Preparation process of composite medical biological membrane
By using raw materials such as sodium hyaluronate, collagen, and modified squalene, combined with the biocrosslinker alginic acid, a stable biofilm is formed, which solves the problem of poor wound repair and antibacterial and antibacterial effects of existing biofilms in wound repair and antibacterial and antibacterial effects. , realizes stability and safety on the skin surface, and has excellent antibacterial, antibacterial and antioxidant properties.
Patent Information
- Application Number
- CN202411175606.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
Existing biofilms have limited effects in wound repair and antibacterial and antibacterial, and commonly used chemical crosslinking agents are highly irritating to the skin, making it difficult to maintain stability and safety.
Sodium hyaluronate, collagen, alginic acid, hydroxypropyl methylcellulose acetate succinate, Inca fruit oil, xanthan gum and squalene are used as the main raw materials, and squalene is modified by hydrogenation and plasma treatment. Combined with the biocrosslinker alginic acid, a stable sodium hyaluronate gel is formed, enhancing the antibacterial, antibacterial and antioxidant properties of the biofilm.
It realizes the formation of a protective layer on the wound surface, promotes tissue repair, has excellent antibacterial, antibacterial and anti-inflammatory effects, and forms Schiff alkaline mass through cross-linking of alginic acid and chitosan, which is not harmful to the skin and can sterilize and improve The stability and cleaning properties of the biofilm are achieved.
Smart Images

Figure BDA0005010635040000081 
Figure BDA0005010635040000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biofilms, in particular to a preparation process of a composite medical biofilm. Background Art
[0002] In recent years, hydrogel materials have become a hot material in the current research of biofilm medical dressings and wound dressings due to their excellent water content, biocompatibility, biodegradability, and adjustable physical and chemical properties. Hydrogel biofilm medical dressings have high water content, strong permeability and skin adhesion, which can provide a moist environment conducive to healing for the skin or wound surface, and give the material excellent tissue adhesion, moisturizing, antibacterial, antioxidant and regulation of inflammatory factor expression functions. Therefore, it has broad prospects in the application field of biofilm medical dressings and wound dressings.
[0003] The present invention is a new product developed using sodium hyaluronate, collagen, glycerin, xanthan gum, hydroxypropyl methylcellulose, maltodextrin, sodium methylparaben, essence and purified water as main raw materials, and has the effects of antibacterial, antibacterial, anti-inflammatory, hemostasis, and promotion of wound healing. By forming a protective layer on the surface of the wound, it acts as a physical barrier. It is suitable for non-chronic wounds such as small wounds, abrasions, cuts, burns (first degree or second degree) and surrounding skin; it is suitable for laser surgery, fruit acid peeling wound care, post-sun skin repair, relieving skin dryness and tightness, skin eczema, acne wound damage, etc.; it is suitable for relieving discomfort symptoms in gynecology, anorectal, dermatology, stomatology and ENT. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation process of a composite medical biofilm to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a composite medical biofilm, wherein the biofilm is a new product developed with sodium hyaluronate, collagen, alginate, chitosan, hydroxypropyl methylcellulose acetate succinate, inca inchi oil, xanthan gum and squalene as main raw materials.
[0006] Furthermore, the squalene is treated with hydrogenation and plasma to generate multiple active ions such as ions, excited molecules, and free radicals, and the activity of the squalene is increased after modification.
[0007] Furthermore, a preparation process of a composite medical biofilm comprises the following preparation steps:
[0008] (1) At a temperature of 120-140°C, the pressure is set to 1-2 MPa, the catalyst is mixed with the squalene raw material and the organic solvent in a mass ratio of 1:0.01-0.05:5, and then hydrogenation is performed slowly and gently; the temperature is then raised to 160-200°C, the pressure is 6-10 MPa, and hydrogenation is performed for 1-5 hours under the catalytic action of the catalyst to prepare hydrogenated squalene; 2 parts of hydrogenated squalane are accurately weighed and dissolved in 10 parts of deionized water, and the suspension is prepared in a conical flask, and placed in a refrigerator at a temperature of 4°C for 24 hours to fully hydrate it; 10 The modified squalane suspension is placed in a culture dish, the gas valve is opened, and high-purity argon gas is first introduced into the low-temperature plasma reactor under normal pressure, and then nitrogen gas is introduced, with a gas flow rate of 10 L / min; the treatment voltage is 5 kV, the treatment frequency is 20 kHz, the temperature is controlled at 22-28 ° C, and the plasma treatment time is 1-10 min; the modified squalane suspension is obtained; the mixture is centrifuged at a speed of 12000-20000 rpm for 20 min, a supernatant containing the modified squalane is taken, and the supernatant is freeze-dried for 24 h to obtain the modified squalane;
[0009] (2) Weigh 0.5-1.5 parts of sodium hydroxide, dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 1-3 parts of sodium hyaluronate and 0.5-5 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 150-250rpm; take 0.1-0.2 parts of sodium alginate and add it to the above solution, stir and react at 30°C for 3-4 hours, and the stirring speed is 400rpm; after the reaction is completed, add hydrochloric acid solution to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer solution, let it stand and swell for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel, and stir at 60rpm. After collecting the precipitate, vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085MPa to obtain sodium hyaluronate gel powder;
[0010] (3) Add 0.5-1.5 parts of sodium hyaluronate gel powder and 0.03-0.08 parts of collagen to 10 parts of purified water at 60-70°C, slowly stir, and stand for 4-5 hours to completely dissolve to obtain a sol solution; add 0.05-0.25 parts of hydroxypropyl methylcellulose acetate succinate and 0.1-0.8 parts of modified squalene to 10 parts of purified water at 40-50°C, stir and dissolve, stand for 2-3 hours to completely dissolve to obtain a mixed solution; lower the temperature of the sol solution to 40-50°C. ℃, pour it into the mixed solution, add 3-5 parts of Inca Inchi oil, stir at 150-200rpm for 1-2h to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80℃, slowly stir for 20min, cool to 40-50℃, slowly add it to the intermediate product, stir slowly while adding, wait until the temperature drops to 20℃, add 0.001 parts of essence, and then add 60 parts of purified water, slowly stir for 20-30min to obtain a skin repair biofilm.
[0011] Furthermore, the reaction time of the steady, slow and mild hydrogenation in step (1) is 2 hours.
[0012] Furthermore, in step (1), the catalyst is Pd / C or Pt / C.
[0013] Furthermore, the organic solvent in step (1) is one of toluene, n-hexane and n-heptane.
[0014] Furthermore, the freeze-drying temperature in step (1) is -40°C.
[0015] Furthermore, the concentration of the hydrochloric acid solution in step (2) is 0.01 mol / L.
[0016] Furthermore, the concentration of the phosphate buffer in step (2) is 0.1 mol / L.
[0017] Furthermore, the slow stirring speed in step (3) is 45 rpm.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The present invention uses sodium hyaluronate, collagen, alginic acid, chitosan, hydroxypropyl methylcellulose acetate succinate, inca inchi oil, xanthan gum, and squalene as main raw materials to develop new products, which can bring peptide growth factors and other structural proteins to the site of action, and then enzymatically degrade and release active proteins to promote tissue repair, and has antibacterial, antibacterial, and anti-inflammatory effects; it is suitable for laser surgery, fruit acid skin peeling wound care, sunburn skin repair, and relieves dry and tight skin, skin eczema, and acne wound damage;
[0020] The squalene added in the present invention generates multiple active ions such as ions, excited molecules, and free radicals after hydrogenation and plasma treatment. The modification increases the activity of squalene, but it contains multiple double bonds and is extremely unstable and easily oxidized, so it is grafted into sodium hyaluronate to interact with the double bonds of gelled sodium hyaluronate to chemically link it to maintain its stability on the skin surface; the commonly used chemical cross-linking agents are highly irritating to the skin, so the present invention uses a biological cross-linking agent, alginate, to combine the aldehyde group on it with the hydroxyl group on sodium hyaluronate, and the gelled sodium hyaluronate is grafted into the sodium hyaluronate by the creation of A protective layer is formed on the surface of the surface, which acts as a physical barrier; when the alginate is cross-linked, the aldehyde group on the alginate is cross-linked with the amino group on the chitosan to form a Schiff base group. While the biofilm covers the skin to form a barrier, the Schiff base plays a role of not hurting the skin but also killing bacteria; the esterified hydroxypropyl methylcellulose, as an auxiliary thickener, has an ionizable terminal carboxyl group, which improves the storage capacity of the biofilm and is easy to clean during use to reduce residues; the biofilm prepared by the present invention contains a large amount of active hydrogen groups, which can effectively remove excess free radicals and achieve excellent antioxidant effects. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a composite medical biofilm prepared in the following examples are as follows:
[0023] Repair rate: 34 healthy New Zealand white rabbits were selected, half of which were male and half were female. The rabbits were depilated and disinfected. Combined anesthesia was performed by intramuscular injection of Su Mian Xin and intravenous injection of sodium pentobarbital. A burn wound of 4 cm was prepared on both sides of the rabbits' backs using a YLS-5Q burn instrument. 2The scalding conditions were as follows: the scalding head temperature was 100°C, the applied pressure was 1000g, and the contact time between the scalding head and the rabbit skin was 5s. Two hours after the modeling, two female and two male rabbits were killed and sent for pathological examination to determine the deep II degree scald model. The remaining 30 model rabbits were randomly divided into 10 groups, namely, the model control group (1 group) and the sample group (9 groups), 3 rabbits / group. The model control group was not given any medicine after modeling, and the sample group was smeared with 150mg of biofilm per wound. The Nagelschmidt method was used to determine the wound healing area on the 7th, 14th, and 21st days of modeling, that is, the scald wound on the back of the rabbit was covered with weighing paper, the edge of the wound was drawn on the transparent weighing paper, the shape of the wound was cut out, and its weight was weighed. The healing rate was calculated according to the following formula: Wound healing rate % = (original wound paper weight - unhealed wound paper weight) / original wound paper weight × 100%. Repair rate = sample wound healing rate - control group healing rate.
[0024] Antibacterial property: Take 10g of each sample from the above-mentioned embodiment and comparative example, and place them in a sterile conical flask as a sample group; at the same time, prepare a blank control group without adding samples, add 70ml of 0.03mol / l PBS and 5ml of Staphylococcus aureus bacterial solution to 10 groups respectively, and culture them under shaking conditions of 25°C and 200rpm / min for 1h. Take samples at 0h and 1h, and calculate the change in the number of bacteria. The test of each sample group and control group was repeated 3 times, and the average antibacterial rate was calculated. Calculation of antibacterial rate: Antibacterial rate = (average number of colonies before sample shaking - average number of colonies after sample shaking) / average number of colonies before sample shaking × 100%
[0025] Example 1
[0026] (1) At a temperature of 120°C and a pressure of 1 MPa, a catalyst Pd / C is mixed with squalene raw material and toluene in a mass ratio of 1:0.01:5, and then hydrogenated slowly and gently for 2 hours; then the temperature is raised to 160°C and the pressure is set to 6 MPa, and hydrogenated for 1 hour under the catalytic action of the catalyst to prepare hydrogenated squalene; 2 parts of hydrogenated squalane are accurately weighed and dissolved in 10 parts of deionized water, and the suspension is prepared in a conical flask and placed in a refrigerator at a temperature of 4°C for 24 hours to fully hydrate; 10 parts of squalane are taken and the mixture is stirred for 2 hours. The squalane suspension is placed in a culture dish, the gas valve is opened, and high-purity argon gas is first introduced into the low-temperature plasma reactor under normal pressure, and then nitrogen gas is introduced, with a gas flow rate of 10 L / min; the treatment voltage is 5 kV, the treatment frequency is 20 kHz, the temperature is controlled at 22° C., and the plasma treatment time is 1 min; thus, a suspension of modified squalane is obtained; the mixture is centrifuged at 12000 rpm for 20 min, a supernatant containing modified squalane is taken, and the supernatant is freeze-dried at -40° C. for 24 h to obtain modified squalane;
[0027] (2) Weigh 0.5 parts of sodium hydroxide and dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 1 part of sodium hyaluronate and 0.5 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 150rpm; take 0.1 parts of sodium alginate and add it to the above solution, stir and react at 30°C for 3 hours, and the stirring speed is 400rpm; after the reaction is completed, add a hydrochloric acid solution with a concentration of 0.01mol / L to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer with a concentration of 0.1mol / L, and let it stand for swelling for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel at a stirring speed of 60rpm, collect the precipitate, and vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085MPa to obtain sodium hyaluronate gel powder;
[0028] (3) Add 0.5 parts of sodium hyaluronate gel powder and 0.03 parts of collagen to 10 parts of 60°C purified water, stir slowly at 45 rpm, and let stand for 4 hours to completely dissolve to obtain a sol solution; add 0.05 parts of hydroxypropyl methylcellulose acetate succinate and 0.1 parts of modified squalene to 10 parts of 40°C purified water, stir and dissolve at 45 rpm, and let stand for 2 hours to completely dissolve to obtain a mixed solution; after the sol solution temperature is lowered to 40°C, pour it into the mixed solution and add Add 3 parts of Inca Inchi oil and stir at 150 rpm for 1 hour to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20 minutes at 45 rpm, cool to 40°C, slowly add it to the intermediate product, slowly stir while adding at 45 rpm, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, slowly stir at 45 rpm for 20 minutes to obtain a skin repair biofilm.
[0029] Example 2
[0030] (1) At a temperature of 130°C, the pressure is set to 1.5 MPa, the catalyst Pd / C is mixed with squalene raw material and n-hexane in a mass ratio of 1:0.03:5, and then hydrogenated slowly and gently for 2 hours; then the temperature is raised to 180°C and the pressure is 8 MPa, and hydrogenated for 3 hours under the catalytic action of the catalyst to prepare hydrogenated squalene; 2 parts of hydrogenated squalane are accurately weighed and dissolved in 10 parts of deionized water, and the suspension is prepared in a conical flask, and placed in a refrigerator at a temperature of 4°C for 24 hours to fully hydrate it; 10 parts The squalane suspension is placed in a culture dish, the gas valve is opened, and high-purity argon gas is first introduced into the low-temperature plasma reactor under normal pressure, and then nitrogen gas is introduced, with a gas flow rate of 10 L / min; the treatment voltage is 5 kV, the treatment frequency is 20 kHz, the temperature is controlled at 25° C., and the plasma treatment time is 5 min; the modified squalane suspension is obtained; the mixture is centrifuged at 16000 rpm for 20 min, a supernatant containing the modified squalane is taken, and the supernatant is freeze-dried at -40° C. for 24 h to obtain the modified squalane;
[0031] (2) Weigh 1 part of sodium hydroxide and dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 2 parts of sodium hyaluronate and 2.75 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 200 rpm; take 0.15 parts of sodium alginate and add it to the above solution, stir and react at 30°C for 3.5 hours, and the stirring speed is 400 rpm; after the reaction is completed, add a hydrochloric acid solution with a concentration of 0.01 mol / L to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer with a concentration of 0.1 mol / L, and let it stand for swelling for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel at a stirring speed of 60 rpm, collect the precipitate, and vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085 MPa to obtain sodium hyaluronate gel powder;
[0032] (3) Add 1 part of sodium hyaluronate gel powder and 0.055 parts of collagen to 10 parts of 65°C purified water, stir slowly at 45 rpm, and let stand for 4.5 hours to completely dissolve to obtain a sol solution; add 0.15 parts of hydroxypropyl methylcellulose acetate succinate and 0.45 parts of modified squalene to 10 parts of 45°C purified water, stir and dissolve at 45 rpm, and let stand for 2.5 hours to completely dissolve to obtain a mixed solution; after the sol solution temperature is lowered to 45°C, pour it into the mixed solution, Add 4 parts of Inca Inchi oil and stir at 175rpm for 1.5h to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20min at 45rpm, cool to 45°C, slowly add it to the intermediate product, stir slowly at 45rpm, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, stir slowly at 45rpm for 25min to obtain a skin repair biofilm.
[0033] Example 3
[0034] (1) At a temperature of 140°C and a pressure of 2 MPa, a catalyst Pd / C is mixed with a squalene raw material and n-heptane in a mass ratio of 1:0.05:5, and then hydrogenated slowly and gently for 2 hours; then the temperature is raised to 200°C and the pressure is 10 MPa, and hydrogenated for 5 hours under the catalytic action of the catalyst to prepare hydrogenated squalene; 2 parts of hydrogenated squalane are accurately weighed and dissolved in 10 parts of deionized water, and the suspension is prepared in a conical flask and placed in a refrigerator at a temperature of 4°C for 24 hours to fully hydrate; 10 parts of squalane are taken and the mixture is stirred for 24 hours. The squalane suspension is placed in a culture dish, the gas valve is opened, and high-purity argon gas is first introduced into the low-temperature plasma reactor under normal pressure, and then nitrogen gas is introduced, with a gas flow rate of 10 L / min; the treatment voltage is 5 kV, the treatment frequency is 20 kHz, the temperature is controlled at 28° C., and the plasma treatment time is 10 min; that is, a suspension of modified squalane is obtained; centrifugation is performed at a speed of 20000 rpm for 20 min, and a supernatant containing modified squalane is taken, and the supernatant is freeze-dried at -40° C. for 24 h to obtain modified squalane;
[0035] (2) Weigh 1.5 parts of sodium hydroxide and dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 3 parts of sodium hyaluronate and 5 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 250rpm; take 0.2 parts of sodium alginate and add it to the above solution, stir and react at 30°C for 4 hours, and the stirring speed is 400rpm; after the reaction is completed, add a hydrochloric acid solution with a concentration of 0.01mol / L to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer with a concentration of 0.1mol / L, and let it stand for swelling for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel at a stirring speed of 60rpm, collect the precipitate, and vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085MPa to obtain sodium hyaluronate gel powder;
[0036] (3) Add 1.5 parts of sodium hyaluronate gel powder and 0.08 parts of collagen to 10 parts of 70°C purified water, stir slowly at 45 rpm, and let stand for 5 hours to completely dissolve to obtain a sol solution; add 0.25 parts of hydroxypropyl methylcellulose acetate succinate and 0.8 parts of modified squalene to 10 parts of 50°C purified water, stir and dissolve at 45 rpm, and let stand for 3 hours to completely dissolve to obtain a mixed solution; after the sol solution temperature is lowered to 50°C, pour it into the mixed solution and add Add 5 parts of Inca Inchi oil and stir at 200 rpm for 2 hours to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20 minutes at 45 rpm, cool to 50°C, slowly add it to the intermediate product, stir slowly at 45 rpm, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, stir slowly at 45 rpm for 30 minutes to obtain a skin repair biofilm.
[0037] Comparative Example 1
[0038] The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (3) is changed to: 1 part of sodium hyaluronate gel powder and 0.055 parts of collagen are added to 10 parts of 65°C purified water, slowly stirred at a speed of 45 rpm, and allowed to stand for 4.5 hours to completely dissolve to obtain a sol solution; 0.15 parts of hydroxypropyl methylcellulose acetate succinate are added to 10 parts of 45°C purified water, stirred and dissolved at a speed of 45 rpm, and allowed to stand for 2.5 hours to completely dissolve to obtain a mixed solution; after the sol solution temperature is lowered to 45°C, pour it into the mixed solution In the solution, 4 parts of Inca Inchi oil were added, and the mixture was stirred at 175 rpm for 1.5 hours to obtain an intermediate product; 0.3 parts of xanthan gum were mixed with 10 parts of purified water, and the mixture was heated to 80°C, and then slowly stirred for 20 minutes at a speed of 45 rpm. After cooling to 45°C, the mixture was slowly added to the intermediate product, and slowly stirred at a speed of 45 rpm. When the temperature dropped to 20°C, 0.001 parts of essence were added, and then 60 parts of purified water were added, and the skin repair biofilm was obtained after slowly stirring at a speed of 45 rpm for 25 minutes. The remaining steps were the same as those in Example 2.
[0039] Comparative Example 2
[0040] The difference between Comparative Example 2 and Example 2 is that there is no step (2), and step (3) is changed to: 1 part of sodium hyaluronate, 1.25 parts of chitosan, 0.1 part of sodium alginate, and 0.055 parts of collagen are added to 10 parts of 65°C purified water, slowly stirred at a speed of 45 rpm, and allowed to stand for 4.5 hours to completely dissolve to obtain a sol solution; 0.15 parts of hydroxypropyl methylcellulose acetate succinate and 0.45 parts of modified squalene are added to 10 parts of 45°C purified water, stirred and dissolved at a speed of 45 rpm, and allowed to stand for 2.5 hours to completely dissolve to obtain a mixed solution; the sol solution is warmed to 450 ° C, and the mixture is stirred and dissolved at a speed of 45 rpm, and the mixture is allowed to stand for 2.5 hours to completely dissolve to obtain a mixed solution. After the temperature drops to 45°C, pour it into the mixed solution, add 4 parts of Inca Inchi oil, and stir at 175rpm for 1.5h to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20min at 45rpm, cool to 45°C, slowly add it to the intermediate product, stir slowly at 45rpm, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, and slowly stir at 45rpm for 25min to obtain a skin repair biofilm; the remaining steps are the same as Example 2.
[0041] Comparative Example 3
[0042] The difference between Comparative Example 3 and Example 2 is that there is no step (1), and step (3) is changed to: 1 part of sodium hyaluronate gel powder and 0.055 parts of collagen are added to 10 parts of 65°C purified water, slowly stirred at a speed of 45 rpm, and allowed to stand for 4.5 hours to completely dissolve to obtain a sol solution; 0.15 parts of hydroxypropyl methylcellulose acetate succinate and 0.45 parts of squalene are added to 10 parts of 45°C purified water, stirred and dissolved at a speed of 45 rpm, and allowed to stand for 2.5 hours to completely dissolve to obtain a mixed solution; after the temperature of the sol solution is lowered to 45°C, Pour into the mixed solution, add 4 parts of Inca Inchi oil, stir at 175rpm for 1.5h to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20min at 45rpm, cool to 45°C, slowly add it to the intermediate product, stir slowly at 45rpm, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, stir slowly at 45rpm for 25min to obtain a skin repair biofilm; the remaining steps are the same as Example 2.
[0043] Comparative Example 4
[0044] The difference between Comparative Example 4 and Example 2 is that step (2) is different, and step (2) is changed to: weigh 1 part of sodium hydroxide, dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 2 parts of sodium hyaluronate and 2.75 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 200 rpm; take 0.15 parts of genipin and add it to the above solution, stir and react at 30°C for 3.5 hours, and the stirring speed is 400 rpm; after the reaction is completed, add a hydrochloric acid solution with a concentration of 0.01 mol / L to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer with a concentration of 0.1 mol / L, and let it stand for swelling for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel, and stir at a speed of 60 rpm. After collecting the precipitate, vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085 MPa to obtain sodium hyaluronate gel powder; the remaining steps are the same as Example 2.
[0045] Comparative Example 5
[0046] The difference between Comparative Example 5 and Example 2 is that step (3) is different. Step (3) is changed to: add 1 part of sodium hyaluronate gel powder and 0.055 parts of collagen to 10 parts of 65°C purified water, slowly stir at a speed of 45 rpm, and stand for 4.5 hours to completely dissolve to obtain a sol solution; add 0.15 parts of hydroxypropyl methylcellulose and 0.45 parts of modified squalene to 10 parts of 45°C purified water, stir and dissolve at a speed of 45 rpm, and stand for 2.5 hours to completely dissolve to obtain a mixed solution; after the sol solution temperature is lowered to 45°C, pour it into Add 4 parts of Inca Inchi oil to the mixed solution, and stir at 175 rpm for 1.5 hours to obtain an intermediate product; mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, and slowly stir for 20 minutes at a speed of 45 rpm. After cooling to 45°C, slowly add it to the intermediate product while slowly stirring at a speed of 45 rpm. When the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water. After slowly stirring at a speed of 45 rpm for 25 minutes, a skin repair biofilm is obtained; the remaining steps are the same as Example 2.
[0047] Effect example
[0048] Table 1 below shows the performance analysis results of a composite medical biomembrane using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0049] Table 1
[0050]
[0051]
[0052] From the comparison of the experimental data of the repair rate of the embodiment and the comparative example, it can be found that the present invention uses sodium hyaluronate, collagen, alginic acid, chitosan, hydroxypropyl methylcellulose acetate succinate, inca inchi oil, xanthan gum, and squalene as the main raw materials to develop new products, which can bring peptide growth factors and other structural proteins to the site of action, and then enzymatically degrade and release active proteins to promote tissue repair, and has antibacterial, antibacterial, and anti-inflammatory effects; it is suitable for laser surgery, fruit acid skin peeling wound care, after-sun skin repair, and relieves skin dryness and tightness, skin eczema, acne wound damage; the present invention adds After hydrogenation and plasma treatment, squalene generates multiple active ions such as ions, excited molecules, and free radicals. The modification increases the activity of squalene, but it contains multiple double bonds and is extremely unstable and easily oxidized, so it is grafted into sodium hyaluronate to interact with the double bonds of gelled sodium hyaluronate to form chemical links to maintain its stability on the skin surface. Commonly used chemical cross-linking agents are highly irritating to the skin, so the present invention uses a biological cross-linking agent, alginate, to combine the aldehyde group on it with the hydroxyl group on sodium hyaluronate, and the gelled sodium hyaluronate forms a protective layer on the wound surface to act as a physical barrier. From the comparison of the experimental data of the antibacterial rate of the embodiment and the comparative example, it can be found that when the alginate of the present invention is cross-linked, the aldehyde group on it is cross-linked with the amino group on the chitosan to form a Schiff base group. While the biofilm covers the skin to form a barrier, the Schiff base plays a role of not hurting the skin but also killing bacteria; the esterified hydroxypropyl methylcellulose, as an auxiliary thickener, has an ionizable terminal carboxyl group, which improves the storage capacity of the biofilm and is easy to clean during use to reduce residues; the biofilm prepared by the present invention contains a large amount of active hydrogen groups, which can effectively remove excess free radicals and achieve excellent antioxidant effects.
[0053] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A composite medical biofilm, characterized in that: The biofilm is a new product developed with sodium hyaluronate, collagen, alginate, chitosan, hydroxypropyl methylcellulose acetate succinate, inca inchi oil, xanthan gum and squalene as main raw materials.
2. A composite medical biofilm according to claim 1, characterized in that: The squalene is treated by hydrogenation and plasma to generate multiple active ions such as ions, excited molecules, free radicals, etc., and the activity of the squalene is increased after modification.
3. A process for preparing a composite medical biofilm, characterized in that: The method comprises the following preparation steps: (1) At a temperature of 120-140°C, the pressure is set to 1-2 MPa, the catalyst is mixed with the squalene raw material and the organic solvent in a mass ratio of 1:0.01-0.05:5, and then hydrogenation is performed slowly and gently; the temperature is then raised to 160-200°C, the pressure is 6-10 MPa, and hydrogenation is performed for 1-5 hours under the catalytic action of the catalyst to prepare hydrogenated squalene; 2 parts of hydrogenated squalane are accurately weighed and dissolved in 10 parts of deionized water, and the suspension is prepared in a conical flask, and placed in a refrigerator at a temperature of 4°C for 24 hours to fully hydrate it; 10 The modified squalane suspension is placed in a culture dish, the gas valve is opened, and high-purity argon gas is first introduced into the low-temperature plasma reactor under normal pressure, and then nitrogen gas is introduced, with a gas flow rate of 10 L / min; the treatment voltage is 5 kV, the treatment frequency is 20 kHz, the temperature is controlled at 22-28 ° C, and the plasma treatment time is 1-10 min; the modified squalane suspension is obtained; the mixture is centrifuged at a speed of 12000-20000 rpm for 20 min, a supernatant containing the modified squalane is taken, and the supernatant is freeze-dried for 24 h to obtain the modified squalane; (2) Weigh 0.5-1.5 parts of sodium hydroxide, dissolve it in 50 parts of deionized water to prepare a sodium hydroxide solution, add 1-3 parts of sodium hyaluronate and 0.5-5 parts of chitosan, stir and dissolve at 40°C for 1 hour, and the stirring speed is 150-250rpm; take 0.1-0.2 parts of sodium alginate and add it to the above solution, stir and react at 30°C for 3-4 hours, and the stirring speed is 400rpm; after the reaction is completed, add hydrochloric acid solution to adjust the pH to neutral to terminate the cross-linking reaction; then add 100 parts of phosphate buffer solution, let it stand and swell for 3 hours; under stirring, add 200 parts of 95% ethanol dropwise to the swollen gel, and stir at 60rpm. After collecting the precipitate, vacuum dry it at 40°C for 12 hours, and the vacuum degree is -0.085MPa to obtain sodium hyaluronate gel powder; (3) adding 0.5-1.5 parts of sodium hyaluronate gel powder and 0.03-0.08 parts of collagen to 10 parts of purified water at 60-70° C., stirring slowly, and standing for 4-5 hours to completely dissolve the sol solution; adding 0.05-0.25 parts of hydroxypropyl methylcellulose acetate succinate and 0.1-0.8 parts of modified squalene to 10 parts of purified water at 40-50° C., stirring and dissolving the sol solution, standing for 2-3 hours to completely dissolve the sol solution, and cooling the sol solution to 40-50° C., pouring the sol solution into the mixed solution, adding 3-5 parts of inca inchi oil, and stirring at 150-200 rpm for 1-2 hours to obtain an intermediate product; Mix 0.3 parts of xanthan gum with 10 parts of purified water, heat to 80°C, slowly stir for 20 minutes, cool to 40-50°C, slowly add it to the intermediate product while slowly stirring, wait until the temperature drops to 20°C, add 0.001 parts of essence, and then add 60 parts of purified water, slowly stir for 20-30 minutes to obtain a skin repair biofilm.
4. The preparation process of a composite medical biofilm according to claim 3, characterized in that: The reaction time of the steady, slow and mild hydrogenation in step (1) is 2 hours.
5. The preparation process of a composite medical biofilm according to claim 3, characterized in that: The catalyst in step (1) is Pd / C or Pt / C.
6. The preparation process of a composite medical biofilm according to claim 3, characterized in that: The organic solvent in step (1) is one of toluene, n-hexane and n-heptane.
7. The preparation process of a composite medical biofilm according to claim 3, characterized in that: The freeze-drying temperature in step (1) is -40°C.
8. The process for preparing a composite medical biofilm according to claim 3, characterized in that: The concentration of the hydrochloric acid solution in step (2) is 0.01 mol / L.
9. The preparation process of a composite medical biofilm according to claim 3, characterized in that: The concentration of the phosphate buffer in step (2) is 0.1 mol / L.