Semiconductor laser chip with buried and butt joint structure and preparation method thereof
Through heterojunction buried structure and docking design, the problem of difficult reduction in the oxidation of AlGaInAs material and the active area cavity length and cavity width in DML chips is solved, which achieves higher response bandwidth and reliability, and simplifies the chip preparation process.
Patent Information
- Application Number
- CN202411007278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
During the preparation process of existing DML chips, AlGaInAs materials are easily oxidized, resulting in device reliability problems. At the same time, it is difficult to effectively reduce the cavity length and cavity width of the active area, affecting the response bandwidth and process difficulty.
Using heterojunction buried structure and docking design, the active area cavity is formed by enclosing the passive waveguide layer to avoid exposure of Al material to the air, and the active area cavity length is reduced through the rectangular high-barrier isolation zone and light exit zone design. and cavity width, reduce junction capacitance, and increase relaxation oscillation frequency.
It effectively avoids the risk of Al element oxidation, improves the reliability and response bandwidth of the device, and simplifies the chip preparation process and reduces the chip cost.
Smart Images

Figure CN118970622A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical communication, and in particular to a semiconductor laser chip with an embedded butt joint structure and a preparation method thereof. Background Art
[0002] With the development and popularization of 5G communications, people are more and more eager for higher network transmission speeds. Optical chips play a vital role in the field of high-speed optical communications. How to achieve high-speed optical chips has become one of the problems that need to be solved urgently.
[0003] At present, high-speed optical chips mainly have two structures: electro-absorption modulation (EML) chip and direct modulation (DML) chip. Among them, EML chip has the advantages of low threshold current of DFB laser and low capacitance of EA modulator, which can achieve high bandwidth modulation above 53G and 106G. However, the monolithic integration problem between DFB and EA devices involved in EML chip and the introduction of integration process have led to the increase of EML chip process difficulty, the decrease of output yield, the increase of reliability failure risk and the significant increase of chip cost.
[0004] The DML chip has a simple structure, high light output characteristics, relatively good single-mode output characteristics, relatively stable side mode suppression ratio, and relatively simple epitaxial design and process tape-out, making it easier to achieve mass production. However, it is more difficult to achieve a higher response frequency for the DML chip. Device parameters such as attenuation coefficient, self-resistance, parasitic capacitance, and relaxation oscillation frequency have a great impact on the rate of the DML chip.
[0005] From the perspective of the preparation process of DML chips, choosing a shorter active area length and a narrower active area width can not only improve the response bandwidth of the DML chip, but also further reduce the self-junction capacitance, thereby further improving the device response bandwidth. However, a shorter cavity length will increase the difficulty of DML chip thinning, bar cleavage, spot measurement and chip bonding, resulting in a loss of chip yield; from the perspective of the performance of epitaxial materials, materials with a larger conduction band bias rate have a stronger ability to bind electrons. Using materials with a larger conduction band bias rate in the active area can make the device have a higher electron mobility and modulation bandwidth. The epitaxial materials currently used are AlGaInAs (AlQ) materials and InGaAsP (PQ) materials. Although the band bias of AlGaInAs (AlQ) materials is greater than that of InGaAsP (PQ) materials, due to the relatively active Al element contained in AlGaInAs (AlQ) materials, the traditional preparation method has the risk of oxidation, which in turn affects the reliability of DML devices.
[0006] In the prior art, such as Chinese patent CN106300013A-An epitaxial growth method and an epitaxial layer of a buried heterostructure, the patent proposes a method for realizing a buried structure by selective epitaxy, by first growing part or all of the n / p / n / p InP or InGaAsP layer, and then epitaxy all Al-containing materials in its structure, thereby realizing a buried structure and avoiding the problem of oxidation of Al-containing materials. The patent adopts a selective epitaxial process to design a buried structure on both sides of the active area. Although the oxidation of Al-containing materials is avoided, the n / p / n / p InP or InGaAsP structure used due to its own process reasons will have a large junction capacitance, which affects the relaxation oscillation frequency of the chip. At the same time, like traditional semiconductor chips, it is also impossible to further reduce the cavity length of the active area.
[0007] Similarly, for example, Chinese patent CN 107623250A - A short cavity long surface emitting laser and its manufacturing method, the patent proposes a method of docking a passive waveguide, reducing the cavity length of the DML device and increasing the relaxation oscillation frequency, thereby realizing a high-speed DML chip of more than 30G. However, in order to increase the relaxation oscillation frequency, the patent process only controls the cavity length of the active area, while the width of the active area remains unchanged; at the same time, the process adopts a method of first growing the active area film layer and then docking the growth of the passive waveguide, so if AlGaInAs (AlQ) material is used in the active area, the risk of aluminum elements being oxidized in the atmosphere will be greatly increased, affecting the reliability performance of the device.
[0008] It can be seen that how to avoid Al oxidation of AlGaInAs (AlQ) materials while effectively reducing the cavity length and width of the chip active area to further improve the response bandwidth of the device is a difficult problem currently faced by the preparation of high-speed DML chips. Summary of the invention
[0009] In order to solve the problems faced by the preparation of the above-mentioned DML chip, the present invention provides a semiconductor laser chip with a buried and butted structure and a preparation method thereof. The buried heterostructure (BH) structure and partitioned burial are adopted to avoid the easy oxidation of aluminum-containing materials in the atmosphere, and the passive waveguide is butted on the light-emitting end face of the active area cavity. On the basis of the existing chips of the same specifications, a shorter active area length and a narrower active area width are obtained, which can effectively reduce the junction capacitance of the active area itself and greatly improve the chip modulation and response bandwidth.
[0010] The technical solution of the present invention is as follows:
[0011] A method for preparing a semiconductor laser chip with a buried and butted structure, comprising the steps of:
[0012] S1. Select a substrate and a passive waveguide layer on the substrate for a first epitaxial growth;
[0013] S2. growing a hard mask on the surface of the passive waveguide layer, selectively etching the passive waveguide layer, and etching the passive waveguide layer into a butt joint structure;
[0014] The docking structure includes two parallel rectangular high-resistance isolation areas and a light-emitting area connecting the two rectangular ends, and the light-emitting area and the high-resistance isolation area enclose an active area cavity;
[0015] S3. sequentially growing a buffer layer, an Al-containing active layer, a spacer layer and a grating layer on the substrate to perform a second epitaxial growth;
[0016] S4. removing the hard mask, sequentially growing a cladding layer and growing an ohmic contact layer to perform a third epitaxial growth;
[0017] S5. Grow the hard mask again, etch the redundant areas on both sides of the chip, form steps, and then make metal upper and lower levels and optical films on the device end faces.
[0018] In this scheme, a passive waveguide layer is first grown, the passive waveguide layer is composed of a high-resistance semiconductor material, and the passive waveguide layer encloses an active region cavity, so that the active region cavity can form a buried heterostructure (BH). Among them, the Al-containing material is epitaxially grown in the active region cavity enclosed by the passive waveguide, forming a passive waveguide layer enclosing the active region cavity structure; in addition, the epitaxially grown Al-containing material will be covered by the subsequently grown Al-free material, so that the Al-containing active region is further isolated from water and oxygen, ensuring that the Al-containing element will not be exposed to the air to avoid oxidation risks; at the same time, the passive waveguide layer design with a docking structure on the light-emitting end face of the device forms an active region cavity with a smaller enclosed area, and the rectangular high-resistance isolation area will form a current blocking effect, and the electric field and the light field will be further restricted, reducing the junction capacitance of the active region and increasing the relaxation oscillation frequency. Moreover, the passive waveguide layer can also make up for the shortened cavity length in the active area of the light-emitting area. Without affecting the power output of the chip, it also ensures that subsequent processes such as chip thinning and bar dissociation can proceed smoothly.
[0019] Preferably, the total thickness of the second epitaxial growth in step S3 is equal to the thickness of the first epitaxial growth in step S1.
[0020] In this scheme, the passive waveguide layer of the first epitaxial growth encloses the active region cavity, making the height of the active region cavity equal to the thickness of the passive waveguide layer. The second epitaxial growth needs to fill the active region cavity, and the positions of the two growths are just complementary, so the thickness of the two growths is guaranteed to be the same, avoiding the formation of stepped terraces by the two epitaxial growths, which affects the subsequent third epitaxial growth and further affects the chip performance.
[0021] Preferably, in the step S1, the substrate uses sulfur (S)-doped InP material, and the passive waveguide layer uses iron (Fe)-doped InP material or InGaAsP (PQ) material.
[0022] In this scheme, the growth of iron (Fe)-doped InP material or InGaAsP (PQ) material has high resistance. The passive waveguide layer preferably uses iron (Fe)-doped InP material, which can well limit the electric field and optical field of the active area after forming the active area cavity, sandwiching the active area, effectively increasing the internal relaxation oscillation frequency, and making the chip have a larger bandwidth.
[0023] Preferably, in the step S1, when growing the passive waveguide layer, the growth temperature is 550° C. to 620° C., the growth chamber pressure is 50 mbar to 200 mbar, and the growth thickness is 1 μm to 2.5 μm.
[0024] In this scheme, the passive waveguide layer with high resistance is first grown on the substrate, and then it is etched into the required morphology, so it is necessary to ensure that the grown passive waveguide layer has good performance and quality. The low-pressure MOCVD machine used in the present invention has a growth temperature of 550°C to 580°C. The growth process in the chamber is mainly gas phase reaction, adsorption and surface reaction, and the film quality of the passive waveguide layer tends to be qualified; but as the temperature increases, the desorption and diffusion reactions in the chamber intensify, which will reduce the performance growth trend of the passive waveguide layer and waste and increase energy consumption. Therefore, the growth temperature range is 550°C to 700°C, preferably 550°C to 580°C. When the chamber pressure is higher than 350mbar, it will affect the air flow field of the chamber environment and cause the piston flow in the chamber to transform into a rotating induced vortex, resulting in poor uniformity of film formation and unqualified film quality. When the pressure is too low, although it will not affect the quality of the passive waveguide layer below 50mba, too low pressure will increase the flow rate of the gas in the chamber, which will consume materials and reduce the growth rate of the InP material.
[0025] Preferably, in step S2, the length of the two high-resistance isolation regions is 10 μm to 100 μm, which is the cavity length of the active region; the spacing between the two high-resistance isolation regions is 1 μm to 2 μm, which is the cavity width of the active region; and the length of the light-emitting end region is 1 μm to 200 μm.
[0026] In this scheme, by controlling the area etched in step S2, the spacing and length of the high-resistance isolation areas are controlled, and then the cavity length and cavity width of the active area are controlled. At the same time, the rectangle formed by the passive waveguide layer and the active area cavity in the middle can avoid the problem of subsequent chip thinning, bar dissociation and other subsequent processes affected by the short cavity length.
[0027] Preferably, in step S3, the buffer layer is made of N-type InP material with a growth thickness of 0.5 μm to 1.5 μm; the Al-containing active layer is made of AlGaInAs material with a growth thickness of 0.1 μm to 0.25 μm; the spacer layer is made of InP material with a growth thickness of 0.2 μm to 0.5 μm; and the grating layer is made of InGaAsP (PQ) material with a growth thickness of 0.1 μm to 0.25 μm.
[0028] Preferably, when etching the ohmic contact layer in step S5, a bromine aqueous solution of (Br:HBr=1:17):H2O=1:5 is used for wet etching, and the etching mesa depth is 2.5 μm to 10 μm.
[0029] In this scheme, since the chip is prepared in a wafer, each layer generally grows in the same plane and at the same height during growth. Since the passive waveguide layer is etched into a certain shape in step S2, during the second epitaxial growth, in addition to the active area cavity, there will be material growth around the passive waveguide layer. In this step, a hard mask is first used to protect the required area, and then the excess part of the passive waveguide layer side is etched away by a bromine aqueous solution, so that the area of the second epitaxial growth is finally retained only in the active area cavity. The solution used for etching is a bromine aqueous solution with a configuration of Br:HBr=1:17 and then diluted 5 times with water.
[0030] Preferably, in step S4, the cladding layer is made of InP material and has a growth thickness of 1 μm to 2.5 μm; the ohmic contact layer is made of InGaAs material and has a growth thickness of 0.15 μm to 0.3 μm.
[0031] Preferably, the first epitaxial growth, the second epitaxial growth and the third epitaxial growth are all grown using a MOCVD machine or an MBE machine.
[0032] In this scheme, the MOCVD machine or MBE machine is used to carry out growth and deposition in a chamber filled with hydrogen. During the second epitaxial growth, multiple materials are grown alternately. The active layer containing Al material will not come into contact with water and oxygen during growth and will be covered by other materials later, directly avoiding exposure to the air.
[0033] A semiconductor laser chip with a buried butt joint structure is manufactured by using any of the above-mentioned methods for manufacturing a semiconductor laser chip with a buried butt joint structure.
[0034] The semiconductor laser chip made by this method uses an active region containing Al elements. At the same time, the cavity length and area of the active region are greatly reduced compared with the existing technology. It has a higher modulation and response bandwidth and is a high-speed DML chip.
[0035] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0036] 1. The present invention first grows a passive waveguide layer and then grows an active layer containing Al elements. At the same time, the passive waveguide layer and the cavity layer of the active area are complementary to each other, which effectively avoids the active layer of Al elements used in the preparation of the chip from being exposed to the atmosphere, solves the problem that the active layer containing Al materials is easily oxidized, and effectively improves the reliability of the device.
[0037] 2. The present invention forms a docking structure by first growing a passive waveguide layer, enclosing an active area cavity with a smaller area, and the rectangular high-resistance isolation area forms a current barrier, which further limits the electric field and the optical field, reduces the junction capacitance of the active area, and increases the relaxation oscillation frequency, thereby increasing the device response frequency; at the same time, the light output area set by the passive waveguide layer makes up for the shortened portion of the source area cavity length, further reducing the active area cavity length without affecting the chip power output, and also ensuring that subsequent chip thinning, bar dissociation and other processes can proceed smoothly.
[0038] 3. The preparation method of the present invention can complete the buried structure of the high-resistance isolation area on both sides of the active area and the passive waveguide docking structure in the light-emitting end area at one time, thereby simplifying the chip preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the accompanying drawings described below are only some embodiments. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0040] In the attached picture:
[0041] Figure 1 A flow chart for preparing a semiconductor laser chip of the present invention;
[0042] Figure 2 This is a schematic diagram of the semiconductor laser chip preparation step S1 of the present invention;
[0043] Figure 3This is a schematic diagram of the semiconductor laser chip preparation step S2 of the present invention;
[0044] Figure 4 This is a schematic diagram of the semiconductor laser chip preparation step S3 of the present invention;
[0045] Figure 5 It is a schematic diagram of the semiconductor laser chip preparation step S4 of the present invention;
[0046] Figure 6 It is a schematic diagram of the semiconductor laser chip preparation step S5 of the present invention;
[0047] Figure 7 For the present invention Figure 6 A top view of
[0048] Figure 8 For the present invention Figure 7 Sectional view of AA in the middle;
[0049] Fig. 9 For the present invention Figure 7 Cross-sectional view of BB.
[0050] Description of symbols in the figure
[0051] 1-substrate, 2-buffer layer, 3-Al-containing active layer, 4-spacer layer, 5-grating layer, 6-cladding layer, 7-ohmic contact layer, 8-passive waveguide layer, 81-high-resistance isolation region, 82-light output region, 9-hard mask, 10-active region cavity.
[0052] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0053] In conjunction with the accompanying drawings, the technical solution of the present invention is clearly and completely described through the specific implementation methods of the embodiments of the present invention.
[0054] Embodiment 1:
[0055] like Figure 1 A method for preparing a semiconductor laser chip with a buried and butt-jointed structure is shown.
[0056] In step S1, a sulfur (S)-doped InP substrate 1 is selected to perform the first epitaxial growth using an Aixtron SSC machine. <100> A passive waveguide layer 8 doped with InP and made of iron (Fe) is grown on a substrate 1 with a crystal surface. When growing the passive waveguide layer 8, the growth temperature is 550° C. to 620° C., the growth chamber pressure is 50 mbar to 200 mbar, and the growth thickness is 1 μm to 2.5 μm, forming a structure as shown in FIG. Figure 2The structure shown.
[0057] Specifically, the iron (Fe) doped InP material has a high resistance value, and after growing and surrounding the active region cavity 10, it can well limit the electric field and optical field of the active region, sandwiching the active region therein, effectively increasing the internal relaxation oscillation frequency, and making the chip have a larger bandwidth. The growth thickness is adjusted according to actual needs.
[0058] Step S2, depositing a 2000A SiO2 film layer as a hard mask 9 on the surface of the passive waveguide layer 8 by plasma enhanced chemical vapor deposition PECVD, and then etching out the shape model required for the second epitaxial growth by yellow light photolithography and SiO2 wet etching process, and selectively etching the passive waveguide layer 8 into a butt joint structure, such as Figure 3 The length of the two high-resistance isolation regions 81 is 10 μm to 100 μm, which is the cavity length of the active region; the spacing between the two high-resistance isolation regions 81 is 1 μm to 2 μm, which is the cavity width of the active region; and the length of the light-emitting end region is 1 μm to 200 μm.
[0059] By controlling the etched area in step S2, controlling the spacing of the high-resistance isolation area 81 and the length of the high-resistance isolation area 81, the cavity length and cavity width of the active area can be controlled. At the same time, the rectangle formed by the passive waveguide layer 8 and the active area cavity 10 enclosed in the middle can avoid the problem of the subsequent chip thinning, bar strip dissociation and other processes being affected by the short cavity length. Specifically, the docking structure includes two parallel rectangular high-resistance isolation areas 81 and a light-emitting area 82 connecting the two rectangular ends. The light-emitting areas 82 of equal height and the high-resistance isolation area 81 are surrounded on three sides as the active area cavity 10; the passive waveguide layer 8 with a docking structure, the enclosed active area cavity 10 with a smaller area, and the rectangular high-resistance isolation area 81 form a current barrier, which restricts the electric field and the light field in one step, reduces the junction capacitance of the active area, and increases the relaxation oscillation frequency. The light-emitting area 82 makes up for the shortened portion of the source area cavity length, does not affect the chip power output, and ensures that the subsequent chip thinning, bar strip dissociation and other processes can proceed smoothly.
[0060] It should be noted that, since the passive waveguide layer 8 from the first epitaxial growth only grows on a part of the surface of the substrate 1 after being etched, the first epitaxial growth can also be called the first selective epitaxial growth.
[0061] In step S3, after removing the photoresist produced by yellow light lithography, a second epitaxial growth is performed. Use MOCVD machine to grow aluminum-containing active area layer, first grow 0.5μm~1.5μm N-type InP buffer layer 2, then grow 0.1μm~0.25μm thick AlGaInAs(AlQ) material active area, then grow 0.2μm~0.5μm InP spacer layer 4, and finally epitaxially grow 0.1μm~0.25μm InGaAsP(PQ) material grating layer 5, and complete the epitaxy of active area cavity 10. The specific structure is as follows Figure 4 shown.
[0062] Similarly, since the upper surface of the passive waveguide layer 8 is protected by the SiO2 hard mask 9 during the second epitaxial growth, the second epitaxial growth will not occur on the upper surface of the passive waveguide layer 8. Therefore, the second epitaxial growth is also carried out on part of the surface of the substrate 1, so it can also be called the second selective epitaxial growth.
[0063] Furthermore, the total thickness of the second selective epitaxial growth in step S3 is equal to the thickness of the first selective epitaxial growth in step S1.
[0064] Specifically, the passive waveguide layer 8 is first grown, and the passive waveguide layer 8 encloses the active region cavity 10, so that the active region cavity 10 can form a buried heterostructure (Buried Heterostructure, BH), and the Al-containing active layer 3 is arranged in the buried heterostructure during the second epitaxial growth of the active region cavity 10. The Al-containing active layer 3 is buried by the subsequently grown material and is also isolated from water and oxygen by the surrounding passive waveguide layer 8, ensuring that the Al-containing element will not be exposed to the air to avoid the risk of oxidation.
[0065] It should be noted that, since the passive waveguide layer 8 of the first epitaxial growth encloses the active region cavity 10, the height of the active region cavity 10 is equal to the thickness of the passive waveguide layer 8. The second epitaxial growth needs to fill the active region cavity 10, and the positions of the two growths are just complementary, so the thickness of the two growths is guaranteed to be the same, avoiding the formation of stepped terraces by the two epitaxial growths, which affects the subsequent third epitaxial growth and further affects the chip performance.
[0066] In step S4, the SiO2 hard mask 9 grown on the surface of the passive waveguide layer 8 needs to be removed first, and then the periodic grating structure is prepared on the PQ grating layer 5 through an electron beam exposure machine. Then, an InP cladding layer 6 with a thickness of 1 μm to 2.5 μm and an InGaAs ohmic contact layer 7 with a thickness of 0.15 μm to 0.3 μm are sequentially grown on the surface of the grating layer 5 to perform the third epitaxial growth. At this time, since the SiO2 hard mask 9 of the passive waveguide layer 8 has been removed, the third epitaxial growth will be performed simultaneously on the surface of the passive waveguide layer 8 and the grating layer 5, such as Figure 5 shown.
[0067] Step S5, using PECVD to deposit 1500A of SiO2 as a hard mask 9, and then using yellow light overlay process and BOE wet etching process to form a long strip SiO2 hard mask 9. At this time, the coverage of the long strip SiO2 hard mask 9 needs to completely cover the position of the active area cavity 10, and the width cannot exceed the outermost side of the high resistance isolation area 81. Use a bromine aqueous solution of (Br:HBr):H2O=(1:17):5 (that is, a bromine aqueous solution configured with Br:HBr=1:17 and then diluted with water 5 times) to perform wet etching to etch the area where the hard mask 9 ohmic contact layer 7 is not grown. The etching table depth is 2.5μm~10μm, and at least the buffer layer 2 must be etched, such as Figure 6 shown.
[0068] Finally, the metal upper and lower levels and the optical films on the device end faces are made to complete the chip preparation.
[0069] Specifically, this is because the chip is prepared in a wafer, and each layer generally grows in the same plane and at the same height during growth. Since the passive waveguide layer 8 is etched into a certain shape in step S2, during the second epitaxial growth, in addition to the active region cavity 10, material will also grow around the passive waveguide layer 8. A long hard mask 9 is used to protect the required area, and then the redundant part of the side of the passive waveguide layer 8 is etched and removed by bromine water, so that the area of the second epitaxial growth is finally retained only in the active region cavity 10, as shown in FIG. Figures 7 to 9 shown.
[0070] Embodiment 2:
[0071] A buried butt-jointed semiconductor laser chip is manufactured by the chip manufacturing method described in the first embodiment. Figures 6 to 9 shown.
[0072] Specifically, the prepared chip is composed of a metal lower layer, a substrate 1, a passive waveguide layer 8, a cladding layer 6, an ohmic contact layer 7, a mask layer and a metal upper layer from bottom to top, wherein an active region cavity 10 is provided in the passive waveguide, the passive waveguide layer 8 is a docking structure composed of two parallel rectangular high-resistance isolation regions 81 and a light-emitting region 82 connecting the two rectangular ends, and the active region cavity 10 is formed by the three. The active region cavity 10 is composed of a buffer layer 2, an Al-containing active layer 3, a spacer layer 4, and a grating layer 5 from bottom to top, the bottom surface of the buffer layer 2 is in contact with the substrate 1, and the upper surface of the grating layer 5 is in contact with the cladding layer 6.
[0073] The semiconductor laser chip made by this method uses an active region containing Al elements, that is, an AlGaInAs (AlQ) material active region; at the same time, the cavity length and area of the active region are also greatly reduced compared with the existing technology, with lower Ith (threshold current), lower parasitic capacitance and junction capacitance, and better reliability performance. Most importantly, it can achieve a higher modulation rate with a higher modulation and response bandwidth, and is a high-speed DML chip.
[0074] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a semiconductor laser chip with a buried and butted structure, characterized in that: Included steps S1. Selecting a substrate and growing a passive waveguide layer on the substrate to perform a first epitaxial growth; S2. growing a hard mask on the surface of the passive waveguide layer, selectively etching the passive waveguide layer, and etching the passive waveguide layer into a butt joint structure; The docking structure includes two parallel rectangular high-resistance isolation areas and a light-emitting area connecting the ends of the two rectangular high-resistance isolation areas, and the light-emitting area and the high-resistance isolation area enclose an active area cavity; S3. sequentially growing a buffer layer, an Al-containing active layer, a spacer layer and a grating layer on the substrate to perform a second epitaxial growth; S4. removing the hard mask, sequentially growing a cladding layer and growing an ohmic contact layer to perform a third epitaxial growth; S5. Grow the hard mask again, etch the redundant areas on both sides of the chip, form steps, and then make metal upper and lower levels and optical films on the device end faces.
2. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 1, characterized in that: The total thickness of the second epitaxial growth in step S3 is equal to the thickness of the first epitaxial growth in step S1.
3. The method for preparing a semiconductor laser chip with a buried and butted structure according to claim 2, characterized in that: In the step S1, the substrate uses sulfur (S)-doped InP material, and the passive waveguide layer uses iron (Fe)-doped InP material or InGaAsP (PQ) material with high resistance.
4. A method for preparing a semiconductor laser chip with a buried and butted structure according to claim 3, characterized in that: In the step S1, when growing the passive waveguide layer, the growth temperature is 550° C. to 620° C., the growth chamber pressure is 50 mbar to 200 mbar, and the growth thickness is 1 μm to 2.5 μm.
5. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 1, characterized in that: In step S2, the length of the two high-resistance isolation regions is 10 μm to 100 μm, which is the cavity length of the active region; the spacing between the two high-resistance isolation regions is 1 μm to 2 μm, which is the cavity width of the active region; and the length of the light-emitting end region is 1 μm to 200 μm.
6. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 2, characterized in that: In the step S3, the buffer layer is made of N-type InP material with a growth thickness of 0.5μm to 1.5μm; the Al-containing active layer is made of AlGaInAs material with a growth thickness of 0.1μm to 0.25μm; the spacer layer is made of InP material with a growth thickness of 0.2μm to 0.5μm; the grating layer is made of InGaAsP (PQ) material with a growth thickness of 0.1μm to 0.25μm.
7. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 1, characterized in that: In the step S5, when etching the ohmic contact layer, a bromine aqueous solution of (Br:HBr=1:17):H2O=1:5 is used for wet etching, and the etching mesa depth is 2.5 μm to 10 μm.
8. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 1, characterized in that: In the step S4, the cladding layer is made of InP material and has a growth thickness of 1 μm to 2.5 μm; the ohmic contact layer is made of InGaAs material and has a growth thickness of 0.15 μm to 0.3 μm.
9. The method for preparing a semiconductor laser chip with a buried butt-jointed structure according to claim 1, characterized in that: The first epitaxial growth, the second epitaxial growth and the third epitaxial growth are all grown using a MOCVD machine or an MBE machine.
10. A semiconductor laser chip with a buried butt-jointed structure, characterized in that: The semiconductor laser chip is manufactured by the method for preparing a buried and butted structure as claimed in any one of claims 1 to 9.
Citation Information
Cited By
Semiconductor laser device and method for manufacturing semiconductor laser device
CN119944437A
Semiconductor laser device and method for manufacturing semiconductor laser device