Site injection method

JP7578345B1Active Publication Date: 2024-11-06KYOKADO ENG CO LTD

Patent Information

Application Number
JP2024089567
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-11-06
Estimated Expiration
2044-05-31

AI Technical Summary

Benefits of technology

【0025】 本発明によれば、地下空間を有するコンクリート構造物をミサイルや核兵器による空爆から保護するための地盤注入工法および地盤固結材であって、固結材の浸透性が良好で、長期耐久性、高強度、耐震性、止水性、特には放射線遮蔽機能に優れ、低炭素型の注入工法にも対応できる地盤注入工法および地盤固結材を提供することができた。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578345000001_ABST
    Figure 0007578345000001_ABST
Patent Text Reader

Abstract

Development of ground injection methods and ground consolidation materials to protect concrete structures with underground spaces from air attacks by missiles and nuclear weapons. [Solution] This is a ground injection method for protecting concrete structures that are buried underground and have underground spaces from air raids. We provide a ground injection method and a ground consolidation material that has good permeability, long-term durability, high strength, earthquake resistance, water cutoff properties, and especially excellent radiation shielding properties, and that can also be used for low-carbon injection methods.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ground injection method used for reinforcing underground concrete structures and a ground consolidation material used therein. [Background technology]

[0002] In recent years, from the perspective of national defense, subways, underground shopping malls, tunnels, etc. are being considered as evacuation shelters. However, these underground concrete structures were not built with such a situation in mind, and since they are currently partially deteriorated, reinforcement work is required.

[0003] In particular, when considering attacks by nuclear weapons as well as missiles, underground concrete structures are required to be not only strong but also to shield against radiation. Conventional radiation shielding technologies include those described in Patent Document 1 and Non-Patent Document 1. In addition, the applicant has demonstrated the long-term durability and earthquake resistance of the technologies described in Patent Documents 2 and 3 and Non-Patent Documents 2 and 3.

[0004] The present invention relates to a ground injection method used to reinforce underground concrete structures, which is a further development of the applicant's injection technology with excellent durability, strength, water cutoff and permeability, and a ground consolidation material used therefor for reinforcement and radiation shielding. The present invention provides a ground injection method and a ground consolidation material that can strengthen concrete structures that have already deteriorated or leaked by injecting a ground consolidation material into the outer periphery of an existing underground structure having a space, thereby protecting the underground space from attacks such as missiles and blocking radiation. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2019 / 031578 [Patent Document 2] JP 2018-193550 A [Patent Document 3] Patent Publication No. 2022-66686 [Patent Document 4] JP 2024-053139 A [Patent Document 5] JP 2020-083959 A [Non-patent literature]

[0006] [Non-Patent Document 1] Report of the Study Group on the Functions of Evacuation Facilities in Civil Protection, July 2008, Civil Protection Office, Fire and Disaster Management Agency, Ministry of Internal Affairs and Communications [Non-Patent Document 2] Yurika Tsunoda, Shunsuke Shimada, Tadao Koyama, Takamitsu Sasaki, Ryozo Yonekura, "Evidence Study on Permanence and Penetration and Consolidation of Ultrafine Composite Silica," 66th Annual Conference of the Japan Society of Civil Engineers, 2011 [Non-Patent Document 3] Takamitsu Sasaki, Ryozo Yonekura, Shunsuke Shimada, "Field verification test of age-related consolidation of consolidated ground using activated silica and ultrafine silica composite," 54th Geotechnical Engineering Research Conference, 0241, 2019 Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors have set the conditions for a ground injection method and a ground consolidation material that are suitable for such purposes as follows. 1) A method of using a radiation shielding material applied to an aboveground structure is already known from Patent Document 1 and Non-Patent Document 1. The present invention aims to realize the reinforcement and protection of an underground structure by an injection method. 2) It must have excellent long-term durability (because we don't know when an air strike will occur), high strength (it needs to be able to withstand the impact of an air strike), and earthquake resistance (an earthquake may occur before an air strike). 3) Excellent permeability (required permeability and solidification ability to cover the injectable limit of high-strength suspension grout) and water-stopping properties (required ability to repair deterioration of existing concrete structures. Also, water-stopping properties are required to prevent groundwater containing radiation from leaking into underground spaces). 4) It is an injection material with radiation shielding properties (it contains particles with radiation shielding properties, penetrates and solidifies into the ground, and it is desirable that the solidified material is a water-containing solidified material). 5) It is preferable that the injection method be low-carbon. (From the viewpoint of preventing global warming, it is preferable to use injection materials that can reduce CO2.)

[0008] Therefore, the object of the present invention is to provide a ground injection method and a ground consolidation material for protecting a concrete structure having an underground space from aerial bombardment by missiles or nuclear weapons, which has good permeability, long-term durability, high strength, earthquake resistance, water stoppage, and especially excellent radiation shielding function, and is also compatible with low-carbon injection methods. [Means for solving the problem]

[0009] In the present invention, the ground injection method for solving the above problem 1) is carried out as shown in Figures 1(a) to 1(c). In order to solve the above problems 2) to 5) in this injection method, the above-mentioned applicant's technology has been further developed. A. Regarding the above problem 2), the development will be based on the prior patent documents 2, 3 and non-patent documents 2, 3, in which long-term durability and earthquake resistance have been demonstrated in indoor tests, large-scale field tests, and actual earthquakes. B. Regarding the above problem 3), we will develop high strength and permeability based on Patent Documents 3 and 4. C. Regarding the above problem 4), development will be based on A and B above and Patent Documents 1 and 5.

[0010] Based on the above findings, the present inventors (1) In order to strengthen underground structures with underground spaces so that they can withstand the impact of air raids, we developed a technology based on the technologies in Patent Documents 3 and 4 that is expected to improve strength, permeability, and watertightness, and (2) In order to protect underground structures having underground spaces from radiation from nuclear missiles, etc., a technology was developed based on the above (1) and further on Non-Patent Document 1 and Patent Document 1, which applies a binder that forms a hydrous gel.

[0011] That is, the ground injection method of the present invention is a ground injection method for protecting a concrete structure buried underground and having an underground space from air raids, The following i) to iii) i) Silica particles comprising any one or more of pyrogenic silica, natural silica having a pozzolanic effect, and hardenable silica particles; ii) Silica particles made of any one or more of slag, fly ash, cement, sewage incineration ash, plant incineration ash, and calcined clay; iii) Silica particles consisting of any one or more of loam soil, volcanic ash, niwa soil and sanwa soil; A ground injection method for protecting a concrete structure by injecting a ground consolidation material consisting of a suspension containing any one of the above-mentioned suspended particles of silica particles as a main component and solution-type silica as an active ingredient into a periphery of the concrete structure from a plurality of injection holes provided in the ground, The silica particles have a Blaine value of 4000 to 20000 cm 2 / g, the amount of the silica particles in the ground consolidation material is 50 to 150 L / 400 L, silica colloid and / or water glass is used as the solution-type silica, and the bleeding liquid of the suspension is gelled, When the solution-type silica is water glass, the ground consolidation material uses water glass at a molar ratio of 1.0 to 5.0, the amount of the water glass in the ground consolidation material is 10 to 150 L / 400 L, the silica concentration of the bleeding liquid is 0.5 w / v% or more, the homogel formed by gelling the bleeding liquid has a strength to stand on its own, and the sand gel solidified by penetration of the bleeding liquid has a strength to stand on its own, The bleeding liquid has permeability to fine soil and penetrates into areas of the ground that the suspended particles could not penetrate, connecting the solidified bodies of the suspended particles from adjacent injection holes, and forming, in the ground around the concrete structure, areas solidified with a high concentration suspension, areas solidified with a low concentration suspension, and areas having water-stopping properties solidified by the gelation of the bleeding liquid, each with a thickness of 1m or more, from the part close to the center to the outside, thereby preventing the concrete structure from being directly affected by the impact of an air raid, making it possible to repair the deteriorated concrete structure, and blocking radiation by preventing groundwater from entering the underground space.

[0012] The ground injection method of the present invention is suitable for use in protecting the concrete structure from air attacks by nuclear missiles by using a ground consolidation material containing radiation shielding particles.

[0013] In the ground injection method of the present invention, it is preferable that the solution-type silica contains silica colloid and / or water glass, and the bleeding liquid of the ground consolidation agent gels.

[0014] In the ground injection method of the present invention, the silica particles preferably contain as an active ingredient any one or more of calcined silica, natural silica having pozzolanic action, and hardened silica particles. The calcined silica is preferably made of any one or more of slag, fly ash, cement, sewage incineration ash, plant incineration ash, and calcined clay, and the natural silica having pozzolanic action is preferably made of any one or more of loam soil, volcanic ash, diploid soil, and triploid soil.

[0015] In the ground injection method of the present invention, the alkaline agent preferably comprises any one or more of the following (1) to (3): (1) An alkaline agent containing gypsum and / or MgO as active ingredients. (2) An alkaline agent containing one or more of Ca salts, Ma salts, Al salts, carbonates, and bicarbonates as active ingredients. (3) An alkaline agent containing one or more of the following active ingredients: lime, cement, caustic alkali, water glass, and silica colloid.

[0016] In the ground injection method of the present invention, the silica particles have a Blaine value of 4000 to 20000 cm 2 It is preferable to use silica particles having a silica content of 50 to 150 L / 400 L in the ground consolidation material, and to set the mixing amount of the silica particles in the ground consolidation material to 50 to 150 L / 400 L. In the ground injection method of the present invention, it is preferable that the silica particles are slag, and the mixing amount of the slag in the ground consolidation material is 10 to 25 mass % when no cement is used, and 10 to 30 mass % when cement is used.

[0017] In the ground injection method of the present invention, it is preferable that the molar ratio of the water glass is 1.0 to 5.0, and the amount of the water glass mixed in the ground consolidation material is 10 to 150 L / 400 L.

[0018] In the ground injection method of the present invention, a suspension containing the silica particles as a main component and the solution-type silica as an active ingredient is used as the ground consolidation material, and the ground consolidation material is injected into the ground from the multiple injection pipes. The bleeding liquid of the ground consolidation material gels, and the homogel has a strength to stand on its own, and the sand gel solidified by the penetration of the bleeding liquid has a strength to stand on its own, The bleeding liquid can penetrate into parts of the ground that the suspension could not penetrate, thereby expanding the solidification range, or can integrate with the parts of the ground that the suspension has penetrated to form a solidified body. Here, in the above, the bleeding liquid gels and the homogel becomes self-supporting means that the silica concentration of the bleeding liquid is 0.5 w / v% or more, and the homogel does not collapse and remains self-supporting even when tilted diagonally within the mold. The sand gel being self-supporting means that the silica concentration of the bleeding liquid is 0.5 w / v% or more, the sand gel is made by a mixing method using No. 6 silica sand and the bleeding liquid so that the relative density is 60%, and the sand gel is self-supporting and has a diameter of 5 cm and a height of 10 cm. The strength of the sand gel measured in a uniaxial compression test is 2.0 kN / m 2 This means that it is more than or equal to this.

[0019] In the ground injection method of the present invention, a formulation for the ground consolidation agent can be set to provide a lightweight, low-alkaline, low-carbon type ground improvement agent.

[0020] In the ground injection method of the present invention, it is preferable that the ground consolidation material contains any one or more of microbubbles, air, a dispersant and a thickener as an active ingredient.

[0021] In the ground injection method of the present invention, the hardener is preferably a polyvalent metal compound, which is one or more of hydroxides, oxides, or salts of Ca, Mg, or Al, and / or gypsum.

[0022] In the ground injection method of the present invention, the improvement effect by injecting the ground consolidation material can be confirmed by non-destructive testing, and the non-destructive testing can be performed using elastic wave velocity logging, acoustic tomography or surface wave exploration.

[0023] The ground consolidation material of the present invention is used in the above-mentioned ground injection method and is intended to protect concrete structures buried in the ground and having underground spaces from air attacks by nuclear missiles, and is characterized in that the ground consolidation material contains radiation-shielding particles.

[0024] The ground consolidation material of the present invention is composed of (B) non-alkaline silica grout having a pH of 1 to 10, and contains as active ingredients one or more of silica colloid and water glass, and one or more of acid and salt as a reactant. When the (B) non-alkaline silica grout is composed of silica colloid, water glass, and acid, it is preferable that the ratio of the silica concentration due to silica colloid to the silica concentration due to water glass is 100:0 to 0:100, the silica concentration is 0.4 to 40 wt%, the molar ratio of silica is 2.0 to 100, and the gelation time is from instantaneous setting to 10,000 minutes. The above-mentioned non-alkali silica (Patent Document 2) and clay grout (Patent Document 5) can be injected further into the periphery of the permeated and solidified area of ​​the above-mentioned suspension-type grout (Figure 13), thereby improving the water-stopping properties and increasing the radiation shielding effect by using a hydrous gel. Effect of the Invention

[0025] According to the present invention, there has been provided a ground injection method and ground consolidation material for protecting concrete structures having underground spaces from air attacks by missiles or nuclear weapons, the consolidation material having good permeability, long-term durability, high strength, earthquake resistance, water stoppage, and especially excellent radiation shielding function, and which can also be used for low-carbon injection methods. [Brief description of the drawings]

[0026] [Figure 1] 1(a) to 1(c) are explanatory diagrams relating to the ground injection method of the present invention, in which 1(a) shows an example of reinforcing injection into the surrounding area of ​​a tunnel, 1(b) shows an example of concrete repair from inside an underground structure in service and reinforcing injection into the surrounding ground, and 1(c) shows an example of strengthening an underground structure. [Diagram 2] FIG. 13 is a photograph showing the bleeding state of the sample of Example 36. [Diagram 3] FIG. 2 is a photograph showing a bleeding state of the sample of Comparative Example 1. [Figure 4] FIG. 13 is a photograph showing the state of the sample of Example 36 several days after permeation. [Diagram 5]FIG. 1 is a photograph showing the state of the sample of Comparative Example 1 several days after infiltration. [Figure 6] 1 is a graph showing the results of a long-length penetration test for Example 36 and Comparative Example 1. [Figure 7] 7 is a graph showing an enlarged portion of the permeation distance of 90 cm to 120 cm in FIG. 6. [Figure 8] This is a photograph showing the state in which the bleeding liquid has gelled and the gel does not collapse (stands on its own) even when tilted. [Figure 9] 1 is a graph showing particle size accumulation curves of various on-site sands that have been treated with liquefaction countermeasures using solution-type grout. [Figure 10] FIG. 13 is a photograph showing the strength measurement status of a test specimen using a bleeding liquid on the 7th day. [Figure 11] FIG. 11 is a photograph showing the state of a test specimen after strength measurement of the test specimen using a bleeding liquid. [Figure 12] 1 is a graph showing the physical properties of the sand used. [Figure 13(a)] FIG. 2 is an explanatory diagram showing the form of infiltration and solidification in the ground injection method of the present invention. [Figure 13(b)] FIG. 2 is an explanatory diagram showing another form of permeation and solidification in the ground injection method of the present invention. [Figure 13(c)] FIG. 10 is an explanatory diagram showing yet another form of infiltration and consolidation in the ground injection method of the present invention. [Figure 13(d)] FIG. 10 is an explanatory diagram showing yet another form of infiltration and consolidation in the ground injection method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. The ground injection method of the present invention is a ground injection method for protecting a concrete structure buried in the ground and having an underground space from air bombing, and is characterized in that the following ground consolidation material (A) and / or (B) is injected from a plurality of injection pipes inserted into the ground into the periphery of the concrete structure to reinforce the concrete structure. (A) A suspension grout whose main component is silica particles and whose active ingredients are one or more of a hardener, an alkali agent, and solution-type silica. (B) Non-alkaline silica grout.

[0028] Specific means for solving the problems in the present invention will be described below. 1) The applicant has already developed a high-strength permanent grout (Patent Documents 3 to 5) that uses silica particles such as slag or fly ash as a permanent grout as a low-carbon injection material and injection method.

[0029] 2) In addition, the applicant has already developed a non-alkali silica grout with excellent permeability and durability (Patent Document 2). These are low-carbon grouts, and their long-term durability and earthquake resistance have been demonstrated (Patent Documents 2 and 3).

[0030] 3) Based on Patent Document 3, the inventors of the present invention have realized ground improvement by simultaneous composite injection of suspension and solution, which integrates the entire target ground with high strength, excellent penetration and solidification properties, and excellent water-stopping properties, by using ultrafine composite silica consisting of silica particles and silica solution to cover the injectable limit of silica particles by the gelling function of the bleeding liquid, and the bleeding liquid penetrates and solidifies even in areas where silica particles cannot penetrate (Figure 13).

[0031] 4) The radiation shielding function is obtained by covering the underground structure with the high-strength solidified material as described above in 3), and then covering the surrounding area with water-stopping hydrated silica gel or clay gel. In addition, by adding a material containing fine particles with radiation shielding function to the high-strength grout, it is possible to create a radiation shielding grout that is high-strength, has excellent water-stopping properties, and has radiation shielding properties. By injecting this into the ground around the concrete structure, it is possible to strengthen the underground structure. Fine particles having a radiation shielding function are already known in Patent Document 1. Also, types of radiation and types of shielding materials are known in Non-Patent Document 1. However, these are all technologies related to the radiation shielding effect of above-ground structures. The present invention relates to a technology that enables the strengthening and radiation shielding of underground structures by an injection method.

[0032] 5) Radiation permeability depends on the type of radiation and the type and thickness of shielding material contained in the grout. The radiation transmission coefficient for the wall thickness of an underground concrete structure (underground shelter) is described in Non-Patent Document 1. Here, it is described that the transmission coefficient is 0.0002 for an underground shelter with a thickness of about 80 cm, and the transmission coefficient is 0.0001 to 0.002 for an underground shelter with a concrete block structure and a wall thickness of about 61 cm. In addition, the type of radiation and the shielding material are described in FIG. 15 of Non-Patent Document 1, and the type and properties of radiation are described in FIG. 15 of Non-Patent Document 1. Furthermore, Patent Document 1 describes carbon nanohorns, nanographite, tungsten, and graphene as shielding particles. Furthermore, since water has a shielding effect, a hydrous gel containing these is effective. Clay grout is described in Patent Document 5, and a hydrous gel containing clay is effective as a radiation shielding part. Therefore, taking these factors into consideration, the solidification thickness and strength of the suspended grout formed on the periphery of the concrete structure can be determined. In the construction of the present invention, however, the construction is carried out as shown in the example of Figures 1(a) to (c), so the distance between the injection holes at which the infiltration range can be connected is set to 1 m, the solidification thickness is set to 1 m or more, and even in ground containing fine-grained soil, this injection material with high-strength penetration solidification and water-stopping properties described below is injected.

[0033] 6) In the above, the shielding of radiation, the type of radiation, and the function of the shielding material are described in Patent Document 1. In addition, the manufacturing method of particles having a radiation shielding function is described in Patent Document 2. The present invention provides a ground injection method and a ground consolidation material that solve the above problems, by injecting a high-strength injection material with excellent permeability and durability, or by injecting the above-mentioned injection material having high-strength permeability and water-stopping effect containing fine particles having a radiation shielding function into the ground, thereby strengthening an underground structure, stopping water and shielding radiation. Therefore, the following describes a method for strengthening an underground structure using a ground injection method that can achieve long-term durability, permeability, high strength, and water-stopping properties.

[0034] From the above, the technology of the present invention is as follows: 1. Strengthening underground structures by injecting high-strength, permeable grouting materials; 2. The gelation of the bleeding liquid of the suspension containing silica solution solidifies fine-grained soil into which silica particles do not penetrate, and the penetration and solidification of the bleeding liquid forms a solidified body larger than that of silica particles, making it possible to reinforce underground structures by simultaneous composite injection of the suspension and solution (Figure 13), which has strength, permeability, water-stopping effect, and radiation shielding effect. 3. A radiation shielding injection method using the above-mentioned injection material containing fine particles with radiation shielding effect. The following will focus on point 2 above, which is the most important technology.

[0035] In conventional injection materials, the main component of suspension grout is cement. Although cement has a high specific gravity of 3.17, its specific surface area is 3,220 cm 2 / g, and the cement particles are heavy. In addition, penetration between soil particles in fine-grained soil is difficult, resulting in a short permeation distance, making it difficult to form large consolidated bodies.

[0036] In the high-pressure jetting method that mainly uses cement, the improved body immediately after construction is in an unsolidified state because sufficient hydration reactions have not yet occurred. Therefore, when construction is carried out near a structure, the function of the structure may be hindered due to a decrease in bearing capacity. Also, in the conventional high-pressure jetting method that relies on the energy of the high-pressure jetting fluid, the cutting area is limited by the distance of the jetted fluid, and the size of the improved body made of cement solidification material is restricted.

[0037] Furthermore, in the high pressure injection method, the soil is removed and replaced with cement to form a solidified body, so the disposal of the removed mud has become a major environmental problem today. Furthermore, in the improvement of soft ground, since soft ground has a low bearing capacity, the improved cement solidified body is prone to sinking, and the displacement of structures is also likely to increase.

[0038] As a result of continuing research into the gelation of the bleeding liquid, the inventors have found that suspensions containing solution-type silica gel even when the bleeding rate is 50% or less or 50% or more (Fig. 2, Fig. 4, Fig. 8, Table 8). They also found that the gelation time and strength of the bleeding can be adjusted by adding a curing agent. They also found the relationship between the gelation of the bleeding liquid and the silica concentration sufficient for the homogel and sand gel to be self-supporting (Table 9, Fig. 2, Fig. 4, Figs. 6 to 8, Fig. 10, Fig. 11).

[0039] Figures 13(a)-(d) show the form of infiltration and consolidation by the ground grouting method of the present invention. Figure 13 shows that by injecting the silica suspension, the suspended particles infiltrate between the soil particles, and the bleeding liquid infiltrates and solidifies, forming an integrated infiltration and consolidation area. Figure 13 corresponds to Figures 6 and 7. Therefore, the silica particles in the suspension, or even the bleeding liquid, can penetrate and solidify into the ground from multiple injection holes, making it possible to improve the ground as a whole (Figures 13(c) and (d)). In addition, the present invention has expanded the injectable limit of suspension grout (Figure 12) to include solution-type grout (Figure 9), and has developed into a ground improvement method based on a new technical concept of simultaneous combined injection of suspension and solution.

[0040] Furthermore, the present invention relates to a ground injection method for improving the soft ground or liquefied ground around the above-mentioned underground structure with high strength and light weight, in which silica particles, slag-based or other solidifying materials are infiltrated into the surrounding area to form large solidified bodies, enabling low-carbon ground improvement. By using a suspension-type solidifying material mainly composed of calcined silica such as slag or fly ash, or silica particles with natural pozzolanic action, a non-cement-based solidifying material or a solidifying material with reduced cement content can be used, which reduces CO emissions. 2 Furthermore, by including solution-type silica in the suspension-type silica particles, the bleeding liquid of the suspension is gelled to expand the range of penetration and solidification, thereby enabling high-strength solidification effects and water-stopping effects, as well as ground improvement that can repair deteriorated underground concrete structures.

[0041] For this reason, the present invention uses artificial calcined silica such as silica powder, slag or fly ash as the main component, or uses natural silica particles with pozzolanic action as the main component, or forms a consolidated body using a small amount of cement, thereby obtaining the advantage that the weight of the improved body is reduced in the entire improved area and settlement caused by the improved body is eliminated. This is because cement has a specific gravity of 3.15, while slag has a specific gravity of 2.9, fly ash has a specific gravity of 2.8, and volcanic ash generally has a specific gravity of 0.9 to 2.5, which is almost the same as ordinary soil.

[0042] Table 1 below shows an example of a consolidated strength test of a mixture with a consolidation agent when the ground is sandy or clayey soil. Tables 1 to 7 show examples of the consolidated strength of the consolidation material or the strength when mixed with the in-situ soil. Table 8 shows the uniaxial compressive strength of the sand gel with the gelling bleeding liquid. In the present invention, by selecting a lightweight suspension mainly made of small silica particles with good fluidity according to the ground conditions, the suspension penetrates into the surrounding ground, and if the suspension contains solution-type silica, the bleeding liquid gels and solidifies, so that the solidification range expands to areas that cannot be penetrated by the suspension alone, and furthermore, a water-stopping effect and continuous solidification between the solidified bodies are possible (Figures 2, 4, and 6 to 11). Figure 9 shows the particle size distribution curve in which the penetration consolidation effect was obtained with the solution-type grout. The suspension-type consolidation material made of the above silica particles containing solution-type silica can penetrate and consolidate up to the ground with the particle size distribution in Figure 9, so that a ground injection method based on a new concept of "simultaneous suspension / solution composite injection" that has the advantages of both the suspension injection method and the solution injection method can be realized. FIG. 12 shows the particle size distribution of the permeability limit of the suspension grout without silica solution.

[0043] The ground consolidation material used in the present invention will be described below. The ground consolidation material of the present invention is used in the ground injection method of the present invention, and is used to protect concrete structures buried in the ground and having underground spaces from air attacks such as nuclear missiles.

[0044] As described above, the ground consolidation material of the present invention is preferably composed of (A) a suspension-type grout containing silica particles as a main ingredient and one or more of a hardener, an alkaline agent, and solution-type silica as active ingredients, and / or (B) a non-alkaline silica grout, and contains radiation-shielding particles.

[0045] (A) Suspension grout is mainly made of silica particles, with one or more of a hardening agent, an alkali agent, and solution-type silica as active ingredients. As a suspension mainly made of silica particles, calcined silica such as slag or fly ash is made into a water suspension, to which water glass and / or a hardening agent such as an alkali agent is mixed and adjusted for use. As the silica particles, it is preferable to use one or more of calcined silica, natural silica having a pozzolanic action, and hardenable silica particles (cement) as active ingredients.

[0046] Among these, the calcined silica includes, in addition to slag and fly ash, cement, paper sludge, sludge incineration ash, sewage incineration ash, plant incineration ash, calcined clay, and the like, and the incineration ash of plants containing a lot of silica, and any one or more of these can be used. In addition, the natural silica having a pozzolanic action includes natural calcined soil such as loam soil, volcanic ash, dip-soil soil, and trip-soil soil, and any one or more of these can be used. These calcined silicas are silica particles having a pozzolanic action, contain soluble silica, and are firmly solidified by forming a crystal structure similar to that of cement through a hydration reaction due to the action of alkalis such as slaked lime, gypsum, magnesium hydroxide, water glass, silica colloid, caustic alkali, carbonates, bicarbonates, aluminum salts, calcium salts, and magnesium salts. In addition, by using aggregates such as soil and clay as thickeners or bulking agents, it becomes possible to economically improve the ground. Furthermore, the on-site soil can be used by making it into a slurry together with the above-mentioned hardener.

[0047] The above silica particles have a Blaine value of 4000 to 20000 cm 2 / g, it is possible for the soil particles to penetrate between them. Also, by using artificial or natural calcined silica as the silica particles and setting the amount of silica particles in the ground consolidation material to 50-150 L per 400 L, high strength can be obtained. The amount of calcined silica such as slag in the consolidation material of the present invention is determined depending on the strength of the hardened product to be aimed for, but it is preferably 10-25 mass% when no cement is used, and 10-30 mass% when cement is used. In particular, when slag is used as the silica particles of the consolidation material, it is preferable to set the amount of slag in the ground consolidation material to 10-25 mass% when no cement is used, and 10-30 mass% when cement is used, because high strength can be obtained.

[0048] The hardener used in the binder of the present invention is a polyvalent metal compound, and may be one or more of hydroxides, oxides, or salts of Ca, Mg, or Al, and / or gypsum. Specifically, it is a Ca melt or an alkali agent such as cement, slaked lime, or gypsum, and in particular, slaked lime is preferable for shortening the gelation time and improving the initial strength. In addition, the binder may be used in combination with slag, bentonite, calcium carbonate, clay, silica powder such as earth and sand, etc. as a filler. As a plastic grout, fly ash, polymers, cement, plasticizers such as aluminum salts, thickeners, clay, etc. may be used as a filler.

[0049] The alkaline agent used in the binder of the present invention may be any one or more of the following (1) to (3). (1) An alkaline agent containing gypsum and / or MgO as active ingredients. (2) An alkaline agent containing one or more of Ca salts, Ma salts, Al salts, carbonates, and bicarbonates as active ingredients. (3) An alkaline agent containing one or more of the following active ingredients: lime, cement, caustic alkali, water glass, and silica colloid.

[0050] The solution-type silica used in the consolidation agent of the present invention preferably contains silica colloid and / or water glass, which gels the bleeding liquid of the consolidation agent. In this case, the molar ratio of water glass is preferably 1.0 to 5.0, and the amount of water glass in the ground consolidation agent is preferably 10 to 150 L / 400 L.

[0051] As the radiation shielding particles used in the binder of the present invention, conventionally known particles such as clay, carbon nanohorn, nanographite, tungsten, graphene, etc. can be used.

[0052] In the present invention, the slag used is finely ground blast furnace slag. In order to increase reactivity, the finer the particle size, the more preferable. For example, the finer the specific surface area (Blaine value) is, the greater the slag is. 2 / g or more, preferably 6000 cm 2 / g~20000cm 2 / g and an average particle size of 10 μm or less is suitable.

[0053] In the present invention, the water glass is preferably one having a high alkali concentration in view of reactivity with slag, and in particular, one having a molar ratio of SiO2 / Na2O of 2.5 or less is preferable. A low molar ratio can provide a high-strength solidified body and a long gelation time. In addition, the water glass may be a mixture of anhydrous sodium orthosilicate and sodium hydroxide, crystalline sodium silicate containing sodium metasilicate, a mixture containing a portion of crystalline sodium silicate, sodium silicate glass (cullet), hydrated glass, dehydrated sodium silicate, semisolid sodium silicate, viscous sodium silicate, a dilute solution of commercially available sodium silicate, or the like. The viscosity, molar ratio, and silica concentration of water glass with a molar ratio of 2.0 to 5.5, a silica solution in which silica colloid is mixed with water glass to further increase the molar ratio, or the like may be changed, or the water glass may be used as it is in powder form. The alkali content of the water glass stimulates the hydraulic properties of the slag. Water glass with a low molar ratio may be a mixture of water glass and caustic alkali. However, when using calcium molten materials such as slaked lime and cement in combination, water glass with a high SiO2 / Na2O molar ratio such as water glass No. 3 and No. 4 can be used. As the silica solution, silica colloid can be used in addition to water glass, and a mixture of silica colloid, calcined silica such as slag, and cement can also be used.

[0054] The salts used in the present invention may be aluminum compounds such as aluminum sulfate and polyaluminum chloride, or compounds obtained by reacting these with caustic alkali. Furthermore, the molar ratio of Na2O / Al2O3 is not particularly limited, but it is preferable that the Na2O concentration in the binder is 5 mass% or more in view of reactivity with slag. Caustic alkali is effective in stimulating the hydraulic properties of slag, and the aluminum content reacts with water glass and silica content of slag to form aluminum silicate or calcium aluminosilicate.

[0055] The amount of water glass and aluminum compound in the binder is such that the hardening time of the binder is several hours, usually within 1 hour, preferably within 30 minutes, and although it varies depending on the molar ratio of Na2O, Al2O3, and SiO2, it is preferable that the amount of Na2O in the binder is 2 mass% or more. However, when a wide area is to be consolidated, the amount is required so that the hardening time is several hours.

[0056] In addition, the solidification material of the present invention can be made lighter by adding a foaming agent or a foaming agent to improve the fluidity, and can be made lighter by adding clay, bentonite, or a polymer-based thickener, i.e., polyvinyl alcohol, carboxymethyl cellulose (CMC), methyl cellulose, etc., to suppress dispersibility in water, reduce precipitation, and improve workability, or to function as a water-retaining material or as a binder for silica particles such as slag, which is the main material, to form a pseudo-gel-like fluid that has a structure that is difficult to disperse while maintaining fluidity. As a result, diffusion and dilution in the ground can be reduced, and the expansion of the solidification body can be promoted.

[0057] In the present invention, microbubbles or microbubbles and air can be mixed into the above-mentioned suspension of slag, fly ash, etc., or the suspension of cement, etc., and then injected into the cutting area. This allows the suspension particles to be covered by the bearing action of the microbubbles or the microbubbles and air, making it possible to construct a wide-area solidified body using suspended particles, and also makes it possible to reduce the weight and strength of the solidified body by increasing the amount of gas in the solidified body. It has also been found that air bubbles present in the solidified body improve the liquefaction prevention effect even if the amount of suspended particles in the solidified body is small and the strength is low. Furthermore, in the consolidation material of the present invention, in addition to microbubbles and air, a dispersant and a thickener can be used, and any one or more of these can be used as the active ingredient.

[0058] Furthermore, the ground consolidation material of the present invention can also be embodied as follows. The ground consolidation material of the present invention comprises (B) non-alkaline silica grout having a pH of 1 to 10, and contains as active ingredients one or more of silica colloid and water glass, and one or more of acid and salt as a reactant. When (B) non-alkaline silica grout comprises silica colloid, water glass, and acid, the ratio of the silica concentration due to silica colloid to the silica concentration due to water glass can be 100:0 to 0:100, the silica concentration can be 0.4 to 40 wt%, the molar ratio of silica can be 2.0 to 100, and the gelation time can be from instantaneous setting to 10,000 minutes.

[0059] In the present invention, a formulation for a ground consolidation agent that is lightweight, low-alkaline, and low-carbon type for ground improvement can be set.

[0060] In the present invention, the binder may be directly mixed and fed to the injection rod as one liquid, or the above-mentioned suspension (liquid A) and water glass and / or alkaline agent (liquid B) may be pumped and mixed before injection. In this case, it is preferable to mix liquid A and liquid B at a ratio of approximately 1:1 (by volume), but they are usually mixed at any ratio within the range of 10:1 to 1:10.

[0061] In the present invention, the improvement effect by injection of the ground consolidation material can be confirmed by a non-destructive test, which can be performed using elastic wave velocity logging, acoustic tomography, or surface wave exploration.

[0062] (test) Clay soil and sandy soil were used, mixed and consolidated with the above-mentioned consolidation material of the present invention. The test results of the example in which the strength of the consolidated body was measured are shown in Table 1.

[0063] As can be seen below, cement-free consolidation materials that are primarily made of calcined silica or natural silica with pozzolanic action, or consolidation materials that use a reduced amount of cement, have a lower specific gravity than cement-based consolidation materials, and therefore consolidate the ground with a material that has almost the same specific gravity as the original ground, or even a lighter material, thereby achieving the effect of a lightweight consolidated body.

[0064] [Materials used] Slag: specific gravity 2.9, Blaine value 8000cm 2 / g, a silica-based non-hardening powder. Fly ash (FA): Coal ash discharged from thermal power plants. It is a silica-based non-hardening powder. Specific gravity: 1.9-2.3g / cm 3 The particle size distribution is 0.1 mm or less for more than 90%. Cement: Ordinary Portland cement: PC, specific gravity 3.15, hardening agent. Aluminum sulfate: Aluminum sulfate, Al2O3=17.2%, gelling agent, specific gravity 1.32. Slaked lime: Industrial calcium hydroxide, gelling accelerator and hardening agent. Gypsum or hemihydrate gypsum: hardening material, specific gravity 2.6. Bentonite: Water retention and thickening material, specific gravity 2.6. Magnesium oxide (gelling agent): Specific gravity 3.65. Calcium chloride (gelling agent): Specific gravity 1.85. Baking soda: Specific gravity 2.2. Dispersant: Specific gravity 1.04. Sulfuric acid: specific gravity 1.67, 75w / w%. No. 5 water glass: specific gravity 1.32, silica concentration 25.5%, Na2O 7.03, molar ratio 3.75. No. 1 water glass: specific gravity 1.35, silica concentration 21.59%, Na2O 10.80%, molar ratio 2.06. No. 3 water glass: specific gravity 1.41, silica concentration 29.16%, Na2O 9.36, molar ratio 3.22. Polyaluminum chloride and foam materials can also be used.

[0065] [Test method and test results] The specimens for the unconfined compression strength tests in Tables 1 to 7 were prepared in accordance with the Japanese Industrial Standards (draft) (JIS A 1216:2020) unconfined compression test method for soil, and cylindrical specimens with a height of 100 mm and a diameter of 50 mm were used. The results of measuring the strength on the 1st day, 7th day, and 28th day, or on the 28th day, are shown, respectively.

[0066] [Table 1]

[0067] [Table 2]

[0068] [Table 3]

[0069] [Table 4]

[0070] [Table 5]

[0071] [Table 6]

[0072] [Table 7]

[0073] [Table 8]

[0074] The consolidation agent of the present invention can penetrate and solidify sandy ground. In particular, when the consolidation agent contains solution-type silica, it can penetrate and solidify fine-grained soil, connect the solidified bodies together, and provide a water-stopping effect.

[0075] Test examples (Figs. 2 to 11) showing the effect of gelling the bleeding liquid in the silica suspension containing the silica solution are described below. Fig. 8 shows the state in which Fig. 2 is tilted. Table 8, Fig. 7, Fig. 10, and Fig. 11 show the state of a strength test of a sand specimen solidified with the bleeding liquid.

[0076] (Permeability test) (Test equipment and test method) Using a one-dimensional infiltration apparatus (length 2m), infiltration tests were carried out on No. 6 silica sand to investigate the infiltration length and strength distribution.

[0077] Test conditions: Acrylic mold h=2m, mixed liquid 3L After the sample was saturated with water, the suspension was poured into the bottom until no more liquid was discharged.

[0078] The specimens were prepared in accordance with the Japanese Industrial Standard (draft) (JIS A 1216:2020) for the unconfined compression test of soil, and cylindrical specimens with a height of 100 mm and a diameter of 50 mm were used for the unconfined compression test.

[0079] The experiments were carried out using the compositions of Example 36 and Comparative Example 1 (FIGS. 4 to 7, 10, and 11).

[0080] The solid lines in Figures 6 and 7 show the results for the formulation of Example 36. It was possible to measure the strength even with a penetration distance of 120 cm. The color of the sand gel did not change after 90 cm, but it is believed that the reason the strength could be measured is because the bleeding liquid solidified after 90 cm. It is believed that the part after 90 cm contains more than 0.5% silica.

[0081] The dotted lines in Figures 6 and 7 show the results for the formulation of Comparative Example 1. The strength could be measured up to 90 cm, but there was no discoloration after 90 cm, so the strength could not be measured, and it was found that the bleeding liquid had not gelled.

[0082] In the penetration test shown in Figure 5, the areas where there was no discoloration of the sand are believed to be areas where the slag had not penetrated. The bleeding fluid was not self-supporting, and the areas where the bleeding fluid had penetrated were also not self-supporting and had not solidified. In contrast, in Figure 6, the bleeding fluid had gelled and was self-supporting, and the sand gel had not discolored but was self-supporting and exhibited strength.

[0083] From the above, under conditions where the soil particle size density and suspended particle size distribution prevent the bleeding liquid from penetrating between soil particles, only the bleeding liquid will penetrate (Figures 9 and 12).

[0084] From Figures 6 and 7, even if the penetration distance of the suspended particles in the suspension is 90 cm, the bleeding liquid penetrates up to 120 cm, and the bleeding liquid has the strength to stand on its own, and the sand gel has the strength to stand on its own. In that case, it can be predicted that the silica concentration is 0.5 to 2% or more (Table 9). Therefore, even if the injection hole interval is long, the homogel of the bleeding liquid will connect the consolidated bodies penetrated by the suspended particles that obtain high strength.

[0085] In this way, an integrated solidified body can be formed even under ground conditions in which suspended particles cannot penetrate, and even if the injection hole spacing is wide, the solidified bodies between the holes can be connected by the self-supporting gel of the bleeding liquid, forming an integrated solidified ground.

[0086] Suspension-type grout can achieve higher strength than solution-type grout, but its large particle size makes it less permeable to fine-grained soil. However, by including solution-type silica, a solidification effect can be obtained even in ground where suspended particles cannot penetrate, making it possible to achieve integrated ground improvement and water-stopping properties (Figure 13).

[0087] As mentioned above, the inventors have also focused on the gelation of the bleeding liquid of the suspension grout, and have studied the gelation of the bleeding liquid, the self-supporting property of the homogel of the bleeding liquid, and the self-supporting property and strength of the sand gel of the bleeding liquid, and by using these as conditions, they have improved the penetration and consolidation property of the suspension grout for fine-grained soil or ground containing fine-grained soil, which was previously thought to be inapplicable, and completed the present invention. Furthermore, according to the present invention, an improvement effect is obtained that enables the self-supporting and watertightness of the excavated surface even in excavated ground.

[0088] In particular, when a suspension containing a silica solution is used in the present invention, the following effects due to gelation of the bleeding liquid are exhibited. These effects cannot be obtained by the conventional high-pressure injection method. (1) Permeation and consolidation of fine-grained soil where permeation and consolidation of suspended particles was previously impossible. (2) Self-supporting and water-tight properties of the cutting surface. (3) Expansion of the area improved by infiltration and solidification. (4) Ground improvement in which adjacent consolidated bodies are connected and integrated. (5) Reduction in the amount of construction work by increasing the hole spacing of the injection pipe. (6) The bleeding liquid has a short-term solidification effect, which improves resistance to earth pressure from adjacent structures and the back of retaining walls, thereby improving the safety of construction, the safety of buried objects through infiltration injection, strengthening the ground surrounding underground structures with spaces, waterproofing, and repairing deterioration.

[0089] An example is given below. (Strength test) (Preparation of sand gel specimen) Using No. 6 silica sand (Figure 12) and bleeding liquid, specimens 5cm in diameter and 10cm in height were prepared using a mixing method to achieve a relative density of 60%, and the unconfined compressive strength was measured after 28 days. The bleeding rate was higher when the amount of water glass was greater, and higher when the amount of slag was reduced. In the case of sand gel using bleeding liquid, greater amounts of water glass and slag produced greater strength. In the case of the combined use of gypsum, the addition of gypsum reduced the bleeding rate and increased the strength.

[0090] The gelation and self-supporting property of the bleeding liquid, as well as the strength and self-supporting property of the sand solidified by the bleeding liquid (sand gel), vary depending on the amount of slag and water glass in the suspension, the silica concentration of the water glass (SiO2) and the CaO content of the slag (CaO / SiO2), the gel time, and the particle size and density of the sand solidified by the bleeding liquid. Therefore, tests were conducted to confirm the gelation and self-supporting property of the bleeding liquid and the minimum strength of the bleeding liquid as conditions that comprehensively affect these several factors (Table 9, Figures 6 and 7). As a result, it became possible to carry out ground improvement by simultaneous composite injection of the suspension and solution, which integrates the fine-grained soil parts where the penetration and solidification of the suspended particles was difficult, or the parts where the penetration did not reach, with the high-strength solidified body in the cutting area, under the condition that the bleeding liquid gels and becomes self-supporting, and the sand gel permeated with the bleeding liquid becomes self-supporting.

[0091] It was found that the gelation occurred whether the bleeding rate was more than 50% or less than 50%, and the bleeding liquid penetrated the mixture, resulting in a composition that allowed the sand gel to stand on its own. The minimum strength at which the sand gel could stand on its own was 2.0 kN / m 2 The strength of the self-supporting sand gel, which was made with 75 g of slag and 100 mL of No. 1 water glass per 400 mL, was 15 kN / m on the 28th day. 2 The strength was also measured on the first and seventh days. The strength on the first day was 2.0 kN / m 2 On the 7th day, the strength was 10 kN / m 2 A similar trend was also observed with Toyoura sand. If the bleeding solution contains salts such as Ca, Mg, and Al, the strength of the sand gel will be further increased (Figures 12 and 13).

[0092] In the present invention, the test specimen is adjusted to the size of the specimen for the uniaxial compression test of soil, and the diameter D0 (mm) is usually 35mm or 50mm, and the height H0 (mm) is 1.8 to 2.5 times the diameter D0 (mm). If it is a self-supporting sand gel, it can be judged at any age. Figure 10 shows the test conditions. From this, it can be judged that the in-situ sand can achieve a strength of 2.0kN / m at an injection rate of 40%. 2It was found that if the strength of the improved ground is obtained, the soil will be self-supporting. 3 The amount of injection liquid per unit is 0.4 m 3 It becomes.

[0093] The gel time was shortened by increasing the amount of slaked lime added, and the strength increased with increasing the amount of slag added. In Comparative Example 1, the solidified portion solidified, but the bleeding portion did not gel. The bleeding liquid of Example 36 gelled. It was found that the bleeding liquid gelled even when either or both of silica colloid and water glass were used in combination.

[0094] (Relationship between silica concentration and strength) A neutral to alkaline solution was poured into an acrylic mold with a removable bottom and allowed to solidify, and the presence or absence of gelation of the homogel at each silica concentration and the self-supporting ability of the gel were confirmed. The same procedure was also carried out with the sand gel, and the solidification and the self-supporting ability of the consolidated sand were confirmed. The results are shown in Table 9.

[0095] At silica concentrations below 0.5%, the homogel and sand gel did not become self-supporting. Further testing revealed that gelation occurred even at a silica concentration of 0.25%, but the gel did not remain self-supporting, and the sand gel did not solidify or remain self-supporting (Table 9).

[0096] [Table 9]

[0097] Even if the entire amount of the bleeding liquid did not gel, the sand gel was able to stand on its own even when it gelled in the bleeding liquid and was tilted in the same way without collapsing (Figure 8). In other words, simply gelling the bleeding solution did not result in the homogel or sand gel being self-supporting (Table 8). It was found that certain conditions were necessary for the homogel and sand gel to be self-supporting.

[0098] In addition, a penetration test using a one-dimensional penetration device (length 2m) revealed that in the water glass-slag system, the bleeding liquid gels and the gel has the strength to stand on its own, but if water glass is not included, the bleeding liquid does not gel, and whether the bleeding rate is 50% or more or less, the bleeding liquid gels and a composition is obtained in which the sand gel penetrated by the bleeding liquid can stand on its own. In this case, the silica concentration of the bleeding liquid was predicted to be 0.5% or more, 0.5 to 2% (Table 9).

[0099] In addition, the penetration test confirmed that in the water glass-slag system and the suspension not containing water glass, the bleeding liquid penetrated and solidified into the sand, which the suspended particles in the bleeding liquid could not penetrate in the suspension containing water glass. Therefore, since this bleeding liquid is capable of penetrating even into ground that follows the particle size accumulation curve of solution-type penetration consolidation, it was found that the penetration potential of solution-type silica grout was achieved (Figure 9).

[0100] In this way, suspension-type grout uses fine silica particles such as slag or fly ash and solution-type silica, and the bleeding liquid penetrates and solidifies even in areas where suspensions cannot penetrate. Therefore, by focusing on the gelation of the bleeding liquid, the following conditions were found under which the bleeding liquid and sand gel can be self-supporting.

[0101] In view of the above, other preferred embodiments of the present invention are as follows. This is an injection method in which a consolidation agent consisting of a suspension containing silica particles such as slag or fly ash as the main material and solution-type silica as the active ingredient is injected into the ground from multiple injection holes provided in the ground to penetrate and consolidate the soil particles. The bleeding liquid of the consolidation agent gels, and the homogel has the strength to stand on its own, and the sand gel solidified by the bleeding liquid has the strength to stand on its own, and the bleeding liquid penetrates into parts of the ground that the suspension could not penetrate, expanding the consolidation range, or integrating with the parts of the ground that the suspension has penetrated to form a consolidation body. This makes it possible to form a large consolidated body by connecting the consolidated bodies of suspended particles from adjacent injection holes (Figure 13). In addition, if CMC, MC, polyacrylamide, clay, etc. are added to the injection agent, it is difficult to disperse in the ground and difficult to dilute even in gravel ground. Furthermore, when a suspension containing solution-type silica as the active ingredient, such as water glass or silica colloid, is used, it is possible to penetrate and consolidate even in areas where suspended particles cannot penetrate.

[0102] Here, in the above, the bleeding liquid gels and the homogel becomes self-supporting means that the silica concentration of the bleeding liquid is 0.5 w / v% or more, and the homogel does not collapse and remains self-supporting even when tilted diagonally within the mold.

[0103] In addition, the sand gel is self-supporting if the silica concentration of the bleeding liquid is 0.5 w / v% or more, the sand gel is made by mixing No. 6 silica sand with a bleeding liquid so that the relative density is 60%, and the sand gel is self-supporting and has a diameter of 5 cm and a height of 10 cm. The strength of the sand gel measured in a uniaxial compression test is 2.0 kN / m 2 This means that it is more than or equal to this.

[0104] In the above, the sand gel produced by bleeding silica grout, which is made of water glass and silica particles containing Ca, increases in strength over time (Table 8). This is thought to be because the Ca ions in the silica particles dissolve into the gel of the bleeding liquid over a long period of time even after gelation and react with the silica, forming calcium silicate, which contributes to the increase in strength. Alternatively, it is thought that the added hardener containing Ca or Mg reacts with the soluble silica in the silica particles over a long period of time through pozzolanic action, resulting in an increase in strength due to the hydration reaction.

[0105] As described above, in this invention, the penetration and consolidation range can be set by the size of the consolidation body, the suspended particles, and the gelation of the bleeding liquid according to the ground conditions and the purpose of ground improvement (strength, range of the consolidated area, etc.). In addition, the penetration and consolidation range of the suspended particles and the penetration and consolidation range of the bleeding liquid can be set by the type and particle size of the silica particles in the suspension, the mixing amount, the hardener and alkali agent, the type and amount of solution-type silica, the bleeding rate, the strength of the bleeding, and the gelation time. As a result, as shown in Figure 13, a new concept of simultaneous combined injection of suspension and solution was created, making ground improvement using suspension-type grout possible.

[0106] Furthermore, according to the present invention, the main materials used as the consolidation materials are natural or artificial silica particles, calcined silica, silica particles with natural pozzolanic action, and fluidized soil made by turning on-site generated soil into a slurry, thereby making it possible to reduce the weight of the solidified body, expand the range of infiltration and consolidation, and provide a ground improvement method that contributes to the global environment by reducing CO2 emissions.

[0107] As described above, the inventors of the present invention have focused on the fact that a solidified body of the suspension with a high silica content is formed in the outer periphery of the suspension containing the above-mentioned silica particles as the main component, and connects adjacent solidified bodies. Conventionally, the fact that there is a lot of bleeding in the suspension has been considered a drawback, but in the present invention, we have focused on the fact that the bleeding liquid can penetrate between soil particles where suspended particles cannot penetrate, and conducted research on the gelation of the bleeding liquid. As a result, it was found that the gelation and strength of the bleeding liquid itself, the permeability of the bleeding liquid into the sand, and the strength of the sand gel have a significant effect on the improvement of the permeation and consolidation of the suspension grout. Based on these findings, we have found the conditions for the penetration and gelation of the bleeding liquid into areas where suspended particles could not penetrate, the homogel of the bleeding liquid, and the strength of the sand gel, and have invented a new ground improvement method based on the concept of simultaneous combined injection of suspension and solution.

[0108] The present invention also provides a ground consolidation method that can be expected to reduce CO2 emissions by using a non-cement based ground consolidation material containing slag as the main component, thereby obtaining a solidified body with excellent durability.

[0109] The radiation shielding grout can be prepared by mixing the above-mentioned particles having radiation shielding properties with the above-mentioned binder to form a hydrous gel. The binder containing the particles having radiation shielding properties can be injected in the same manner as the binder injection. Thus, the injection of the binder provides high strength against air bombing, a water-stopping effect against the infiltration of water containing radiation into the space, and a solidified material having a radiation shielding effect, making it possible to protect an underground structure having an underground space.

[0110] The binder of the present invention has, in particular, the following properties: (1) By setting the composition of the suspension, which is mainly made of small, lightweight, and highly fluid silica particles, it is possible to achieve penetration over a wide area (Figures 5 to 7). (2) The inclusion of solution-type silica causes the bleeding liquid to gel, and the bleeding liquid penetrates into the fine particle areas where silica particles cannot penetrate (Fig. 4, Figs. 6-8), causing the fine particle areas to solidify and become self-supporting. Since the bleeding liquid has the same permeability as solution-type silica grout, the fine soil permeability range shown in Fig. 9 can be expected. Fig. 2 shows the state in which a silica suspension containing silica is left to stand, where the suspended matter solidifies and the bleeding liquid gels. Figs. 3 and 5 show the state in which a silica suspension not containing silica is left to stand, where only the suspended matter solidifies and the bleeding liquid does not gel. (3) The self-supporting properties of homogel at low silica concentrations of solution-type grout, the solidification of sand gel, and the self-supporting properties of consolidated sand are shown (Table 9). (4) From the particle size distribution of the sand used in the infiltration test (Figure 12), it can be seen that the suspended particles used in the present invention infiltrate and solidify into the sandy ground.

[0111] The particle size distribution of the sand used in the infiltration tests (Figures 4-7) is No. 6 silica sand in Figure 12. With this particle size distribution, suspended particles can infiltrate between soil particles up to 80 cm (Figures 6 and 7). With Toyoura sand, which is finer than this, the infiltration distance was almost half that. Furthermore, if the above suspension containing solution silica is used, the infiltration range shown in Figure 9, which is the same as the particle size of the infiltrable range of the solution type, can be obtained, and although the infiltration distance varies depending on the soil conditions, it is possible to form an improved body as shown in Figure 13. Figures 13(c) and (d) are plan views of the infiltrated solidified body. The type and size of the silica particles in the suspension can be selected depending on the soil conditions. In addition, since infiltration injection is possible as shown in Figure 13(d), it is possible to stabilize surrounding structures without causing damage to underground buried objects. Furthermore, by strengthening and water-stopping the surrounding ground, it is possible to strengthen underground structures with spaces.

[0112] As described above, the inventors have found that when a suspension containing the above-mentioned silica particles as a main component containing solution-type silica is injected, the area near the center becomes a high-strength area with many suspended particles, and the strength of the suspended particles decreases as the area moves away from the center, resulting in a low-strength area (Figures 6, 7, and 13). However, outside of that, a solidified body with a high silica content is formed due to gelation of the bleeding liquid of the solution-type silica, and connects adjacent solidified bodies. Conventionally, a large amount of bleeding in a suspension has been considered a disadvantage, but in the present invention, focusing on the fact that the bleeding liquid can penetrate between soil particles where suspended particles cannot penetrate, research was conducted on the gelation of the bleeding liquid. As a result, it was found that the gelation and strength of the bleeding liquid itself, the permeability of the bleeding liquid into the sand, and the strength of the sand gel have a significant effect on the improvement of the penetration and consolidation of the suspension-type grout. Based on these findings, the conditions were examined that not only can the suspension penetrate into the surrounding ground, but also can allow the bleeding liquid to penetrate and gel into fine-grained soil areas where suspended particles cannot penetrate, thereby enabling the formation of large solidified bodies.

[0113] In suspensions that do not contain silica solution, the bleeding liquid does not gel, and the sand that the bleeding liquid has penetrated does not stand up, and no strength is obtained (Figs. 3 and 5). However, sufficient strength is not obtained if the bleeding liquid only gels (Table 9). From this point of view, it was found that the strength condition for the self-supporting homogel of the bleeding liquid and the sand gel is that the silica concentration of the bleeding liquid is 0.5 w / v% or more (Table 8), and this is considered to be penetration and solidification by solution-type silica. As a result, the conditions for the penetration and gelation of the bleeding liquid into areas where suspended particles could not penetrate, and the strength of the homogel of the bleeding liquid and the sand gel were found, and it was possible to invent a new ground improvement method based on the concept of simultaneous combined injection of suspension and solution.

[0114] The present invention also provides a ground consolidation method that can be expected to reduce CO2 emissions by using a non-cementitious ground consolidation material whose main component is silica particles with natural pozzolanic action, including artificially calcined silica such as slag or fly ash, or soluble silica such as loam soil, thereby producing a solidified body with excellent durability.

Claims

1. In a ground injection method for protecting a concrete structure buried underground and having an underground space from air raids, The following i) to iii) i) Silica particles consisting of any one or more of pyrogenic silica, natural silica having pozzolanic action, and hardenable silica particles; ii) Silica particles made of any one or more of slag, fly ash, cement, sewage incineration ash, plant incineration ash, and calcined clay; iii) Silica particles consisting of any one or more of loam soil, volcanic ash, diploid soil, and triploid soil; A ground injection method for protecting a concrete structure by injecting a ground consolidation material consisting of a suspension containing any one of the above-mentioned suspended particles of silica particles as a main component and solution-type silica as an active ingredient into a periphery of the concrete structure from a plurality of injection holes provided in the ground, the silica particles have a Blaine value of 4,000 to 20,000 cm 2 / g, the amount of the silica particles in the ground consolidation material is 50 to 150 L / 400 L, silica colloid and / or water glass is used as the solution-type silica, and the bleeding liquid of the suspension is gelled; When the solution-type silica is water glass, the ground consolidation material uses water glass at a molar ratio of 1.0 to 5.0, the amount of the water glass in the ground consolidation material is 10 to 150 L / 400 L, the silica concentration of the bleeding liquid is 0.5 w / v% or more, a homogel formed by gelling the bleeding liquid has a strength to stand on its own, and a sand gel solidified by penetration of the bleeding liquid has a strength to stand on its own, A ground injection method characterized in that the bleeding liquid, having permeability to fine soil, penetrates into areas of the ground that the suspended particles could not penetrate, connecting solidified bodies of the suspended particles from adjacent injection holes, and forming, in the ground around the concrete structure, areas solidified with a high concentration suspension, areas solidified with a low concentration suspension, and areas having water-stopping properties solidified by gelation of the bleeding liquid, each with a thickness of 1 m or more, from the part close to the center to the outside, thereby preventing the concrete structure from being directly affected by the impact of an air bombing, enabling the repair of a deteriorated concrete structure, and blocking radiation by preventing groundwater from entering the underground space.

2. The ground injection method as described in claim 1, wherein the homogel formed by gelling the bleeding liquid is self-supporting means that the silica concentration of the bleeding liquid is 0.5 w / v% or more, and the homogel is self-supporting even when tilted diagonally in a mold without collapsing, and the sand gel is self-supporting means that the silica concentration of the bleeding liquid is 0.5 w / v% or more, the sand gel prepared by a mixing method using No. 6 silica sand and the bleeding liquid to have a relative density of 60% and measuring 5 cm in diameter and 10 cm in height is self-supporting, and the minimum strength in a uniaxial compression test measured using the sand gel is 2.0 kN / m2 or more.

3. 2. The ground grouting method according to claim 1, wherein the ground consolidation material contains radiation shielding particles and is used to protect the concrete structure from an aerial bombardment by a nuclear missile.

4. The ground injection method according to claim 1, wherein the ground consolidation material contains an alkaline agent consisting of any one or more of the following (1) to (3). (1) An alkaline agent containing either or both of gypsum and MgO as active ingredients. (2) An alkaline agent containing, as an active ingredient, one or more of Ca salts, Mg salts, Al salts, carbonates and bicarbonates. (3) An alkaline agent having as its active ingredient one or more of lime, cement, caustic alkali, water glass, and silica colloid.

5. The ground injection method according to claim 1, wherein the silica particles are slag, and the amount of the slag in the ground consolidation material is 10 to 25% by mass when no cement is used, and 10 to 30% by mass when cement is used.

6. 2. The ground injection method according to claim 1, wherein a mixing recipe for the ground consolidation material is set to provide a lightweight, low-alkaline, low-carbon type ground improvement material.

7. 2. The ground injection method according to claim 1, wherein the ground consolidation material contains one or more of microbubbles, air, a dispersant, and a thickener as active ingredients.

8. 2. The ground injection method according to claim 1, wherein the improvement effect of the injection of the ground consolidation material is confirmed by a non-destructive test.

9. 9. The ground grouting method according to claim 8, wherein the non-destructive testing is carried out by elastic wave velocity logging, acoustic tomography or surface wave exploration.

10. A ground injection method as described in claim 1, in which the peripheral portion of the concrete structure is consolidated with a ground consolidation material consisting of the suspension, and then a solution-type consolidation material as described below is further injected into the outer periphery to form a consolidated layer. A consolidation agent comprising a non-alkaline silica grout having a pH of 1 to 10, and containing as active ingredients one or more of silica colloid and water glass, and one or more of an acid and a salt as a reactant, and when the non-alkaline silica grout comprises silica colloid, water glass, and acid, the ratio of the silica concentration resulting from silica colloid to the silica concentration resulting from water glass is 100:0 to 0:100, the silica concentration is 0.4 to 40 wt%, the molar ratio of silica is 2.0 to 100, and the gelation time is from instantaneous setting to 10,000 minutes.

Citation Information

Patent Citations

  • Earthquake-proof reinforcing method for existing tunnel

    JP2001026922A

  • Foundation improving material and method for construction of large sectional tunnel

    JP2006316221A

  • Ground injection method

    JP2011241674A

  • Reinforcement method of existing tunnel and tunnel reinforcement device

    JP2017145641A

  • Durable silica grout and ground improvement method using durable silica grout

    JP2018193550A

Cited By

  • Construction materials and ground improvement methods using them

    JP2026181708A

  • Construction materials and ground improvement methods using them

    JP7884810B1

  • Tbm method using grout material with fixed carbon dioxide

    KR102965485B1

  • Deep cement mixing method using grout material with fixed carbon dioxide

    KR102965487B1