarns and A glass cloth having a thickness of 8 μm to 16 μm and a matrix resin are woven as weft yarns. The prepreg (hereinafter referred to as prepreg B) is composed of a matrix. The glass cloth is impregnated with the resin. Prepreg B is the following 1) to 3); 1) Resin content is 50% or more and 76% or less by mass. 2) The thickness of the first resin layer located on one side of the glass cloth and the thickness of the other side of the glass cloth the thickness ratio of the second resin layer located on the surface side of the first resin layer to the first resin layer is 0.8 or more and 1.2 or less; 3) The amount of waviness is less than 3 mm. Meet the following.
[0058] The glass cloth constituting the prepreg of this embodiment is preferably By using the glass cloth of this embodiment, the prepreg coating can be performed with a minimum of This reduces waviness and provides a prepreg with excellent stability against dimensional changes.
[0059] The resin content in the prepreg B of this embodiment is determined based on the total amount of the prepreg B being 100 mass%. When the amount of the saturation agent is 50% by mass or more and 76% by mass or less, preferably 52% by mass or more and 73% by mass or less. The resin content is more preferably 54% by mass or more and 70% by mass or less. With a content of 76% by mass or more, it is possible to meet the increasing functionality of electronic devices.
[0060] In the prepreg B of this embodiment, the first The ratio of the thickness of the resin layer to the thickness of the second resin layer located on the other side of the glass cloth is 0. The ratio is 0.70 or more and 1.30 or less, preferably 0.80 or more and 1.20 or less, and more preferably or 0.85 or more and 1.15 or less. The ratio of the thickness of the first resin layer to the thickness of the second resin layer is 0.70 or more and 1.30 or less. This prevents the prepreg from waviness even when using thin glass cloth with a thickness of 16 μm or less. can be done.
[0061] In addition, the amount of waviness in the prepreg B of this embodiment is 3 mm or less, and preferably It is 2 mm or less, more preferably 1 mm or less. The waviness of the prepreg is 3 mm or less, so that the prepreg can be molded by heating and pressurizing. In addition, it is presumed that this is because it is possible to suppress the occurrence of distortion such as bending of the glass yarns that form the glass cloth. However, this is preferred because it has excellent stability against dimensional changes. Here, the waviness of the prepreg is a value determined as follows. The prepreg was cut to a size of 340 mm x 510 mm and used as a test piece for measuring the amount of waviness. As shown in FIG. 2, the prepreg 2 is placed on a flat surface of a measuring table 1, and the waviness of the prepreg 2 is measured. The height of each wave is measured, and the maximum value is defined as the “amount of waviness.”
[0062] The prepreg of the present embodiment can be produced by a conventional method. For example, The matrix resin is impregnated with a varnish made by diluting it with an organic solvent, and then the organic solvent is removed in a drying oven. The agent is volatilized and the thermosetting resin is hardened to a B-stage state, i.e., a semi-hardened state. Resin impregnated prepregs can be made.
[0063] As the matrix resin, either a thermosetting resin or a thermoplastic resin can be used. The thermosetting resin is not particularly limited, but examples thereof include a) a compound having an epoxy group. and epoxy groups, amino groups, phenol groups, acid anhydride groups, hydrazide groups, iso groups, A compound having at least one of a cyanate group, a cyanate group, and a hydroxyl group, etc., Reaction of imidazole compounds, tertiary amine compounds, urea compounds, phosphorus compounds, etc. with a catalyst Epoxy resin that is cured by adding a catalyst with catalytic ability; b) Allyl group, meth A compound having at least one of an acrylic group and an acryl group is subjected to a thermal decomposition type catalyst or a photochemical reaction. c) radical polymerization type curing resin that is cured using a decomposition catalyst as a reaction initiator; A maleimide compound is cured by reacting a compound having a maleimide group with a compound having a maleimide group. d) Imidotriazine resin; e) Thermosetting polyimide resins that are produced by thermal polymerization of compounds having benzoxazine rings; Examples of the resin include benzoxazine resins that are crosslinked and hardened. The thermoplastic resin is not particularly limited, but may be, for example, polyphenylene ether. , modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyether Tersulfone, polyarylate, aromatic polyamide, polyether ether ketone, heat Examples of the material include plastic polyimide, insoluble polyimide, polyamideimide, and fluororesin. A thermosetting resin and a thermoplastic resin may be used in combination.
[0064] <Printed wiring board> One embodiment of the present invention is a printed wiring board manufactured using the prepreg of the present embodiment. That is, the printed wiring board is manufactured using the prepreg of the present embodiment. By manufacturing printed wiring boards using prepregs, we can achieve high quality and accurate wiring circuits. Thus, a printed wiring board can be provided. EXAMPLES
[0065] The present invention will now be described in detail with reference to examples. In the examples and comparative examples, the physical properties were measured by the following methods.
[0066] (1) Physical properties of glass cloth The physical properties of the glass cloth, specifically, the thickness of the glass cloth, the mass of the glass cloth, the warp yarn and The mass of the weft and warp threads, the diameter of the filaments constituting the warp and weft threads, the number of filaments, and the density of the warp threads The degree of twist was measured according to JIS R3420. The gap width between adjacent wefts is 100mm x 100mm at any position on the glass cloth. This was determined by observing areas measuring 1 mm or more.
[0067] (2) Evaluation of waviness of prepreg The prepregs obtained in the examples and comparative examples were cut to a size of 340 mm x 510 mm. As shown in FIG. 2, the test piece was placed on a flat surface of the measurement table 1. The height of the waviness 3 that occurred in 2 was measured, and the maximum value was taken as the “amount of waviness.”
[0068] (3) Pinhole The prepregs obtained in the examples and comparative examples were cut to dimensions of 500 mm x 500 mm. The test pieces were observed with a 20x magnifying glass to count the number of pinholes.
[0069] (4) Evaluation of dimensional stability in the weft direction The prepregs obtained in the examples and comparative examples were cut to a size of 340 mm x 340 mm. Two sheets of the prepreg were laminated, and then copper foil with a thickness of 12 μm was placed on both surfaces. , 40kgf / cm 2 The test substrate was obtained by compression molding at 125 mm. A total of nine points were marked, three vertically and three horizontally, to create a gap. The gauge intervals between two adjacent gauge points were measured at six points in both the vertical and horizontal directions ( Measurement value a). Next, the steel foil was removed by etching, and the specimen was heated at 170°C for 30 minutes. Then, the gauge interval was measured again (measurement value b). The ratio of the difference to the measured value a was calculated, and the dimensional change rate between each reference point in the weft direction was calculated (total 6 The above test was performed three times. Calculate the average value of the dimensional change rate between each reference point for three times (6 points x 3 times = 18 dimensional change rate values). The standard deviation of all 18 dimensional change rates was calculated and the weft direction dimensional change rate was calculated. The variation in the dimensional change rate in the yarn direction was taken as the variation.
[0070] <Example 1> The warp yarn has an average filament diameter of 4.0 μm, 50 filaments, and a twist of 1.0Z. , weight per unit length 1.65×10 -6 kg / m of E-glass yarn, as weft, average fill Lament diameter 4.5μm, filament count 50, twist count 1.0Z, weight per unit length 2 .07×10 -6 Using E-glass yarn of 93 kg / m, an air jet loom is used, and the warp thread is 93 The glass cloth was woven with a weaving density of 0.5 threads / 25 mm and 60 weft threads / 25 mm. The grey fabric was heat treated at 400℃ for 24 hours to remove the size. Then, a silane coupling agent, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane The glass cloth was immersed in a treatment solution using SZ6032 (manufactured by Dow Corning Toray Co., Ltd.), After squeezing, the fabric is dried at 120°C for 1 minute, then opened with a high-pressure water spray, weighing 11. 2g / m 2 Thus, a glass cloth A having a thickness of 12 μm was obtained. The widths are 134 μm and 267 μm, respectively, the weft occupancy rate is 64%, and the weft gap is 15. 0 μm. Glass cloth A was processed to a width of 650 mm for coating tests and was pre-coated with epoxy resin varnish. A repreg coating test was conducted. The epoxy resin varnish used was low-brominated bisphenol A type. Epoxy resin 80 parts by mass, cresol novolac type epoxy resin 20 parts by mass, dicyandi 2 parts by weight of 2-ethyl-4-methylimidazole, 0.2 parts by weight of 2-methoxy- The glass cloth was conveyed at a speed of 3 m / min. Then, glass cloth A was immersed in epoxy resin varnish so that the resin content became 68% by mass. After scraping off excess varnish through a slit with an adjusted gap, the plate is dried at 170°C. Dry for 1 minute 30 seconds to semi-harden the epoxy resin (B stage) and print. Preg A was obtained.
[0071] <Example 2> The glass cloth was prepared in the same manner as in Example 1, except that the weaving density of the weft yarn was 70 threads / 25 mm. Loss weaving and subsequent processing, weight 12.1 g / m 2 , 13μm thick glass cross section The yarn widths of the warp and weft of the glass cloth B were 139 μm and 285 μm, respectively. The weft occupancy rate was 80%, and the weft gap was 72 μm. Prepreg B was obtained in the same manner as in Example 1, except that glass cloth B was used. Ta.
[0072] <Example 3> The glass cloth was prepared in the same manner as in Example 1, except that the weaving density of the weft yarn was 75 threads / 25 mm. Loss weaving and subsequent processing, weight 12.5g / m 2 , 14μm thick glass cross section Glass cloth C was obtained. The warp and weft widths of glass cloth C were 137 μm and 276 μm, respectively. The weft occupancy rate was 83%, and the weft gap was 57 μm. Prepreg C was obtained in the same manner as in Example 1, except that glass cloth C was used. Ta.
[0073] <Example 4> The glass cloth was prepared in the same manner as in Example 1, except that the weaving density of the weft yarn was 78 threads / 25 mm. Loss weaving and subsequent processing, weight 12.8g / m 2 , 14μm thick glass cross section The yarn widths of the warp and weft of glass cloth D were 135 μm and 274 μm, respectively. The weft occupancy rate was 85%, and the weft gap was 47 μm. Prepreg D was obtained in the same manner as in Example 1, except that glass cloth D was used. Ta.
[0074] <Example 5> The glass cloth was prepared in the same manner as in Example 1, except that the weaving density of the weft yarn was 81 threads / 25 mm. Loss weaving and subsequent processing, weight 13.0 g / m 2 , 15μm thick glass cross section The yarn widths of the warp and weft of the glass cloth E were 134 μm and 268 μm, respectively. The weft occupancy rate was 87%, and the weft gap was 41 μm. Prepreg E was obtained in the same manner as in Example 1, except that glass cloth E was used. Ta.
[0075] <Example 6> The glass cloth was prepared in the same manner as in Example 1, except that the weaving density of the weft yarn was 85 / 25 mm. Loss weaving and subsequent processing, weight 13.3 g / m 2 , 16μm thick glass cross section The yarn widths of the warp and weft of the glass cloth F were 131 μm and 266 μm, respectively. The weft occupancy rate was 90%, and the weft gap was 28 μm. Prepreg F was obtained in the same manner as in Example 1, except that glass cloth F was used. Ta.
[0076] <Example 7> The average weft filament diameter is 4.0 μm, the number of filaments is 67, and the twist is 1.0Z. Weight per length 2.20 x 10 -6 The glass yarn is woven at a density of 6 kg / m. The glass cloth was woven in the same manner as in Example 1, except that the number of strands was 5 / 25 mm. The next treatment resulted in a weight of 11.9 g / m 2 Thus, a glass cloth G having a thickness of 13 μm was obtained. The warp and weft widths of the cross G are 150 μm and 284 μm, respectively, and the weft occupancy rate is The weft gap was 74% and 101 μm. Prepreg G was obtained in the same manner as in Example 1, except that glass cloth G was used. Ta.
[0077] <Example 8> The glass cloth was prepared in the same manner as in Example 7, except that the weaving density of the weft yarn was 72 threads / 25 mm. Loss weaving and subsequent processing, weight 12.5g / m 2 , 14μm thick glass cross section The yarn widths of the warp and weft of the glass cloth H were 148 μm and 281 μm, respectively. The weft occupancy rate was 81%, and the weft gap was 66 μm. Prepreg H was obtained in the same manner as in Example 1, except that glass cloth H was used. Ta.
[0078] <Example 9> The glass cloth was prepared in the same manner as in Example 7, except that the weaving density of the weft yarn was 75 threads / 25 mm. Loss weaving and subsequent processing, weight 12.8g / m 2 , 14μm thick glass cross section The yarn widths of the warp and weft of the glass cloth I were 146 μm and 277 μm, respectively. The weft occupancy rate was 83%, and the weft gap was 56 μm. Prepreg I was obtained in the same manner as in Example 1, except that Glass Cloth I was used. Ta.
[0079] <Example 10> Weft filament average diameter 5.0μm, filament count 50, twist count 1.0Z, unit Weight per length 2.76 x 10 -6 The glass yarn is 5 kg / m thick and the weft density is 5 The glass cloth was woven in the same manner as in Example 1, except that the number of strands was 7 / 25 mm. The next treatment resulted in a weight of 12.6 g / m 2 Thus, a glass cloth J having a thickness of 15 μm was obtained. The warp and weft widths of Cross J are 161 μm and 273 μm, respectively, and the weft occupancy rate is The weft gap was 62% and 166 μm. Prepreg J was obtained in the same manner as in Example 1, except that glass cloth J was used. Ta.
[0080] <Comparative Example 1> Weft filament average diameter 4.0μm, filament count 50, twist count 1.0Z, unit Weight per length 1.65 x 10 -6 The glass yarn is 9 kg / m thick and the weft density is 9 The glass cloth was woven and spun in the same manner as in Example 1, except that the thickness was 3.5 strands / 25 mm. The next treatment resulted in a weight of 12.5g / m 2 As a result, a glass cloth K having a thickness of 14 μm was obtained. The warp and weft widths of the Lath Cloth K are 132 μm and 222 μm, respectively. The prevalence was 83% and the weft gap was 45 μm. Prepreg K was obtained in the same manner as in Example 1, except that glass cloth K was used. Ta.
[0081] <Comparative Example 2> The weft and warp have an average filament diameter of 4.0 μm, 40 filaments, and a twist of 1. 0Z, weight per unit length 1.32×10 -6 kg / m of glass yarn is used, and the warp and The glass cloth was woven in the same manner as in Example 1, except that the weaving density of the weft yarn was 95 / 25 mm. Loss weaving and subsequent processing, weight 10.2 g / m 2 , 11μm thick glass cross section The yarn widths of the warp and weft of the glass cloth L were 156 μm and 175 μm, respectively. The weft occupancy rate was 67%, and the weft gap was 88 μm. Prepreg L was obtained in the same manner as in Example 1, except that glass cloth L was used. Ta.
[0082] <Comparative Example 3> The warp has an average filament diameter of 4.0 μm, 40 filaments, and 1.0Z twist. Weight per length 1.32 x 10 -6 kg / m of glass yarn, average filament diameter of weft yarn: 4.0 μm, filament count 50, twist count 1.0Z, weight per unit length 1.65×10 -6 k The glass yarn used is 100 g / m, and the warp density is 95 / 25 mm, the weft density is 9 The glass cloth was woven and then processed in the same manner as in Example 1, except that the number of strands per meter was 5. Weight 10.4g / m 2 Thus, a glass cloth M having a thickness of 13 μm was obtained. The warp and weft widths of M are 156 μm and 213 μm, respectively, and the weft occupancy rate is 81%. The gap between the weft yarns was 50 μm. Prepreg M was obtained in the same manner as in Example 1, except that glass cloth M was used. Ta.
[0083] <Comparative Example 4> The glass cloth was prepared in the same manner as in Comparative Example 2, except that the weaving density of the weft yarn was 76 threads / 25 mm. Loss weaving and subsequent processing, weight 9.1 g / m 2 , 12μm thick glass cloth The yarn widths of the warp and weft of the glass cloth N were 160 μm and 228 μm, respectively. The weft occupancy rate was 69%, and the weft gap was 101 μm. Prepreg M was obtained in the same manner as in Example 1, except that glass cloth N was used. Ta.
[0084] <Comparative Example 5> A glass cloth was woven in the same manner as in Comparative Example 1. The obtained green fabric was subjected to a 4.9 N / Fiber opening processing using high-pressure water spray under tension of 196 N / cm 2 ) method was applied. After that, it was heated at 400℃ for 24 hours to remove the glue. β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane;S A glass cloth was immersed in a treatment solution using Z6032 (Toray, Dow Corning) and squeezed. After drying at 120°C for 1 minute, the weight was 12.5g / m 2 , 14 μm thick glass cloth O The chemical and physical treatment of the glass cloth was described in Patent Document 4: Japanese Patent No. 3897789. The method of Example 2 of No. 2 was followed. The yarn widths of the warp and weft of the glass cloth O were 14 The weft occupancy rate was 62%, and the weft gap was 102 μm. A prepreg M was obtained in the same manner as in Example 1, except that glass cloth O was used. Ta.
[0085] <Comparative Example 6> Both warp and weft have an average filament diameter of 4.0 μm, 100 filaments, and 1 twist. .0Z, weight per unit length 3.31 x 10 -6 kg / m of E-glass yarn is used, and The same method as in Example 1 was used, except that the weaving density of both the warp and weft yarns was 100 / 25 mm. The glass cloth was woven and subsequently processed by the method, and the weight was 22.0 g / m 2 , thickness 20μm Thus, glass cloth P was obtained. A prepreg P was obtained in the same manner as in Example 1, except that glass cloth P was used. Ta.
[0086] <Comparative Example 7> The warp yarn has an average filament diameter of 4.0 μm, 100 filaments, 1.0Z twist, and single Weight per length 3.30 x 10 -6 kg / m E-glass yarn, average filament in weft Diameter 4.5μm, filament count 100, twist count 1.0Z, weight per unit length 4.1 3×10 -6 The fabric is made of E-glass yarn of 1.0 kg / m2, and the warp density is 75 threads / 25 mm. The glass cloth was woven in the same manner as in Example 1, except that the weaving density of the weft yarn was 60 threads / 25 mm. The fabric is woven and then processed to a weight of 20.0 g / m 2 , 19μm thick glass cloth I got a Q. Prepreg Q was obtained in the same manner as in Example 1, except that glass cloth Q was used. Ta.
[0087] [Performance test] Various evaluations were performed on the prepregs A to Q obtained in Examples 1 to 10 and Comparative Examples 1 to 7. The results are shown in Tables 1 and 2.
[0088] [Table 1]
[0089] [Table 2]
[0090] From the results in Table 1, all of the prepregs A to J obtained in Examples 1 to 10 were free from waviness. The fabric had little looseness, and the dimensional change in the weft direction and its variation were small. Prepregs K, L, and Q, 2, 6, are registered with IPC and are available on the market. The prepreg is made using 1010 and 1027 style glass cloth. The prepreg of the present example has less waviness and a weft width compared to the prepregs of Comparative Examples 1, 2, and 6. All of the samples were excellent in terms of the amount of dimensional change in the yarn direction and the variation therein.
[0091] The prepreg M of Comparative Example 3 was made using the same yarn as in Example 1 of Patent Document 1 and Example 1 of Patent Document 2. The prepreg was made using glass cloth having the same composition as that of the prepreg M in Comparative Example 3. In comparison with glass cloth L (IPC registered 1010) of Comparative Example 2, which has the same warp yarn structure, Although the amount of change in the weft dimensions was reduced, there was still a large variation.
[0092] In Comparative Example 5, as disclosed in Patent Document 4, the weft and warp yarns were processed under low tension conditions. The yarn width is the same, that is, the weft / warp ratio is in the range of 0.8 to 1.2. The prepreg obtained from the glass cloth corresponds to the above-mentioned glass cloth. However, prepreg O has a large waviness and a large variation in dimensional change. It was.
[0093] The prepreg Q of Comparative Example 7 is a glass fiber prepreg having the same warp and weft configuration as Example 3 of Patent Document 3. It corresponds to a prepreg made using glass cloth Q. The thickness of glass cloth Q is 19 μm. However, the thickness of the glass cloth was not thin. The thickness of the resin layer on both sides of the mold was not uniform, causing some waviness. It was larger than those in Examples 1 to 10. [Industrial Applicability]
[0094] The glass cloth and prepreg of the present invention are used in printed wiring boards used in the electronic and electrical fields. The present invention has industrial applicability as a substrate for plates. [Explanation of symbols]
[0095] 1: Measuring table 2: Prepreg 3: Height of the waves
Claims
1. A prepreg comprising a glass cloth having a thickness of 8 μm to 16 μm and formed by weaving glass yarns consisting of a plurality of glass filaments as warp yarns and weft yarns, and a matrix resin, The following 1) to 3); 1) Resin content is 50% or more and 76% or less by mass; 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 to 1.
3. 3) The amount of waviness is less than 3 mm; Fulfilling Either 4) or 5) below is satisfied: 4) The average filament count of the warp and weft yarns is substantially the same; and The average filament diameter of the warp yarn is 3.7 μm or more and 4.3 μm or less, The average filament diameter of the weft yarn is 4.2 μm or more and 5.3 μm or less, The ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) is 1.07 or more and 1.40 or less; 5) The average filament diameters of the warp and weft yarns are substantially the same, and The average number of warp filaments is 45 or more and 70 or less, The average number of filaments in the weft yarn is 55 or more and 80 or less, The ratio of the average number of filaments of the weft to the average number of filaments of the warp (weft / warp ratio) is greater than 1.25 and less than or equal to 1.50; Prepreg.
2. 2. The prepreg according to claim 1, wherein a gap width between adjacent weft yarns in the longitudinal direction (MD direction) is 40 μm or more and 80 μm or less.
3. A printed wiring board produced by using the prepreg according to claim 1 or 2.
Citation Information
Patent Citations
JP1975027335A
Television receiver
JP1983031665A
Precursor pitch fiber for carbon fiber
JP1984036726A
Glass fiber woven fabric for printed circuit board
JP1998245743A
Production method of prepreg, prepreg and multilayer board
JP2001269931A