Hot-dip Al-Zn-plated steel sheet, surface-treated steel sheet, painted steel sheet, and method for manufacturing hot-dip Al-Zn-plated steel sheet

The optimized composition and structure of the hot-dip Al-Zn coated steel sheet with controlled thickness and hardness, combined with a chemical conversion coating, effectively addresses the peeling issue at the unbent portion, enhancing adhesion and corrosion resistance.

JP7577817B1Active Publication Date: 2024-11-05JFE GALVANIZING & COATING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023189639
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-06
Publication Date
2024-11-05
Estimated Expiration
2043-11-06

Smart Images

  • Figure 0007577817000001_ABST
    Figure 0007577817000001_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a hot-dip Al-Zn plated steel sheet which has excellent plating adhesion in a bent-back portion even when the plating coating weight is large. [Solution] In order to achieve the above object, the present invention provides a hot-dip Al-Zn plated steel sheet having a coating layer formed thereon having a composition containing 40-70 mass% Al and 0.5-3.0 mass% Si, with the balance being Zn and unavoidable impurities, the coating layer having dendrites mainly composed of Al primary crystals and dendritic gaps containing Al-Zn eutectic, and a thickness X (μm) of the coating layer and a Vickers hardness HV of the Al primary crystals are 0.01 and satisfy the following relationships (1) and (2). HV 0.01 ≦-4X+205 (1) X≧23 (2)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot-dip Al-Zn coated steel sheet having excellent coating adhesion in a bent-back portion even when the coating weight is large, and a method for producing the same. [Background technology]

[0002] Hot-dip Al-Zn-plated steel sheets, which contain 20 to 95 mass% Al in the plating layer, such as 55% Al-Zn-plated steel sheets, are known to exhibit high corrosion resistance among hot-dip galvanized steel sheets because they combine the sacrificial corrosion protection properties of Zn with the high corrosion resistance of Al. For this reason, hot-dip Al-Zn-plated steel sheets are widely used in the field of building materials such as roofs and walls that are exposed to the outdoors for long periods of time, and in the field of civil engineering and construction such as guardrails, wiring and piping, soundproof walls, etc. In particular, for applications such as factory buildings, hot-dip Al-Zn-plated steel sheets are suitably used as long metal walls and roofing materials in shapes such as folded plates, square spans, and square corrugations, because of their low cost and excellent workability.

[0003] When hot-dip Al-Zn-plated steel sheets are used for long metal roofing materials, etc., they may be subjected to severe processing in order to be applied to weatherproofing areas such as wall edges and eaves. Specifically, after the steel sheets are first bent 180 degrees so as to overlap, a process called "rebending" may be required to return a portion of the sheet to its original smooth state. When such a bending process is performed, there is a problem that the plating layer around the bent-back portion (the portion returned to the smooth state after the 180-degree bending) of the hot-dip Al-Zn-plated steel sheet may peel off.

[0004] Here, Figure 1 shows an electron microscope observation of a cross section of a 55% Al-Zn-based plated steel sheet that has been subjected to a 180° close contact bend, and Figure 2 shows an electron microscope observation of a cross section of the 55% Al-Zn-based plated steel sheet after the 180° close contact bent portion has been returned to its original smooth state. As can be seen from Figure 1, after the 180° close bending, the inside of the plating layer in the bent part is subjected to compressive strain and bulges inward like a wave. The plating layer itself peels off from the Al-Fe alloy layer that exists at the interface between the plating layer and the steel sheet due to the bulge caused by the compressive stress, so when the bent part is subsequently returned to its original position, the plating layer in the returned part peels off significantly, as shown in Figure 2. In addition, peeling of the plating layer at the bent back section tends to occur more significantly when the plating layer is thicker, and the minimum coating weight on both sides, averaged over three points, is 150 g / m 2 If the coating weight is a general-purpose coating weight (for example, coating weight indication symbol AZ150 in JIS G 3322), there is little problem with peeling of the coating layer at the bent back part. However, for the purpose of high durability and high corrosion resistance, a minimum coating weight of 170 g / m2 on both sides (average of three points) is required. 2 In hot-dip Al-Zn coated steel sheets with the above coating weights (coating weight designations AZ170, AZ185, AZ200, etc. in JIS G 3322), peeling of the coating layer in the bent back portion is a major problem.

[0005] For this reason, various attempts have been made to improve the bending workability and corrosion resistance of bent parts of hot-dip Al-Zn plated steel sheets (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-156729 A [Patent Document 2] JP 2001-288551 A [Patent Document 3] JP 2002-363722 A [Patent Document 4] Patent Application No. 2022-113532 Summary of the Invention [Problem to be solved by the invention]

[0007] However, Patent Document 1 is a technology related to the resistance to bending back of 55% Al-Zn-plated steel sheet, i.e., the prevention of cracks caused by necking of the base steel during repeated bending back, while Patent Document 2 is a technology that suppresses the peeling phenomenon of the plating by nitriding the surface of the original sheet before forming the plating layer, thereby forming a discontinuous Al-Fe-based alloy layer that causes peeling. Therefore, neither of these technologies suppresses peeling of the plating layer in the bent back portion. In addition, Patent Documents 3 and 4 disclose a method for improving the elongation processability of plating without compressing the outer surface of the bent portion by measuring the Vickers hardness (HV 0.01 ) to be 120 or less, but the effect of the thickness of the coating layer is not taken into consideration, and further improvement was needed to address the phenomenon of coating peeling in parts of thick hot-dip Al-Zn coated steel sheets that have been bent back.

[0008] In view of the above circumstances, the present invention has an object to provide a hot-dip Al-Zn-plated steel sheet, a surface-treated steel sheet, and a painted steel sheet, which have excellent coating adhesion in a bent-back portion even when the coating weight is high, and a method for manufacturing the hot-dip Al-Zn-plated steel sheet. [Means for solving the problem]

[0009] The present inventors have conducted studies to solve the above-mentioned problems regarding hot-dip Al-Zn plated steel sheets having a coating layer having a composition containing 40 to 70 mass % Al, 0.5 to 3.0 mass % Si, with the balance being Zn and unavoidable impurities. As a result, they have found that by optimizing the relationship between the thickness of the coating layer and the Vickers hardness of the primary Al crystals constituting the dendrites in the coating layer, it is possible to improve the coating adhesion in the bent-back portion even when the coating weight is large.

[0010] The present invention has been made based on the above findings, and the gist of the present invention is as follows. 1. A hot-dip Al-Zn plated steel sheet having a plating layer formed thereon having a composition containing 40 to 70 mass% Al, 0.5 to 3.0 mass% Si, and the remainder being Zn and unavoidable impurities, The plating layer has dendrites mainly composed of Al primary crystals and dendritic gaps containing Al-Zn eutectic, The thickness X (μm) of the plating layer and the Vickers hardness HV 0.01 and (2) satisfy the following relationships (1) and (2): HV 0.01 ≦-4X+205 (1) X≧23 (2)

[0011] 2. The hot-dip Al-Zn plated steel sheet according to claim 1, characterized in that in a bending test conforming to JIS G 3322 (2019), a 180-degree close contact bend is performed with a width of 125 mm without placing a plate in the inner space between the bends, the close contact bent portion is returned and smoothed, and then an adhesive tape is applied to the surface of the returned portion that was on the inside during the close contact bend, and the tape is peeled off in a direction perpendicular to the bend line of the returned portion, and the maximum width of the peeled plating layer adhering to the adhesive tape in the direction perpendicular to the bend line is 1 mm or less.

[0012] 3. A surface-treated steel sheet, comprising the hot-dip Al-Zn-plated steel sheet according to 1 or 2 above, and a chemical conversion coating formed on the hot-dip Al-Zn-plated steel sheet.

[0013] 4. A coated steel sheet comprising the hot-dip Al-Zn-plated steel sheet according to 1 or 2 above, and a coating film formed directly or via an intermediate layer on the hot-dip Al-Zn-plated steel sheet.

[0014] 5. A step of forming a plating layer having a plating thickness of X (μm) per side on a base steel sheet using a plating bath having a composition containing 40 to 70 mass% Al and 0.5 to 3.0 mass% Si, with the remainder being Zn and unavoidable impurities; and reheating the steel sheet on which the plating layer is formed. a manufacturing method for a hot-dip Al-Zn coated steel sheet, characterized in that the following relationships (2), (3) and (4) are satisfied, where T°C is the maximum temperature reached by the steel sheet during reheating, and y (hr) is the cooling time from T°C to 100°C: X≧23 (2) 150≦T≦300 (3) 0.5≦y≦24 (4) Effect of the Invention

[0015] Effects of the Invention The present invention can provide a hot-dip Al-Zn-plated steel sheet, a surface-treated steel sheet, and a painted steel sheet, which have excellent coating adhesion in the unbent portion even when the coating weight is high, and a method for manufacturing a hot-dip Al-Zn-plated steel sheet. [Brief description of the drawings]

[0016] [Figure 1] This is an electron microscope photograph of the cross section of a 55% Al-Zn coated steel sheet that has been subjected to 180 degree close bending. [Diagram 2] This is an electron microscope photograph of the cross section of a 55% Al-Zn plated steel sheet that had peeled off of the plating layer when it was returned to its original flat and smooth state after being subjected to a 180 degree close bending. [Diagram 3] This is an electron microscope photograph of the cross section of a 55% Al-Zn plated steel sheet in which peeling of the plating layer was suppressed when the sheet was returned to its original flat and smooth state after being subjected to a 180-degree close bending. [Figure 4] 1 is a graph showing the relationship between the thickness of the plating layer, the Vickers hardness HV0.01 of the Al primary crystal in the plating layer, and the presence or absence of peeling of the plating layer in the unbent portion for each sample of coated steel sheet produced in Examples and Comparative Examples. [Diagram 5] FIG. 1 is a schematic diagram showing a state in which adhesive tape is applied to the surface of a bent-back portion of an Al-Zn-plated steel sheet in order to measure the maximum width of the peeled plating layer in the direction perpendicular to the bend line. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] (Hot-dip Al-Zn coated steel sheet) The hot-dip Al-Zn plated steel sheet of the present invention has a plating layer on the surface of the steel sheet. Here, the coating layer has a composition containing 40 to 70 mass% Al, 0.5 to 3.0 mass% Si, and the balance being Zn and unavoidable impurities. When the coating layer of the hot-dip galvanized steel sheet has the above-mentioned composition, good corrosion resistance can be achieved. The plating layer is composed of an interface alloy layer present at the interface side with the base steel sheet and a main layer present on the interface alloy layer.

[0018] The Al content in the plating layer is 40 to 70 mass %, and preferably 50 to 60 mass %, in view of the balance between corrosion resistance and operability. If the Al content in the coating layer is at least 40 mass%, dendritic solidification of Al primary crystals occurs, and a structure consisting of a portion where Al is solidified into dendrites (α-Al dendritic phase) and the remaining portion between the dendrites (interdendritic phase) can be obtained, in which the dendritic phase is laminated in the thickness direction of the coating layer. By adopting a structure in which the dendritic solidification structure is laminated in the thickness direction of the coating layer, the corrosion progression path of the coating layer becomes complex, and the corrosion resistance can be improved. In addition, the more dendrites are laminated, the more complex the corrosion progression path becomes, making it difficult for corrosion to easily reach the base steel sheet, and improving the corrosion resistance. On the other hand, if the Al content in the plating layer exceeds 70 mass%, the content of Zn, which has a sacrificial corrosion protection effect against Fe, decreases, and corrosion resistance deteriorates. For this reason, the Al content in the plating layer is set to 70 mass% or less. Also, if the Al content in the plating layer is 60 mass% or less, even when the coating weight of the plating is reduced and the base steel sheet is easily exposed, the plating layer has a sacrificial corrosion protection effect against Fe, and sufficient corrosion resistance can be obtained. For this reason, the Al content in the plating main layer is preferably set to 60 mass% or less.

[0019] Si is added to the plating layer to suppress the growth of an interfacial alloy layer that forms at the interface with the base steel sheet, and to improve the adhesion, corrosion resistance, workability, etc. between the plating layer and the base steel sheet. In the case of the hot-dip Al-Zn-plated steel sheet of the present invention, when the steel sheet is immersed in an Al-Zn-plating bath containing Si, the Fe on the steel sheet surface reacts with the Al and Si in the plating bath to form a layer of Fe-Al and / or Fe-Al-Si intermetallic compounds at the interface between the base steel sheet and the plating layer (an interfacial alloy layer is formed). Since the growth rate of this Fe-Al-Si alloy is slower than that of the Fe-Al alloy, the higher the ratio of the Fe-Al-Si alloy, the more the growth of the entire alloy phase can be suppressed. Therefore, the Si content in the plating layer must be 0.5 mass% or more. On the other hand, the excess Si that is not consumed in the formation of the interface alloy layer precipitates as a Si phase in the plating layer, but the Si phase is electrochemically more noble than the Al primary crystal and the Al-Zn eutectic and acts as a cathode, which promotes corrosion of the plating layer and reduces its corrosion resistance. Specifically, when the Si content in the plating layer exceeds 3.0 mass%, not only does the effect of inhibiting the growth of the alloy phase described above saturate, but the amount of the Si phase increases and corrosion is promoted, so the Si content is set to 3.0 mass% or less. From the same viewpoint, the Si content in the plating layer is more preferably 2.5 mass % or less.

[0020] The plating layer contains Zn as a main component of the plating layer. By including Zn in the plating layer, a sacrificial anticorrosive effect can be obtained, and it becomes possible to improve the corrosion resistance. The content of Zn is not particularly limited, but when it is 80 mass% or less, it is preferable in that the Al content can be secured and the above-mentioned corrosion resistance due to the dendrite phase and the interdendritic phase can be realized.

[0021] Moreover, the plating layer contains unavoidable impurities. The unavoidable impurities include components of the base steel sheet that are incorporated into the plating due to a reaction between the plating bath and the base steel sheet during the plating process, unavoidable impurities contained in the ingots used when preparing the plating bath, and unavoidable impurities that are slightly eluted from equipment in the bath. The components of the base steel sheet taken in during the plating may include a few percent of Fe. Examples of the types of unavoidable impurities in the plating bath include Fe, Mn, P, S, C, Nb, Ti, B, etc. as the components of the base steel sheet. Furthermore, examples of impurities in the ingot include Fe, Pb, Sb, Cd, As, Ga, V, etc. Furthermore, examples of impurities from the equipment in the bath include Cr, Ni, W, Co, etc. It is not possible to quantitatively determine Fe in the coating layer by distinguishing between Fe taken in from the base steel sheet and Fe in the coating bath. The total content of the unavoidable impurities is not particularly limited, but from the viewpoint of maintaining the corrosion resistance and uniform solubility of the coating, the total amount of unavoidable impurities excluding Fe is preferably 1.0 mass% or less. Furthermore, the total content including the unavoidable impurity Fe is not particularly limited, but if contained in excess, it may affect various properties of the plated steel sheet, and therefore the total content is preferably 5.0 mass% or less, and more preferably 3.0 mass% or less.

[0022] Furthermore, the hot-dip Al-Zn plated steel sheet of the present invention may contain up to 5 mass % of optional additive elements in addition to the above-mentioned components. The optional additive components can be appropriately selected depending on the performance required for the plating layer, and examples thereof include alkaline earth metals such as Ca and Mg, and additive components such as Mn, V, Cr, Mo, Ti, Sr, Ni, Co, Sb, and B. Although these optional components have the effect of further improving corrosion resistance, they may reduce the workability of the plating layer and deteriorate the ultimate elongation of the hot-dip Al-Zn plated steel sheet. Therefore, the content of these optional components is preferably 5 mass% or less.

[0023] The optional addition of Mg and Ca results in the corrosion product containing Mg and / or Ca when the plating layer corrodes, improving the stability of the corrosion product and slowing down the progression of corrosion, resulting in improved corrosion resistance. The total content of Ca and / or Mg in the plating layer is not particularly limited as long as it is 5 mass% or less, but is preferably 0.01 to 5 mass%. By setting the total content to 0.01 mass% or more, a sufficient corrosion retardation effect can be obtained, while by setting the total content to 5 mass% or less, the effect does not become saturated, an increase in production costs is suppressed, and the composition of the plating bath can be easily controlled.

[0024] Furthermore, the plating layer preferably contains at least Mg as the optional added component. When the plating layer contains Mg, Mg2Si can be produced together with Si, and a corrosion retardation effect can be obtained. Here, the content of Mg in the plating layer is preferably 0.01 to 5 mass%, more preferably 2 to 4.9 mass%.

[0025] The means for forming the plating layer on the base steel sheet is not particularly limited, and a typical continuous hot-dip plating facility can be used. For example, a base steel sheet is heated to a predetermined temperature in an annealing furnace maintained in a reducing atmosphere, and while annealing, rolling oil and the like adhering to the steel sheet surface is removed, and an oxide film is reduced and removed, and then the steel sheet is immersed in a hot-dip galvanizing bath containing predetermined concentrations of Al and Zn through a snout whose lower end is immersed in the coating bath. The steel sheet immersed in the coating bath is then pulled up above the coating bath via a sink roll, and pressurized gas is sprayed from a gas wiping nozzle arranged above the coating bath toward the surface of the steel sheet to adjust the coating weight, and the steel sheet is then cooled by a cooling device, thereby forming a coating layer. The cooling rate after plating (after the steel sheet is removed from the plating bath) is not particularly limited, and can be set to normal conditions (for example, 12° C. / s or more).

[0026] The composition of the plating layer can be confirmed, for example, by immersing the plating layer in hydrochloric acid or the like to dissolve it, and subjecting the solution to ICP emission spectrometry, atomic absorption spectrometry, etc. This method is merely one example, and any method that can accurately quantify the composition of the plating layer may be used, and is not particularly limited.

[0027] The coating layer of the hot-dip Al-Zn coated steel sheet obtained according to the present invention has a composition substantially equivalent to that of the coating bath as a whole, and therefore the composition of the coating layer can be controlled with high precision by controlling the composition of the coating bath.

[0028] In the hot-dip Al-Zn-coated steel sheet of the present invention, the thickness X (μm) of the coating layer and the Vickers hardness HV of the primary Al crystals constituting the dendrites in the coating layer are 0.01 and satisfy the following relationships (1) and (2). HV 0.01 ≦-4X+205 (1) X≧23 (2)

[0029] Regarding the adhesion of the coating layer in the bent-back portion of the above-mentioned hot-dip Al-Zn coated steel sheet, it has been found that there is a correlation between the thickness X of the coating layer and the hardness of the coating layer. In the present invention, the Vickers hardness HV of the Al primary crystal, which has a large effect on the hardness of the plating layer, 0.01 By appropriately controlling in accordance with the thickness of the coating layer, that is, by satisfying formula (1), when a steel sheet is bent by 180 degrees in close contact, a reaction force (a reaction force directly leading to peeling of the coating) that tends to cause the coating layer to bulge further inward, which is generated due to compressive strain in the bent coating layer on the inner side of the bent part, can be suppressed. As a result, the hot-dip Al-Zn coated steel sheet of the present invention can maintain a high level of coating adhesion in the unbent part even when the coating adhesion is high.

[0030] Specifically, in the case of the hot-dip Al-Zn-plated steel sheet of the present invention, in a bending test conforming to JIS G 3322 (2019), a 180-degree close bending is performed with a width of 125 mm without sandwiching a plate in the inner interval of the bend, and after the close bending portion is returned and smoothed, as shown in FIG. 5, an adhesive tape is applied to the surface of the bent back portion that was on the inside during the close bending, and then peeled off in a direction perpendicular to the bend line of the bent back portion. It is preferable that the maximum width A of the peeled plating layer attached to the adhesive tape in the direction perpendicular to the bend line is 1 mm or less, and it is more preferable that there is no peeling of the plating layer. The range of the adhesive tape to be applied to the bent back portion of the hot-dip Al-Zn-plated steel sheet is not particularly limited, but from the viewpoint of being able to more reliably confirm the presence or absence of peeling of the plating layer, it is preferable that the width W of the applied adhesive tape in the direction along the bend line of the bent back portion is 18 mm or more. It is more preferable to apply multiple sheets of adhesive tape in parallel to widen the evaluation range. This makes it possible to obtain plating adhesion at the bent-back portion at a level sufficient for practical use.

[0031] In the hot-dip Al-Zn coated steel sheet of the present invention, the thickness X of the coating layer is 23 μm or more (satisfies formula (2): X≧23). Since peeling of the coating layer around the bent-back portion of the hot-dip Al-Zn coated steel sheet, which is a problem in the present invention, tends to occur more significantly when the coating layer is thick, the effect of improving coating adhesion in the bent-back portion according to the present invention can be more effectively achieved when the thickness X of the coating layer is as large as 23 μm or more.

[0032] The thickness of the coating layer can be measured, for example, by embedding a cross section of the hot-dip Al-Zn-coated steel sheet in a room-dry resin, cutting, polishing, and then observing it with a scanning electron microscope (SEM). In this case, the accuracy can be improved by sampling from multiple points, for example, about five points, along the width direction of the hot-dip Al-Zn-coated steel sheet (usually about 1,000 mm), and calculating the average value. Another method for calculating the thickness of the coating layer is the coating weight test method described in JIS H 0401, in which the coating film of a sample of a certain area (approximately 70 mmφ) is removed with a remover or the like, weighed, and then the coating layer is dissolved in a test solution prepared by dissolving 3.5 g of hexamethylenetetramine in 1 liter of 1+1 hydrochloric acid, and then weighed again to calculate the coating weight per unit area. This value can be used as the specific gravity of the coating layer of hot-dip Al-Zn coated steel sheet, 3.7 g / μm m. 2 The plating thickness can be calculated by dividing by . In this case, too, accuracy can be improved by sampling from multiple points, for example, three points.

[0033] Regarding the thickness of the plating layer, in the present invention, a coating weight equal to or greater than the coating weight designation symbol AZ170 described in JIS G 3321 is considered to be thick. The three-point average minimum coating weight of AZ170 is 170 g / m 2 In this case, the plating thickness per side is: 170 g / m 2 ÷2÷3.7 g / μm m 2 Therefore, it is 23 μm. Similarly, AZ185: 185 g / m 2 ÷2÷3.7 g / μm m 2 Approximately 25 μm AZ200: 20 g / m 2 ÷2÷3.7 g / μm m 2 Approximately 27 μm The peeling of the coating layer around the bent back portion on the inner bend side of the hot-dip Al-Zn coated steel sheet, which is the subject of the present invention, tends to occur significantly as the coating layer becomes thicker. Therefore, in formula (2), X≧23 is specified.

[0034] Here, the Vickers hardness is measured with a 10g indentation load (HV 0.01 ) testing is being carried out. For example, a sample of hot-dip Al-Zn plated steel sheet is embedded in resin and polished so that the cross section of the sample can be observed. The primary Al crystal part of the cross section is then indented with a Vickers tester using an indenter, and the Vickers hardness can be calculated from the average horizontal and vertical lengths of the indentation made with a test force of 98.07 mN and a holding time of 10 seconds.

[0035] The plating layer has dendrites mainly composed of Al primary crystals and dendritic gaps containing Al-Zn eutectic, the Al primary crystals contain an α-Al phase matrix and Zn precipitates, and the Zn content in the matrix is ​​preferably 30 mass% or less. In the present invention, the coating layer is reheated to soften it and thereby improve its workability. This softening occurs due to the crystallization of Zn from the Al primary crystals as described above. In this case, the Zn concentration in the Al primary crystal matrix decreases compared to that before the heat treatment due to the crystallization of Zn; specifically, it is preferable that the Zn concentration be 30 mass % or less.

[0036] The Vickers hardness HV of the primary Al crystal 0.01 The method for controlling the hardness is not particularly limited, and the coating layer is softened by the cooling conditions after hot-dip coating or the reheating treatment of the coating layer described later, so that the Vickers hardness HV of the Al primary crystal satisfies the above formula (1). 0.01 can be controlled.

[0037] The interfacial alloy layer in the coating layer is a layer of the coating layer that exists at the interface with the base steel sheet and is a lamellar interfacial alloy layer containing Fe, Al, Si, Zn and unavoidable impurities. As described above, the interfacial alloy layer is inevitably formed by an alloying reaction between Fe on the surface of the base steel sheet and Al and Si in the coating bath. This interface alloy layer is hard and brittle, and if it grows too thick, it will become the starting point of cracks during processing, so it needs to be as thin as possible. Therefore, in the hot-dip Al-Zn-plated steel sheet of the present invention, the thickness of the interface alloy layer needs to be 2 μm or less, and is preferably 1 μm or less. If the thickness of the interface alloy layer exceeds 2 μm, the plating adhesion of the bent-back portion will be reduced.

[0038] The interfacial alloy layer is the average of the measured average thicknesses of the interfacial alloy layer present in three or more fields of view when the cross section of the plating layer is observed using a scanning electron microscope (SEM) or the like. The method for suppressing the thickness of the interface alloy layer is not particularly limited, and examples thereof include the method of adjusting the Si content in the plating layer as described above, and the method of adjusting the cooling time when applying a thermal history after forming the plating layer as described below.

[0039] (Surface-treated steel sheet) The surface-treated steel sheet of the present invention is characterized in that a chemical conversion coating is formed on the hot-dip Al-Zn plated steel sheet of the present invention. The chemical conversion coating is not particularly limited and can be appropriately selected according to the required performance. For example, both chromate chemical conversion coating and chromate-free chemical conversion coating can be used. For example, a chromate-free chemical conversion coating can be used, which is a composite of a resin component and an inorganic component, and contains 70 to 90 mass% of a mixture of a urethane resin and an epoxy resin containing a curing agent, and contains 2 to 10 mass% of phosphorus oxide and 8 to 20 mass% of zirconium oxide as inorganic components.

[0040] The coating weight of the chemical conversion coating is 0.025 to 0.5 g / m 2 It is preferable that the thickness is 0.025 g / m 2 If the thickness is less than 0.5 g / m, the adhesion to the underlying aluminum-zinc alloy plated steel sheet and the upper primer coating film may decrease, and the corrosion resistance may decrease. 2If it exceeds this value, the chemical conversion coating will be prone to destruction (peeling off) when subjected to severe bending, and the corrosion resistance may also decrease.

[0041] The chemical conversion coating can be obtained by continuously applying a chemical conversion solution to a hot-dip Al-Zn-plated steel sheet using a roll coater or the like, and then drying the sheet at a peak metal temperature (PMT) of about 60°C to 200°C using hot air or induction heating.

[0042] (painted steel plate) The coated steel sheet of the present invention is characterized in that a coating film is formed directly or via an intermediate layer on the hot-dip Al-Zn plated steel sheet of the present invention. By forming the coating film, it is possible to impart a beautiful appearance and also to improve various performances such as processability, weather resistance, chemical resistance, stain resistance, water resistance, and corrosion resistance.

[0043] The type of the coating film and the method for forming the coating film are not particularly limited, and can be appropriately selected depending on the required performance. Examples of the paint used to form the coating film include polyester resin paints, silicone polyester resin paints, polyurethane resin paints, acrylic resin paints, and fluororesin paints. In particular, fluororesin paints are preferred from the standpoint of corrosion resistance and weather resistance.

[0044] The thickness of the coating film is not particularly limited. For example, the thickness of the coating film can be 5 to 30 μm. By making the thickness 5 μm or more, the color tone and appearance can be stabilized, and by making the thickness 30 μm or less, the decrease in processability (the occurrence of cracks in the coating film) can be more reliably suppressed.

[0045] Depending on the purpose and application, the coating film may contain appropriate amounts of additives other than chromate compounds, such as titanium oxide, red iron oxide, mica, carbon black, and other various coloring pigments, metallic pigments such as aluminum powder and mica, extender pigments made of carbonates or sulfates, or various fine particles such as silica fine particles, nylon resin beads, and acrylic resin beads, curing catalysts such as p-toluenesulfonic acid and dibutyltin dilaurate, wax, and other additives.

[0046] There is no particular restriction on the method of applying the coating composition to form the coating film, but the coating composition can be preferably applied by a method such as roll coater coating, curtain flow coating, etc. After the coating composition is applied, the coating film is obtained by baking using a heating means such as hot air heating, infrared heating, induction heating, etc. The baking process is usually performed at a maximum plate temperature of about 180 to 270°C for about 30 seconds to 3 minutes in this temperature range.

[0047] The intermediate layer is not particularly limited as long as it is a layer formed between the coating layer of the hot-dip plated steel sheet and the coating film. Examples of the intermediate layer include a paint base chemical conversion coating film and a primer such as an adhesive layer. The paint base chemical conversion coating film can be formed by, for example, a chromate paint base treatment or a chrome-free paint base chemical conversion coating film, which is applied with a chromate paint base treatment liquid or a chrome-free paint base chemical conversion coating liquid, and dried at a steel sheet temperature of 80 to 300°C without rinsing with water. These paint base chemical conversion coating films may be single-layered or multi-layered, and in the case of multi-layered, multiple paint base chemical conversion treatments may be performed sequentially.

[0048] (Method of manufacturing hot-dip Al-Zn coated steel sheet) The method for producing a hot-dip Al-Zn-plated steel sheet of the present invention (hereinafter, sometimes referred to as "the production method of the present invention") includes the steps of forming a plating layer having a plating thickness of X (μm) per side on a base steel sheet using a plating bath having a composition containing 40 to 70 mass% Al and 0.5 to 3.0 mass% Si, with the balance being Zn and unavoidable impurities; and reheating the steel sheet on which the plating layer is formed.

[0049] In addition, the means for forming the plating in the step of forming the plating layer on the base steel sheet is not particularly limited. For example, the base steel sheet can be produced by cleaning, heating, and immersing in a plating bath in a continuous hot-dip galvanizing facility.

[0050] The type of base steel sheet used in the manufacturing method of the present invention is not particularly limited. For example, a hot-rolled steel sheet or strip that has been pickled and descaled, or a cold-rolled steel sheet or strip obtained by cold rolling the hot-rolled steel sheet or strip may be used. Furthermore, the steel components are not particularly limited in the present invention, but for example, a steel containing 0.01 to 0.10 mass% C can be used. However, the present invention does not exclude steel sheets containing less than 0.01% C. In addition to the component elements C, Al, Si, Mn, and P, it is also possible to add N, S, O, B, V, Nb, Ti, Cu, Mo, Cr, Co, Ni, Ca, Sr, In, Sn, Sb, etc. as trace additive elements.

[0051] In addition, the method for obtaining the base steel sheet is not particularly limited. For example, in the case of the hot-rolled steel sheet, one that has been subjected to a hot rolling process and a pickling process can be used, and in the case of the cold-rolled steel sheet, it can be manufactured by further adding a cold rolling process. Furthermore, in order to obtain the properties of the steel sheet, it is also possible to go through a recrystallization annealing process or the like before the hot-dip plating process.

[0052] As described above, the plating bath used in forming the plating layer has a composition that is substantially the same as the plating bath as a whole, and therefore contains 40 to 70 mass % Al, 0.5 to 3.0 mass % Si, and the remainder being Zn and unavoidable impurities.

[0053] In the manufacturing method of the present invention, the thickness of the plating layer is controlled so as to satisfy the following formula (2). X ≧ 23(μm) (2) The thickness and coating weight of the coating layer can be controlled by adjusting the air pressure sprayed from slit nozzles from both sides of the steel sheet when the steel sheet is immersed in a hot-dip coating bath in a continuous hot-dip coating facility and then pulled out, thereby changing the amount of material scraped off. The gas used for the air wiping is not particularly limited, and air, nitrogen, etc., can be used.

[0054] The manufacturing method of the present invention includes a step of reheating the steel sheet on which the plating layer has been formed, and when the maximum temperature that the steel sheet reaches during the reheating is T°C and the cooling time from T°C to 100°C is y (hr), the following relationships (3) and (4) are satisfied. 150≦T≦300 (3) 0.5≦y≦24 (4)

[0055] The above formula (3) specifies the range of the maximum temperature T to be reached when reheating the steel sheet on which the coating layer is formed. The reason why the maximum temperature T is set to 150°C or more is that if the temperature is not this temperature or higher, sufficient softening of the coating layer does not occur, and sufficient bending workability of the hot-dip Al-Zn-coated steel sheet cannot be obtained. From the same viewpoint, the maximum temperature T is preferably set to 160°C or more. On the other hand, the reason why the maximum temperature T is set to 300°C or less is that if the temperature is higher than this temperature, the thickness of the interfacial alloy layer generated at the interface between the coating and the steel sheet becomes thick, resulting in a decrease in bending workability. From the same viewpoint, the maximum temperature T is preferably set to 280°C or less.

[0056] The above formula (4) is defined in order to maintain high levels of plating adhesion and productivity in the bent-back portion, taking into consideration the thickness T of the formed plating layer and the maximum temperature T reached during reheating. If the cooling time (residence time) y in the above formula (4) is less than 0.5 hours, the plating layer cannot be sufficiently softened, and good bending workability and plating adhesion in the bent-back portion cannot be ensured. On the other hand, if the cooling time (residence time) y exceeds 24 hours, productivity decreases. From the same viewpoint, the cooling time (residence time) y is preferably 0.5≦y≦12.

[0057] In the manufacturing method of the present invention, the average heating rate from room temperature to the maximum temperature T°C when reheating the steel sheet is preferably 3°C / hr or more, more preferably 4°C / hr, and even more preferably 5°C / hr, in order to prevent the residence time in the high temperature range from becoming excessively long in order to improve the workability, although this is not particularly limited. Furthermore, the average cooling rate from the maximum temperature T°C to room temperature when cooling the reheated steel sheet is preferably 20°C / hr or less, more preferably 15°C / hr or less, and even more preferably 10°C / hr or less, in order to ensure the minimum residence time in the high temperature range required to improve the workability.

[0058] In the manufacturing method of the present invention, when a chemical conversion coating is formed on the plating layer, the chemical conversion coating may be formed either before or after the reheating. However, when the chemical conversion coating is formed before the reheating, it is preferable to reduce the resin component of the chemical conversion coating, add an aggregate, or prevent the chemical conversion coatings from adhering to each other when reheating with a coil.

[0059] In the manufacturing method of the present invention, as described above, it is sufficient to satisfy the conditions in the step of forming a coating layer and the step of reheating the steel sheet on which the coating layer has been formed, and other manufacturing conditions are not particularly limited. They can be appropriately selected from known manufacturing conditions for hot-dip Al-Zn coated steel sheets depending on the required performance.

[0060] The method may further include a step of forming a chemical conversion coating on the hot-dip Al-Zn-plated steel sheet obtained by the above-mentioned method for producing a hot-dip Al-Zn-plated steel sheet of the present invention. The type and method of forming the chemical conversion coating are the same as those explained in the surface-treated steel sheet of the present invention.

[0061] Furthermore, the method may further include a step of forming a coating film directly or via an intermediate layer on the hot-dip Al-Zn-plated steel sheet obtained by the above-mentioned method for producing a hot-dip Al-Zn-plated steel sheet of the present invention. The types and methods of forming the coating film and intermediate layer are the same as those explained in the coated steel sheet of the present invention. EXAMPLES

[0062] <Samples 1-14> (1) Formation of plating layer, reheating A cold-rolled steel sheet having a thickness of 0.35 mm manufactured by a conventional method was used as a base steel sheet (steel sheet consisting of C: 0.06 mass%, Si: 0.02 mass%, Mn: 0.3 mass%, Al: 0.05 mass%, P: 0.02 mass%, S: 0.02 mass%, N: 0.01 mass%, the balance being Fe and unavoidable impurities), and was subjected to annealing treatment, plating treatment, and skin pass treatment in a continuous hot-dip plating facility. Note that, for all samples, the plating treatment was performed under the following conditions: the bath temperature of the plating bath was 590°C, the entry sheet temperature was 600°C, and the skin pass reduction rate was 0.5%. After that, the steel sheets were subjected to heat treatment (reheating treatment) in a batch heating furnace under the conditions shown in Table 1. The temperature of the steel sheets during the reheating treatment was measured using a thermocouple attached to the steel sheets. Furthermore, this coil was subjected to a paint base conversion treatment in a continuous painting line, and a primer and top coat were painted. For some samples, an elongation of 0.1% was given to the steel sheets using a tension leveler after painting.

[0063] (2) Thickness of plating layer, Vickers hardness HV of primary aluminum 0.01 The thickness of the plating layer of each sample was measured by cross-sectional observation of the plating layer using an SEM (X1000), and the average value of 10 points was calculated. In addition, the Vickers hardness HV of the primary Al crystals in the dendritic phase in the plating layer of each sample was 0.01For the Vickers hardness, each sample was embedded in a room temperature drying resin, polished, and the dendrite phase of the plating layer was selected from the cross section, and the Vickers hardness of the selected dendrite phase was measured using a microhardness tester (Shimadzu Corporation, Shimadzu Microhardness Tester HMV-G21). The measurement method was in accordance with JIS Z 2244, and the indentation load was 10 gf.

[0064] (3) Formation of chemical conversion coatings, primers, and coatings (3-1) Chemical conversion coating for paint base Thereafter, a paint base chemical conversion coating, a primer, and a paint film were successively formed on each of the obtained sample hot-dip Al-Zn-plated steel sheets. The resin component in the base coating was "Yuka Resin RE-1050" manufactured by Yoshimura Oil Chemical Co., Ltd., an epoxy resin having a bisphenol skeleton, and was used in an amount of 43 mass% in terms of solid content in the base coating. The vanadium compound contained in the paint base chemical conversion coating was 6 mass% of an organic vanadium compound chelated with acetylacetone, the zirconium compound contained in the paint base chemical conversion coating was 50 mass% ammonium zirconium carbonate, and the fluorine compound contained in the paint base chemical conversion coating was 1 mass% ammonium fluoride, calculated as fluorine atoms, each of which was used in terms of the solid content in the paint base chemical conversion coating. These raw materials were mixed to obtain a chemical conversion treatment liquid. The pH of the paint base chemical conversion treatment liquid was set to 8-10. This paint base conversion treatment liquid was applied with a roll coater, then heated in an oven at 200°C for 2 seconds and air-dried, resulting in a coating weight of 0.1 g / m 2 A chemical conversion coating was formed as a base for painting. (3-2) Primer The paint for forming the primer was prepared in the following manner. The resin component of the primer was a mixture of a bisphenol A type epoxy resin (product name "JER 1009", manufactured by Mitsubishi Chemical Corporation), which is an epoxy resin having a urethane bond, reacted with a blocked polyisocyanate compound (product name "Desmodur BL-3175", manufactured by Sumika Bayer Urethane Co., Ltd.) in a mass ratio of 85:15, and a melamine resin, n-butylated melamine resin (product name "U-Ban 122", manufactured by Mitsui Chemicals, Inc.), in a ratio of 9:1. In addition, magnesium vanadate was used as the vanadium compound of the rust-preventive pigment contained in the primer, and calcium phosphate was used as the phosphate compound contained in the primer, each of which was used at 12 mass % in the coating film. After adding a solvent and an anti-rust pigment to the above resin, 0.3 parts of dibutyltin dilaurate (DBTDL) was added as a reaction catalyst and mixed uniformly to obtain a chrome-free primer coating composition. (3-3) Coating The following paints were used for the coating. Melamine-cured polyester paint (black) "Precolor HD-0030HR" (Akzo Nobel Coatings Co., Ltd.) The above coating paint was applied onto the formed primer using a roll coater, baked at PMT 260°C for a baking time of 40 seconds, and then cooled with water to form a coating film so that the film thickness after baking was 17 μm as shown.

[0065] <Evaluation> The following evaluations were carried out on each of the coated steel sheet samples obtained as described above. The evaluation results are shown in Table 1.

[0066] (1) Bending adhesion A bending test was conducted on each sample of coated steel sheet in accordance with JIS G 3322 (2019). After cutting into a width of 125 mm, a 180-degree close bending (hereinafter sometimes referred to as "0T bending") was performed without sandwiching a plate between the inner spaces of the bend so that the surface on which the coating film was formed was on the inside. Then, a scraper was inserted on the inner side of the bent part to open the close contact part, and after smoothing it to a certain extent, it was pressed with a vice to completely smooth the bent part, forming a bent-back part. Then, cellophane adhesive tape was applied to the entire bent-back part on the inner side, and peeled off in a direction perpendicular to the bend line of the bent-back part. Then, the width of the peeled-off plating layer adhering to the peeled adhesive tape in the direction perpendicular to the bend line was measured to obtain the maximum width. This measurement was performed at five points in the coil width direction, and the average value was evaluated according to the following criteria. ○: No peeled pieces attached to the tape, or only tiny peeled pieces less than 1 mm in size △: 1 to 2 mm peeled off piece on tape ×: Tape has peeled pieces of 3 mm or more In addition, for each sample, the thickness of the plating layer and the Vickers hardness HV of the primary Al crystals in the plating layer were 0.01 A graph was created showing the relationship between the evaluation of peeling of the plating layer at the bent-back portion and the test results, and is shown in Figure 4.

[0067] (2) Corrosion resistance of bent back parts As described above, each sample of coated steel sheet was bent 180 degrees in accordance with JIS G 3322 (2019) and returned to a smooth state (after forming the bent-back portion), after which an outdoor exposure test was conducted in Chuo-ku, Chiba City. After 4 years and 8 months of exposure testing, the bent-back portion was visually observed and evaluated according to the following criteria. The evaluation results are shown in Table 1. (Evaluation Criteria) 1 point: Clear red rust 2 points: Slight red rust 3 points: No red rust

[0068] [Table 1]

[0069] From the results in Table 1 and FIG. 4, it can be seen that the samples of the invention are excellent in both plating adhesion and corrosion resistance of the unbent portion in a well-balanced manner compared to the samples of the comparative examples. [Industrial Applicability]

[0070] Effects of the Invention The present invention can provide a hot-dip Al-Zn-plated steel sheet, a surface-treated steel sheet, and a painted steel sheet, which have excellent coating adhesion in the unbent portion even when the coating weight is high, and a method for manufacturing a hot-dip Al-Zn-plated steel sheet.

Claims

1. A hot-dip Al-Zn plated steel sheet having a plating layer formed thereon, the plating layer having a composition containing 40 to 70 mass% Al, 0.5 to 3.0 mass% Si, and the balance being Zn and unavoidable impurities, The plating layer has dendrites mainly composed of Al primary crystals and dendritic gaps containing Al-Zn eutectic, The Zn content in the matrix of the α-Al phase in the Al primary crystal is 30 mass% or less, The thickness X (μm) of the plating layer and the Vickers hardness HV 0.01 and (2) satisfy the following relationships (1) and (2): HV 0.01 ≦-4X+205...(1) X≧23 ... (2)

2. The hot-dip Al-Zn coated steel sheet according to claim 1, characterized in that in a bending test in accordance with JIS G 3322 (2019), a 180-degree close bending is performed with a width of 125 mm without placing a plate in the inner space of the bend, the close bending portion is returned to be smooth, and then an adhesive tape is applied to the surface of the returned portion that was on the inside during the close bending, and the tape is peeled off in a direction perpendicular to the bend line of the returned portion, and the maximum width of the peeled plating layer adhering to the adhesive tape in the direction perpendicular to the bend line is 1 mm or less.

3. A surface-treated steel sheet, comprising the hot-dip Al-Zn plated steel sheet according to claim 1 or 2, and a chemical conversion coating formed on the hot-dip Al-Zn plated steel sheet.

4. A coated steel sheet comprising the hot-dip Al-Zn plated steel sheet according to claim 1 or 2, and a coating film formed directly or via an intermediate layer on the hot-dip Al-Zn plated steel sheet.

5. forming a plating layer having a plating thickness of X (μm) per side on a base steel sheet using a plating bath having a composition containing 40 to 70 mass% Al, 0.5 to 3.0 mass% Si, and the balance being Zn and unavoidable impurities; and reheating the steel sheet on which the plating layer is formed. When the maximum temperature reached by the steel plate during the reheating is T°C and the cooling time from T°C to 100°C is y (hr), the following relationships (2), (3), and (4) are satisfied: X≧23 ... (2) 160≦T≦300 ... (3) 0.5≦y≦5 ... (4) The average cooling rate from the maximum temperature T°C to room temperature is 10°C / hr or less, A method for producing a hot-dip Al-Zn plated steel sheet, characterized in that an average heating rate from room temperature to the maximum temperature T°C during the reheating is 3°C / hr or more.

Citation Information

Patent Citations

  • Hot dip aluminized steel sheet excellent in plating adhesion

    JP2001288551A

  • Coated hot dip al-zr alloy plated steel sheet having excellent workability and corrosion resistance

    JP2002363722A

  • Surface-treated steel plate of excellent machinability and corrosion resistance of machined part, and manufacturing method thereof

    JP2003213396A

  • Zn-Al-BASED PLATING-COATED STEEL SHEET EXCELLENT IN UNBENDING RESISTANCE, AND ITS PRODUCTION METHOD

    JP2008156729A

  • FUSION Al-Zn BASED ALLOY PLATING STEEL SHEET EXCELLENT IN PROCESSING PART CORROSION RESISTANCE AND PRODUCTION METHOD FOR THE SAME

    JP2021031759A