Manufacturing method of molded body
The sequential three-step pressurization process with specific punch movements addresses non-uniform density in powder press molding, resulting in high-quality molded bodies with minimal defects and uniform density.
Patent Information
- Application Number
- JP2021029235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-02-25
AI Technical Summary
Existing powder press molding methods result in non-uniform density distribution and dimensional variations within molded bodies, leading to increased processing difficulties and internal defects.
A sequential three-step pressurization process using two punches, where the second punch's movement is equal to the sum of the first and third punch's movements, with the third punch's movement being smaller than the second, to promote uniform density distribution.
The method achieves a high-quality molded body with reduced density variations and internal defects, ensuring consistent dimensions and improved sintering outcomes.
Smart Images

Figure 0007578508000002 
Figure 0007578508000003 
Figure 0007578508000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a compact from powder using a molding die. [Background technology]
[0002] In recent years, there is an increasing need for products with excellent functionality, such as ceramics and carbide. For example, powder press molding, which allows for mass production, is often used to manufacture chip products for cutting tools. In powder press molding, a molding die consisting of a die and a punch is used, and the punch is inserted into the die filled with raw material powder to pressurize the raw material powder to produce a cylindrical, cylindrical, rectangular, or other shaped body. The shaped body is sintered to produce a blank, and the blank's outer shape is then processed into the final product shape to manufacture the product. In products manufactured by these powder press moldings, if there are parts with uneven density inside the shaped body, there is a risk of increased dimensional variation in the blank's outer shape and damage occurring during the processing of the blank. Dimensional variation in the blank's outer shape leads to an increase in the amount of processing in the subsequent processing steps and an increase in internal defects in the blank.
[0003] In powder press molding, in order to obtain high-precision blanks, molding is sometimes performed using a CNC powder molding machine that can precisely control the punch with a servo motor. However, even when molding is performed using this method, the powder around the punch inserted into the die tends to have a higher density than other areas due to friction with the die wall, resulting in differences in density distribution inside the compact. In particular, cylindrical and rectangular compacts are prone to uneven density distribution during molding because powder movement within the die is difficult.
[0004] In order to eliminate such differences in density distribution inside the compact, various methods have been devised, such as a two-sided molding method in which a load is applied to the powder from above and below using an upper and lower punch, and a withdrawal process method in which the punch is driven and the die is moved in the same direction as the punch to form the compact. Patent Document 1 proposes a two-stage pressing method in which a first punch is moved first and then a second punch is moved during powder press molding, and discloses an example in which the amount of movement of the first punch (upper punch) is set to 1 to 5 times the amount of movement of the second punch (lower punch). Patent Document 2 also proposes a method of molding with a tapered die. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-272942 A [Patent Document 2] JP 2001-3104 A Summary of the Invention [Problem to be solved by the invention]
[0006] For example, in the molding method described in Patent Document 1, the movement amount of the first punch and the second punch are made different, so that the movement amount of the raw material powder in the process of moving each punch is different, and a large density variation occurs on the punch side with a larger movement amount, and it is not possible to fully eliminate the quality deterioration due to dimensional variation and density unevenness in the blank sintered into the molded body. Also, even with the molding method described in Patent Document 2, although it is expected that the unevenness of the density distribution inside the molded body can be reduced by reducing the pressure applied to the molded body, it cannot be said to be sufficient. In view of the above problems, the present invention provides a manufacturing method for a molded body for manufacturing a molded body with a small density distribution difference inside the molded body. [Means for solving the problem]
[0007] A method for manufacturing a molded body, comprising: filling a raw material powder into a space formed by a through hole provided in a die and a first punch inserted into the through hole; inserting a second punch into the through hole so as to face the first punch; and relatively moving the first punch and the second punch to compress and mold the raw material powder, the method comprising: a first pressurizing step of moving the second punch a first predetermined amount toward the first punch from a position where the second punch contacted the raw material powder; a second pressurizing step of moving the first punch toward the second punch by a second predetermined amount; and a third pressurizing step of moving the second punch toward the first punch by a third predetermined amount, wherein the first pressurizing step, the second pressurizing step, and the third pressurizing step are carried out in sequence. Furthermore, the second predetermined amount is equal to the sum of the first predetermined amount and the third predetermined amount in the method for producing a molded body. Furthermore, the third predetermined amount is smaller than the second predetermined amount in the method for producing a molded article. Effect of the Invention
[0008] According to the present invention, it is possible to obtain a high-quality product having a small density distribution inside a molded body and having few dimensional variations and few internal defects after sintering the molded body. [Brief description of the drawings]
[0009] [Figure 1] 1A to 1C are diagrams for explaining an embodiment of the method for producing a molded body of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a method for producing a molded body of Comparative Example 1. [Diagram 3] FIG. 13 is a diagram for explaining a method for producing a molded body of Comparative Example 3. [Figure 4-1] FIG. 2 is a photograph of a pinhole formation state in a cross section of a blank in Example 1. [Figure 4-2] FIG. 13 is a photograph of a pinhole formation state in a cross section of a blank in Comparative Example 2. [Figure 4-3] FIG. 13 is a photograph of a pinhole formation state in a cross section of a blank in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method for manufacturing a molded body of the present invention involves filling a space formed by a through hole in a die and a first punch inserted into the through hole with raw material powder, inserting a second punch into the through hole so as to face the first punch, and moving the first punch and the second punch relative to one another to compress the raw material powder, in which the second punch is moved to pressurize the raw material powder, then the first punch is moved to pressurize the raw material powder, and then the second punch is moved to pressurize the raw material powder to produce a molded body.
[0011] 1 is a diagram for explaining an embodiment of a method for producing a molded body of the present invention. In this embodiment, the present invention will be explained by taking a method for producing a cylindrical molded body as an example. The molded body is produced by a powder molding press equipped with a cylindrical die 3 with a through hole 3a, and a die having a cylindrical lower punch 1 and an upper punch 2 inserted into the through hole 3a of the die 3. The lower punch 1 and the upper punch 2 are inserted into the through hole 3a of the die 3, and each is independently movable on the axis of the through hole 3a.
[0012] [Raw material powder filling process: Figure 1(a)] First, the lower punch 1 is inserted into one open end of the through hole 3a, and raw material powder 4 for the compact is supplied into the recess of the die 3 formed by the bottom surface of the lower punch 1 and the inner wall surface of the through hole 3a of the die 3.
[0013] [First pressurization step: Figure 1(b)] Next, the upper punch 2 is inserted from the other open end of the through hole 3a, and the upper punch 2 is moved toward the lower punch 1 to pressurize and compress the raw material powder 4. At this time, the positions of the die 3 and the lower punch 1 are fixed, and the upper punch 2 moves a preset distance A from the position where it contacted the raw material powder 4 toward the lower punch 1. This process mainly moves the raw material powder 4 on the upper punch 2 side, and the raw material powder 4 is partially compressed due to friction with the inner wall surface of the through hole 3a, causing an increase in density near the upper punch 2. Note that there is no significant movement of the raw material powder 4 around the lower punch 1, so no significant increase in density occurs, and the density of the entire raw material powder 4 is non-uniform.
[0014] [Second pressurization step: Figure 1(c)] Next, with the die 3 and upper punch 2 held in fixed positions, the lower punch 1 is moved a preset distance a toward the upper punch 2 to pressurize and compress the raw material powder 4. This process mainly moves the raw material powder 4 on the lower punch 1 side, causing an increase in density near the lower punch 1. At this time, the raw material powder 4 is in a state compressed to some extent by the first pressurizing process, and a larger increase in density occurs around the lower punch 1 than the increase in density around the upper punch 2 in the first pressurizing process. The amount of movement of the lower punch 1 in this process (predetermined distance a) is set to be larger than the amount of movement of the upper punch 2 in the first pressurizing process (predetermined distance A).
[0015] [Third pressurization step: Figure 1(d)] Next, with the die 3 and lower punch 1 held in fixed positions, the upper punch 2 is moved a preset distance α toward the lower punch 1 to pressurize and compress the raw material powder. After the second pressurizing step is completed, the density around the lower punch 1 is greater than that around the upper punch 2, but by carrying out this step, the density mainly around the upper punch 2 increases.
[0016] In this way, by sequentially applying pressure from the upper punch 2 (first pressure application process), pressure from the lower punch 1 (second pressure application process), and pressure from the upper punch 2 (third pressure application process), the raw material powder 4 is more likely to move (rearrange) in the center of the recess of the die 3, compared to the case where pressure from the upper punch 2 and pressure from below are applied once simultaneously or separately, thereby promoting even compression of the raw material powder 4 and making it possible to reduce differences in density distribution inside the molded body 10.
[0017] Furthermore, it is preferable to set the amount of movement of the upper punch 2 in the third pressurizing step (predetermined distance α) smaller than the amount of movement of the upper punch 2 in the first pressurizing step (predetermined distance A) and the amount of movement in the second pressurizing step (predetermined distance a), and set the sum of the amount of movement of the upper punch 2 in the first and third pressurizing steps (predetermined distance A + predetermined distance α) to be equal to the amount of movement of the lower punch 1 in the second processing step (predetermined distance a).In other words, by making the amount of movement of the upper punch 2 and the amount of movement of the lower punch 1 throughout each step equal, it is possible to produce a molded body 10 with a more uniform density.
[0018] [Discharge process: Figure 1(e)] Finally, the upper punch 2 and the lower punch 1 are moved to the other open end of the through hole 3a of the die 3, and the green compact 10 made of the raw material powder 4 compressed and molded in the through hole 3a is discharged from the die 3. In this way, the green compact 10 made of the raw material powder 4 is completed. The green compact 10 is then sintered to become a blank, and the outer shape of the blank is polished to become a product with the desired outer diameter.
[0019] Next, the results of verifying the state of each of the molded bodies will be described using a blank (Example) sintered from a molded body manufactured by the molded body manufacturing method of the present invention and a blank (Comparative Example) sintered from a molded body manufactured by another manufacturing method not employing the present invention. Here, the examples and comparative examples will be described using the symbols explained in the above embodiment. In both the examples and comparative examples, a carbide die 3 with a through hole 3a of 1.2 mm in diameter, a carbide lower punch 1, and a carbide upper punch 2 were used as a molding die for manufacturing the molded body 10, and alumina powder to which a molding binder was added as raw material powder 4 was powder press molded to manufacture the molded body 10. The molded body 10 was created with an outer shape of 1.2 mm in diameter and 1.2 mm in height. In both the examples and comparative examples, molding conditions, sintering conditions, etc. not described in the steps described below were all the same, The condition of the molded body 10 was evaluated by observing the difference in diameter between the upper surface (upper punch 2 side) and the lower surface (lower punch 1 side) of each blank in the examples and comparative examples, and the state of pinhole formation in the cross section of each blank.
[0020] [Example 1] In Example 1, a molded body 10 was produced according to the embodiment of the present invention described above, and the total movement amount of each of the upper punch 2 and the lower punch 1 was set to 2.7 mm, the movement amount of the upper punch 2 in the first pressurizing step was 1.2 mm, the movement amount of the lower punch 1 in the second pressurizing step was 1.35 mm, and the movement amount of the upper punch 2 in the third pressurizing step was 0.15 mm, and the raw material powder 4 was compressed to produce the molded body 10.
[0021] [Example 2] In Example 2, a green compact 10 was also manufactured according to the embodiment of the present invention described above, with the total movement amount of each of the upper punch 2 and the lower punch 1 set to 2.7 mm, the movement amount of the upper punch 2 in the first pressurizing step being 1.15 mm, the movement amount of the lower punch 1 in the second pressurizing step being 1.35 mm, and the movement amount of the upper punch 2 in the third pressurizing step being 0.20 mm, to compress the raw material powder 4 and manufacture the green compact 10. The difference from Example 1 is that the movement amount of the upper punch 2 in the first pressurizing step was reduced by 0.05 mm, and the movement amount of the upper punch 2 in the third step was increased by 0.05 mm.
[0022] [Comparative Example 1] In Comparative Example 1, the upper punch 2 and the lower punch 1 are moved once each in sequence, and the raw material powder 4 is compressed to produce a molded body 10. FIG. 2 is a diagram for explaining the method for producing a molded body in Comparative Example 1. In Comparative Example 1, the lower punch 1 is first inserted from one open end of the through hole 3a, and the raw material powder 4 of the molded body is supplied to the recess of the die 3, which is formed by the bottom surface of the lower punch 1 and the inner wall surface of the through hole 3a of the die 3 (FIG. 2(a): raw material powder filling step). Next, the upper punch 2 is inserted from the other open end of the through hole 3a, and the raw material powder 4 is compressed by moving the upper punch 2 toward the lower punch 1 (FIG. 2(b): first pressurizing step). At this time, the positions of the die 3 and the lower punch 1 are fixed, and the upper punch 2 is moved 2.25 mm from the position where it contacted the raw material powder 4 toward the lower punch 1, and the raw material powder 4 is compressed. Next, with the die 3 and upper punch 2 held in fixed positions, the lower punch 1 was moved 0.45 mm toward the upper punch 2 to pressurize and compress the raw material powder 4 (FIG. 2(c): second pressurizing step). Finally, the upper punch 2 and lower punch 1 were moved toward the other open end of the through hole 3a of the die 3, and the molded body 10 made of the raw material powder 4 compressed within the through hole 3a was ejected from the die 3 (FIG. 2(d): ejection step).
[0023] [Comparative Example 2] In Comparative Example 2, a compact 10 was produced by the same process as in Comparative Example 1. The difference from Comparative Example 1 is that the movement amount of the upper punch 2 in the first pressurizing step in Comparative Example 1 was 2.55 mm, and the movement amount of the lower punch 1 in the second pressurizing step was 0.15 mm.
[0024] [Comparative Example 3] Comparative Example 3 is an example in which the upper punch 2 and the lower punch 1 are moved simultaneously to pressurize the raw material powder 4 to produce a molded body 10. FIG. 3 is a diagram for explaining the method for producing a molded body of Comparative Example 3. In Comparative Example 3, first, the lower punch 1 is inserted from one open end of the through hole 3a, and the raw material powder 4 of the molded body is supplied to the recess of the die 3 formed by the bottom surface of the lower punch 1 and the inner wall surface of the through hole 3a of the die 3 (FIG. 3(a): raw material powder filling step). Next, the upper punch 2 is inserted from the other open end of the through hole 3a, and while the position of the die 3 is fixed, the upper punch 2 and the lower punch 1 are moved toward the opposing punches, respectively, to pressurize and compress the raw material powder 4 (FIG. 3(b): first pressurizing step). At this time, the upper punch 2 and the lower punch 1 are simultaneously moved 1.35 mm from the position where the upper punch 2 contacts the raw material powder 4, respectively, to pressurize and compress the raw material powder 4. Finally, the upper punch 2 and the lower punch 1 were moved to the other open end of the through hole 3a of the die 3, and the compact 10 made of the raw material powder 4 compressed and molded within the through hole 3a was ejected from the die 3 (Figure 3(c): ejection process).
[0025] Table 1 shows the manufacturing conditions of the molded bodies of the examples and comparative examples, and the dimensional difference in diameter between the upper surface side (upper punch side) and the lower surface side (lower punch side) of each blank obtained by sintering the molded body 10 manufactured by each example and comparative example. The dimensional difference of each blank was calculated by measuring the dimensions of the upper surface side and the lower surface side with a micrometer. Also, FIG. 4-1 is a diagram of an image of a pinhole formation state in the blank cross section of Example 1, FIG. 4-2 is a diagram of an image of a pinhole formation state in Comparative Example 2, and FIG. 4-3 is a diagram of an image of a pinhole formation state in the blank cross section of Comparative Example 3. The cross section of the blank is a cross section cut horizontally in the pressure direction of the upper punch and the lower punch during molding (the axial direction of the through hole of the die), and the state of the pinhole was observed and photographed by a stereomicroscope magnification of 100 times. The black dots in the figure indicate pinholes.
[0026] [Table 1]
[0027] From Table 1, Figures 4-1, 4-2 and 4-3, Example 1 has the smallest dimensional difference between the top and bottom surfaces of the blank, and although pinholes are present in the cross section of the blank, the amount is the smallest and they are uniformly distributed throughout the inside of the blank. From the above results, it can be said that the inside of the blank (molded body 10) has a uniform density throughout, there is little difference in density distribution, and a good molded body 10 was obtained.
[0028] In Example 2, the dimensional difference between the upper and lower surfaces of the blank is moderate compared to the other examples, and the dimensional difference is large compared to Example 1. In Example 1 and Example 2, the total movement amount of the upper punch 2 is the same, but in Example 2, the movement amount of the upper punch 2 in the first pressurizing step is reduced and the movement amount of the upper punch 2 in the third pressurizing step is increased compared to Example 1. The upper diameter of the blank in Example 2 is larger than the lower diameter. This is considered to be due to the fact that in the first pressurizing step, the raw material powder 4 in a state where the raw material powder is filled in the recess formed by the die 3 and the lower punch 1 is pressed, whereas in the third pressurizing step, the raw material powder 4 in a state compressed to some extent through the first pressurizing step and the second pressurizing step is pressed. The state of the pinholes is not shown, but the number and distribution were the same as in Example 1. In Example 2, the dimensional difference between the top and bottom surfaces of the blank is larger than in Example 1, and therefore the density difference inside the blank is thought to be large; however, the dimensional difference is moderate and the pinhole condition is the same as in Example 1, so the density distribution difference within the molded body 10 is not very large, and it can be said that a good molded body 10 was obtained.
[0029] In Comparative Example 1, the compact broke into two at the center between the upper and lower sides during the compact ejection process, making it impossible to mold. This is believed to be because the density in the center was low due to the small amount of powder movement in the center of the compact, resulting in a large difference in density between the center and the lower or upper side. In Comparative Example 3, the dimensions of the lower side were larger than those of the upper side, so the density of the lower side was thought to be very high in this comparative example.
[0030] In Comparative Example 2, the movement amount of the lower punch was adjusted in the manufacturing method of Comparative Example 1. In Comparative Example 2, a green body could be manufactured, but the dimensional difference between the upper and lower surfaces of the blank obtained by sintering the green body was 9 μm, and the lower surface was larger. Furthermore, more pinholes were observed than in Example 1. Therefore, it can be seen that the density distribution difference inside the blank is very large.
[0031] In Comparative Example 3, the dimensional difference between the upper and lower surfaces of the blank was smaller than in the other examples. However, the number of pinholes observed was greater than in Example 1, as in Comparative Example 2. From this, it is presumed that, in the manufacturing method of Comparative Example 3, although the outer shape of the blank (molded body 10) can be formed with high precision, the density distribution inside the blank is non-uniform.
[0032] Although specific examples of the method for producing a molded body of the present invention have been described in detail above, these are merely examples, and it goes without saying that they can be appropriately modified and applied within the scope of the gist of the method. For example, in the embodiment, the molded body is produced by sequentially performing the first pressurizing step, the second pressurizing step, and the third pressurizing step, but the third step may include a step of further compressing the raw material powder. Even in this case, by pressing the raw material powder by moving the upper punch and the lower punch alternately multiple times, the movement of the raw material powder located in the center of the molded body, where movement is difficult, can be promoted, and the density distribution difference inside the molded body can be reduced. [Explanation of symbols]
[0033] 1 Lower punch 2 Upper punch 3 Die 3a Through hole 4 Raw material powder 10 Molded body
Claims
[Claim 1] A method for manufacturing a molded body, comprising the steps of: filling a raw material powder into a space formed by a through hole provided in a die and a first punch inserted into the through hole; inserting a second punch into the through hole so as to face the first punch; and relatively moving the first punch and the second punch to compress and mold the raw material powder, a first pressurizing step of moving the second punch by a first predetermined distance from a position where the second punch contacts the raw material powder toward the first punch; a second pressing step of moving the first punch toward the second punch by a second predetermined amount; a third pressurizing step of moving the second punch toward the first punch by a third predetermined amount; and a discharge step of discharging the molded body from the die, The first pressurizing step, the second pressurizing step, the third pressurizing step, and the discharging step are sequentially performed; the first predetermined amount, the second predetermined amount, and the third predetermined amount satisfy a magnitude relationship of the third predetermined amount < the first predetermined amount < the second predetermined amount, the third predetermined amount is 0.1 to 0.15 times the second predetermined amount; The ejection step ejects the compact from an open end of a through hole provided in the die on the second punch side. The method for producing a molded body comprising the steps of:
Citation Information
Patent Citations
Oil feeding nozzle
JP1977036315A
Bidirectional simultaneous compressing apparatus for powder molding press
JP1982007399A
Method for forming green compact from powder
JP2001003104A
Wet molding method for magnet, wet molding device and rare earth sintered magnet
JP2001049303A
Method of manufacturing permanent magnet
JP2003272942A