Polyimide, polyimide composition, adhesive film, laminate, coverlay film, resin-coated copper foil, metal-clad laminate, circuit board, and multilayer circuit board
By controlling the molecular weight of polyimide using a purified dimer diamine composition and forming a crosslinked structure with a metal salt of organic phosphinic acid, the challenges of brittleness and high transmission loss in FPCs are addressed, enhancing signal reliability and durability.
Patent Information
- Application Number
- JP2020064080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-03-31
AI Technical Summary
The polyimide films used in flexible printed circuits (FPCs) face challenges in controlling molecular weight, leading to brittleness and increased transmission loss of high-frequency signals due to the presence of trimer and monomer components in diamine derived from dimer acid, which affects the adhesiveness and dielectric properties.
The use of a dimer diamine composition purified to control the weight average molecular weight (Mw) and number average molecular weight (Mn) of polyimide within specific ranges, combined with a metal salt of organic phosphinic acid and a crosslinking agent, to form a crosslinked structure, thereby enhancing dielectric properties and reducing brittleness.
The controlled polyimide composition effectively reduces transmission loss and maintains flexibility, improving the reliability and durability of electronic equipment by suppressing brittleness and maintaining low dielectric constants and loss tangents, especially in high-frequency signal transmission.
Smart Images

Figure 0007578408000007 
Figure 0007578408000008 
Figure 0007578408000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide useful as a material for electronic components, and a polyimide composition, an adhesive film, a laminate, a coverlay film, a resin-coated copper foil, a metal-clad laminate, a circuit board, and a multilayer circuit board each using the polyimide. [Background technology]
[0002] In recent years, with the progress of miniaturization, weight reduction, and space saving of electronic devices, there is an increasing demand for flexible printed circuits (FPCs) that are thin, lightweight, flexible, and have excellent durability even when repeatedly bent. Because FPCs allow three-dimensional and high-density mounting even in a limited space, their applications are expanding to include wiring for electronic devices such as HDDs, DVDs, and smartphones, as well as components such as cables and connectors.
[0003] Meanwhile, in addition to higher density, the performance of devices has also improved, making it necessary to accommodate higher frequencies of transmitted signals. When transmitting high-frequency signals, if there is a large transmission loss in the transmission path, problems such as loss of electrical signals and longer signal delay times occur. Therefore, in the future, it will be important to further reduce the transmission loss of high-frequency signals in FPCs as well.
[0004] One type of FPC is known to have a structure in which a circuit pattern is formed on a polyimide film having excellent heat resistance and flexibility, and a coverlay film having an adhesive layer is laminated to the surface of the polyimide film.As a material for the adhesive layer of a coverlay film having such a structure, it has been proposed to use a polyimide made from a diamine derived from a dimer acid in which two terminal carboxylic acid groups of the dimer acid are substituted with primary aminomethyl groups or amino groups (for example, Patent Document 1).
[0005] In addition, in a double-sided metal-clad laminate having a structure in which two single-sided metal-clad laminates are bonded together by an adhesive layer, it has been proposed to use a polyimide containing a predetermined amount or more of diamine residues derived from a diamine derived from a dimer acid in the adhesive layer (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 6488170 [Patent Document 2] JP 2018-170417 A Summary of the Invention [Problem to be solved by the invention]
[0007] The polyimide films made from the diamine derived from dimer acid used in Patent Documents 1 and 2 exhibit excellent adhesion and low dielectric constant and dielectric loss tangent. However, since the diamine derived from dimer acid is a mixture containing trimer components and monomer components other than dimer components, it has an aspect that it is difficult to control the molecular weight of the polyimide made from it. If the molecular weight control of the polyimide is insufficient, for example, when a filler is blended, there is a problem that the resin film is easily weakened, and an improvement in this respect has been desired.
[0008] Therefore, an object of the present invention is to provide a polyimide that is made from a diamine derived from a dimer acid, that can effectively reduce the transmission loss of high-frequency signals while suppressing the embrittlement of the resin film. [Means for solving the problem]
[0009] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by using a dimer diamine composition that is purified as a diamine derived from dimer acid, and by controlling the weight average molecular weight and number average molecular weight of a polyimide within predetermined ranges, and have thus completed the present invention.
[0010] The polyimide of the present invention is a polyimide containing a tetracarboxylic acid residue derived from a tetracarboxylic acid anhydride component and a diamine residue derived from a diamine component, and is characterized by satisfying the following conditions a to d. a) The diamine composition contains 40 mol% or more of diamine residues derived from a dimer diamine composition mainly composed of a dimer diamine in which the two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine residues. b) The weight average molecular weight (Mw) is within the range of 25,000 to 100,000. c) The number average molecular weight (Mn) is within the range of 15,000 to 32,000. d) The ratio of Mw to Mn (Mw / Mn) is within the range of 1.8 to 3.4.
[0011] The polyimide composition of the present invention comprises the following components (A) and (B); (A) the polyimide; and (B) a metal salt of an organic phosphinic acid; and the weight ratio of the component (B) to the component (A) is within the range of 10 to 70% by weight.
[0012] The polyimide composition of the present invention is a polyimide composition comprising the component (A) having a ketone group in the molecule, and further comprising the following component (C): (C) a crosslinking agent having a functional group that undergoes a nucleophilic addition reaction with the ketone group; It may also contain:
[0013] The adhesive film of the present invention is characterized by containing the above-mentioned polyimide.
[0014] The adhesive film of the present invention comprises the following components (A) and (B); (A) the polyimide; And, (B) a metal salt of an organic phosphinic acid; and the weight ratio of the component (B) to the component (A) is within the range of 10 to 70% by weight.
[0015] The adhesive film of the present invention comprises the following components (A') and (B); (A') a crosslinked polyimide having a crosslinked structure formed by a reaction between the above polyimide having a ketone group in the molecule and a crosslinking agent having a functional group which undergoes a nucleophilic addition reaction with the ketone group; And, (B) a metal salt of an organic phosphinic acid; and the weight ratio of the component (B) to the component (A') is within the range of 10 to 70% by weight.
[0016] The laminate of the present invention is a laminate having a substrate and an adhesive layer laminated on at least one surface of the substrate, the adhesive layer being made of the above-mentioned adhesive film.
[0017] The coverlay film of the present invention is a coverlay film having a coverlay film material layer and an adhesive layer laminated on the coverlay film material layer, and the adhesive layer is made of the above-mentioned adhesive film.
[0018] The resin-coated copper foil of the present invention is a resin-coated copper foil in which an adhesive layer and a copper foil are laminated together, and the adhesive layer is made of the above-mentioned adhesive film.
[0019] The metal-clad laminate of the present invention is a metal-clad laminate having an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, and at least one layer of the insulating resin layer is made of the above-mentioned adhesive film.
[0020] The metal-clad laminate of the present invention is a metal-clad laminate having an insulating resin layer, an adhesive layer laminated on at least one side of the insulating resin layer, and a metal layer laminated on the insulating resin layer via the adhesive layer, wherein the adhesive layer is made of the above-mentioned adhesive film.
[0021] The metal-clad laminate of the present invention includes a first single-sided metal-clad laminate having a first metal layer and a first insulating resin layer laminated on at least one surface of the first metal layer; a second single-sided metal-clad laminate having a second metal layer and a second insulating resin layer laminated on at least one surface of the second metal layer; An adhesive layer is arranged so as to abut against the first insulating resin layer and the second insulating resin layer, and is laminated between the first single-sided metal-clad laminate and the second single-sided metal-clad laminate, The adhesive layer is made of the above adhesive film.
[0022] The metal-clad laminate of the present invention comprises a single-sided metal-clad laminate having an insulating resin layer and a metal layer laminated on one side of the insulating resin layer, and an adhesive layer laminated on the other side of the insulating resin layer, the adhesive layer being made of the above-mentioned adhesive film.
[0023] The circuit board of the present invention is obtained by wiring the metal layer of the metal-clad laminate.
[0024] The circuit board of the present invention is a circuit board comprising a first base material, a wiring layer laminated on at least one surface of the first base material, and an adhesive layer laminated on the surface of the first base material facing the wiring layer so as to cover the wiring layer, wherein the adhesive layer is made of the above-mentioned adhesive film.
[0025] The circuit board of the present invention is a circuit board comprising a first substrate, a wiring layer laminated on at least one surface of the first substrate, an adhesive layer laminated on the surface of the first substrate facing the wiring layer so as to cover the wiring layer, and a second substrate laminated on the surface of the adhesive layer opposite the first substrate, wherein the adhesive layer is made of the adhesive film described above.
[0026] The circuit board of the present invention is a circuit board comprising a first substrate, an adhesive layer laminated on at least one side of the first substrate, a second substrate laminated on the side of the adhesive layer opposite the first substrate, and wiring layers laminated on the sides of the first substrate and the second substrate opposite the adhesive layer, respectively, wherein the adhesive layer is made of the above-mentioned adhesive film.
[0027] The multilayer circuit board of the present invention is a multilayer circuit board comprising a laminate including a plurality of stacked insulating resin layers and at least one wiring layer embedded inside the laminate, wherein at least one of the plurality of insulating resin layers is formed of an adhesive layer having adhesive properties and covering the wiring layer, and the adhesive layer is made of the above-mentioned adhesive film. Effect of the Invention
[0028] The polyimide of the present invention is made from a dimer diamine composition and has a controlled weight average molecular weight and number average molecular weight, and therefore has excellent dielectric properties and can suppress weakening of the resin film. Therefore, when an adhesive film formed using the polyimide of the present invention is applied to a circuit board or the like that transmits high-frequency signals in the GHz band, it can effectively reduce transmission loss and has excellent strength and durability, thereby contributing to improving the reliability of electronic devices. [Brief description of the drawings]
[0029] [Figure 1] 1 is a schematic diagram showing a cross-sectional configuration of a laminate according to an embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing a cross-sectional configuration of a metal-clad laminate according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic diagram showing a cross-sectional configuration of a metal-clad laminate according to another embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing a cross-sectional configuration of a metal-clad laminate according to yet another embodiment of the present invention. [Diagram 5]1 is a schematic diagram showing a cross-sectional configuration of a circuit board according to an embodiment of the present invention; [Figure 6] FIG. 13 is a schematic diagram showing a cross-sectional configuration of a circuit board according to another embodiment of the present invention. [Figure 7] FIG. 13 is a schematic diagram showing a cross-sectional configuration of a circuit board according to still another embodiment of the present invention. [Figure 8] 1 is a schematic diagram showing a cross-sectional configuration of a multilayer circuit board according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described with reference to the accompanying drawings.
[0031] [Polyimide] The polyimide according to one embodiment of the present invention has adhesiveness and satisfies the conditions a to d described below. Hereinafter, the polyimide according to the present embodiment may be referred to as "adhesive polyimide". The adhesive polyimide contains a tetracarboxylic acid residue derived from a tetracarboxylic acid anhydride component and a diamine residue derived from a diamine component. In the present invention, the "tetracarboxylic acid residue" refers to a tetravalent group derived from a tetracarboxylic acid dianhydride, and the "diamine residue" refers to a divalent group derived from a diamine compound. When the raw materials tetracarboxylic acid anhydride and diamine compound are reacted in approximately equal moles, the types and molar ratios of the tetracarboxylic acid residue and diamine residue contained in the polyimide can be made to correspond approximately to the types and molar ratios of the raw materials. In the present invention, the term "polyimide" refers to a resin made of a polymer having an imide group in the molecular structure, such as polyimide, polyamideimide, polyetherimide, polyesterimide, polysiloxaneimide, polybenzimidazoleimide, etc.
[0032] (acid anhydride) The adhesive polyimide may be made of any tetracarboxylic anhydride generally used in thermoplastic polyimides as a raw material, without any particular limitations. However, it is preferable to use a raw material containing 90 mol % or more of tetracarboxylic anhydrides represented by the following general formula (1) and / or (2) in total relative to the total tetracarboxylic anhydride components. In other words, it is preferable for the adhesive polyimide to contain 90 mol % or more of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (1) and / or (2) in total relative to the total tetracarboxylic acid residues. By containing 90 mol % or more of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (1) and / or (2) in total relative to the total tetracarboxylic acid residues, it is preferable that the adhesive polyimide is easily compatible with flexibility and heat resistance. If the total amount of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (1) and / or (2) is less than 90 mol %, the adhesive polyimide tends to have a low solvent solubility.
[0033] [ka]
[0034] In general formula (1), X represents a single bond or a divalent group selected from the following formulas, and in general formula (2), the cyclic moiety represented by Y represents the formation of a cyclic saturated hydrocarbon group selected from a 4-membered ring, a 5-membered ring, a 6-membered ring, a 7-membered ring, or an 8-membered ring.
[0035] [ka]
[0036] In the above formula, Z is -C 6 H 4 -, -(CH 2 )n- or -CH 2 -CH(-OC(=O)-CH 3 )-CH 2 -, where n is an integer from 1 to 20.
[0037] Examples of the tetracarboxylic acid anhydride represented by the above general formula (1) include 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), 4,4'-oxydiphthalic anhydride (ODPA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), p-phenylenebis(trimellitic acid monoester anhydride) (TAHQ), ethylene glycol bisanhydrotrimellitate (TMEG), etc. Among these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is particularly preferred. When BTDA is used, the carbonyl group (ketone group) contributes to adhesion, so that the adhesion of the adhesive polyimide can be improved. In addition, the ketone group present in the molecular skeleton of BTDA may react with the amino group of an amino compound for crosslinking, which will be described later, to form a C=N bond, which is likely to exhibit the effect of improving heat resistance. From this viewpoint, it is preferable that the tetracarboxylic acid residue derived from BTDA is contained in an amount of preferably 50 mol % or more, more preferably 60 mol % or more, of the total tetracarboxylic acid residues.
[0038] Examples of the tetracarboxylic acid anhydride represented by the general formula (2) include 1,2,3,4-cyclobutane tetracarboxylic acid dianhydride, 1,2,3,4-cyclopentane tetracarboxylic acid dianhydride, 1,2,4,5-cyclohexane tetracarboxylic acid dianhydride, 1,2,4,5-cycloheptane tetracarboxylic acid dianhydride, and 1,2,5,6-cyclooctane tetracarboxylic acid dianhydride.
[0039] The adhesive polyimide may contain tetracarboxylic acid residues derived from acid anhydrides other than the tetracarboxylic acid anhydrides represented by the above general formulas (1) and (2) as long as the effects of the invention are not impaired.Such a tetracarboxylic acid residue is not particularly limited, and examples thereof include pyromellitic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'- or 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-diphenylethertetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3'',4,4''-, 2,3,3'',4''- or 2,2'',3,3''-p-terphenyltetracarboxylic dianhydride, 2,3',3,4''- ... ,2-Bis(2,3- or 3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3- or 3,4-dicarboxyphenyl)methane dianhydride, bis(2,3- or 3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3- or 3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-, 1,2,6,7- or 1,2,9,10-phenanthrene-tetracarboxylic acid dianhydride, 2,3,6,7-anthracene tetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl) ) tetrafluoropropane dianhydride, 1,2,5,6-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6- or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8-)tetrachloronaphthalene-1,4,5,8-(or 2, 3,6,7-tetracarboxylic acid dianhydride, 2,3,8,9-, 3,4,9,10-, 4,5,10,11- or 5,6,11,12-perylene-tetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic acid dianhydride, thiophene-2,3,4,5-tetracarboxylic acid dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride and other aromatic tetracarboxylic acid dianhydrides.
[0040] (Diamine) The adhesive polyimide may be made of any diamine compound generally used for thermoplastic polyimides as a raw material without any particular restrictions, but a raw material containing 40 mol % or more of a dimer diamine composition mainly composed of a dimer diamine in which two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine components, is used. In other words, as described in condition a below, the adhesive polyimide contains 40 mol % or more of diamine residues derived from a dimer diamine composition mainly composed of a dimer diamine in which two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine residues.
[0041] The dimer diamine composition is a refined product containing the following component (a) as a main component with the amounts of components (b) and (c) being controlled.
[0042] (a) dimer diamine; The dimer diamine of component (a) is a dimer acid in which the two terminal carboxylic acid groups (-COOH) of the dimer acid are replaced by primary aminomethyl groups (-CH 2 -NH 2 ) or amino group (-NH 2) is substituted. Dimer acid is a known dibasic acid obtained by intermolecular polymerization of unsaturated fatty acids, and its industrial production process is almost standardized in the industry, and is obtained by dimerizing unsaturated fatty acids having 11 to 22 carbon atoms using a clay catalyst or the like. Industrially obtained dimer acid is mainly composed of a dibasic acid having 36 carbon atoms obtained by dimerizing unsaturated fatty acids having 18 carbon atoms, such as oleic acid, linoleic acid, and linolenic acid, but contains any amount of monomer acid (having 18 carbon atoms), trimer acid (having 54 carbon atoms), and other polymerized fatty acids having 20 to 54 carbon atoms depending on the degree of purification. In addition, although double bonds remain after the dimerization reaction, in the present invention, those which have been further subjected to a hydrogenation reaction to reduce the degree of unsaturation are also included in the dimer acid. The dimer diamine of the component (a) can be defined as a diamine compound obtained by substituting the terminal carboxylic acid group of a dibasic acid compound having 18 to 54 carbon atoms, preferably 22 to 44 carbon atoms, with a primary aminomethyl group or an amino group.
[0043] As a feature of dimer diamine, it is possible to impart characteristics derived from the skeleton of dimer acid. That is, since dimer diamine is an aliphatic macromolecule with a molecular weight of about 560 to 620, it is possible to increase the molar volume of the molecule and relatively reduce the polar group of the polyimide. It is considered that such a feature of dimer diamine contributes to improving the dielectric properties by reducing the relative dielectric constant and dielectric tangent while suppressing the deterioration of the heat resistance of the adhesive polyimide. In addition, since it has two freely moving hydrophobic chains with 7 to 9 carbon atoms and two chain-like aliphatic amino groups with a length close to 18 carbon atoms, it is not only possible to impart flexibility to the polyimide, but also possible to make the polyimide have an asymmetric chemical structure or a non-planar chemical structure, and therefore it is considered that it is possible to reduce the dielectric constant of the polyimide.
[0044] The dimer diamine composition used may be one in which the dimer diamine content of component (a) is increased to 96% by weight or more, preferably 97% by weight or more, more preferably 98% by weight or more by a purification method such as molecular distillation. By increasing the dimer diamine content of component (a) to 96% by weight or more, the broadening of the molecular weight distribution of the polyimide can be suppressed. If technically possible, it is best that the entire dimer diamine composition (100% by weight) is composed of component (a) dimer diamine.
[0045] (b) a monoamine compound obtained by substituting a terminal carboxylic acid group of a monobasic acid compound having 10 to 40 carbon atoms with a primary aminomethyl group or an amino group; The monobasic acid compound having 10 to 40 carbon atoms is a mixture of a monobasic unsaturated fatty acid having 10 to 20 carbon atoms derived from the raw material of dimer acid, and a monobasic acid compound having 21 to 40 carbon atoms which is a by-product during the production of dimer acid. The monoamine compound is obtained by substituting the terminal carboxylic acid group of these monobasic acid compounds with a primary aminomethyl group or an amino group.
[0046] The monoamine compound (b) is a component that suppresses an increase in the molecular weight of the polyimide. During polymerization of the polyamic acid or polyimide, the monofunctional amino group of the monoamine compound reacts with the terminal acid anhydride group of the polyamic acid or polyimide to cap the terminal acid anhydride group, thereby suppressing an increase in the molecular weight of the polyamic acid or polyimide.
[0047] (c) an amine compound obtained by substituting a terminal carboxylic acid group of a polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms with a primary aminomethyl group or an amino group (excluding the above-mentioned dimer diamine); The polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms is a polybasic acid compound mainly composed of a tribasic acid compound having 41 to 80 carbon atoms, which is a by-product during the production of dimer acid. It may also contain a polymerized fatty acid other than dimer acid having 41 to 80 carbon atoms. The amine compound is obtained by substituting the terminal carboxylic acid group of these polybasic acid compounds with a primary aminomethyl group or an amino group.
[0048] The amine compound (c) is a component that promotes an increase in the molecular weight of the polyimide. The trifunctional or higher amino group, the main component of which is a triamine derived from a trimer acid, reacts with the terminal acid anhydride group of the polyamic acid or polyimide, rapidly increasing the molecular weight of the polyimide. In addition, amine compounds derived from polymerized fatty acids other than dimer acids having 41 to 80 carbon atoms also increase the molecular weight of the polyimide, causing gelation of the polyamic acid or polyimide.
[0049] When each component is quantified by measurement using gel permeation chromatography (GPC), in order to easily confirm the peak start, peak top, and peak end of each component of the dimer diamine composition, a sample of the dimer diamine composition treated with acetic anhydride and pyridine is used, and cyclohexanone is used as an internal standard. Using the sample thus prepared, each component is quantified by the area percentage of the GPC chromatogram. The peak start and peak end of each component are the minimum values of each peak curve, and the area percentage of the chromatogram can be calculated based on this.
[0050] In addition, the dimer diamine composition has a total area percentage of components (b) and (c) of 4% or less, preferably less than 4%, in a chromatogram obtained by GPC measurement. By keeping the total area percentage of components (b) and (c) at 4% or less, the broadening of the molecular weight distribution of the polyimide can be suppressed.
[0051] The area percentage of the chromatogram of the (b) component is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. By setting it in such a range, it is possible to suppress the decrease in the molecular weight of the polyimide, and further to widen the range of the molar ratio of the tetracarboxylic anhydride component and the diamine component. It is not necessary for the (b) component to be contained in the dimer diamine composition.
[0052] The area percentage of the chromatogram of component (c) is 2% or less, preferably 1.8% or less, and more preferably 1.5% or less. By setting it in such a range, a sudden increase in the molecular weight of the polyimide can be suppressed, and further, an increase in the dielectric tangent of the resin film over a wide frequency range can be suppressed. Note that component (c) does not have to be contained in the dimer diamine composition.
[0053] In addition, when the ratio (b / c) of the area percentages of the chromatograms of the components (b) and (c) is 1 or more, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably 0.97 or more and less than 1.0. By setting such a molar ratio, it becomes easier to control the molecular weight of the polyimide.
[0054] Furthermore, when the ratio (b / c) of the area percentages of the components (b) and (c) in the chromatograms is less than 1, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably 0.97 or more and 1.1 or less. By setting such a molar ratio, it becomes easier to control the molecular weight of the polyimide.
[0055] The dimer diamine composition is available as a commercially available product, and is preferably purified to reduce the amount of components other than the dimer diamine of the component (a), for example, the component (a) is preferably 96% by weight or more. The purification method is not particularly limited, but known methods such as distillation and precipitation purification are suitable. Examples of commercially available products include PRIAMINE 1073 (trade name), PRIAMINE 1074 (trade name), and PRIAMINE 1075 (trade name) manufactured by Croda Japan.
[0056] The adhesive polyimide may contain a diamine residue derived from a diamine component other than the above. As such a diamine residue, for example, a diamine residue derived from a diamine compound represented by the general formulas (B1) to (B7) is preferable.
[0057] [ka]
[0058] In formulas (B1) to (B7), R 1 each independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms; the linking group A is independently -O-, -S-, -CO-, -SO-, -SO 2 -, -COO-, -CH 2 -, -C(CH 3 ) 2 represents a divalent group selected from -, -NH-, or -CONH-, n 1 independently represent an integer of 0 to 4. However, in formula (B3), those which overlap with formula (B2) are excluded, and in formula (B5), those which overlap with formula (B4) are excluded. Here, "independently" means that in one or more of the above formulas (B1) to (B7), a plurality of linking groups A, a plurality of R 1 or multiple n 1 may be the same or different. In the above formulas (B1) to (B7), the hydrogen atoms in the two terminal amino groups may be substituted, for example, -NR 2 R 3 (where R 2 ,R3 may be independently any substituent such as an alkyl group.
[0059] The diamine represented by formula (B1) (hereinafter sometimes referred to as "diamine (B1)") is an aromatic diamine having two benzene rings. This diamine (B1) has an amino group directly bonded to at least one benzene ring and a divalent linking group A at the meta position, which increases the degree of freedom of the polyimide molecular chain and provides high flexibility, which is thought to contribute to improving the flexibility of the polyimide molecular chain. Therefore, the use of diamine (B1) enhances the thermoplasticity of the polyimide. Here, examples of the linking group A include -O-, -CH 2 -, -C(CH 3 ) 2 -, -CO-, -SO 2 - and -S- are preferred.
[0060] Examples of the diamine (B1) include 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, and (3,3'-bisamino)diphenylamine.
[0061] The diamine represented by formula (B2) (hereinafter sometimes referred to as "diamine (B2)") is an aromatic diamine having three benzene rings. In this diamine (B2), the amino group directly bonded to at least one benzene ring and the divalent linking group A are at the meta position, so that the degree of freedom of the polyimide molecular chain is increased and the polyimide molecular chain has high flexibility, which is thought to contribute to improving the flexibility of the polyimide molecular chain. Therefore, by using diamine (B2), the thermoplasticity of the polyimide is increased. Here, the linking group A is preferably -O-.
[0062] Examples of the diamine (B2) include 1,4-bis(3-aminophenoxy)benzene, 3-[4-(4-aminophenoxy)phenoxy]benzeneamine, and 3-[3-(4-aminophenoxy)phenoxy]benzeneamine.
[0063] The diamine represented by formula (B3) (hereinafter, sometimes referred to as "diamine (B3)") is an aromatic diamine having three benzene rings. In this diamine (B3), two divalent linking groups A directly bonded to one benzene ring are in meta positions with respect to each other, so that the degree of freedom of the polyimide molecular chain is increased and the polyimide molecular chain has high flexibility, which is considered to contribute to improving the flexibility of the polyimide molecular chain. Therefore, by using diamine (B3), the thermoplasticity of the polyimide is increased. Here, as the linking group A, -O- is preferable.
[0064] Examples of diamine (B3) include 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), 4,4'-[2-methyl-(1,3-phenylene)bisoxy]bisaniline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy]bisaniline, and 4,4'-[5-methyl-(1,3-phenylene)bisoxy]bisaniline.
[0065] The diamine represented by formula (B4) (hereinafter sometimes referred to as "diamine (B4)") is an aromatic diamine having four benzene rings. This diamine (B4) has high flexibility due to the fact that at least one amino group directly bonded to the benzene ring and the divalent linking group A are at the meta position, and is considered to contribute to improving the flexibility of the polyimide molecular chain. Therefore, the use of diamine (B4) enhances the thermoplasticity of the polyimide. Here, examples of the linking group A include -O-, -CH 2 -, -C(CH 3 ) 2 -, -SO 2 -, -CO- and -CONH- are preferred.
[0066] Examples of the diamine (B4) include bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, and bis[4,4'-(3-aminophenoxy)]benzanilide.
[0067] The diamine represented by formula (B5) (hereinafter sometimes referred to as "diamine (B5)") is an aromatic diamine having four benzene rings. In this diamine (B5), two divalent linking groups A directly bonded to at least one benzene ring are mutually at meta positions, so that the degree of freedom of the polyimide molecular chain is increased and the polyimide molecular chain has high flexibility, which is considered to contribute to improving the flexibility of the polyimide molecular chain. Therefore, by using diamine (B5), the thermoplasticity of the polyimide is increased. Here, as the linking group A, -O- is preferable.
[0068] Examples of the diamine (B5) include 4-[3-[4-(4-aminophenoxy)phenoxy]phenoxy]aniline, 4,4'-[oxybis(3,1-phenyleneoxy)]bisaniline, and the like.
[0069] The diamine represented by formula (B6) (hereinafter sometimes referred to as "diamine (B6)") is an aromatic diamine having four benzene rings. This diamine (B6) has high flexibility due to having at least two ether bonds, and is considered to contribute to improving the flexibility of the polyimide molecular chain. Therefore, the use of diamine (B6) enhances the thermoplasticity of the polyimide. Here, the linking group A is -C(CH 3 ) 2 -, -O-, -SO 2 - and -CO- are preferred.
[0070] Examples of diamines (B6) include 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), and bis[4-(4-aminophenoxy)phenyl]ketone (BAPK).
[0071] The diamine represented by formula (B7) (hereinafter sometimes referred to as "diamine (B7)") is an aromatic diamine having four benzene rings. This diamine (B7) has a highly flexible divalent linking group A on both sides of the diphenyl skeleton, which is believed to contribute to improving the flexibility of the polyimide molecular chain. Therefore, the use of diamine (B7) enhances the thermoplasticity of the polyimide. Here, the linking group A is preferably -O-.
[0072] Examples of the diamine (B7) include bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, and the like.
[0073] The adhesive polyimide preferably contains diamine residues derived from at least one diamine compound selected from diamines (B1) to (B7) in an amount of 1 mol % to 40 mol %, more preferably 5 mol % to 35 mol %, based on the total diamine residues. Since diamines (B1) to (B7) have flexible molecular structures, the use of at least one diamine compound selected from these in an amount within the above range can improve the flexibility of the polyimide molecular chain and impart thermoplasticity.
[0074] The adhesive polyimide may further contain diamine residues other than those mentioned above, provided that the effect of the invention is not impaired.
[0075] The adhesive polyimide can be produced by reacting the above-mentioned acid anhydride component and diamine component in a solvent, generating polyamic acid, and then heating to close the ring. For example, the acid anhydride component and diamine component are dissolved in an organic solvent in approximately equimolar amounts, and the mixture is stirred at a temperature in the range of 0 to 100°C for 30 minutes to 24 hours to cause a polymerization reaction, thereby obtaining polyamic acid, which is a precursor of polyimide. In the reaction, the reaction components are dissolved in the organic solvent so that the generated precursor is in the range of 5 to 50% by weight, preferably in the range of 10 to 40% by weight. Examples of organic solvents used in the polymerization reaction include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, methylcyclohexane, dioxane, tetrahydrofuran, diglyme, triglyme, methanol, ethanol, benzyl alcohol, and cresol. Two or more of these solvents can be used in combination, and aromatic hydrocarbons such as xylene and toluene can also be used in combination. The amount of such an organic solvent is not particularly limited, but it is preferable to adjust the amount so that the concentration of the polyamic acid solution obtained by the polymerization reaction is about 5 to 50% by weight.
[0076] The synthesized polyamic acid is usually advantageously used as a solution in a reaction solvent, but it can be concentrated, diluted, or replaced with another organic solvent if necessary. Polyamic acid is also advantageously used because it generally has excellent solubility in solvents. The viscosity of the polyamic acid solution is preferably within the range of 500 mPa·s to 100,000 mPa·s. If it is outside this range, defects such as uneven thickness and streaks are likely to occur in the film during coating using a coater or the like.
[0077] The method for imidizing polyamic acid to form polyimide is not particularly limited, and for example, a heat treatment in which the polyamic acid is heated in the above-mentioned solvent at a temperature in the range of 80 to 400° C. for 1 to 24 hours is preferably used. The temperature may be constant, or the temperature may be changed during the process.
[0078] In the adhesive polyimide, by selecting the types of the acid anhydride component and the diamine component, or by selecting the molar ratio of each when two or more types of acid anhydride components or diamine components are used, it is possible to control physical properties such as dielectric properties, thermal expansion coefficient, tensile modulus, glass transition temperature, etc. When the adhesive polyimide has a plurality of structural units, they may be present as blocks or randomly, but are preferably present randomly.
[0079] The adhesive polyimide of the present embodiment satisfies the following conditions a to d.
[0080] Condition a) The diamine composition contains 40 mol % or more of diamine residues derived from a dimer diamine composition mainly composed of a dimer diamine in which two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, relative to the total diamine residues: The adhesive polyimide can be made solvent-soluble by making the content of the diamine residue derived from the dimer diamine composition 40 mol % or more relative to the total diamine residues. The content of the diamine residue derived from the dimer diamine composition is preferably 60 mol % or more, more preferably 60 to 100 mol %, relative to the total diamine residues. If it is less than 60 mol %, the relative dielectric constant and dielectric loss tangent tend to increase due to the relatively increased polar groups contained in the adhesive polyimide, but by making the content 60 mol % or more, the relative dielectric constant and dielectric loss tangent of the adhesive polyimide can be reduced.
[0081] Condition b) Weight average molecular weight (Mw) is within the range of 25,000 to 100,000: By making the Mw 25,000 or more, it is possible to improve the tear strength and adhesive strength when made into a film, and to increase the storage stability of the varnish. If the Mw is less than 25,000, the film becomes brittle, and in a film containing a filler (e.g., a metal salt of an organic phosphinic acid, which is a flame retardant), stress is generated at the interface between the filler and the resin when the film is bent or stretched, which causes breakage or the generation of voids at the interface between the filler and the resin. On the other hand, if Mw exceeds 100,000, the viscosity of the varnish increases and the handleability tends to decrease. Within the above range, the lower the Mw, the narrower the molecular weight distribution tends to be, so the Mw is preferably in the range of 50,000 to 100,000, and more preferably in the range of 50,000 to 70,000.
[0082] Condition c) Number average molecular weight (Mn) is within the range of 15,000 to 32,000: Since Mn represents the number of polyimide chain ends more directly than Mw, an increase in highly polar ends in the polyimide molecular chain can be suppressed, and an increase in the relative dielectric constant and dielectric loss tangent can be suppressed by setting Mn to 15,000 or more, preferably 24,000 or more. Mn can be controlled by increasing the content of dimer diamine in the dimer diamine composition (i.e., by reducing the trimer component and monomer component), which can suppress the spread of the molecular weight of the adhesive polyimide.
[0083] Condition d) The ratio of the Mw to the Mn (Mw / Mn) is within the range of 1.8 to 3.4: The ratio Mw / Mn represents the degree of polydispersity, and in the adhesive polyimide of this embodiment, the ratio Mw / Mn is set to 1.8 or more. Even if Mn is about the same, the higher the degree of polydispersity, the higher the frequency of high molecular weight bodies, which increases the suppression of movement due to molecular entanglement, thereby achieving a low dielectric tangent and improved tear strength. In addition, by setting the ratio Mw / Mn to 3.4 or less and achieving a balance with Mn while ensuring a certain degree of polydispersity, it is possible to suppress an increase in highly polar ends in the polyimide molecular chain and suppress an increase in the relative dielectric constant and dielectric tangent.
[0084] The imide group concentration of the adhesive polyimide is preferably 22% by weight or less, more preferably 20% by weight or less. Here, the "imide group concentration" refers to the ratio of the imide group (-(CO) 2 The imide group concentration is calculated by dividing the molecular weight of the imide (-N-) by the molecular weight of the entire polyimide structure. If the imide group concentration exceeds 22% by weight, the molecular weight of the resin itself decreases, and the low moisture absorption property deteriorates due to an increase in polar groups, and Tg and elastic modulus increase.
[0085] The adhesive polyimide is most preferably a completely imidized structure. However, a part of the polyimide may be an amic acid. The imidization rate can be determined by measuring the infrared absorption spectrum of the polyimide thin film by a single reflection ATR method using a Fourier transform infrared spectrophotometer (commercially available: FT / IR620 manufactured by JASCO Corporation) at 1015 cm -1 Based on the benzene ring absorber near 1780cm -1 It can be calculated from the absorbance of the C=O stretching derived from the imide group.
[0086] (Crosslinking of adhesive polyimide) When the adhesive polyimide has a ketone group, a crosslinked structure can be formed by reacting the ketone group with a crosslinking agent having a functional group that undergoes a nucleophilic addition reaction. The formation of the crosslinked structure can improve heat resistance. A polyimide having such a crosslinked structure (hereinafter sometimes referred to as "crosslinked polyimide") is an application example of an adhesive polyimide, and is a preferred embodiment. Since the weight average molecular weight varies greatly due to crosslinking, it is sufficient that the adhesive polyimide before crosslinking satisfies conditions a to d, and the crosslinked polyimide does not have to satisfy these conditions.
[0087] As the crosslinking agent, for example, an amino compound having at least two primary amino groups as functional groups (hereinafter, sometimes referred to as "amino compound for crosslinking") is preferably used. A crosslinked structure can be formed by reacting a ketone group of the adhesive polyimide with an amino group of the amino compound for crosslinking to form a C=N bond. In other words, the two primary amino groups in the amino compound function as functional groups that undergo a nucleophilic addition reaction with the ketone group. The primary amino group is particularly advantageous because it does not involve the generation of a hydroxyl group (-OH) that deteriorates the dielectric properties.
[0088] A preferred tetracarboxylic anhydride for forming an adhesive polyimide having a ketone group is, for example, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and a preferred diamine compound is, for example, an aromatic diamine such as 4,4'-bis(3-aminophenoxy)benzophenone (BABP) or 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene (BABB). For the purpose of forming a crosslinked structure, it is particularly preferred to allow an amino compound for crosslinking to act on the above adhesive polyimide, which contains, with respect to the total tetracarboxylic acid residues, preferably 50 mol % or more, more preferably 60 mol % or more of BTDA residues derived from BTDA. In the present invention, the term "BTDA residue" refers to a tetravalent group derived from BTDA.
[0089] Examples of the amino compound for forming a crosslink include (I) a dihydrazide compound, (II) an aromatic diamine, and (III) an aliphatic amine. Among these, a dihydrazide compound is preferred. Aliphatic amines other than dihydrazide compounds are likely to form a crosslinked structure even at room temperature, which raises concerns about the storage stability of the varnish, while aromatic diamines require high temperatures to form a crosslinked structure. In this way, when a dihydrazide compound is used, it is possible to achieve both the storage stability of the varnish and a shortened curing time. Examples of the dihydrazide compound include oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglyceryl ester dihydrazide, ... Preferred are dihydrazide compounds such as cholic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoedioic acid dihydrazide, 4,4-bisbenzene dihydrazide, 1,4-naphthoic acid dihydrazide, 2,6-pyridine diacid dihydrazide, itaconic acid dihydrazide, etc. The above dihydrazide compounds may be used alone or in combination of two or more.
[0090] In addition, the above amino compounds, such as (I) dihydrazide compounds, (II) aromatic diamines, and (III) aliphatic amines, can also be used in combination of two or more kinds beyond categories, such as a combination of (I) and (II), a combination of (I) and (III), or a combination of (I), (II) and (III).
[0091] In addition, from the viewpoint of making the network structure formed by the crosslinking by the crosslinking amino compound denser, the crosslinking amino compound used in the present invention preferably has a molecular weight (weight average molecular weight when the crosslinking amino compound is an oligomer) of 5,000 or less, more preferably 90 to 2,000, and even more preferably 100 to 1,500. Among these, crosslinking amino compounds having a molecular weight of 100 to 1,000 are particularly preferred. When the molecular weight of the crosslinking amino compound is less than 90, only one amino group of the crosslinking amino compound forms a C=N bond with a ketone group of the adhesive polyimide, and the periphery of the remaining amino group becomes three-dimensionally bulky, so that the remaining amino group tends to have difficulty in forming a C=N bond.
[0092] When crosslinking the ketone group in the adhesive polyimide with the crosslinking amino compound, the crosslinking amino compound is added to a resin solution containing the adhesive polyimide to cause a condensation reaction between the ketone group in the adhesive polyimide and the primary amino group of the crosslinking amino compound. This condensation reaction hardens the resin solution to become a hardened product.
[0093] A ketone group in the adhesive polyimide and a functional group of the crosslinking agent are subjected to a nucleophilic addition reaction to form a crosslink, resulting in a crosslinked polyimide, which is a cured product. The conditions of the nucleophilic addition reaction for forming the crosslink are not particularly limited and can be selected according to the type of the crosslinking agent. For example, when a primary amino group of an amino compound for forming a crosslink is reacted with a ketone group in the adhesive polyimide, an imine bond (C=N bond) is generated by a condensation reaction by heating, and a crosslinked structure is formed. The conditions of the condensation reaction for forming the crosslink are not particularly limited as long as the ketone group in the adhesive polyimide and the primary amino group of the amino compound for forming the crosslink form an imine bond (C=N bond). The temperature of the heat condensation is preferably within the range of 120 to 220°C, more preferably within the range of 140 to 200°C, for example, in order to release water generated by condensation out of the system, or to simplify the condensation step when a heat condensation reaction is performed subsequently after the synthesis of the adhesive polyimide. The reaction time is preferably about 30 minutes to 24 hours. The end point of the reaction can be determined by measuring the infrared absorption spectrum using, for example, a Fourier transform infrared spectrophotometer (commercially available: FT / IR620 manufactured by JASCO Corporation) at 1670 cm -1 The decrease or disappearance of the absorption peak due to the ketone group in the polyimide resin near 1635 cm -1 This can be confirmed by the appearance of an absorption peak derived from a nearby imine group.
[0094] The thermal condensation of the ketone group of the adhesive polyimide with the primary amino group of the crosslinking amino compound can be carried out, for example, by the following method: (1) A method in which, following the synthesis (imidization) of adhesive polyimide, an amino compound for crosslinking is added and heated; (2) A method in which an excess amount of an amino compound is charged in advance as a diamine component, and following the synthesis (imidization) of an adhesive polyimide, the remaining amino compound that is not involved in imidization or amidation is used as an amino compound for crosslinking and heated together with the adhesive polyimide; Or, (3) A method in which the adhesive polyimide composition containing the above-mentioned crosslinking amino compound is processed into a predetermined shape (for example, after being applied to a substrate or formed into a film), and then heated; This can be done by, etc.
[0095] In the above description, an example of a crosslinked polyimide having a crosslinked structure formed by the formation of an imine bond has been given in order to impart heat resistance to the adhesive polyimide. However, the present invention is not limited to this example. As a method for curing the polyimide, it is also possible to mix and cure the polyimide with a compound having an unsaturated bond, such as an epoxy resin, an epoxy resin curing agent, maleimide, an activated ester resin, or a resin having a styrene skeleton.
[0096] [Polyimide composition] The polyimide composition according to one embodiment of the present invention comprises the following components (A) and (B); (A) adhesive polyimide; and (B) a metal salt of an organic phosphinic acid; The polyimide composition contains an adhesive polyimide as a main component of the resin components, preferably 70% by weight or more of the resin components, more preferably 90% by weight or more of the resin components, and most preferably the entire resin components. The main component of the resin components means a component contained in an amount of more than 50% by weight of the entire resin components.
[0097] The metal salt of an organic phosphinic acid of component (B) is a flame retardant that does not deteriorate the dielectric properties of the polyimide. As the metal salt of an organic phosphinic acid of component (B), for example, an aluminum salt of an organic phosphinic acid represented by the following general formula (3) is preferable.
[0098] [ka]
[0099] In the general formula (3), two R's each independently represent an alkyl group, and R is preferably a lower alkyl group having 1 to 4 carbon atoms.
[0100] As the metal salt of an organic phosphinic acid of component (B), commercially available products can be used, for example, Exolit OP935 (trade name, manufactured by Clariant) and the like.
[0101] In the polyimide composition according to the present embodiment, when the adhesive polyimide of component (A) is a polyimide having a ketone group in the molecule, the polyimide composition further contains, as an optional component, component (C); (C) a crosslinking agent having a functional group that undergoes a nucleophilic addition reaction with the ketone group; Here, the details of the polyimide having a ketone group in the molecule and the component (C) crosslinking agent are as described above.
[0102] [Composition ratio] In the polyimide composition, the weight ratio of the metal salt of organic phosphinic acid of component (B) to the adhesive polyimide of component (A) is preferably within the range of 10 to 70% by weight. If the weight ratio of component (B) to component (A) is less than 10% by weight, the flame retardant effect of component (B) is not fully exhibited, and if it exceeds 70% by weight, the resin film (adhesive film) formed by the polyimide composition becomes brittle. For example, when the weight ratio of the metal salt of organic phosphinic acid of component (B) to the adhesive polyimide of component (A) is 25% by weight, the film elongation is 168%, whereas when it is 70% by weight, the film elongation is about 12%.
[0103] The polyimide composition preferably contains component (C) such that the functional groups of the crosslinking agent of component (C) are in the range of 0.04 to 0.50 mol, preferably 0.06 to 0.40 mol, in total, per 1 mol of ketone groups contained in the adhesive polyimide of component (A). For example, when a crosslinking amino compound is used as component (C), the primary amino groups can be in the range of 0.04 to 0.50 mol, preferably 0.06 to 0.40 mol, in total, per 1 mol of ketone groups. If the total number of functional groups in the crosslinking agent is less than 0.04 moles per mole of ketone group, crosslinking does not proceed sufficiently, and heat resistance after curing tends to be difficult to achieve. On the other hand, if the number exceeds 0.5 moles, the dielectric tangent tends to increase. This is presumably because the mobility of the polyimide molecular chain is restricted by the excess crosslinking agent, inhibiting the formation of an ordered molecular chain structure that is effective in suppressing the dielectric tangent during curing. In addition, if the amount of crosslinking agent is too large, the unreacted crosslinking agent acts as a thermoplasticizer, tending to reduce the heat resistance of the adhesive layer.
[0104] In addition, since the adhesive polyimide is soluble in a solvent, it can be used in the form of a composition containing a solvent. That is, the polyimide composition preferably contains, as an optional component, a solvent capable of dissolving the adhesive polyimide.
[0105] The solvent is not particularly limited as long as it can dissolve the adhesive polyimide, and examples thereof include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, methylcyclohexane, dioxane, tetrahydrofuran, diglyme, triglyme, methanol, ethanol, benzyl alcohol, cresol, acetone, etc. Two or more of these solvents can be used in combination, and aromatic hydrocarbons such as xylene and toluene can also be used in combination.
[0106] In the polyimide composition, the blending ratio of the adhesive polyimide and the solvent is not particularly limited as long as the viscosity of the composition can be maintained to a level that allows coating. The viscosity of the polyimide composition is preferably within a range of, for example, 500 mPa·s to 100,000 mPa·s. If it is outside this range, defects such as uneven thickness and streaks are likely to occur in the resin film during coating.
[0107] The polyimide composition may contain, as appropriate, optional components, such as a plasticizer, another curable resin component such as an epoxy resin, a curing agent, a curing accelerator, an organic filler, an inorganic filler, a coupling agent, a solvent, and a flame retardant, provided that the effects of the invention are not impaired.
[0108] [Adhesive film] The adhesive film according to one embodiment of the present invention is a resin film obtained by processing the adhesive polyimide or crosslinked polyimide into a film. The adhesive film may be a film containing the adhesive polyimide or crosslinked polyimide as the main component of the resin component, preferably 70% by weight or more of the resin component, more preferably 90% by weight or more of the resin component, and most preferably the entire resin component. The main component of the resin component means a component that is contained in an amount of more than 50% by weight of the total resin component. The adhesive film may be a film (sheet) made of adhesive polyimide or crosslinked polyimide, or may be laminated on a resin base material such as an inorganic material such as copper foil or glass plate, or a polyimide film, polyamide film, or polyester film. The adhesive film may be appropriately blended with optional components such as plasticizers, other curable resin components such as epoxy resins, curing agents, curing accelerators, organic fillers, inorganic fillers, coupling agents, and flame retardants.
[0109] A preferred form of adhesive film of the present invention comprises the following components (A) and (B); (A) adhesive polyimide; And, (B) a metal salt of an organic phosphinic acid; In this regard, the contents of the adhesive polyimide of component (A) and the metal salt of an organic phosphinic acid of component (B) are as described above.
[0110] Another preferred embodiment of the adhesive film of the present invention comprises the following components (A') and (B); (A') a crosslinked polyimide which is an adhesive polyimide having a ketone group in the molecule and which forms a crosslinked structure by a reaction between a polyimide and a crosslinking agent having a functional group which undergoes a nucleophilic addition reaction with the ketone group; And, (B) a metal salt of an organic phosphinic acid; In this regard, the contents of the crosslinked polyimide of component (A') and the metal salt of an organic phosphinic acid of component (B) are as described above.
[0111] The adhesive film is conditioned for 24 hours under constant temperature and humidity conditions (normal conditions) of 23°C and 50% RH, and then the dielectric loss tangent (Tanδ) at 10 GHz measured by a split post dielectric resonator (SPDR) is 10 ) is preferably 0.003 or less, more preferably 0.0025 or less, and the relative dielectric constant (E 10 It is preferable that the dielectric tangent (Tanδ) is 3.0 or less. 10 ) and relative dielectric constant (E 10 ) is equal to or less than the above-mentioned numerical value, when applied to a circuit board, an increase in dielectric loss is suppressed, and the occurrence of inconveniences such as loss of electrical signals on the transmission path of high-frequency signals can be suppressed.
[0112] In addition, the adhesive film was conditioned for 24 hours under constant temperature and humidity conditions (normal conditions) of 23°C and 50% RH, and then the dielectric loss tangent (Tanδ) at 20 GHz was measured using a split post dielectric resonator (SPDR). 20 ) is preferably 0.003 or less, more preferably 0.0025 or less, and the relative dielectric constant (E 20 It is preferable that the dielectric tangent (Tanδ) is 3.0 or less. 20 ) and relative dielectric constant (E 20 ) is equal to or less than the above-mentioned numerical value, when applied to a circuit board, an increase in dielectric loss is suppressed, and the occurrence of inconveniences such as loss of electrical signals on the transmission path of high-frequency signals can be suppressed.
[0113] Furthermore, the adhesive film was conditioned for 24 hours under constant temperature and humidity conditions (normal conditions) of 23°C and 50% RH, and then the dielectric loss tangent (Tanδ) at 20 GHz was measured using a split post dielectric resonator (SPDR).20 ) and dielectric loss tangent (Tanδ) at 10GHz 10 ) and the difference (Tan δ 20 - Tan δ 10 ) is preferably 0 or less. 20 - Tan δ 10 ) being 0 or less means that the transmission loss at 10 to 20 GHz does not increase, but remains the same or even decreases.
[0114] The tensile modulus of the adhesive film is preferably 3000 MPa or less, more preferably 100 MPa or more and 2500 MPa or less, more preferably 200 MPa or more and 2000 MPa or less. If the tensile modulus is less than 100 MPa, the film is likely to wrinkle, and handling properties may be deteriorated due to air entrapment during lamination. If the tensile modulus exceeds 3000 MPa, warping may occur or dimensional stability may decrease when the substrate and the adhesive film are laminated. By setting the tensile modulus to the above range, a laminate having good handling properties, suppressing warping and excellent dimensional stability can be obtained.
[0115] The elongation of the adhesive film is preferably 50% or more, more preferably 100% or more, and more preferably 150% or more. If the elongation is less than 50%, the flexibility of the laminate, such as a circuit board, is reduced, which may cause breakage when the laminate is bent. In addition, if the elongation is small during handling, voids may occur between the filler and the adhesive, causing the entire film to become cloudy, which may cause defects in appearance and characteristics. By setting the elongation to the above range, a laminate that has good handling properties and sufficient bending resistance after being made into a multilayer FPC can be obtained.
[0116] The method for producing the adhesive film of the present embodiment is not particularly limited, but the following methods [1] to [3] can be exemplified. [1] A method in which an adhesive polyimide is applied in a solution state (e.g., in the form of a polyimide composition) to any substrate to form a coating film, which is then dried at a temperature of, for example, 80 to 180°C to form a film, and then peeled off from the substrate as necessary. [2] A method in which a solution of polyamic acid, which is a precursor of adhesive polyimide, is applied to any substrate, dried, and then imidized to form a film, which is then peeled off from the substrate as necessary. [3] A method in which a solution of polyamic acid, a precursor of adhesive polyimide, is applied to any substrate and dried, and then the polyamic acid gel film is peeled off from the substrate and imidized to produce an adhesive film. The method for applying the adhesive polyimide solution (or polyamic acid solution) onto the substrate is not particularly limited, and it is possible to apply it using, for example, a coater such as a comma, die, knife or lip coater.
[0117] Next, specific examples of laminates, metal-clad laminates, circuit boards, and multilayer circuit boards, which are preferred embodiments to which a resin film is applied, will be described.
[0118] [Laminate] As shown in FIG. 1, the laminate 100 according to an embodiment of the present invention has a substrate 10 and an adhesive layer 20 laminated on at least one surface of the substrate 10, and the adhesive layer 20 is made of the adhesive film. The laminate 100 may include any layer other than the above. Examples of the substrate 10 in the laminate 100 include substrates made of inorganic materials such as copper foil and glass plate, and substrates made of resin materials such as polyimide films, polyamide films, and polyester films. The laminate 100 can be manufactured according to any one of the methods [1] to [3] for manufacturing the adhesive film, except that the laminate 100 is not peeled off from the substrate 10. The laminate 100 may also be manufactured by preparing the substrate 10 and the adhesive film separately and bonding them together. Preferred embodiments of the laminate 100 include a coverlay film, a copper foil with resin, and the like.
[0119] (Coverlay film) The coverlay film, which is one embodiment of the laminate 100, is used to protect a wiring layer in a circuit board, and although not shown, has a coverlay film material layer as a base material 10 and an adhesive layer 20 laminated on one side of the coverlay film material layer, the adhesive layer 20 being made of the above-mentioned adhesive film. The coverlay film may include any layer other than those described above.
[0120] The material of the coverlay film material layer is not particularly limited, but for example, polyimide-based films such as polyimide resins, polyetherimide resins, and polyamideimide resins, polyamide-based films, and polyester-based films can be used. Among these, it is preferable to use polyimide-based films with excellent heat resistance. In addition, the coverlay film material can contain a black pigment in order to effectively exhibit light-shielding properties, concealing properties, design properties, and the like, and can also contain optional components such as matte pigments that suppress the gloss of the surface, within a range that does not impair the effect of improving the dielectric properties.
[0121] The thickness of the coverlay film material layer is not particularly limited, but is preferably within the range of, for example, 5 μm or more and 100 μm or less. The thickness of the adhesive layer 20 is not particularly limited, but is preferably within the range of, for example, 10 μm or more and 75 μm or less.
[0122] The coverlay film of the present embodiment can be produced by the method exemplified below. First, as a first method, polyimide that will become the adhesive layer 20 is applied in a solution state (for example, a varnish state containing a solvent is preferable, and a polyimide composition is preferable) to one side of a film material layer for the coverlay, and then the adhesive layer 20 is formed by drying at a temperature of, for example, 80 to 180°C, thereby forming a coverlay film having a film material layer for the coverlay and the adhesive layer 20.
[0123] As a second method, polyimide for adhesive layer 20 is applied in a solution state (for example, a varnish containing a solvent is preferable, and a polyimide composition is preferable) onto any substrate, dried at a temperature of, for example, 80 to 180°C, and then peeled off to form a resin film for adhesive layer 20, and this resin film is thermocompression bonded to a film material layer for the coverlay at a temperature of, for example, 60 to 220°C to form a coverlay film.
[0124] (Copper foil with resin) The resin-coated copper foil, which is another embodiment of the laminate 100, is used as a circuit board material, and although not shown, is obtained by laminating an adhesive layer 20 on at least one side of a copper foil as a substrate 10, and the adhesive layer 20 is made of the above-mentioned adhesive film. The resin-coated copper foil of this embodiment may include any layer other than those described above.
[0125] The thickness of the adhesive layer 20 in the resin-coated copper foil is preferably within the range of 0.1 to 125 μm, and more preferably within the range of 0.3 to 100 μm. If the thickness of the adhesive layer 20 is less than the above lower limit, problems such as insufficient adhesion may occur. On the other hand, if the thickness of the adhesive layer 20 exceeds the above upper limit, problems such as reduced dimensional stability may occur. In addition, from the viewpoint of lowering the dielectric constant and the dielectric loss tangent, the thickness of the adhesive layer 20 is preferably 3 μm or more.
[0126] The material of the copper foil in the resin-coated copper foil is preferably one mainly composed of copper or a copper alloy. The thickness of the copper foil is preferably 35 μm or less, more preferably in the range of 5 to 25 μm. From the viewpoint of production stability and handling, the lower limit of the thickness of the copper foil is preferably 5 μm. The copper foil may be a rolled copper foil or an electrolytic copper foil. In addition, a commercially available copper foil can be used as the copper foil.
[0127] The resin-attached copper foil may be prepared, for example, by sputtering a metal onto an adhesive film to form a seed layer, and then forming a copper layer, for example, by copper plating, or by laminating an adhesive film and a copper foil by a method such as thermocompression bonding. Furthermore, the resin-attached copper foil may be prepared by casting a coating solution of an adhesive polyimide or a precursor thereof onto the copper foil, drying the coating film to form an adhesive layer 20, and then carrying out the necessary heat treatment.
[0128] [Metal-clad laminate] (First aspect) The metal-clad laminate according to one embodiment of the present invention is used as a circuit board material and includes an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, at least one of the insulating resin layers being made of the adhesive film. Note that the metal-clad laminate according to this embodiment may include any layer other than those described above.
[0129] (Second aspect) A metal-clad laminate according to another embodiment of the present invention is a so-called three-layer metal-clad laminate 101 including an insulating resin layer 30, an adhesive layer 20 laminated on at least one surface of the insulating resin layer 30, and a metal layer M laminated on the insulating resin layer 30 via the adhesive layer 20, as shown in FIG. 2, and the adhesive layer 20 is made of the above-mentioned adhesive film. The three-layer metal-clad laminate 101 may include any layer other than the above. The three-layer metal-clad laminate 101 may have the adhesive layer 20 on one or both surfaces of the insulating resin layer 30, and the metal layer M may have the adhesive layer 20 on one or both surfaces of the insulating resin layer 30. In other words, the three-layer metal-clad laminate 101 may be a single-sided metal-clad laminate or a double-sided metal-clad laminate. A single-sided or double-sided FPC can be manufactured by performing wiring circuit processing such as etching the metal layer M of the three-layer metal-clad laminate 101.
[0130] The insulating resin layer 30 in the three-layer metal-clad laminate 101 is not particularly limited as long as it is made of a resin having electrical insulation properties, and examples thereof include polyimide, epoxy resin, phenolic resin, polyethylene, polypropylene, polytetrafluoroethylene, silicone, ETFE, etc., but is preferably made of polyimide. The polyimide layer constituting the insulating resin layer 30 may be a single layer or multiple layers, but preferably includes a non-thermoplastic polyimide layer.
[0131] The thickness of the insulating resin layer 30 in the three-layer metal-clad laminate 101 is preferably within a range of, for example, 1 to 125 μm, and more preferably within a range of 5 to 100 μm. If the thickness of the insulating resin layer 30 is less than the above lower limit, problems such as inability to ensure sufficient electrical insulation may occur. On the other hand, if the thickness of the insulating resin layer 30 exceeds the above upper limit, problems such as the metal-clad laminate being more likely to warp may occur.
[0132] The thickness of the adhesive layer 20 in the three-layer metal-clad laminate 101 is preferably within a range of, for example, 0.1 to 125 μm, and more preferably within a range of 0.3 to 100 μm. In the three-layer metal-clad laminate 101 of the present embodiment, if the thickness of the adhesive layer 20 is less than the above lower limit, problems such as insufficient adhesion may occur. On the other hand, if the thickness of the adhesive layer 20 exceeds the above upper limit, problems such as reduced dimensional stability may occur. In addition, from the viewpoint of reducing the dielectric constant and dielectric loss tangent of the entire insulating layer, which is a laminate of the insulating resin layer 30 and the adhesive layer 20, the thickness of the adhesive layer 20 is preferably 3 μm or more.
[0133] Moreover, the ratio of the thickness of the insulating resin layer 30 to the thickness of the adhesive layer 20 (thickness of the insulating resin layer 30 / thickness of the adhesive layer 20) is preferably within a range of, for example, 0.1 to 3.0, and more preferably within a range of 0.15 to 2.0. By setting such a ratio, it is possible to suppress warping of the three-layer metal-clad laminate 101. Moreover, the insulating resin layer 30 may contain a filler as necessary. Examples of the filler include silicon dioxide, aluminum oxide, magnesium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, and metal salts of organic phosphinic acid. These can be used alone or in combination of two or more kinds.
[0134] (Third aspect) A metal-clad laminate according to still another embodiment of the present invention is, for example, as shown in Fig. 3, a laminated type metal-clad laminate 102 formed by laminating at least two single-sided metal-clad laminates via an adhesive layer 20. The laminated type metal-clad laminate 102 comprises a first single-sided metal-clad laminate 41, a second single-sided metal-clad laminate 42, and an adhesive layer 20 laminated between the first single-sided metal-clad laminate 41 and the second single-sided metal-clad laminate 42, and the adhesive layer 20 is made of the above-mentioned adhesive film. Here, the first single-sided metal-clad laminate 41 has a first metal layer M1 and a first insulating resin layer 31 laminated on at least one side of the first metal layer M1. The second single-sided metal-clad laminate 42 has a second metal layer M2 and a second insulating resin layer 32 laminated on at least one side of the second metal layer M2. The adhesive layer 20 is disposed so as to abut against the first insulating resin layer 31 and the second insulating resin layer 32. The laminated metal-clad laminate 102 may include any layer other than those described above.
[0135] The first insulating resin layer 31 and the second insulating resin layer 32 in the laminated metal-clad laminate 102 may have the same configuration as the insulating resin layer 30 in the three-layer metal-clad laminate 101 of the second embodiment. The laminated metal-clad laminate 102 can be manufactured by preparing a first single-sided metal-clad laminate 41 and a second single-sided metal-clad laminate 42, and placing an adhesive film between the first insulating resin layer 31 and the second insulating resin layer 32 and laminating them together.
[0136] (Fourth aspect) 4, a metal-clad laminate according to still another embodiment of the present invention is a metal-clad laminate 103 with an adhesive layer, which includes a single-sided metal-clad laminate having an insulating resin layer 33 and a metal layer M laminated on one side of the insulating resin layer 33, and an adhesive layer 20 laminated on the other side of the insulating resin layer 33, and the adhesive layer 20 is made of the above-mentioned adhesive film. Note that the metal-clad laminate 103 with an adhesive layer may include any layer other than those described above. The insulating resin layer 33 in the adhesive layer-attached metal-clad laminate 103 may have a configuration similar to that of the insulating resin layer 30 in the three-layer metal-clad laminate 101 of the second embodiment. The adhesive layer-attached metal-clad laminate 103 can be manufactured by preparing a single-sided metal-clad laminate having an insulating resin layer 33 and a metal layer M, and laminating an adhesive film to the insulating resin layer 33 side.
[0137] In the metal-clad laminate of any of the first to fourth exemplary embodiments above, the material of the metal layer M (including the first metal layer M1 and the second metal layer M2, the same applies below) is not particularly limited, and examples thereof include copper, stainless steel, iron, nickel, beryllium, aluminum, zinc, indium, silver, gold, tin, zirconium, tantalum, titanium, lead, magnesium, manganese, and alloys thereof. Among these, copper or a copper alloy is particularly preferred. The material of the wiring layer in the circuit board described below is also the same as that of the metal layer M.
[0138] The thickness of the metal layer M is not particularly limited, but when a metal foil such as copper foil is used, it is preferably 35 μm or less, more preferably in the range of 5 to 25 μm. From the viewpoint of production stability and handling, the lower limit of the thickness of the metal foil is preferably 5 μm. When copper foil is used, it may be rolled copper foil or electrolytic copper foil. In addition, commercially available copper foil may be used as the copper foil. In addition, the metal foil may be subjected to a surface treatment such as siding, aluminum alcoholate, aluminum chelate, silane coupling agent, etc., for the purpose of, for example, rust prevention treatment or improvement of adhesive strength.
[0139] [Circuit board] (First aspect) The circuit board according to the embodiment of the present invention is obtained by wiring the metal layer of the metal-clad laminate according to any of the above embodiments. One or more metal layers of the metal-clad laminate are patterned by a conventional method to form a wiring layer (conductor circuit layer), thereby manufacturing a circuit board such as an FPC. The circuit board may include a coverlay film that covers the wiring layer.
[0140] (Second aspect) 5, a circuit board 200 according to another embodiment of the present invention includes a first base material 11, a wiring layer 50 laminated on at least one surface of the first base material 11, and an adhesive layer 20 laminated on the surface of the first base material 11 facing the wiring layer 50 so as to cover the wiring layer 50, the adhesive layer 20 being made of the adhesive film. Note that the circuit board 200 may include any layer other than those described above. The first base material 11 in the circuit board 200 may have the same configuration as the insulating resin layer of the metal-clad laminate. The circuit board 200 can be manufactured by laminating an adhesive film to the side of the wiring layer 50 of a circuit board including the first base material 11 and the wiring layer 50 laminated on at least one surface of the first base material 11.
[0141] (Third aspect) As shown in FIG. 6, a circuit board 201 according to another embodiment of the present invention includes a first base material 11, a wiring layer 50 laminated on at least one surface of the first base material 11, an adhesive layer 20 laminated on the surface of the first base material 11 facing the wiring layer 50 so as to cover the wiring layer 50, and a second base material 12 laminated on the surface of the adhesive layer 20 opposite the first base material 11, and the adhesive layer 20 is made of the adhesive film. The circuit board 201 may include any layer other than those described above. The first base material 11 and the second base material 12 in the circuit board 201 may have the same configuration as the insulating resin layer of the metal-clad laminate. The circuit board 201 can be manufactured by bonding a second substrate 12 to the wiring layer 50 side of a circuit board having a first substrate 11 and a wiring layer 50 laminated on at least one surface of the first substrate 11 via an adhesive film.
[0142] (Fourth aspect) As shown in FIG. 7, the circuit board 202 according to another embodiment of the present invention includes a first base material 11, an adhesive layer 20 laminated on at least one surface of the first base material 11, a second base material 12 laminated on the surface of the adhesive layer 20 opposite the first base material 11, and wiring layers 50, 50 laminated on the surfaces of the first base material 11 and the second base material 12 opposite the adhesive layer 20, respectively, and the adhesive layer 20 is made of the adhesive film. The circuit board 202 may include any layer other than the above. The first base material 11 and the second base material 12 in the circuit board 202 may have the same configuration as the insulating resin layer of the metal-clad laminate. The circuit board 202 can be manufactured by preparing a first circuit board having a first substrate 11 and a wiring layer 50 laminated on at least one surface of the first substrate 11, and a second circuit board having a second substrate 12 and a wiring layer 50 laminated on at least one surface of the second substrate 12, and then placing an adhesive film between the first substrate 11 of the first circuit board and the second substrate 12 of the second circuit board and bonding them together.
[0143] [Multilayer circuit board] A multilayer circuit board according to an embodiment of the present invention includes a laminate in which a plurality of insulating resin layers are stacked, and one or more wiring layers embedded inside the laminate, and at least one of the plurality of insulating resin layers is formed of an adhesive layer 20 that has adhesiveness and covers the wiring layer, and the adhesive layer 20 is made of the adhesive film. Note that the multilayer circuit board of this embodiment may include any layer other than those described above. For example, as shown in FIG. 8, the multilayer circuit board 203 of the present embodiment has at least two insulating resin layers 34 and at least two wiring layers 50, and at least one of the wiring layers 50 is covered with an adhesive layer 20. The adhesive layer 20 covering the wiring layer 50 may partially cover the surface of the wiring layer 50, or may cover the entire surface of the wiring layer 50. The multilayer circuit board 203 may also have a wiring layer 50 exposed on the surface of the multilayer circuit board 203. The multilayer circuit board 203 may also have an interlayer connection electrode (via electrode) in contact with the wiring layer 50. The wiring layer 50 is formed by forming a conductor circuit in a predetermined pattern on one or both sides of the insulating resin layer 34. The conductor circuit may be patterned on the surface of the insulating resin layer 34, or may be patterned in a damascene (embedded) manner. The insulating resin layer 34 in the multilayer circuit board 203 may have the same configuration as the insulating resin layer of the metal-clad laminate.
[0144] The circuit board and multilayer circuit board of each of the above embodiments include the adhesive layer 20 containing an adhesive polyimide or crosslinked polyimide whose Mw and Mn are controlled, and therefore have excellent adhesiveness, and even if a filler is contained, the decrease in mechanical strength is suppressed, and it is possible to reduce transmission loss in the transmission of high-frequency signals. EXAMPLES
[0145] The features of the present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to the examples. In the following examples, various measurements and evaluations are as follows, unless otherwise specified.
[0146] [Method for measuring amine value] Approximately 2 g of the dimer diamine composition is weighed into a 200-250 mL Erlenmeyer flask, and phenolphthalein is used as an indicator. A 0.1 mol / L ethanolic potassium hydroxide solution is dropped into the solution until the solution turns light pink, and the solution is dissolved in approximately 100 mL of neutralized butanol. 3-7 drops of phenolphthalein solution are added thereto, and titration is performed with 0.1 mol / L ethanolic potassium hydroxide solution while stirring until the sample solution turns light pink. Five drops of bromophenol blue solution are added thereto, and titration is performed with 0.2 mol / L hydrochloric acid / isopropanol solution while stirring until the sample solution turns yellow. The amine value is calculated according to the following formula (1). Amine value = {(V 2 ×C 2 )-(V 1 ×C 1 )}×M KOH / m (1) Here, the amine value is expressed as mg-KOH / g, and M KOH is the molecular weight of potassium hydroxide, 56.1. V and C are the volume and concentration of the solution used in the titration, respectively, and the subscripts 1 and 2 represent 0.1 mol / L ethanolic potassium hydroxide solution and 0.2 mol / L hydrochloric acid / isopropanol solution, respectively. Furthermore, m is the sample weight in grams.
[0147] [Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn) of polyimide] Measurement was performed using a gel permeation chromatograph (manufactured by Tosoh Corporation, product name: HLC-8220GPC). Polystyrene was used as the standard substance, and tetrahydrofuran (THF) was used as the developing solvent.
[0148] [Calculation of GPC and chromatogram area percentage] For GPC, 20 mg of the dimer diamine composition was pretreated with 200 μL of acetic anhydride, 200 μL of pyridine, and 2 mL of THF to prepare a 100 mg solution, which was then diluted with 10 mL of THF (containing 1000 ppm of cyclohexanone) to prepare a sample. The prepared sample was measured using a Tosoh Corporation product name: HLC-8220GPC under the following conditions: column: TSK-gel G2000HXL, G1000HXL, flow rate: 1 mL / min, column (oven) temperature: 40° C., injection volume: 50 μL. Cyclohexanone was used as a standard substance to correct the elution time.
[0149] In this case, the retention times were adjusted so that the peak top of the cyclohexanone main peak was at a retention time of 27 to 31 minutes, and the period from the peak start to the peak end of the cyclohexanone main peak was 2 minutes, and the peak top of the main peak excluding the cyclohexanone peak was at a retention time of 18 to 19 minutes, and the period from the peak start to the peak end of the main peak excluding the cyclohexanone peak was at a retention time of 2 minutes to 4 minutes 30 seconds, (a) Component represented by the main peak; (b) A component represented by a GPC peak detected at a time later than the minimum retention time of the main peak; (c) Components represented by GPC peaks detected at earlier retention times than the minimum value of the main peak on the earlier side; was detected.
[0150] [Dielectric property evaluation] Using a vector network analyzer (manufactured by Agilent, product name: Vector Network Analyzer E8363C) and a split post dielectric resonator (SPDR), a resin sheet was heat-treated with a small precision press machine manufactured by Kitagawa Seiki under conditions of temperature: 160°C, pressure: 2 MPa, and 1.0 hour, and then left for 24 hours under conditions of temperature: 23°C and humidity: 50%, and then the relative dielectric constant (Dk) and dielectric loss tangent (Df) were measured at frequencies of 5 GHz, 10 GHz, and 20 GHz.
[0151] [Measurement of tensile modulus, strength, and elongation] A tension tester (trade name Tensilon, manufactured by Orientec Co., Ltd.) was used to carry out a tensile test at 50 mm / min using a test piece having a width of 12.7 mm and a length of 127 mm, and the tensile modulus, strength and elongation were measured.
[0152] The abbreviations used in the examples represent the following compounds. BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride DDA1: Product name: PRIAMINE 1074, manufactured by Croda Japan Co., Ltd., purified (component a: 97.9% by weight, component b: 0.3%, component c: 1.8%, amine value: 210 mg KOH / g, mixture of dimer diamines having a cyclic structure and a chain structure) DDA2: product name: PRIAMINE 1075, manufactured by Croda Japan Co., Ltd., purified (component a: 98.3% by weight, component b: 0%, component c: 1.7%, amine value: 210 mg KOH / g, mixture of dimer diamines having a cyclic structure and a chain structure) N-12: Dodecanedioic acid dihydrazide NMP: N-methyl-2-pyrrolidone OP935: Aluminum salt of phosphinic acid (manufactured by Clariant, trade name: Exolit OP935, aluminum diethylphosphinate, phosphorus content: 23% by mass, particle size D 50 ;2μm) In the above DDA1 and DDA2, the "%" of the b component and the c component means the area percentage of the chromatogram in the GPC measurement. The molecular weights of DDA1 and DDA2 were calculated by the following formula (1). Molecular weight = 56.1 × 2 × 1000 / amine value (1)
[0153] (Reference example 1) <Preparation of polyimide solution> A polyamic acid solution was prepared by charging 34.94g of BTDA (0.108 mol), 55.06g of DDA1 (0.103 mol), 126g of NMP, and 84g of xylene into a 1000ml separable flask and thoroughly mixing at 40°C for 1 hour. The polyamic acid solution was heated to 190°C, heated and stirred for 4 hours, and 64g of xylene was added to complete the imidization, preparing polyimide solution 1 (solid content: 30% by weight, Mw: 20,165, Mn: 12,259, Mw / Mn: 1.64).
[0154] <Preparation of Polyimide Composition> 1.575 g of N-12 (equivalent to 0.35 mol of primary amine group per 1 mol of BTDA ketone group) was mixed with 150 g of polyimide solution 1, and 5.0 g of NMP was added to dilute it. Further, 11.25 g of OP935 (25 wt % with respect to the solid content of polyimide, equivalent to 0.09 mol of phosphorus per 1 mol of dimer diamine) was mixed and stirred for another 1 hour to prepare polyimide composition 1.
[0155] <Preparation of Resin Sheet> The polyimide composition 1 was applied to one side of a release PET film (manufactured by Higashiyama Film Co., Ltd., product name: HY-S05, length x width x thickness = 200 mm x 300 mm x 25 μm), dried at 80°C for 15 minutes, and peeled off from the release PET film to prepare a resin sheet 1 with a thickness of 25 μm.
[0156] The various properties of the resin sheet 1 are as follows. Dielectric constant at 5GHz: 2.7, dissipation factor: 0.0031 Dielectric constant at 10GHz: 2.7, dissipation factor: 0.0027 Dielectric constant at 20GHz: 2.6, dissipation factor: 0.0020 Tensile modulus: 0.6GPa, strength: 21MPa, elongation: 222%
[0157] (Reference example 2) A polyamic acid solution was prepared by charging 34.53 g of BTDA (0.106 mol), 55.47 g of DDA1 (0.104 mol), 126 g of NMP, and 84 g of xylene into a 1000 ml separable flask and thoroughly mixing at 40° C. for 1 hour. The polyamic acid solution was heated to 190° C., heated and stirred for 4 hours, and 64 g of xylene was added to complete the imidization, preparing polyimide solution 2 (solid content: 30 wt %, Mw: 25,779, Mn: 14,853, Mw / Mn: 1.74).
[0158] Polyimide composition 2 and resin sheet 2 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 1.546 g.
[0159] The various properties of the resin sheet 2 are as follows: Dielectric constant at 5GHz: 2.7, dissipation factor: 0.0030 Dielectric constant at 10GHz: 2.7, dissipation factor: 0.0025 Dielectric constant at 20GHz: 2.6, dissipation factor: 0.0019 Tensile modulus: 0.6GPa, strength: 23MPa, elongation: 215%
[0160] [Example 1] A polyamic acid solution was prepared by charging 33.94g of BTDA (0.105 mol), 55.06g of DDA2 (0.105 mol), 126g of NMP, and 84g of xylene into a 1000ml separable flask and thoroughly mixing at 40°C for 1 hour. The polyamic acid solution was heated to 190°C, heated and stirred for 4 hours, and 84g of xylene was added to complete the imidization, preparing polyimide solution 3 (solid content: 30% by weight, Mw: 38,818, Mn: 20,569, Mw / Mn: 1.89).
[0161] Polyimide composition 3 and resin sheet 3 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 1.531 g.
[0162] The various properties of the resin sheet 3 are as follows: Dielectric constant at 5GHz: 2.7, dissipation factor: 0.0026 Dielectric constant at 10GHz: 2.7, dissipation factor: 0.0022 Dielectric constant at 20GHz: 2.6, dissipation factor: 0.0016 Tensile modulus: 0.4GPa, strength: 16MPa, elongation: 235%
[0163] [Example 2] A polyamic acid solution was prepared by charging 28.05g of BTDA (0.087 mol), 46.95g of DDA2 (0.86 mol), 105g of NMP, and 70g of xylene into a 1000ml separable flask and thoroughly mixing at 40°C for 1 hour. The polyamic acid solution was heated to 190°C, heated and stirred for 4 hours, and 70g of xylene was added to complete the imidization, preparing polyimide solution 4 (solid content: 30% by weight, Mw: 48,452, Mn: 23,399, Mw / Mn: 2.07).
[0164] Polyimide composition 4 and resin sheet 4 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 1.269 g.
[0165] The various properties of the resin sheet 4 are as follows: Dielectric constant at 5GHz: 2.8, dissipation factor: 0.0028 Dielectric constant at 10GHz: 2.7, dissipation factor: 0.0024 Dielectric constant at 20GHz: 2.7, dissipation factor: 0.0015 Tensile modulus: 0.6GPa, strength: 24MPa, elongation: 191%
[0166] [Example 3] A polyamic acid solution was prepared by charging 33.73 g of BTDA (0.104 mol), 56.27 g of DDA2 (0.105 mol), 126 g of NMP, and 84 g of xylene into a 1000 ml separable flask and thoroughly mixing at 40° C. for 1 hour. The polyamic acid solution was heated to 190° C., heated and stirred for 4 hours, and 84 g of xylene was added to complete the imidization, preparing polyimide solution 5 (solid content: 30 wt %, Mw: 63,338, Mn: 29,207, Mw / Mn: 2.17).
[0167] Polyimide composition 5 and resin sheet 5 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 1.517 g.
[0168] The resin sheet 5 has the following characteristics. Dielectric constant at 5GHz: 2.6, dissipation factor: 0.0025 Dielectric constant at 10GHz: 2.6, dissipation factor: 0.0021 Dielectric constant at 20GHz: 2.7, dissipation factor: 0.0016 Tensile modulus: 0.4GPa, strength: 20MPa, elongation: 210%
[0169] [Example 4] A polyamic acid solution was prepared by charging 33.63 g of BTDA (0.104 mol), 56.37 g of DDA2 (0.106 mol), 126 g of NMP, and 84 g of xylene into a 1000 ml separable flask and thoroughly mixing at 40° C. for 1 hour. The polyamic acid solution was heated to 190° C., heated and stirred for 4 hours, and 84 g of xylene was added to complete the imidization, preparing polyimide solution 6 (solid content: 30 wt %, Mw: 85,454, Mn: 30,797, Mw / Mn: 2.77).
[0170] Polyimide composition 6 and resin sheet 6 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 1.517 g.
[0171] The various properties of the resin sheet 6 are as follows: Dielectric constant at 5GHz: 2.6, dissipation factor: 0.0025 Dielectric constant at 10GHz: 2.6, dissipation factor: 0.0021 Dielectric constant at 20GHz: 2.6, dissipation factor: 0.0016 Tensile modulus: 0.4GPa, strength: 15MPa, elongation: 224%
[0172] [Example 5] A polyamic acid solution was prepared by charging 55.88g of BTDA (0.173 mol), 94.12g of DDA1 (0.175 mol), 210g of NMP and 140g of xylene into a 1000ml separable flask and thoroughly mixing for 1 hour at 40°C. The polyamic acid solution was heated to 190°C, heated and stirred for 4 hours, and 120g of xylene was added to complete the imidization, preparing polyimide solution 7 (solid content: 30% by weight, Mw: 95,519, Mn: 30,544, Mw / Mn: 3.13).
[0173] Polyimide composition 7 and resin sheet 7 were prepared in the same manner as in Reference Example 1, except that the amount of N-12 was 2.523 g.
[0174] The various properties of the resin sheet 7 are as follows. Dielectric constant at 5GHz: 2.6, dissipation factor: 0.0025 Dielectric constant at 10GHz: 2.7, dissipation factor: 0.0022 Dielectric constant at 20GHz: 2.7, dissipation factor: 0.0018 Tensile modulus: 0.6GPa, strength: 24MPa, elongation: 229%
[0178] The above results are summarized in Tables 1 and 2.
[0179] [Table 1]
[0180] [Table 2]
[0181] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment, and various modifications are possible. [Explanation of symbols]
[0182] REFERENCE SIGNS LIST 10...substrate, 11...first substrate, 12...second substrate, 20...adhesive layer, 30, 33, 34...insulating resin layer, 31...first insulating resin layer, 32...second insulating resin layer, 41...first single-sided metal-clad laminate, 42...second single-sided metal-clad laminate, 50...wiring layer, M...metal layer, M1...first metal layer, M2...second metal layer, 100...laminate, 101...three-layer metal-clad laminate, 102...laminated metal-clad laminate, 103...metal-clad laminate with adhesive layer, 200, 201, 202...circuit board, 203...multilayer circuit board
Claims
1. A polyimide containing a tetracarboxylic acid residue derived from a tetracarboxylic acid anhydride component and a diamine residue derived from a diamine component, the polyimide being capable of being produced by the following conditions a to d: a) containing 40 mol % or more of diamine residues derived from a dimer diamine composition mainly composed of a dimer diamine obtained by substituting two terminal carboxylic acid groups of a dimer acid with primary aminomethyl groups or amino groups, relative to the total diamine residues; b) a weight average molecular weight (Mw) in the range of 25,000 to 100,000; c) a number average molecular weight (Mn) in the range of 15,000 to 32,000; d) the ratio of Mw to Mn (Mw / Mn) is in the range of 1.8 to 3.4; While satisfying the above, The dimer diamine composition comprises the following components (a) to (c): (a) dimer diamine; (b) a monoamine compound obtained by substituting a terminal carboxylic acid group of a monobasic acid compound having 10 to 40 carbon atoms with a primary aminomethyl group or an amino group; (c) Amine compounds obtained by substituting the terminal carboxylic acid group of a polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms with a primary aminomethyl group or an amino group (excluding the above-mentioned dimer diamine); The content of the component (a) in the dimer diamine composition is 97.9% by weight or more.
2. 2. The polyimide according to claim 1, wherein the area percentage of the chromatogram of the dimer diamine composition measured by gel permeation chromatography is 3% or less.
3. 3. The polyimide according to claim 2, wherein the total area percentage of said component (b) and said component (c) is 4% or less in said chromatogram.
4. Components (A) and (B) below; (A) the polyimide according to claim 1, and (B) a metal salt of an organic phosphinic acid; and wherein the weight ratio of the component (B) to the component (A) is within the range of 10 to 70% by weight.
5. The polyimide of the component (A) is a polyimide having a ketone group in the molecule, and further comprises the following component (C): (C) a crosslinking agent having a functional group that undergoes a nucleophilic addition reaction with the ketone group; The polyimide composition according to claim 4, comprising:
6. An adhesive film comprising the polyimide according to claim 1.
7. Components (A) and (B) below; (A) the polyimide according to claim 1; And, (B) a metal salt of an organic phosphinic acid; and wherein the weight ratio of the component (B) to the component (A) is within the range of 10 to 70% by weight.
8. Components (A') and (B) below; (A') a crosslinked polyimide having a crosslinked structure formed by a reaction between the polyimide according to claim 1 having a ketone group in the molecule and a crosslinking agent having a functional group which undergoes a nucleophilic addition reaction with the ketone group; And, (B) a metal salt of an organic phosphinic acid; and wherein the weight ratio of the component (B) to the component (A') is within the range of 10 to 70% by weight.
9. A laminate having a substrate and an adhesive layer laminated on at least one surface of the substrate, A laminate, wherein the adhesive layer comprises the adhesive film according to any one of claims 6 to 8.
10. A coverlay film having a coverlay film material layer and an adhesive layer laminated on the coverlay film material layer, A coverlay film, characterized in that the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
11. A resin-coated copper foil in which an adhesive layer and a copper foil are laminated, A resin-coated copper foil, characterized in that the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
12. A metal-clad laminate having an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, 9. A metal-clad laminate, wherein at least one of the insulating resin layers is made of the adhesive film according to claim 6.
13. A metal-clad laminate having an insulating resin layer, an adhesive layer laminated on at least one surface of the insulating resin layer, and a metal layer laminated on the insulating resin layer via the adhesive layer, A metal-clad laminate, wherein the adhesive layer comprises the adhesive film according to any one of claims 6 to 8.
14. A first single-sided metal-clad laminate having a first metal layer and a first insulating resin layer laminated on at least one surface of the first metal layer; a second single-sided metal-clad laminate having a second metal layer and a second insulating resin layer laminated on at least one surface of the second metal layer; An adhesive layer is disposed so as to abut against the first insulating resin layer and the second insulating resin layer, and is laminated between the first single-sided metal-clad laminate and the second single-sided metal-clad laminate, A metal-clad laminate, wherein the adhesive layer comprises the adhesive film according to any one of claims 6 to 8.
15. A metal-clad laminate comprising: a single-sided metal-clad laminate having an insulating resin layer and a metal layer laminated on one side of the insulating resin layer; and an adhesive layer laminated on the other side of the insulating resin layer, wherein the adhesive layer is made of the adhesive film described in any one of claims 6 to 8.
16. A circuit board obtained by wiring the metal layer of the metal-clad laminate according to any one of claims 12 to 15.
17. A circuit board comprising: a first base material; a wiring layer laminated on at least one surface of the first base material; and an adhesive layer laminated on a surface of the first base material facing the wiring layer so as to cover the wiring layer, A circuit board, wherein the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
18. A circuit board comprising: a first base material; a wiring layer laminated on at least one surface of the first base material; an adhesive layer laminated on a surface of the first base material facing the wiring layer so as to cover the wiring layer; and a second base material laminated on a surface of the adhesive layer opposite to the first base material, A circuit board, wherein the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
19. A circuit board comprising: a first base material; an adhesive layer laminated on at least one surface of the first base material; a second base material laminated on a surface of the adhesive layer opposite to the first base material; and wiring layers laminated on each of the first base material and the second base material opposite to the adhesive layer, A circuit board, wherein the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
20. A multilayer circuit board comprising a laminate including a plurality of laminated insulating resin layers, and at least one wiring layer embedded in the laminate, At least one of the plurality of insulating resin layers is formed of an adhesive layer having adhesiveness and covering the wiring layer, A multilayer circuit board, wherein the adhesive layer is made of the adhesive film according to any one of claims 6 to 8.
Citation Information
Patent Citations
Battery voltage detecting device
JP1989088170A
Crosslinked polyimide resin, adhesive resin composition and cured product thereof, cover lay film and circuit board
JP2013001730A
Polyamide acid composition, polyimide, resin film, and metal-clad laminate
JP2015127370A
Metal-clad laminate, adhesive sheet, adhesive polyimide resin composition, and circuit board
JP2018140544A
Metal-clad laminate sheet and circuit board
JP2018170417A