Polyphenylene Sulfone
Patent Information
- Application Number
- JP2023513257
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-08-24
Smart Images

Figure 0007577833000001 
Figure 0007577833000002 
Figure 0007577833000003
Abstract
Description
[Technical field]
[0001] The present invention relates to polyphenylene sulfones based on phenylene sulfone segments linked together by benzophenone groups. [Background technology]
[0002] Polyarylene ether sulfone and polyarylene ether ketone are classified as high performance thermoplastics. A specific preparation method and specific properties of a copolymer of polyarylene ether sulfone and polyarylene ether ketone are disclosed.
[0003] Thus, EP 278 720 A2 discloses crystalline copolymers of ketone units with a molar content of 50 to 92 mol % and polyphenylene sulfone (PPSU)-containing units with a chain length of 1 to 3.5, which are obtained by a process in which a block containing the ketone units is polymerized first.
[0004] Patent document 2 (CN 106167548 A) discloses the reaction of DCDPS to which 3-fluoro-4-chloro-benzophenone is added in ppm amounts, followed by the addition of biphenyl, and further discloses that the reaction is stopped by the addition of 3-fluoro-4-chlorobenzophenone.
[0005] For example, US Pat. No. 4,268,635 describes the preparation of block copolymers in which a suspension of crystalline polyetherketone or etherketone / sulfone copolymer is used.
[0006] Polyphenylene sulfone ketones prepared from a mixture of 4,4'-biphenol, 4,4'-dichlorodiphenyl sulfone (DCDPS) and benzophenones substituted at the 4,4' positions with fluoro, chloro or hydroxy groups are described in EP 2225328.
[0007] Block polycondensates prepared from 4,4'-biphenol, DCDPS, 4,4-difluro and / or dihydroxybenzophenone are disclosed in EP 332 012 as components of high-temperature resistant thermoplastic compositions. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] EP 278 720 A2 [Patent Document 2] CN 106167548A [Patent Document 3] US 4,268,635 [Patent Document 4] EP2225328 [Patent Document 5] EP 332 012 Summary of the Invention [Problem to be solved by the invention]
[0009] The problem addressed by the present disclosure is to present new polyphenylene sulfones that exhibit good resistance to hydraulic fluids, gasoline and / or fuels, especially with a view to resistance to flame-retardant hydraulic fluids. Furthermore, the new polyphenylene sulfones should provide good processing stability at high temperatures, in combination with good resistance, especially to flame-retardant hydraulic fluids (hydraulic fluids). Furthermore, said polyphenylene sulfones should support the production of coatings, fibers, films, foams and moldings. One of the motivations was to provide new polyphenylene sulfones that are suitable for the production of membranes. The membranes produced that are suitable for the purification of water were intended in particular for use in fuel and oil production. Furthermore, a method for the production of said new polyphenylene sulfones should be provided, which is easy and therefore particularly suitable for production on an industrial scale, and for example salt separation should be possible with short filtration times. [Means for solving the problem]
[0010] Below, Formula I [ka] (wherein segments A and B can be the same or different), and Formula II [ka] (where x is in the range of 4.5 to 9.) Disclosed is a polyphenylene sulfone (PPSU) consisting essentially of benzophenone-linked phenylene sulfone segments A and B of the formula:
[0011] Further disclosed is a solution comprising PPSU. Also disclosed is a method for producing PPSU, comprising reacting at least one dihalodiphenylsulfone with at least one dihydroxybiphenyl to obtain a phenylenesulfone oligomer having a number average degree of polymerization of 4.5 to 9 (hereinafter also referred to as chain length x) and reacting said oligomer with at least one dihalobenzophenone. Also disclosed is the use of the PPSU thus obtained as well as a solution comprising said PPSU in the production of coatings, fibers, films, foams, mouldings and / or membranes. Also disclosed is a membrane comprising the above or above thus obtained PPSU and an article comprising said membrane. Furthermore disclosed is the use of the membrane in water purification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] It should be noted that "at least one" below generally means one or more than one, for example, three or four or five or more, where "more than" can mean multiple or uncountable. For example, "at least one" can mean a mixture of one or more than one. When used in relation to compounds, "at least one" is used in the sense that one or more compounds that differ in their chemical constitution, i.e., chemical properties, are described.
[0013] Hereinafter, "polymer" may mean homopolymer or copolymer or a mixture thereof. Those skilled in the art understand that any polymer, whether homopolymer or copolymer, is essentially a mixture of polymeric individuals that typically differ in their composition, such as number-average degree of polymerization, degree of branching, or nature of the end groups. Such a fact is often also described as distribution. Thus, the following "at least one" as a prefix to a polymer means that different types of polymers may be included, each type may have the above-mentioned given distribution.
[0014] Those skilled in the art will further appreciate that any polymer may be derived from monomers or oligomers, or mixtures thereof, which then comprise the polymer in reacted, polymerized form.
[0015] In the following: The starting compounds are at least one dihalodiphenyl sulfone and at least one dihydroxybiphenyl.
[0016] The coupling agent is at least one dihalobenzophenone.
[0017] The solvent L is at least one solvent.
[0018] Compound C is at least one compound having (one) functional group reactive towards the reactive groups in the polymer chain.
[0019] Polyphenylene sulfone (PPSU) is essentially composed of benzophenone-linked phenylene sulfone segments A and B of formula I. Thus, PPSU is completely or essentially completely composed of the above-mentioned linking segments. Optionally, PPSU may contain small amounts of structurally different units. If PPSU contains such structurally different units, the content is generally preferably 10 mol % or less, for example 5 mol % or less, more preferably 1 mol % or less, based on the moles of the raw material compounds. Generally, PPSU may most preferably be free of such structurally different units.
[0020] Segments A and B may be identical or different. Segments A and B may differ in chain length x, for example, in the range of 4.5 to 9, such as 4.5 to 8, 4.5 to 7 or 4.5 to 6, or 4.5 to 5. Very good results in terms of the desired properties have been obtained with PPSU essentially composed of benzophenone-linked phenylene sulfone segments A and B, where segments A and B of formula I may be identical or different and have a chain length x of 4.5 to 7.
[0021] It is also possible for segments A and B to have different degrees of linearity. Thus, both segments may be linear (straight-chained). One or both segments may be non-linear. It is also possible for A and B to differ in chain length x and degree of linearity. Typically, and preferably, segments A and B are both linear and have the same or different chain length x.
[0022] The units structurally distinct from the linking segments are not particularly limited, so long as they support the technical properties required for PPSU, in particular good resistance to hydraulic fluids, gasoline and / or fuels, processing stability, and ease of manufacture. Such units may, for example, be derived from monomers typically used in the manufacture of polyarylene ether sulfones and / or polyarylene ether ketones.
[0023] The nature of the end groups of the PPSU is not particularly limited. This may generally depend on whether reactive or non-reactive end groups are desired as end groups. Reactive end groups may be preferred if it is intended to polymerize the PPSU with at least one further monomer or polymer to produce a copolymer, such as a block copolymer or a polymer network. Possible end groups are phenolic OH end groups or phenolate end groups, and phenolic alkoxy end groups, among others, -OCH 3 Terminal groups may be preferred, with amino terminal groups being among them -NH 2 may be preferred, the halogen end groups being especially -F or -Cl. Of the halogen end groups, Cl may be the most preferred. It is also possible for the end groups to be phthalic anhydride end groups. The end groups can be of one type or different types. In general, the end groups are Cl-, OH- and / or OCH 3 In many cases, the inactive end groups are accessible by end-capping the reactive end groups. If the PPSU is intended for applications accessible by solution-based manufacturing methods such as solution spinning or casting from solution, end-capping may not be required. Non-end-capped PPSU may be useful, especially in combination with membrane production. In this case, PPSU with Cl and / or OH end groups may be advantageous. Very good results have been obtained for the production of membranes or articles containing them, especially for the treatment of water, more particularly for the treatment of production water (produced water), with -OCH 3 and for PPSU containing end groups, wherein the end groups are essentially -OCH 3 For example, 98% or more, for example, 99% or more of all terminal groups are -OCH 3 Terminal groups are typically more preferred.
[0024] The PPSU may preferably have a relative viscosity of 0.20 to 1.30 dl / g, in particular 0.30 to 0.95. Depending on the solubility of the PPSU, the relative viscosity can be measured in a 1% by weight solution in N-methylpyrrolidone or in a mixture of phenol and dichlorobenzene, in each case at 20° C. or 25° C.
[0025] The PPSU can preferably have an average molecular weight Mn (number average) in the range of 7.500 to 60000 g / mol, in particular 8000 to 45000 g / mol, as determined by gel permeation chromatography (GPC). The weight-average molar mass Mw of the PPSU, as determined by GPC, can preferably be 14000 to 120000 g / mol, in particular 18000 to 100000 g / mol, particularly preferably 25000 to 80000 g / mol. Here Mn and Mw can be determined by GPC in dimethylacetamide as solvent against narrow-distribution polymethylmethacrylate as standard (calibration between 800 and 1820000 g / mol) using 4 columns (precolumn, 3 separation columns based on polyester copolymer) operated at 80° C. and a flow rate of 1 ml / min with an injection volume of 100 pl. For detection, an Rl detector can be used.
[0026] From the standpoint of ease of manufacture from a PPSU solution, PPSU is essentially composed of benzophenone-linked linear segments A and B, which can be the same or different, where x ranges from 4.5 to 9, Mw ranges from 25,000 to 80,000 g / mol (determined as above), and PPSU is -OCH 3 and -Cl end groups, where it may be preferred that the further units are included in an amount of 1 mol % or less based on the moles of starting compound, and it may be more preferred that the further units are not included.
[0027] Considering the ease of extrusion or injection molding of PPSU, it is advantageous to have good melt stability. Melt stability can be determined by comparing the apparent melt viscosity at a given time with the apparent melt viscosity at a later time. The ratio of the two, Q, is a measure of melt stability. It is preferred that the Q value of PPSU is equal to or less than 1.5, more preferably less than 1.5, and Q can be determined as given in the examples.
[0028] The disclosed PPSU can advantageously be prepared by a process comprising, more preferably consisting of, reacting at least one dihalodiphenylsulfone with at least one dihydroxybiphenyl to obtain a phenylenesulfone oligomer having a chain length x between 4.5 and 9, and reacting said oligomer with at least one dihalobenzophenone, such that the structure of the phenylenesulfone oligomer chain can be represented diagrammatically by formula (II):
[0029] Considering the ease of production on an industrial scale, it may be preferable to react one or two, particularly one, dihalophenylsulfone with one or two, particularly one, dihydroxybiphenyl to obtain phenylenesulfone oligomer. For the same reason, it may be preferable to react phenylenesulfone oligomer with one or two, particularly one, dihalobenzophenone. Thus, very good results have been observed in reacting phenylenesulfone oligomer (obtained by reacting dihalodiphenylsulfone with dihydroxybiphenyl) with dihalobenzophenone to obtain PPSU.
[0030] The at least one dihalophenylsulfone can be a 4,4'-substituted phenylsulfone. Dihalophenylsulfones with other substitution patterns, such as 2,4'- or 2,2'-substituted dihalophenylsulfones, can also be used. The at least one dihydroxybiphenyl can be a 4,4'-substituted biphenyl. Dihydroxybiphenyls with other substitution patterns, such as 2,4'- or 2,2'-substituted dihydroxybiphenyls, can also be used. Reacting at least one 4,4'-substituted dihalophenylsulfone with at least one 4,4'-substituted biphenyl results in a linear phenylenesulfone oligomer. Those skilled in the art will appreciate that otherwise non-linear phenylenesulfone oligomers are obtained. Those skilled in the art will further appreciate that the degree of linearity of the phenylenesulfone oligomer can vary depending on the combination and amount of dihalophenylsulfone, dihydroxybiphenyl, and other substitution patterns.
[0031] The at least one dihalobenzophenone can be a 2,2'-, or 2,4'-, or 4,4'-substituted benzophenone. Reacting a linear phenylene sulfone oligomer with a 4,4'-substituted benzophenone results in a PPSU consisting essentially of benzophenone-linked linear phenylene sulfone segments A and B and a linear PPSU. Those skilled in the art will appreciate that otherwise non-linear PPSUs are obtained. Those skilled in the art will further appreciate that depending on the combination and amount of non-linear polyphenylene oligomers and / or dihalobenzophenones with 2,2' or 2,4'-substitution patterns, PPSUs with different linearities are obtained. They may have lower solution viscosities compared to the corresponding linear PPSUs with comparable molecular weights and therefore generally better processability from solution, especially in the manufacture of membranes. Linear PPSUs may be particularly preferred in terms of ease of manufacture, especially on an industrial scale, as well as the better overall technical results observed. Under this aspect, it may be further preferred that the PPSU is linear, where x is in the range of 4.5 to 7, and M w is in the range of 25000-80000 g / mol (determined as above) and the end groups are essentially -OCH 3 and Cl, wherein 60 to 90%, particularly 70 to 85%, of the terminal groups are -OCH 3 where the further units are not included in the PPSU.
[0032] Although other halogen groups are possible, typically fluorine and / or chlorine are the preferred halogens in the at least one dihalodiphenylsulfone and at least one dihalobenzophenone, respectively.
[0033] Examples of dihalodiphenylsulfones are 4,4'-dichlorodiphenylsulfone, 4,4'-difluorodiphenylsulfone, 4,4'-dibromodiphenylsulfone, 2,2'-dichlorodiphenylsulfone, 2,2'-difluorodiphenylsulfone, and when linear PPSU is required, 4,4'-dichlorodiphenylsulfone (DCDPS) and / or 4,4'-difluorodiphenylsulfone are particularly preferred. Examples of dihalobenzophenones are 4,4'-dichlorobenzophenone, 4,4'-difluorobenzophenone, 2,2-dichlorobenzophenone, 2,4-dichlorobenzophenone, 2,2'-fluorobenzophenone, and / or 2,4'-difluorobenzophenone, and when linear PPSU is required, 4,4'-dichlorobenzophenone and / or 4,4'-difluorobenzophenone are particularly preferred.
[0034] The process for producing PPSU may preferably comprise, and essentially consist of, reacting starting compounds to obtain phenylene sulfone oligomers of the chain length defined above, and reacting said oligomers with a coupling agent. The process may also comprise using preformed oligomers, for example oligomers formed in a separate reactor, or oligomers isolated before reacting them with a coupling agent. A process is primarily preferred that comprises carrying out the reaction as a one-pot reaction, and may thus preferably comprise the process essentially. Such a one-pot reaction is typically a convenient and robust process. In this case, the starting compounds are reacted to obtain oligomers until the desired chain length is reached, and are reacted with a coupling agent without isolating the oligomers.
[0035] The starting compounds enter into a polycondensation reaction to obtain phenylene sulfone oligomers, which can usually be carried out in the presence of at least a catalytic amount of a base. This can be carried out in the absence of a solvent L, preferably in the presence of a solvent L. A reaction mixture is formed. The components of the reaction mixture are generally reacted simultaneously. The individual components can be mixed in an upstream process and reacted subsequently. It is also possible to feed the individual starting components to a reactor, where they are mixed and then reacted. The polycondensation reaction to obtain phenylene sulfone oligomers can preferably be carried out in one step. This means that the deprotonation of the starting compound bearing an OH-group and the condensation reaction with the starting compound bearing a halo group take place in one single reaction step without isolation of intermediate products.
[0036] The general knowledge about the preparation of polymers in the field of polyarylene ether sulfones with simultaneous control can be applied to phenylene sulfone oligomers and will be explained in more detail below.In the case of phenylene sulfone oligomers, for example, this can be achieved by controlling the amount of functional groups of the starting compounds, i.e. the amount of functional groups they have before they are polymerized.The ratio of the starting compounds used is in principle derived from the stoichiometry of the polycondensation reaction that proceeds with the theoretical removal of hydrogen halide such as hydrogen chloride, and is established by a person skilled in the art in a known manner.
[0037] In general, it is preferred to control or adjust the molar ratio of the functional groups of the starting compounds that are reactive with each other. Thus, the molar ratio of halogen and hydroxy groups can be varied depending on factors such as control of the end groups of the phenylene sulfone oligomer or control of the reaction rate and the chain length x. Thus, the chain length x of a phenylene sulfone oligomer containing, for example, phenolate end groups can be adjusted using a defined offset of the stoichiometric ratio between the starting compounds having halogen and hydroxy groups. In general, the molar ratio is 0.80:1 to 0.895:1 or less, such as 0.80:1 to 0.85:1.
[0038] The phenylene sulfone oligomer having a phenolic end group can be reacted with a dihalobenzophenone. The molar ratio of the phenylene sulfone oligomer to the dihalobenzophenone can be varied depending on factors such as control of the end groups of the PPSU or control of the reaction rate and molecular weight. This usually establishes a defined molar offset of the phenylene sulfone oligomer and the dihalobenzophenone. In terms of ease of production, it is generally preferred to prepare the phenylene sulfone oligomer with an excess of a starting compound having a hydroxy group and react the phenylene sulfone oligomer with the dihalobenzophenone. On a molar basis, the ratio of the phenylene sulfone oligomer OH group to the benzophenone halogen group can be in this case 0.70:1 to 1:1, in particular 0.75:1 to 0.95:1, most preferably 0.75:1 to 0.90:1.
[0039] In principle, the method can be carried out in the absence of a solvent, but the process can be most advantageously carried out in the presence of at least one solvent (solvent L), especially if a very light color of the PPSU is aimed for.
[0040] Preferred solvents L in the context of the present method are N-methyl-2-pyrrolidone (NMP) or N-ethyl-2-pyrrolidone (NEP), dimethylacetamide (DMAC), sulfolane or any combination thereof. To increase the solubility, the solvent L can be, for example, a mixture of 2-3 solvents. In most cases, it may be sufficient to use two or more, preferably only one, solvent. The solvent L may in particular be DMAC, NMP or NEP, or any mixture thereof. For industrial production purposes, it is often easier to employ one of the above-mentioned preferred solvents.
[0041] In order to separate the water released during the reaction to obtain the phenylene oligomer and / or PPSU, a co-solvent forming an azeotrope, such as toluene or chlorobenzene, may be used. Usually, it may be preferable not to employ such a co-solvent azeotrope. Separation of the water together with the solvent L during the heating step may generally be preferred. Losses of solvent L can be accounted for, for example, by starting with more solvent L or by adding solvent L during the reaction. Control of the viscosity increase during the reaction can also be a means to control the molecular weight of the PPSU. The disclosed method generally includes, or preferably consists essentially of, the reaction of the starting compound and / or the phenylene oligomer with the coupling agent in the presence of at least one base. Those skilled in the art know that it is preferred that the phenolic OH group react in the presence of at least one base in order to increase the reactivity towards halogen substituents. The at least one base can typically be a hydroxide, a carbonate or a bicarbonate. It may therefore be a mixture of at least one hydroxide and at least one carbonate, or a mixture of at least one carbonate and at least one bicarbonate. This may result in the preference for at least one anhydrous alkali metal carbonate. For example, it is also possible to use a mixture of different hydroxides or different carbonates or different bicarbonates. It may be preferred to use one base. It may be preferred that one base is one of the alkali metal carbonates. In particular, sodium carbonate, potassium carbonate, calcium carbonate or mixtures thereof may be preferred, and in particular potassium carbonate may be used as the base.In view of the rate of reaction and the reduction of the amount of by-products, potassium carbonate is particularly preferred having a volume weighted average particle size of less than 100 micrometers, for example potassium carbonate having a volume weighted average particle size of 5 to 80 μm, preferably 10 to 60 μm, for example 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or 55 μm, or a non-uniform μm size in the range of 5 to 100 μm, as measured on a suspension of the solids in chlorobenzene / sulfolane 60 / 40 (by weight) using a Malvern Mastersizer 2000 instrument.
[0042] Particularly preferred combinations are DMAC, NMP or NEP or any mixture thereof as solvent and potassium carbonate as base, especially potassium carbonate of a size less than 100 μm. One combination that may be particularly preferred is NMP as solvent and potassium carbonate as base, especially potassium carbonate of a size less than 100 μm, measured as above, for example potassium carbonate of 5-80 μm, preferably 10-60 μm, for example 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or 55 μm, or any non-uniform μm size between 5-100 μm.
[0043] The reaction of the raw material compounds to obtain the phenylene sulfone oligomers and their reaction with the coupling agent can be carried out at a temperature at which the reaction proceeds at an acceptable rate and produces phenylene sulfone oligomers and PPSU of acceptable quality, such as the desired molecular weight and molecular weight distribution. In general, the process can be carried out at a temperature of 80 to 250°C, preferably 100 to 220°C. If the process is carried out in the presence of a solvent L and at ambient pressure, the upper temperature limit is usually determined by the boiling point of the solvent L. The stability of the reactants can be a limiting factor for the reaction temperature, especially if the process is carried out in the presence of a solvent.
[0044] Those skilled in the art can adapt the reaction temperature and time to the particular PPSU being produced, but reaction temperatures in the range of 180-205°C may be applicable, with temperatures of 185-195°C being preferred. At the latter temperatures, the reaction of the starting compounds to obtain the phenylene sulfone oligomer is usually quite fast. This initial reaction time may therefore range from about 1 to about 2 hours. It is possible to have a reaction time of less than 2 hours, usually more than 1 hour. The reaction of the oligomer with the coupling agent at this temperature may require an additional 2-20 hours, for example 3-18 hours, for example 3-15 hours. The above conditions may be preferred, especially when the treatment is carried out in a solvent L such as NMP.
[0045] In the process, it may be possible to employ at least one compound (compound C) having one functional group that reacts with the reactive groups contained in the polymer chain. One compound C may preferably be used. This may allow the chain length of the PPSU to be controlled. In general, a reaction with compound C may be preferred, followed by a polycondensation reaction after reaching a conversion of, for example, at least 90%. Compound C may preferably be at least one aliphatic organohalogen. This leads to further reaction of the reactive end groups, in particular the hydroxy end groups. The PPSU therefore contains compound C in reacted form. Such PPSU is usually stabilized against further extension of the polymer chain, especially during further processing steps.
[0046] The preferred at least one aliphatic organohalogen is at least one alkyl halide, in particular an alkyl chloride, which may in particular be a primary alkyl chloride, having a linear or branched alkyl group having 1 to 10 carbon atoms, and is particularly preferably a methyl halide, in particular methyl chloride.
[0047] The reaction with compound C can be carried out at a temperature preferably between 90° C. and 160° C., where a temperature in the range between 100° C. and 150° C. may be preferred. The time can vary widely and is usually at least 5 minutes, in particular at least 15 minutes. The reaction time can generally be preferably between 15 minutes and 8 hours, where the reaction time can in particular be between 30 minutes and 4 hours.
[0048] Various methods can be used for the reaction of compound C, more particularly at least one aliphatic organic halogen.The amount of compound C, more particularly at least one aliphatic organic halogen used can be stoichiometric or represent excess, where excess can be, for example, up to 5-fold excess.For example, it may be preferred that at least one aliphatic organic halogen is added continuously, particularly via continuous introduction in the form of a gas stream.
[0049] The reaction with compound C can take place in a separate process unit or it may be preferred to carry it out directly in the polycondensation reactor.
[0050] If the step is carried out in the presence of solvent L and after the reaction is complete, further solvent L, which can be the solvent in which the reaction was carried out, such as DMAC, NMP, NEP, sulfolane or any mixture thereof, such as DMAC, NMP, NEP or any mixture thereof, where NMP may be preferred, is typically added to cool the reaction mixture. The reaction mixture can be cooled, for example, to a temperature range in which compound C can react with PPSU in a separate unit or polycondensation reactor as described above. The reaction mixture can then be further cooled, if necessary, where a temperature of around 80° C. may be preferred. If PPSU does not react with compound C, it may be preferred to cool the reaction mixture to about 80° C. At this temperature, the reaction mixture, which is typically a suspension, is removed from the respective reaction unit, which typically comprises a reaction vessel, and transferred to at least one separation unit. Said separation unit may preferably comprise a filtration unit for separating salts formed during the reaction, such as potassium chloride, from the reaction mixture. Depending on the viscosity of the suspension, this step can take several minutes or several hours, such as 30 minutes to 24 hours, preferably 1 to 12 hours. The product may then be isolated, for example via precipitation by contacting the filtrate with a non-solvent. This may for example be a mixture of water and at least one polar aprotic solvent. It may be preferred to use a mixture of water and solvent L, for example DMAC, NMP, NEP, sulfolane or any mixture thereof, for example DMAC, NMP, NEP or any mixture thereof, NMP may be preferred. Here water may generally be used in a larger portion than solvent L (NMP may be preferred), such as DMAC, NMP, NEP, sulfolane or any mixture thereof, for example DMAC, NMP, NEP or any mixture thereof. Precipitation in a water / NMP mixture (80 / 20 by mass) may be most preferred. Precipitation may also be carried out in an acidic medium, such as a water / NMP mixture containing an acid. Suitable acids are for example organic or inorganic acids, for example carboxylic acids, for example acetic acid, propionic acid, succinic acid or citric acid, and mineral acids, for example hydrochloric acid, sulfuric acid or phosphoric acid.The resulting particulate solid, e.g., powder or pearls, can be collected, typically filtered, then typically washed and finally dried, where temperatures below the glass transition temperature, 80-150°C in vacuum, can be advantageously used.
[0051] In addition to the above disclosure, a person skilled in the art can rely on methods accessible to him by applying his general knowledge. The preparation process leading to polyarylene ether sulfones is described, for example, in Herman F. Mark, "Encyclopedia of Polymer Science and Technology", Third edition, volume 4, 2003, chapter "Polysulfons" pages 2-8, and Hans R. Kricheldorf, "Aromatic Polyethers" in: Handbook of Polymer Synthesis, Second edition, 2005, pages 427-443. Further details on the synthesis of OH-terminated polyarylene ether sulfones are given, for example, in R. Viswanathan, BC Johnson, JE McGrath, Polymer 25 (1984) 1827. Information on molecular weight control is disclosed, for example, in A. Noshay, M. Matzner, CN Merriam, J. Polym.Sci. A-1 9 (1971) 3147.
[0052] The PPSU disclosed herein is an essentially amorphous polymer, which has the advantages of being soluble in a variety of solvents and can be processed at high temperatures.
[0053] A solution comprising at least one PPSU is also disclosed. The solution comprises at least one liquid capable of dissolving at least one PPSU (hereinafter also referred to as solute). The solution may result from a process for producing PPSU. In this case, the solution may comprise a solid. The process may comprise that the solution is filtered at a temperature higher than room temperature. This allows the solution to be filtered at a temperature below the boiling point of the solute. The temperature may be constant or may vary over the time of the filtration. The filtration may in principle be carried out in any filtration device suitable for the required pressure and temperature conditions. Pore sizes that can be employed are in the μm range and may preferably be 10 pm or less, for example 5 pm or less. The time required for filtration varies depending on factors such as the temperature and the pore size used. In general, filtration of a solution comprising at least one PPSU can be achieved in a time that is reasonable for industrial scale production. Usually, it may be preferred that the solution comprises one PPSU - or may be essentially composed of one PPSU and the solute. Thus, typically the filtrate is a solution that essentially consists of one PPSU and the solute. In particular, when the solution results from the process, the solution usually contains only one PPSU. The solution can also be prepared by contacting at least one PPSU, preferably one PPSU, with a solute. In view of solvent removal after use, it is preferable to minimize the amount of solute. The amount of solute often depends on the temperature at which the solution is handled and the desired viscosity of the solution for the intended use. The amount of solute should be sufficient to dissolve at least one PPSU at the temperature at which it is desired to handle the solution. Advantageously, the solute is at least one solvent L, such as DMAC, NMP, NEP, sulfolane or any mixture thereof, such as DMAC, NMP, NEP, or any mixture thereof, where NMP may be preferred. A solution containing PPSU usually has a reduced tendency to gel. Therefore, there is usually a convenient time span to process it.
[0054] This solution can be used in particular for the preparation of coatings, films, fibers or membranes. For this purpose, the solution may be mixed with further compounds, such as processing adjuvants and / or further polymers. Thus, the solution may, for example, comprise at least one other polyarylene (ether) sulfone and / or at least one polyvinyl-pyrrolidone, the latter usually being preferred in terms of membrane formation. Thus, the solution may comprise or be preferred as further components as mentioned above - but essentially consists of at least one PPSU, at least one solute and at least one other polyarylene (ether) sulfone and / or at least one polyvinyl pyrrolidone.
[0055] Also disclosed herein is the use of at least one PPSU as disclosed herein or obtainable by the process disclosed herein for the production of coatings, fibers, films, foams, molded articles and / or membranes.
[0056] Fibers are, for example, more or less flexible structures that are thin relative to their length. They can be compact or hollow. They can be circular or nearly circular or have different cross-sectional shapes. They can be, for example, flat. They can be tubular. They can have a smooth surface or have holes or holes. They can be obtained, for example, by extrusion. It may be more preferred that the fibers from at least one PPSU are obtained by a spinning process, where one PPSU is usually preferred. Spinning from a solution can be advantageous when the thermal stress on the at least one PPSU is important. Spinning can be carried out, for example, immediately after separating the PPSU from the salt. It is also possible to first isolate the PPSU and then dissolve it in the solvent used for spinning. To improve the mechanical properties of the fibers, it may be advantageous to spin at least one PPSU, where one PPSU is generally preferred, which can be and may be preferred to be spun from a solution by electrospinning methods, including magnetic electrospinning. Electrospinning may be most preferred for producing fibers, e.g. nanofibers. Magnetoelectrospinning may be employed for producing nonwoven fabrics from at least one PPSU, where one PPSU is generally preferred. Electrospinning requires that the melt, or preferably the solution, is conductive, so that it may not be necessary to separate all or substantially all of the salt from the reaction mixture after the reaction. A solution containing one PPSU, consisting essentially of benzophenone-linked phenylene sulfone segments A and B of formula I, and free of structurally distinct units, may be preferred for producing fibers by electrospinning.
[0057] The molding can essentially be a solid geometric body that can be produced, for example, by molding, injection molding, extrusion, calendaring, rotational molding, foaming, blow molding, molding or joining processes. The molding can be prepared from PPSU. Similarly, the molding can be prepared from a mixture comprising at least one PPSU, where the mixture can also comprise at least one further polymer resin. Typically, in addition to at least one PPSU and optionally at least one further polymer resin, the mixture used to produce the molding comprises at least one processing aid and / or filler. The molding comprising at least one PPSU generally exhibits excellent flame retardancy and excellent resistance to hydraulic oils. Examples of preferred moldings are airplane connectors and spacers for airplane fuselage exteriors, which are usually aluminum shells.
[0058] A membrane is, for example, a separating layer. A membrane may be understood to mean an impermeable, partially impermeable or selectively permeable membrane, or a membrane that is permeable in one direction or a permeable membrane. The type of membrane is generally not limited. Also, the membrane may be, for example, a reverse osmosis (RO) membrane, a forward osmosis (FO) membrane, a nanofiltration (NF) membrane, an ultrafiltration (UF) membrane or a microfiltration (MF) membrane. In many cases, it is preferred that the membrane is a UF, NF or MF membrane.
[0059] The PPSU disclosed herein can be used in different filter membrane configurations, for example flat membranes and / or capillary and hollow fiber membranes, and the flow towards these membranes can be in dead-end or cross-flow conditions.
[0060] The membrane may be produced with at least one PPSU, and preferably from one PPSU. Typically, the membrane can be prepared according to methods known to those skilled in the art. The membrane may be produced, for example, by casting from a solution. This allows the preparation of a casting solution. The casting solution typically contains at least one (often preferably one) compound that can be removed from the membrane by washing. The compound is often also called a pore former. In this case, the solution therefore also contains the pore former. For the purpose of producing a membrane from at least one PPSU, polyvinylpyrrolidone and / or polyethylene glycol (PEG) can often be used as a pore former in the casting solution.
[0061] The membranes can be used in contact with water. In particular, the membranes can be used in conjunction with water purification. More specifically, the membranes can be used to purify water contaminated or loaded with hydraulic fluids, gasoline and / or fuel, such as from spills in daily life or from industrial processing environments. Advantageously, the membranes can be used in particular to purify produced water, such as water originating from oil and gas production processes, which may be fracking processes or recirculation of desalted water on oil platforms. The article comprising at least one membrane can be, for example, a filtration system, such as a filtration device, a module train or a module rack. EXAMPLES
[0062] Working Example: The following examples provide further illustration of the present invention without, however, limiting it.
[0063] Definitions and Abbreviations: Reaction time: The time the reaction mixture was held at 190°C. DCDPS: 4,4'-dichlorodiphenyl sulfone BP: 4,4'-dihydroxybiphenyl NMP: N-methyl-2-pyrrolidone The particle size of potassium carbonate was determined in a suspension of the solid in chlorobenzene / sulfolane 60 / 40 (by weight) using a Malvern Mastersizer 2000 instrument as described above.
[0064] The chain length x of the oligomers was determined by potentiometric titration of OH groups and elemental analysis of the organic Cl content of the precipitate and dried samples taken from the reactor before the addition of 4,4'-dichlorobenzophenone, and the calculated value corresponds to the number average molecular weight of the oligomers.
[0065] The time required to filter the polymer solution was determined.
[0066] The obtained polymer was processed into granules using a ZSK18 extruder. The throughput was 2.5 kg / h at 300 rpm and the melt temperature, measured by a thermometer placed directly on the melt cake, was below 385° C. From the granules thus obtained, ISO bars (80 mm×1 mm×4 mm) and S2 tensile bars were prepared at a mass temperature of 370° C. and a tool temperature of 140° C.
[0067] The solution viscosity (VN) was determined using a solution of 0.01 g / ml polymer in N-methylpyrrolidone at 25° C. (DIN EN ISO 1628-1 (October 2012)).
[0068] The glass transition temperature (Tg) and melting point (Tm) of the polymers were determined by DSC analysis at a heating rate of 20 K / min. The reported values for glass transition temperature, melting point, and heat of fusion were determined in the second heating run.
[0069] The melt stability of the samples was measured using a capillary rheometer at a mass temperature of 400 °C for 60 min. The apparent viscosity of the melt was measured at 55 s every 5 min. -1 The quotient (Q) of the apparent viscosity determined at 60 minutes over the apparent viscosity determined at 5 minutes is a measure of melt stability.
[0070] The resistance of the products to hydraulic fluids, gasoline and / or fuel was determined as resistance to Skydrol® LD4 (58 wt% tributyl phosphate, 20-30 wt% dibutylphenyl phosphate, 5-10 wt% butyldiphenyl phosphate, 1-5 wt% 2,6-ditertyl-p-cresol, less than 10 wt% carboxylates). The S2 tensile bars were stored in Skydrol® LD4 for 24 hours. In each case, two S2 tensile bars were bent with a stencil to a bending radius of 132 mm before their storage. Pictures were taken every minute using a camera to determine the time to failure.
[0071] The measurement results are shown in Table 1.
[0072] Preparation of the polymer - general procedural procedures used in each case A vessel equipped with stirrer, Dean-Stark trap, nitrogen inlet and temperature control was used. 304.05 g (2.20 moles) of potassium carbonate with a volume average particle size of 34.5 μm was used. The water formed in the reaction was continuously removed by distillation. No azeotrope former was used. Lost NMP was replaced.
[0073] After the reaction time, 1500 ml of NMP was added to the vessel and the temperature of the reaction mixture was adjusted to 135° C. Methyl chloride was then added to the vessel for 60 minutes. Nitrogen was then purged through the reaction mixture for an additional 30 minutes. The reaction mixture was then cooled to 80° C. and then transferred to a heated pressure filter (80° C.) and the potassium chloride formed in the reaction mixture was separated by filtration.
[0074] Filtration was performed using a 3 μm pore size filter at 2.0 bar nitrogen pressure.
[0075] The polymer was isolated from the filtrate by precipitating it into a bath of demineralized water at room temperature (fall distance 0.5 m, throughput about 2.5 l / h). The resulting pearls were collected and washed with water at 85°C for 20 hours (water throughput 160 l / h). The pearls were then dried at a temperature below the glass transition temperature. The residual water content was less than 0.1% by weight.
[0076] A small amount of material precipitated for the samples that could not be filtered. These were then washed with water and dried at 120° C. for 24 hours. The residual moisture content was less than 0.1% by weight.
[0077] Comparative copolymer C1 In a vessel, 522.63 g (1.82 mol) of DCDPS, 372.41 g (2.00 mol) of BP, 50.22 g (0.20 mol) of 4,4'-dichlorobenzophenone, and potassium carbonate were dissolved, and suspended in 1152 ml of NMP in a nitrogen atmosphere.
[0078] The mixture was heated to 190° C. within 1 hour, after which the reaction time was 5 hours.
[0079] The filtration took 8 hours. The polymer was then isolated from the filtrate and dried.
[0080] Comparative copolymer C2 In a vessel, 522.63 g (1.82 mol) of DCDPS, 372.41 g (2.00 mol) of BP, and potassium carbonate were dissolved, and suspended in 952 ml of NMP in a nitrogen atmosphere.
[0081] The mixture was heated to 190° C. within 1 hour. The initial reaction time was 70 minutes.
[0082] After that, 20 ml of the suspension was separated. Then, 50.22 g (0.200 mol) of 4,4'-dichlorobenzophenone dissolved in 200 ml NMP was charged into the vessel. The reaction was continued at 190°C. The reaction time was 4 hours.
[0083] The filtration took 8.5 h. The resulting polymer was then isolated and dried.
[0084] Comparative copolymer C3 In a vessel, 508.28 g (1.77 mol) of DCDPS, 372.41 g (2.00 mol) of BP, 62.78 g (0.25 mol) of 4,4'-dichlorobenzophenone, and potassium carbonate were dissolved and suspended in 1152 ml of NMP in a nitrogen atmosphere.
[0085] The mixture was heated to 190° C. within 1 hour. The reaction time was 5 h.
[0086] The filtration took 10 h.
[0087] The polymer was then isolated from the filtrate and dried.
[0088] PPSU1 508.28 g (1.77 mol) of DCDPS, 372.41 g (2.00 mol) of BP, and potassium carbonate were dissolved in a vessel, and suspended in 952 ml of NMP in a nitrogen atmosphere.
[0089] The mixture was heated to 190° C. within 1 hour. The initial reaction time was 70 minutes.
[0090] Afterwards, 20 ml of the suspension was separated.Then, 62.78 g (0.250 mol) of 4,4'-dichlorobenzophenone dissolved in 200 ml of NMP was charged to the vessel.
[0091] The reaction was continued at 190° C. The reaction time was 4 hours. The filtration took 7.5 hours.
[0092] The polymer was then isolated from the filtrate and dried.
[0093] Comparative example C4 In a vessel, 493.92 g (1.72 mol) of DCDPS, 372.41 g (2.00 mol) of BP, 75.33 g (0.3 mol) of 4,4'-dichlorobenzophenone, and potassium carbonate were dissolved and suspended in 1152 ml of NMP in a nitrogen atmosphere.
[0094] The mixture was heated to 190° C. within 1 hour. The reaction time was 5.5 hours. The filtration took 12 hours.
[0095] The polymer was then isolated from the filtrate and dried.
[0096] PPSU 2 In a vessel, 493.92 g (1.72 mol) of DCDPS, 373.41 g (2.00 mol) of BP, and potassium carbonate were dissolved and suspended in 952 ml of NMP in a nitrogen atmosphere.
[0097] The mixture was heated to 190° C. within 1 hour. The initial reaction time was 70 minutes.
[0098] After that, 20 ml of the suspension was separated. Then, 75.33 g (0.30 mol) of 4,4'-dichlorobenzophenone dissolved in 200 ml of NMP was charged into the vessel. The reaction was continued at 190°C. The reaction time was 5 hours. Filtration took 8 hours.
[0099] The polymer was then isolated from the filtrate and dried.
[0100] Comparative copolymer C5 In a vessel, 465.20 g (1.62 mol) of DCDPS, 372.41 g (2.00 mol) of BP, and 100.44 g (0.4 mol) of 4,4'-dichlorobenzophenone were dissolved and suspended in 1152 ml of NMP under a nitrogen atmosphere.
[0101] The mixture was heated to 190° C. within 1 h. The reaction time was 6 h. The filtration took 14 h.
[0102] The resulting polymer was then isolated from the filtrate and dried.
[0103] PPSU 3 465.20 g (1.62 mol) of DCDPS, 372.41 g (2.00 mol) of BP, and potassium carbonate were dissolved in a vessel and suspended in 952 ml of NMP in a nitrogen atmosphere.
[0104] The mixture was heated to 190° C. within 1 hour. The initial reaction time was 70 minutes.
[0105] Afterwards, 20 ml of suspension was separated. Then, 100.44 g (0.40 mol) of 4,4'-dichlorobenzophenone dissolved in 200 ml of NMP was charged into the vessel. The reaction was continued at 190°C. The reaction time was 5.5 hours. Filtration took 10 hours. The polymer was then isolated from the filtrate and dried.
[0106] Comparative copolymer C6 In a vessel, 450.86 g (1.57 mol) of DCDPS, 372.41 g (2.00 mol) of BP, and potassium carbonate were each dissolved, and suspended in 952 ml of NMP in a nitrogen atmosphere.
[0107] The mixture was heated to 190° C. within 1 hour. The initial reaction time was 70 minutes.
[0108] Then, 20 ml of the suspension was separated. Next, 113.00 g (0.45 mol) of 4,4'-dichlorobenzophenone dissolved in 200 ml of NMP was charged into the vessel. The reaction was continued at 190°C. The reaction time was 6 hours.
[0109] Even after 24 hours of filtration time, only a trace portion of the solution was filtered.
[0110] After 24 hours the solution became a gel and precipitation was possible only after diluting 20 ml solution / gel with 20 ml NMP and heating to 120°C.
[0111] The polymer that was possible to obtain was then isolated from the filtrate and dried.
[0112] Comparative copolymer C7 In a vessel, 450.86 g (1.57 mol) of DCDPS, 372.41 g (2.00 mol) of BP, 113.00 g (0.45 mol) of 4,4'-dichlorobenzophenone, and potassium carbonate were dissolved, and suspended in 1152 ml of NMP in a nitrogen atmosphere.
[0113] The mixture was heated to 190° C. within 1 hour. The reaction time was 6 h.
[0114] Even after 24 hours filtration time, only a very small amount of solution was filtered.
[0115] After 24 hours the solution became a gel and precipitation was only possible after diluting 20 ml solution / gel with 20 ml NMP and heating to 120°C.
[0116] The resulting polymer was then isolated from the filtrate and dried.
[0117] As can be seen from the measurement results given in Table 1 below, the desired properties were observable for PPSU consisting essentially of benzophenone-linked segments with chain lengths x ranging from 4.5 to 9. Longer chain lengths did not provide resistance to Skydrol®. Shorter chain lengths did not allow the samples to be easily processed.
[0118] [Table 1]
Claims
1. Formula I 【Chemistry 1】 A polyphenylene sulfone (PPSU) consisting essentially of benzophenone-linked phenylene sulfone segments A and B of the formula II, wherein segments A and B may be the same or different, 【Chemistry 2】 and x is 4.5 to 9.
2. 2. The polyphenylene sulfone according to claim 1, wherein x is 4.5 to 7.
3. The polyphenylene sulfone according to claim 1 or 2, which is linear.
4. A solution comprising the polyphenylene sulfone according to any one of claims 1 to 3.
5. 5. The solution of claim 4, comprising N-methyl-2-pyrrolidone, dimethylacetamide and / or sulfolane.
6. The method for producing polyphenylene sulfone according to any one of claims 1 to 3, comprising reacting at least one dihalodiphenyl sulfone with at least one dihydroxybiphenyl to obtain a phenylene sulfone oligomer having a number average degree of polymerization in the range of 4.5 to 9, and reacting the oligomer with at least one dihalobenzophenone.
7. The method of claim 6, wherein the reaction is carried out as a one-pot reaction.
8. The process according to claim 6 or 7, comprising carrying out the reaction in the presence of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethylacetamide and / or sulfolane.
9. 9. The method of claim 8, comprising filtering the solution of claim 4 at a temperature above room temperature.
10. Use of the polyphenylene sulfone according to any one of claims 1 to 3 or the polyphenylene sulfone obtained by the process according to any one of claims 6 to 9 for the production of a coating, a film, a fiber, a foam, a membrane or a molded article.
11. 6. Use of the solution according to claim 4 or 5 in the manufacture of a coating, film, fibre or membrane.
12. 12. The method according to claim 10 or 11 for use in the manufacture of a membrane.
13. A membrane comprising at least one polyphenylene sulfone according to any one of claims 1 to 3.
14. An article comprising the membrane of claim 13.
15. 15. Use of the membrane of claim 13 or the article of claim 14 in the purification of water.
16. 16. The method of claim 15, wherein the produced water is used in a fracking process or for circulating desalted water on an oil platform.
Citation Information
Patent Citations
High-performance polysulfone resin and synthesis thereof
CN106167548A
Aromatic polymer
EP0278720A2
High temperature resistant polyarylethersulfone- / polyaryleneetherketone moulding compounds with improved phase cohesion
EP0332012A1
Polyphenyl sulfone ketone copolymers
EP2225328A1
Production of aromatic block copolymer ether
JP1987172020A