Semiconductor optical device and its manufacturing method
By bonding a III-V compound semiconductor element to a silicon substrate with a groove, terrace, and wall structure, the method addresses positional misalignment and etchant intrusion, ensuring the semiconductor optical device's integrity and reducing light loss.
Patent Information
- Application Number
- JP2021032021
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-01
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-03-01
AI Technical Summary
The misalignment of semiconductor elements during bonding to a substrate can cause positional variations, leading to unintended etching and reduced bonding strength due to etchant intrusion, which damages the semiconductor element.
A method involving bonding a III-V group compound semiconductor element with a silicon substrate, followed by wet etching and forming a mesa with a groove, terrace, and wall structure to block etchant intrusion, thereby preventing unintended etching and maintaining the semiconductor element's integrity.
This approach effectively suppresses etchant-induced damage to the semiconductor element, maintains positional accuracy, and reduces light loss by confining light within the silicon layer, enhancing the semiconductor optical device's performance.
Smart Images

Figure 0007578025000001 
Figure 0007578025000002 
Figure 0007578025000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor optical device and a method for manufacturing the same. [Background technology]
[0002] There is a known technique for bonding a semiconductor element formed of a III-V group compound semiconductor to a substrate such as an SOI (Silicon On Insulator) substrate (so-called silicon photonics) on which a waveguide is formed (for example, Patent Document 1, etc.). The substrate is provided with a waveguide formed of, for example, silicon (Si). The III-V group compound semiconductor is of the direct transition type and has a high optical gain. The semiconductor element is evanescently optically coupled to the substrate, and the emitted light of the semiconductor element propagates through the waveguide of the substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-53527 A Summary of the Invention [Problem to be solved by the invention]
[0004] The position of the semiconductor element within the plane of the substrate may vary due to misalignment when bonding the semiconductor element to the substrate. After bonding, the semiconductor element can be shaped by wet etching or other methods to eliminate the positional variation at the time of bonding. After molding, a mesa or other structure that becomes the light-emitting region can be formed to suppress misalignment.
[0005] However, etchant may get into the grooves (trench) in the substrate, and the mesa of the semiconductor element may be etched from the bonding interface side. Such unintended etching may cause damage to the semiconductor element and may reduce the bonding strength. Therefore, the objective of the present invention is to provide a semiconductor optical element that can suppress damage caused by etching, and a method for manufacturing the same. [Means for solving the problem]
[0006] A method for manufacturing a semiconductor optical device according to the present disclosure includes the steps of: bonding a semiconductor device having optical gain, formed of a III-V compound semiconductor, onto a substrate containing silicon; shaping the semiconductor device by wet etching after the bonding step; and forming a mesa in the semiconductor device after the molding step, wherein the substrate has a waveguide, a groove extending along the waveguide, a terrace located on an opposite side of the groove from the waveguide, and a wall closing the groove, and the bonding step is a step of bonding the semiconductor device onto the waveguide, the groove, the terrace and the wall of the substrate.
[0007] A semiconductor optical device according to the present disclosure comprises a substrate including silicon, the substrate having a waveguide, a groove along the waveguide, and a terrace facing the waveguide across the groove, and a semiconductor device bonded onto the waveguide and the terrace, the semiconductor device being formed of a III-V compound semiconductor and having optical gain, the waveguide having a first portion and a second portion, the first portion and the second portion being aligned in a direction in which the waveguide extends and connected to each other, the second portion having a width greater than that of the first portion in a direction intersecting the direction in which the waveguide extends, and the substrate having a wall connected to the second portion and the terrace and closing the groove, or the second portion closing the groove. Effect of the Invention
[0008] According to the present disclosure, damage caused by etching can be suppressed. [Brief description of the drawings]
[0009] [Figure 1A] FIG. 1A is a perspective view illustrating a semiconductor optical device according to the first embodiment. [Figure 1B] FIG. 1B is a cross-sectional view taken along line AA in FIG. 1A. [Figure 2A] FIG. 2A is a perspective view illustrating the substrate. [Figure 2B] FIG. 2B is a plan view illustrating the substrate. [Figure 2C] FIG. 2C is a cross-sectional view taken along line BB in FIG. 2B. [Diagram 3] FIG. 3 is a diagram illustrating the transmittance. [Figure 4A] FIG. 4A is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 4B] FIG. 4B is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 5A] FIG. 5A is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 5B] FIG. 5B is a cross-sectional view taken along line CC in FIG. 5A. [Figure 6A] FIG. 6A is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 6B] FIG. 6B is a cross-sectional view taken along line CC in FIG. 6A. [Figure 7A] FIG. 7A is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 7B] FIG. 7B is a perspective view illustrating a method for manufacturing a semiconductor optical device. [Figure 8] FIG. 8 is a plan view illustrating the substrate of the semiconductor optical device according to the second embodiment. [Figure 9] FIG. 9 is a plan view illustrating a substrate of the semiconductor optical device according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Description of the embodiments of the present disclosure] First, the contents of the embodiments of the present disclosure will be listed and described.
[0011] One embodiment of the present disclosure is a method for manufacturing a semiconductor optical device, comprising: (1) a step of bonding a semiconductor element having optical gain formed of a III-V compound semiconductor onto a substrate containing silicon; a step of shaping the semiconductor element by wet etching after the bonding step; and a step of forming a mesa on the semiconductor element after the shaping step, wherein the substrate has a waveguide, a groove extending along the waveguide, a terrace located on the opposite side of the groove from the waveguide, and a wall closing the groove, and the bonding step is a step of bonding the semiconductor element onto the waveguide, the groove, the terrace, and the wall of the substrate. The wall blocks the etchant for wet etching, thereby preventing the etchant from penetrating inward from the wall. Unintended etching of the semiconductor element can be suppressed. (2) In the step of molding the semiconductor element, the semiconductor element may be molded so that an end of the semiconductor element is located on the wall. The wall prevents the intrusion of an etchant, thereby preventing unintended etching of the semiconductor element. Since the semiconductor element does not protrude beyond the wall, the etchant is less likely to remain under the semiconductor element. Light loss due to the etchant is suppressed. (3) The waveguide may have a first portion and a second portion, the first portion and the second portion being aligned in an extension direction of the waveguide and connected to each other, the second portion having a width greater than that of the first portion in a direction intersecting the extension direction of the waveguide, and the wall may be connected to the second portion and the terrace. This makes it possible to suppress the effect of the wall on the propagation of light and to suppress light loss. (4) The wall may be connected to a center portion of the second portion in the extension direction of the waveguide, thereby making it possible to suppress the effect of the wall on the propagation of light and to suppress light loss. (5) The length of the second portion in the extension direction of the waveguide may be 50 μm or more, which can suppress the effect of walls on light propagation and reduce light loss. (6) The wall may have a thickness of 5 μm or more. After wet etching, an edge of the semiconductor element may be formed on the wall. (7) The waveguide may have a first portion and a second portion, the first portion and the second portion being aligned in an extension direction of the waveguide and connected to each other, the second portion having a width greater than that of the first portion in a direction intersecting the extension direction of the waveguide, the second portion being connected to the terrace and functioning as the wall. The wall may block an etchant for wet etching, thereby suppressing unintended etching of a semiconductor element. (8) The semiconductor element may have a compound semiconductor substrate and a compound semiconductor layer laminated on the compound semiconductor substrate, the compound semiconductor layer and the substrate may be bonded in the bonding step, the bonding step may include a step of removing the compound semiconductor substrate of the semiconductor element by wet etching, and the step of molding the semiconductor element may be performed after the step of removing the compound semiconductor substrate. Damage caused to the semiconductor element during etching of the compound semiconductor substrate can be removed by wet etching. (9) The substrate may be an SOI substrate having a silicon layer, and the waveguide, the terrace, and the wall may be formed in the silicon layer. The heights of the waveguide, the terrace, and the wall may be approximately the same, so that the intrusion of an etchant can be effectively suppressed. Since light is confined in the silicon layer, loss can be suppressed. (10) The method may further include a step of covering the substrate with an insulating film after the wet etching step, and the step of forming a mesa in the semiconductor element may include a step of dry etching the semiconductor element after the step of covering with the insulating film. By covering with the insulating film, damage to the substrate caused by dry etching is suppressed. (11) A semiconductor optical element comprising: a substrate including silicon, the substrate having a waveguide, a groove along the waveguide, and a terrace facing the waveguide across the groove; and a semiconductor element bonded onto the waveguide and the terrace, the semiconductor element being formed of a III-V compound semiconductor and having optical gain, the waveguide having a first portion and a second portion, the first portion and the second portion being aligned in the extension direction of the waveguide and connected to each other, the second portion having a width greater than that of the first portion in a direction intersecting the extension direction of the waveguide, the substrate having a wall connected to the second portion and the terrace and closing the groove, or the second portion closing the groove. The wall blocks the etchant, thereby suppressing unnecessary etching.
[0012] [Details of the embodiment of the present disclosure] Specific examples of semiconductor optical devices and manufacturing methods thereof according to embodiments of the present disclosure will be described below with reference to the drawings. Note that the present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0013] First Embodiment (Semiconductor optical element) FIG 1A is a perspective view illustrating a semiconductor optical device 100 according to a first embodiment. FIG 1B is a cross-sectional view taken along line AA in FIG 1A. As shown in FIG 1A and FIG 1B, the semiconductor optical device 100 is a hybrid type laser device having a substrate 10 and a semiconductor device 20. The upper surface of the substrate 10 extends in the XY plane, and the semiconductor device 20 is bonded to the upper surface. The Z-axis direction is the normal direction to the upper surface of the substrate 10. The X-axis direction, the Y-axis direction, and the Z-axis direction are mutually perpendicular.
[0014] (substrate) Fig. 2A is a perspective view illustrating the substrate 10. Fig. 2B is a plan view illustrating the substrate 10, enlarging the vicinity of the wall 40. Fig. 2C is a cross-sectional view taken along line BB in Fig. 2B.
[0015] The substrate 10 is an SOI substrate including a substrate 12, a silicon oxide (SiO2) layer 14, and a silicon (Si) layer 16, which are stacked in this order in the Z-axis direction. The substrate 12 is made of Si. The SiO2 layer 14 has a thickness of, for example, 3 μm. The Si layer 16 has a thickness of, for example, 220 nm. The upper surface of the substrate 10 is covered with an insulating film 18. The insulating film 18 is made of SiO2 with a thickness of, for example, 1 μm. The Si layer 16 has a refractive index of 3.45. The refractive index of the SiO2 layer 14 and the insulating film 18 is lower than that of the Si layer 16, that is, 1.45.
[0016] As shown in FIG. 2A, the Si layer 16 of the substrate 10 has a waveguide 11, two grooves 13, two terraces 15, and four walls. The waveguide 11 and the groove 13 extend in the X-axis direction. The two grooves 13 are located on both sides of the waveguide 11 in the Y-axis direction. The terrace 15 is a flat surface of the Si layer 16 and is located on the opposite side of the groove 13 from the waveguide 11. In FIGS. 1A to 2C, the bottom surface of the groove 13 is the Si layer 16, but may be the SiO2 layer 14. The walls 40 are spaced apart from the semiconductor element 20. Of the four walls 40, two are located on one end side of the semiconductor element 20 in the X-axis direction, and the other two are located on the other end side.
[0017] As shown in FIG. 2A, the waveguide 11 has three narrow portions 42 (first portions) and two wide portions 44 (second portions). The narrow portions 42, wide portions 44, narrow portions 42, wide portions 44, and narrow portions 42 are arranged in this order along the X-axis direction. A tapered portion 46 is provided between the narrow portions 42 and the wide portions 44. The narrow portions 42 and the wide portions 44 are connected to each other via the tapered portion 46. One of the three narrow portions 42 extends to one end of the substrate 10 in the X-axis direction. Another of the three narrow portions 42 extends to the other end of the substrate 10 in the X-axis direction. Of the three narrow portions 42, the one in the center in the X-axis direction is located between the two wide portions 44. The semiconductor element 20 shown in FIG. 1A is provided on the narrow portions 42.
[0018] FIG. 2B illustrates two narrow portions 42, one wide portion 44, and two tapered portions 46 of the waveguide 11. The narrow portion 42, tapered portion 46, wide portion 44, tapered portion 46, and narrow portion 42 are arranged in order along the X-axis direction. In the Y-axis direction, the wide portion 44 has a width greater than that of the narrow portion 42. The tapered portions 46 are provided at both ends of the wide portion 44 in the X-axis direction. The tapered portion 46 tapers toward the side away from the wide portion 44 along the X-axis direction. The narrow portion 42 is connected to the tip of the tapered portion 46. The narrow portion 42 extends in the X-axis direction. The narrow portion 42, the wide portion 44, and the tapered portion 46 are formed in the Si layer 16 of the substrate 10, and grooves 13 are provided on both sides of these portions.
[0019] As shown in FIG. 2B, the portion of the wide portion 44 close to the tapered portion 46 is defined as region 44a, and the central portion in the X-axis direction is defined as region 44b. Two walls 40 protrude from region 44b of the wide portion 44 in the Y-axis direction. One end of one wall 40 is connected to region 44b of the wide portion 44, and the other end is connected to terrace 15. In other words, the wall 40 extends in the Y-axis direction, crosses the groove 13, and closes the groove 13. The wall 40 is connected to the central portion in the X-axis direction of region 44b of the wide portion 44. The wall 40 is formed in the Si layer 16 of the substrate 10, similarly to the waveguide 11. The upper surfaces of the waveguide 11, the terrace 15, and the wall 40 are located at the same height in the Z-axis direction. Since the wall 40 closes the groove 13, it is possible to suppress the intrusion of an etchant during wet etching in the manufacturing process of the semiconductor optical device 100, and to prevent unintended etching of the semiconductor device 20.
[0020] The width W1 of the narrow portion 42 shown in FIG. 2B is, for example, 0.5 μm. The width W2 of the wide portion 44 in the Y-axis direction is, for example, 4 μm, and the length L1 in the X-axis direction is, for example, 20 μm or more and 60 μm or less. The width W3 of the tapered portion 46 at the connection position with the wide portion 44 is, for example, 1.5 μm or more and 2 μm or less. The length L2 of the tapered portion 46 is, for example, 10 μm to 15 μm. The width W4 of the groove 13 is, for example, 1 μm. The thickness T1 of the wall 40 is, for example, 5 μm.
[0021] As shown in Fig. 2C, the inside of groove 13 is filled with insulating film 18. That is, as shown in Fig. 1B, below semiconductor element 20, the upper surfaces of waveguide 11 and terrace 15 are in contact with semiconductor element 20, and groove 13 is hollow. As shown in Fig. 2C, at a position separated from semiconductor element 20, insulating film 18 covers the upper and side surfaces of waveguide 11, covers the upper surface of terrace 15, and fills the inside of groove 13.
[0022] (Semiconductor element) As shown in FIG. 1B, the semiconductor device 20 has a cladding layer 22, a core layer 24, a cladding layer 26, and a contact layer 28, which are stacked in this order from the substrate 10 side. The cladding layer 22 is formed of, for example, n-type indium phosphide (n-InP) having a thickness of 400 nm. The cladding layer 26 is formed of, for example, p-InP having a thickness of 2 μm. The contact layer 28 is formed of, for example, (p+)-gallium indium arsenide (GaInAs) or the like. The core layer 24 includes a plurality of well layers and barrier layers alternately stacked, and has a multi-quantum well structure (MQW: Multi Quantum Well). The well layers and barrier layers are formed of, for example, non-doped gallium indium arsenide phosphide (i-GaInAsP) or the like. The core layer 24 has a thickness of, for example, 300 nm. The core layer 24 has optical gain and emits light having a wavelength of, for example, 1.55 μm. Each layer of the semiconductor device 20 may be formed of a III-V compound semiconductor other than those mentioned above.
[0023] 1A, the semiconductor element 20 has a mesa 30 and electrodes 32 and 34. The mesa 30 of the semiconductor element 20 is located on the waveguide 11. The tip of the mesa 30 in the X-axis direction has a tapered shape that tapers along the waveguide 11. In the X-axis direction, one wide portion 44 is located on one end side of the mesa 30, and another wide portion 44 is located on the other end side. The mesa 30, the wide portion 44, and the wall 40 are spaced apart from each other.
[0024] 1B, the mesa 30 is formed of the core layer 24, the cladding layer 26, and the contact layer 28, and is located on the waveguide 11 of the substrate 10. The cladding layer 22 is located between the mesa 30 and the substrate 10, and extends outside the mesa 30 in the XY plane. The cladding layer 22 contacts the upper surface of the waveguide 11 of the substrate 10 and the upper surface of the terrace 15. The surfaces of the mesa 30 and the cladding layer 22 are covered with an insulating film 18. The insulating film 18 has openings on the mesa 30 and on the cladding layer 22.
[0025] 1B, the electrode 32 extends from above the mesa 30 to the upper surface of the insulating film 18 outside the mesa 30, and is electrically connected to the contact layer 28 through an opening in the insulating film 18. The electrode 32 is formed of, for example, a laminate of titanium, platinum, and gold (Ti / Pt / Au). The electrode 34 is spaced apart from the electrode 32, provided on the upper surface of the insulating film 18, and electrically connected to the cladding layer 22 through the opening in the insulating film 18. The electrode 34 is formed of, for example, a metal such as an alloy of gold, germanium, and nickel (AuGeNi). The electrodes 32 and 34 may be provided with an Au plating layer or the like.
[0026] An electric signal is input to the electrodes 32 and 34, and carriers are injected into the core layer 24 of the semiconductor element 20, causing it to emit light. The semiconductor element 20 and the substrate 10 are evanescently optically coupled, and the light transitions to the substrate 10. The light propagates through the waveguide 11 and is emitted to the outside from the end of the substrate 10.
[0027] The narrow portion 42 and the wide portion 44 of the waveguide 11 function as a one-input, one-output MMI (Multi-Mode Interface). The narrow portion 42 is a single-mode waveguide. The wide portion 44 functions as a multi-mode waveguide. Single-mode light propagates through the narrow portion 42 and enters the wide portion 44 through the tapered portion 46. The tapered portion 46 suppresses light reflection, and suppresses light loss between the narrow portion 42 and the wide portion 44. The light propagates in multi-mode in the wide portion 44, enters the narrow portion 42 through the tapered portion 46, and propagates again in single mode.
[0028] FIG. 3 is a diagram illustrating transmittance. The horizontal axis indicates the thickness of the wall 40, and the vertical axis indicates transmittance. A width of 0 μm on the horizontal axis means that there is no wall 40. The transmittance is calculated by changing the dimensions in the dashed line example and the solid line example in FIG. 3. The dashed line is an example in which the length L1 of the wide portion 44 is 27 μm, and the solid line is an example in which the length L1 of the wide portion 44 is 54 μm.
[0029] As shown in FIG. 3, in the example of the dashed line, when the thickness T1 of the wall 40 is in the range of 0 to 4 μm, the transmittance is 0.95 or more. When the thickness T1 is greater than 4 μm, the transmittance drops sharply. Light is tightly confined in the narrow portion 42, but when it enters the wide portion 44, it tends to spread in the width direction. The light is affected by the wall 40 and leaks out to the terrace 15 side. In the example of the dashed line, the length L1 of the wide portion 44 is 27 μm, and the wall 40 is relatively thicker than the wide portion 44. The influence of the wall 40 becomes greater, and the transmittance drops.
[0030] In the example of the solid line, the transmittance is maintained at 0.95 or more until the thickness of the wall 40 is in the range of 0 to 8 μm or more. The length L1 of the wide portion 44 is 54 μm, which is about twice as long as that of the example of the dashed line. In the region 44a of the wide portion 44 shown in FIG. 2A, the light is distributed widely in the Y-axis direction. On the other hand, in the region 44b, the light is imaged on the center side in the Y-axis direction. Although the walls 40 are connected to both ends of the region 44b, the light is distributed concentratedly on the center side of the region 44b, and is therefore less affected by the walls 40. Since the light is less likely to leak, a high transmittance can be obtained as shown by the solid line in FIG. 3.
[0031] (Manufacturing method) 4A to 5A, 6A, 7A, and 7B are perspective views illustrating a manufacturing method of the semiconductor optical device 100. Fig. 5B is a cross-sectional view taken along line CC in Fig. 5A, and Fig. 6B is a cross-sectional view taken along line CC in Fig. 6A, both of which show the vicinity of the wall 40 in an enlarged view.
[0032] Dry etching is performed on the Si layer 16 of the substrate 10 in a wafer state to form the waveguide 11, the groove 13 and the wall 40 as shown in FIG. 2A.
[0033] A contact layer 28, a cladding layer 26, a core layer 24, and a cladding layer 22 are epitaxially grown in this order on a surface of a III-V compound semiconductor substrate 50 by organometallic vapor phase epitaxy (OMVPE) or the like. The substrate 50 is diced to form a plurality of semiconductor elements 20 shown in FIG. 4A.
[0034] 4B, the surfaces of the semiconductor element 20 and the substrate 10 are plasma-activated or the like, and the semiconductor element 20 is bonded to the substrate 10. No adhesive or the like is used for bonding, and the cladding layer 22 of the semiconductor element 20 is brought into contact with the upper surfaces of the waveguide 11, the terrace 15, and the walls 40 of the substrate 10. The semiconductor element 20 covers the two wide portions 44 and the four tapered portions 46 of the waveguide 11, and the four walls 40. A substrate 50 is located on top of the semiconductor element 20.
[0035] As shown in Fig. 5A, the substrate 50 of the semiconductor element 20 is removed by wet etching using, for example, hydrochloric acid as an etchant. After the wet etching, the contact layer 28 is exposed. As shown in Fig. 5B, the cladding layer 22, the core layer 24, the cladding layer 26, and the contact layer 28 are not removed and cover the waveguide 11 and the wall 40. Side etching may progress during the wet etching, causing damage to the semiconductor element 20.
[0036] As shown in FIG. 6A and FIG. 6B, a mask 52 made of, for example, SiO2 is provided on the semiconductor element 20 by photolithography or the like. The end of the mask 52 is located on the wall 40. The portion of the semiconductor element 20 exposed from the mask 52 is removed by wet etching using, for example, buffered hydrofluoric acid (BHF) as an etchant, and is molded into, for example, a rectangle. After the wet etching, the portion of the semiconductor element 20 protected by the mask 52 remains, and the end of the semiconductor element 20 in the X-axis direction is located on the wall 40. The etchant used in the wet etching enters the groove 13 of the substrate 10, but the wall 40 blocks the groove 13 and acts as a dike to hold back the etchant. The inflow of the etchant inside the wall 40 (to the right in FIG. 6B) is suppressed, and etching of the semiconductor element 20 from the bonding interface side is also suppressed.
[0037] 6A and 6B, the portions of the substrate 50 that were damaged by the wet etching can be removed. When the semiconductor element 20 is bonded to the substrate 10, positional deviation may occur. By forming the semiconductor element 20 into a fixed shape by wet etching as shown in FIG. 6A, the positional deviation during bonding is eliminated. After the wet etching, the semiconductor element 20 remains in a specified position in the substrate 10.
[0038] As shown in FIG. 7A, a mask 54, for example, made of SiO2, is provided on the upper surface of the substrate 10 and on a part of the semiconductor element 20. After providing the mask 54, dry etching is performed to form a mesa 30 in the semiconductor element 20. The mesa 30 is located on the narrow portion 42 of the waveguide 11 and is spaced apart from the wide portion 44 and the wall 40. After the mesa 30 is formed, a SiO2 film is provided on the exposed upper surface of the substrate 10 and the surface of the semiconductor element 20. This SiO2 film forms the insulating film 18 together with the mask 54. As shown in FIG. 7B, electrodes 32 and 34 are provided by vacuum deposition or the like. The substrate 10 is diced along a dicing line surrounding one semiconductor element 20 to form a semiconductor optical element 100.
[0039] According to the first embodiment, the wall 40 of the substrate 10 closes the groove 13. In the process of wet etching the semiconductor element 20 shown in Fig. 5A to Fig. 6B, the etchant is blocked by the wall 40 and is prevented from penetrating further inward than the wall 40. Etching from the bonding interface to the portion of the semiconductor element 20 that will become the gain region in the semiconductor optical element 100, such as the mesa 30, is prevented. By preventing damage to the semiconductor element 20, the semiconductor element 20 is less likely to peel off from the substrate 10 and deterioration of the characteristics is also prevented.
[0040] Misalignment may occur when bonding the semiconductor element 20 to the substrate 10. Damage may occur to the semiconductor element 20 during the process of etching the substrate 50. Damaged portions of the semiconductor element 20 can be removed by wet etching as shown in FIGS. 6A and 6B. As shown in FIG. 6A, the semiconductor element 20 can be molded into a certain shape by wet etching to suppress the effect of misalignment on subsequent processes. As shown in FIG. 7A, a mesa 30 can be formed at an intended position in the substrate 10.
[0041] As shown in Figures 6A and 6B, it is preferable that the end of the semiconductor element 20 after wet etching is located on the wall 40. If the end is located inside the wall 40 in the X-axis direction (to the right in Figure 6B), the etchant will invade beyond the wall 40. If the end protrudes beyond the wall 40 to the left in Figure 6B, the etchant will remain under the semiconductor element 20 protruding beyond the wall 40. The remaining etchant will become a deposit and increase light loss. By positioning the end of the semiconductor element 20 on the wall 40, it is possible to prevent the etchant from invading and also suppress the remaining etchant.
[0042] As shown in FIG. 1A, the wall 40 is connected to the waveguide 11 and is spaced apart from the mesa 30 in the extension direction of the waveguide 11. Light emitted from the mesa 30 propagates through the waveguide 11. In order to suppress a decrease in optical output, it is important to suppress the influence of the wall 40 on the light. As shown in FIG. 2B, the wall 40 is connected to a wide portion 44 of the waveguide 11, which has a width greater than that of a narrow portion 42. Compared to a case in which the wall 40 is connected to the narrow portion 42, the influence of the wall 40 can be suppressed, and optical loss can be suppressed.
[0043] As shown in FIG. 2B, the wall 40 is preferably connected to the central region 44b of the wide portion 44. In the region 44a on the end side of the wide portion 44, the light is distributed spreading in the Y-axis direction. In contrast, in the central region 44b, the light is imaged and distributed concentratedly in the center in the Y-axis direction. By connecting the wall 40 to the region 44b, the influence of the wall 40 is further suppressed, the light is less likely to leak in the lateral direction, and the loss of light is suppressed. If the wide portion 44 is long in the X-axis direction, the light is imaged in the central region 44b, and the leakage of light can be effectively suppressed. The length L1 of the wide portion 44 is preferably 50 μm or more. As shown in the example of the solid line in FIG. 3, even if the wall 40 is thick, high transmittance can be maintained and the loss of light can be suppressed. The shape of the wide portion 44 in the XY plane does not have to be rectangular, but is preferably rectangular. Except for the connection part of the wall 40, the equivalent refractive index of the wide portion 44 in the X-axis direction is almost constant, so the loss of light is suppressed.
[0044] The thickness T1 of the wall 40 shown in FIG. 2B is preferably 5 μm or more. Even when the accuracy of photolithography is taken into consideration, the end of the mask 52 for wet etching can be formed on the wall 40 as shown in FIG. 6B. By forming the end of the mask 52 on the wall 40, the end of the semiconductor element 20 after wet etching can be formed on the wall 40. If the thickness T1 is 5 μm or more, even if the semiconductor element 20 is side-etched in wet etching, the end is located on the wall 40. Since the wall 40 is connected to the wide portion 44, the influence on light can be suppressed even if the wall 40 is made thicker, such as 5 μm or more. The thickness T1 of the wall 40 may be, for example, 8 μm or more, 10 μm or more. When the length L1 of the wide portion 44 is about 54 μm as shown in FIG. 3, the transmittance can be 90%. In order to suppress the influence of the wall 40 on the propagation of light, the thickness T1 is preferably, for example, 20 μm or less.
[0045] The waveguide 11, the terrace 15, and the wall 40 are formed in the Si layer 16 of the substrate 10. The height of the wall 40 is equal to the height of the waveguide 11 and the terrace 15, and it is preferable that their upper surfaces are located in the same plane. The semiconductor element 20 and the wall 40 are in contact with each other, so that the intrusion of the etchant can be more effectively suppressed. The height of the wall 40 does not need to be exactly the same as the height of the waveguide 11 and the terrace 15, and may be, for example, slightly lower. The etchant is unlikely to intrude through a minute gap between the semiconductor element 20 and the wall 40. As shown in FIG. 2B, a SiO2 layer 14 is provided under the Si layer 16, and an insulating film 18 of SiO2 is provided on top, and both sides of the waveguide 11 are filled with the insulating film 18. Since the refractive index of the Si layer 16 is higher than the surroundings, light can be strongly confined in the waveguide 11 and loss can be suppressed.
[0046] The substrate 10 may be an SOI substrate or a substrate other than an SOI substrate. The substrate 10 is preferably a substrate containing Si. The waveguide 11 of the substrate 10 has a refractive index higher than that of an insulator such as SiO2 and air, thereby enhancing optical confinement.
[0047] It is preferable to cover the substrate 10 with an insulating mask 54 before forming the mesa 30. This makes it possible to suppress damage to the substrate 10 due to dry etching. Since the mask 54 is provided after molding the semiconductor element 20 as shown in FIG. 5A, most of the substrate 10 is protected by the mask 54, and damage to the waveguide 11 can be suppressed.
[0048] <Second embodiment> The semiconductor optical device according to the second embodiment is also a hybrid type laser device, similar to the example in Figures 1A and 1B. The waveguide 11 of the substrate 10 in the second embodiment is different from that in the first embodiment. The configuration other than the waveguide 11 is the same as that in the first embodiment.
[0049] Fig. 8 is a plan view illustrating the substrate 10 of the semiconductor optical device according to the second embodiment, with an enlarged view of the vicinity of the wide portion 44 of the waveguide 11. In Fig. 8, the waveguide 11 has two narrow portions 42, two tapered portions 46, and one wide portion 44. Of the grooves 13, grooves 13a are located on both sides of the narrow portion 42 and the tapered portion 46. Of the grooves 13, grooves 13b are located on both sides of the wide portion 44.
[0050] The shape of the wide portion 44 in the XY plane is rectangular, and the vertex of the wide portion 44 is connected to the terrace 15. The wide portion 44 functions as a wall that closes the gap between the groove 13a and the groove 13b. The width W5 of the connection portion between the wide portion 44 and the terrace 15 is, for example, 0.5 μm. The length of the wide portion 44 in the X-axis direction is, for example, 27 μm.
[0051] In the second embodiment, the same manufacturing method as in the first embodiment is performed. Dry etching is performed on the substrate 10 to form a waveguide as shown in FIG. 8. After wet etching as shown in FIG. 6A and FIG. 6B, the end of the semiconductor element 20 is located, for example, on the narrow portion 42, and the semiconductor element 20 after wet etching extends to the opposite side to the wide portion 44 (upper side in FIG. 8). The semiconductor element 20 may extend to the wide portion 44 side (lower side). The end of the semiconductor element 20 may be located on the wide portion 44. The end of the semiconductor element 20 may be parallel to the Y-axis direction or inclined with respect to the Y-axis direction. Dry etching is performed on the semiconductor element 20 formed by wet etching to form a mesa 30. The mesa 30 is located on the narrow portion 42 of the waveguide 11 and is separated from the wide portion 44.
[0052] According to the second embodiment, the wide portion 44 serves as a wall that blocks the gap between the groove 13a and the groove 13b. The etchant is blocked by the wide portion 44, and etching from the bonding interface side of the semiconductor element 20 is suppressed. Damage to the semiconductor element 20 due to etching can be suppressed.
[0053] The wide portion 44 of the waveguide 11 does not need to have a wall protruding in the Y-axis direction. The equivalent refractive index of the wide portion 44 does not change discontinuously along the X-axis direction, but is almost uniform. The decrease in transmittance is suppressed, and for example, the transmittance for fundamental mode light with a wavelength of 1.55 μm is 98%. Light loss can be suppressed.
[0054] <Third embodiment> The semiconductor optical device according to the third embodiment is also a hybrid type laser device, similar to the example in Figures 1A and 1B. The waveguide 11 of the substrate 10 in the third embodiment is different from that in the first embodiment. The configuration other than the waveguide 11 is the same as that in the first embodiment.
[0055] 9 is a plan view illustrating the substrate 10 of the semiconductor optical device according to the third embodiment, with the vicinity of the wide portion 44 of the waveguide 11 enlarged. The waveguide 11 has two narrow portions 42, two tapered portions 46, and one wide portion 44. One of the two narrow portions 42 in FIG. 9 is referred to as narrow portion 42a, and the other is referred to as narrow portion 42b. One of the two tapered portions 46 is referred to as tapered portion 46a, and the other is referred to as tapered portion 46b. One end of the wide portion 44 in the X-axis direction is referred to as end portion 44c, and the other end is referred to as end portion 44d.
[0056] In the X-axis direction, the tapered portion 46a is connected to the end 44c of the wide portion 44, and the narrow portion 42a is connected to the tip of the tapered portion 46a. The tapered portion 46b is connected to the end 44d of the wide portion 44, and the narrow portion 42b is connected to the tip of the tapered portion 46b. In the Y-axis direction, the narrow portion 42a and the tapered portion 46a are connected to one side of the wide portion 44 (the left side in FIG. 9). The narrow portion 42b and the tapered portion 46b are connected to the other side of the wide portion 44 (the right side in FIG. 9). In other words, the narrow portion 42a and the narrow portion 42b do not face each other along the X-axis direction.
[0057] Among the grooves 13, the grooves 13c and 13d are located on both sides of the narrow portion 42a and the tapered portion 46a. The groove 13c reaches the end 44c of the wide portion 44. The groove 13d extends longer than the groove 13c and is adjacent to the end 44d of the wide portion 44 in the Y-axis direction. Among the grooves 13, the grooves 13e and 13f are located on both sides of the narrow portion 42b and the tapered portion 46b. The groove 13e reaches the end 44d of the wide portion 44. The groove 13f extends longer than the groove 13e and is adjacent to the end 44c of the wide portion 44 in the Y-axis direction. The width W6 on the base side of the tapered portion 46a and the width W7 between the grooves 13c and 13f are, for example, 1.5 μm. The length of the wide portion 44 is, for example, 109 μm.
[0058] In the third embodiment, the same manufacturing method as in the first embodiment is performed. Dry etching is performed on the substrate 10 to form a waveguide as shown in Fig. 9. After the wet etching shown in Fig. 6A and Fig. 6B, the end of the semiconductor element 20 is located, for example, on the wide portion 44. The end of the semiconductor element 20 may be parallel to the Y-axis direction or may be inclined with respect to the Y-axis direction.
[0059] According to the third embodiment, the wide portion 44 functions as a wall that blocks the gap between the grooves 13c and 13d and the grooves 13e and 13f. The etchant is blocked by the wide portion 44, suppressing damage to the semiconductor element 20. The grooves 13c and 13d and the groove 13f are aligned in the Y-axis direction. The grooves 13e and 13d are aligned in the Y-axis direction, and the wide portion 44 is located between them. The grooves 13c and 13e face each other in the X-axis direction, and the wide portion 44 is also located between them. The wide portion 44 can effectively suppress the intrusion of the etchant.
[0060] The wide portion 44 of the waveguide 11 does not need to have a wall protruding in the Y-axis direction. The equivalent refractive index of the wide portion 44 is uniform along the X-axis direction. Reduction in transmittance is suppressed, and for example, the transmittance for fundamental mode light with a wavelength of 1.55 μm is 97%. Light loss can be suppressed. Light loss can be suppressed.
[0061] Although the embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present disclosure described in the claims. [Explanation of symbols]
[0062] 10, 12, 50 boards 11 Waveguide 13, 13a~13f groove 14 SiO2 layer 15. Terrace 16 Si layer 18 Insulating film 20 Semiconductor elements 22, 26 Cladding layer 24 Core Layer 28 Contact layer 30 Mesa 32, 34 electrodes 40 Wall 42, 42a~42b Narrow part (1st part) 44 Wide part (2nd part, wall) 44a, 44b area 46, 46a, 46b Tapered section 52, 54 Mask 100 Semiconductor optical element
Claims
1. A step of bonding a semiconductor element having optical gain, which is formed of a III-V compound semiconductor, onto a substrate containing silicon; After the bonding step, a step of shaping the semiconductor element by wet etching; forming a mesa in the semiconductor element after the step of molding the semiconductor element; the substrate has a waveguide, a groove extending along the waveguide, a terrace located on an opposite side of the groove to the waveguide, and a wall closing the groove; the bonding step is a step of bonding the semiconductor element onto the waveguide, the groove, the terrace and the wall of the substrate, the waveguide has a first portion and a second portion; the first portion and the second portion are aligned in an extension direction of the waveguide and connected to each other; the second portion has a width greater than that of the first portion in a direction intersecting with an extension direction of the waveguide; A method for manufacturing a semiconductor optical device, wherein the wall is connected to the second portion and the terrace.
2. 2. The method for manufacturing a semiconductor optical device according to claim 1, wherein in the step of molding the semiconductor device, the semiconductor device is molded so that an end portion of the semiconductor device is located on the wall.
3. The method for manufacturing a semiconductor optical device according to claim 1 , wherein the wall is connected to a central portion of the second portion in an extension direction of the waveguide.
4. 4. The method for manufacturing a semiconductor optical device according to claim 1, wherein the length of the second portion in the extending direction of the waveguide is 50 [mu]m or more.
5. 5. The method for manufacturing a semiconductor optical device according to claim 1, wherein the wall has a thickness of 5 [mu]m or more.
6. The waveguide has a first portion and a second portion, the first portion and the second portion are aligned in an extension direction of the waveguide and connected to each other; the second portion has a width greater than that of the first portion in a direction intersecting with an extension direction of the waveguide; 3. The method for manufacturing a semiconductor optical device according to claim 1, wherein the second portion is connected to the terrace and functions as the wall.
7. The semiconductor device includes a compound semiconductor substrate and a compound semiconductor layer laminated on the compound semiconductor substrate, In the bonding step, the compound semiconductor layer and the substrate are bonded to each other, After the bonding step, a step of removing the compound semiconductor substrate of the semiconductor element by wet etching is included; 7. The method for manufacturing a semiconductor optical device according to claim 1, further comprising the step of molding the semiconductor device after the step of removing the compound semiconductor substrate.
8. the substrate having a silicon layer; 8. The method for manufacturing a semiconductor optical device according to claim 1, wherein the waveguide, the terrace and the wall are formed in the silicon layer.
9. After the step of molding the semiconductor element, a step of covering the substrate with an insulating film is included, 9. The method for manufacturing a semiconductor optical device according to claim 1, wherein the step of forming a mesa in the semiconductor device includes a step of performing dry etching on the semiconductor device after the step of covering with the insulating film.
10. a substrate including silicon, the substrate having a waveguide, a groove along the waveguide, and a terrace facing the waveguide across the groove; a semiconductor element bonded onto the waveguide and the terrace, the semiconductor element being made of a III-V compound semiconductor and having an optical gain; the waveguide has a first portion and a second portion; the first portion and the second portion are aligned in an extension direction of the waveguide and connected to each other; the second portion has a width greater than that of the first portion in a direction intersecting with an extension direction of the waveguide; The substrate has a wall connected to the second portion and the terrace and closing the groove, or the second portion closes the groove.
Citation Information
Patent Citations
Method for manufacturing silicon-based mixing laser achieving complete metal limitation
CN103887705A
Semiconductor laser light emitting device and electronic equipment
JP2009277833A
Semiconductor device, method for manufacturing the same, integrated substrate, optical module, and optical communication device
JP2012014002A
Method of manufacturing optical semiconductor element
JP2020017650A
Optical semiconductor element and manufacturing method thereof
JP2020053527A