SiC substrate, SiC epitaxial substrate, SiC ingot, and manufacturing method thereof
A heat treatment process addresses defects in SiC substrates and epitaxial layers by removing strained layers and basal plane dislocations, improving the quality and reliability of SiC semiconductor devices.
Patent Information
- Application Number
- JP2021537362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-06
- Filing Date
- 2020-08-05
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-08-05
AI Technical Summary
SiC substrates and epitaxial layers suffer from crystal defects such as basal plane dislocations (BPD) and step bunching, which adversely affect the performance and reliability of SiC semiconductor devices.
A heat treatment process involving strained layer removal, bunching removal, and basal plane dislocation reduction steps is applied to SiC substrates, utilizing a semi-closed space and temperature gradients to etch and grow high-quality SiC substrates and epitaxial layers, reducing or eliminating defects like BPD and step bunching.
The process results in high-quality SiC substrates and epitaxial layers with reduced defects, enhancing the operational performance and reliability of SiC semiconductor devices.
Smart Images

Figure 0007578870000003 
Figure 0007578870000004 
Figure 0007578870000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-quality SiC substrate, a SiC epitaxial substrate, a SiC ingot, and methods for producing these. [Background technology]
[0002] SiC (silicon carbide) semiconductor devices are capable of higher voltage resistance, higher efficiency, and higher temperature operation than Si (silicon) and GaAs (gallium arsenide) semiconductor devices, and therefore their development is underway with the aim of industrialization.
[0003] However, many crystal defects and dislocations still exist in SiC substrates and SiC epitaxial substrates on which SiC epitaxial layers (hereinafter referred to as epilayers) are grown, and these have a detrimental effect on the characteristics of SiC semiconductor devices.
[0004] For example, basal plane dislocations (BPDs) in epitaxial layers expand into stacking faults when SiC semiconductor devices are operated in bipolar mode. These stacking faults increase the on-voltage of SiC semiconductor devices and lead to bipolar degradation, so there is a strong demand for technology to reduce BPDs in SiC substrates and epitaxial layers.
[0005] To address these problems, various techniques have been proposed for converting BPDs into Threading Edge Dislocations (TEDs).For example, Patent Documents 1 and 2 describe techniques for forming pits corresponding to dislocations contained in a SiC substrate and performing epitaxial growth on the surface on which the pits are formed, thereby reducing the density of BPDs in the epilayer.
[0006] In addition, during the device manufacturing process, the formation of step bunching, which is caused by the bunching of steps on the surface of the SiC substrate, is considered to be a problem, and it is known that this step bunching has a detrimental effect on the characteristics of SiC semiconductor devices.
[0007] Specifically, when epitaxial growth is performed on a surface on which step bunching has been formed, defects due to step bunching may occur on the surface of the epitaxial layer. In addition, in MOSFETs in which an oxide film is formed on the epitaxial layer surface and current is passed through the interface, the presence of step bunching may have a fatal effect on the operating performance and reliability.
[0008] In response to such problems, various techniques have been proposed to suppress the occurrence of step bunching. For example, Patent Document 1 describes a technique for etching the surface of a SiC substrate to obtain a molecular level flat surface by "a heat treatment process including a heat treatment process in which the single crystal silicon carbide substrate is stored in a storage container made of tantalum metal and fitted at the top and bottom so as to expose the tantalum carbide layer to the internal space, and the storage container is uniformly heated at a temperature of 1500°C to 2300°C while maintaining the internal pressure of the storage container higher than the external pressure and in a vacuum under the saturated vapor pressure of silicon." [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Special Publication No. 2007-506289 [Patent Document 2] JP 2017-71525 A [Patent Document 3] JP 2008-16691 A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a new technique capable of producing high-quality SiC substrates, SiC epitaxial substrates, and SiC ingots. [Means for solving the problem]
[0011] The present invention, which solves the above-mentioned problems, is a method for manufacturing a SiC substrate, which includes a heat treatment step of heat-treating an original SiC substrate, the heat treatment step including two or more of the following steps (a), (b), and (c): (a) a strained layer removing step of removing the strained layer of the SiC base substrate; (b) a bunching removal step for removing macrostep bunching on the SiC substrate (c) a basal plane dislocation reduction step of forming a growth layer having reduced basal plane dislocations on the original SiC substrate;
[0012] In this manner, by including two or more steps among the strained layer removing step, the bunching removing step, and the basal plane dislocation reducing step, a higher quality SiC substrate can be manufactured.
[0013] In a preferred embodiment of the present invention, the heat treatment step is a step of heat treating the original SiC substrate in a semi-closed space in which a SiC material is exposed. In this way, by performing the heat treatment process in a semi-closed space where the SiC material is exposed, a higher quality SiC substrate can be manufactured.
[0014] In a preferred embodiment of the present invention, the heat treatment step is a step of heat treating the original SiC substrate in a main body container made of a SiC material. In this way, by carrying out the heat treatment process in a main body vessel made of SiC material, each process (strained layer removal process, bunching removal process, basal plane dislocation reduction process) can be carried out in the same equipment system.
[0015] In a preferred embodiment of the present invention, the heat treatment step is a step of disposing the original SiC substrate and the SiC material so as to face each other, and heating the original SiC substrate and the SiC material so as to form a temperature gradient between the original SiC substrate and the SiC material. In this way, by transporting the raw material between the original SiC substrate and the SiC material using the temperature gradient, a higher quality SiC substrate can be manufactured.
[0016] In a preferred embodiment of the present invention, the strained layer removing step is a step of placing the original SiC substrate and the SiC material opposite to each other and heating the original SiC substrate to a low temperature side and the SiC material to a high temperature side. In this manner, by etching the original SiC substrate using the temperature gradient as a driving force, it is possible to manufacture a SiC substrate in which the strained layer has been removed or reduced.
[0017] In a preferred embodiment of the present invention, the bunching removal step includes a step of arranging the SiC original substrate and the SiC material so as to face each other, and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so as to form a temperature gradient between the SiC original substrate and the SiC material. In this way, by heat-treating the original SiC substrate using the temperature gradient as a driving force in a SiC-Si equilibrium vapor pressure environment, it is possible to manufacture a high-quality SiC substrate in which macrostep bunching is eliminated or reduced.
[0018] In a preferred embodiment of the present invention, the bunching removal step includes a step of placing the SiC original substrate and the SiC material opposite each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate and the SiC material so as to form a temperature gradient between the SiC original substrate and the SiC material. In this way, by heat treating the SiC substrate in a quasi-closed space in which the atomic ratio Si / C exceeds 1, a high-quality SiC seed crystal in which macrostep bunching is eliminated or reduced can be produced.
[0019] In a preferred embodiment of the present invention, the bunching removal step includes a step of disposing the SiC original substrate and the SiC material opposite to each other, and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so that the SiC original substrate is on the high temperature side and the SiC material is on the low temperature side. In addition, in a preferred embodiment of the present invention, the bunching removal step includes a step of arranging the SiC original substrate and the SiC material opposite to each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate to be on the high temperature side and the SiC material to be on the low temperature side. In this manner, by etching the original SiC substrate in a SiC-Si equilibrium vapor pressure environment or in a space in which the atomic ratio Si / C exceeds 1, a high-quality SiC substrate in which macrostep bunching is eliminated or reduced can be manufactured (etching bunching removal process).
[0020] In a preferred embodiment of the present invention, the bunching removal step includes a step of disposing the SiC original substrate and the SiC material opposite to each other, and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so that the SiC original substrate is on the low temperature side and the SiC material is on the high temperature side. In addition, in a preferred embodiment of the present invention, the bunching removal step includes a step of placing the SiC original substrate and the SiC material opposite each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate to be on the low temperature side and the SiC material to be on the high temperature side. In this way, by growing the crystal of the SiC original substrate in a SiC-Si equilibrium vapor pressure environment or in a space in which the atomic ratio Si / C exceeds 1, a high-quality SiC substrate in which macro-step bunching is eliminated or reduced can be manufactured (growth bunching removal process).
[0021] In a preferred embodiment of the present invention, the basal plane dislocation reduction step includes a step of disposing the SiC original substrate and the SiC material opposite to each other, and heating the SiC original substrate and the SiC material in a SiC-C equilibrium vapor pressure environment so that the SiC original substrate is on the high temperature side and the SiC material is on the low temperature side. In addition, in a preferred embodiment of the present invention, the basal plane dislocation reduction step includes a step of placing the SiC original substrate and the SiC material opposite each other in a quasi-closed space having an atomic ratio Si / C of 1 or less, and heating the SiC original substrate to be on the high temperature side and the SiC material to be on the low temperature side. In this way, basal plane dislocations can be converted to other dislocations with high efficiency by growing the crystal of the original SiC substrate in a SiC-C equilibrium vapor pressure environment or in a space where the atomic ratio Si / C is 1 or less. This makes it possible to manufacture a SiC substrate in which basal plane dislocations exposed on the surface are removed or reduced.
[0022] In a preferred embodiment of the present invention, the doping concentration of the SiC material is lower than the doping concentration of the original SiC substrate. In this way, by using a SiC material with a lower doping concentration than the SiC base substrate, a growth layer that functions as a voltage-resistant layer can be formed, i.e., an epitaxial layer can be formed.
[0023] In a preferred embodiment of the present invention, the doping concentration of the SiC material is 1×10 17 cm -3 The following is the result. By using a SiC material with such a doping concentration, a grown layer with a doping concentration suitable for a voltage-resistant layer can be formed.
[0024] In a preferred embodiment of the present invention, the heat treatment step includes the bunching removal step followed by the strained layer removal step. In this manner, by carrying out the bunching removal process on the surface of the original SiC substrate from which the strained layer has been removed, a high-quality SiC substrate from which the strained layer and macrostep bunching have been removed or reduced can be manufactured.
[0025] In a preferred embodiment of the present invention, the heat treatment step includes the bunching removal step followed by the basal plane dislocation reduction step. In this way, by performing the basal plane dislocation reduction process on the surface of the original SiC substrate from which macrostep bunching has been removed, a high-quality SiC substrate having a growth layer from which basal plane dislocations have been removed can be manufactured.
[0026] In a preferred embodiment of the present invention, the heat treatment step includes the bunching removal step subsequent to the basal plane dislocation reduction step. In this way, by subjecting the growth layer from which basal plane dislocations have been removed or reduced to the bunching removal process, a high-quality SiC substrate having a growth layer from which basal plane dislocations and macrostep bunching have been removed or reduced can be manufactured.
[0027] The present invention also relates to a SiC substrate manufactured by the above-mentioned manufacturing method. The SiC substrate of the present invention has one or more of the following characteristics that adversely affect the characteristics of SiC semiconductor devices: strained layer, macro step bunching, and basal plane dislocations removed or reduced, which can contribute to improving the operating performance and reliability of SiC semiconductor devices.
[0028] The present invention also relates to a method for producing a SiC epitaxial substrate, which includes an epitaxial growth step of growing an epilayer on the above-mentioned SiC substrate. In this way, epitaxial growth is performed using a SiC substrate with a good surface in which one or more of the following are reduced: strained layer, basal plane dislocations, and macro step bunching. This makes it possible to suppress the generation and propagation of defects, and to manufacture a higher quality SiC epitaxial substrate. The present invention also relates to a SiC epitaxial substrate manufactured by the above-mentioned manufacturing method.
[0029] The present invention also relates to a method for producing a SiC ingot, which includes an ingot growing step of growing single crystal SiC on the above-mentioned SiC substrate. In this way, the ingot is grown using a SiC substrate with a good surface where one or more of the following are reduced: strained layer, basal plane dislocation, and macro step bunching. This makes it possible to suppress the generation and propagation of defects, and to produce a higher quality SiC ingot. The present invention also relates to a SiC ingot produced by the above-mentioned production method. Effect of the Invention
[0030] According to the present invention, it is possible to manufacture a SiC substrate having a good surface with reduced strained layers, basal plane dislocations, and macrostep bunching, and therefore it is possible to provide a high-quality SiC epitaxial substrate and a high-quality SiC ingot.
[0031] Other objects, features and advantages will become apparent from a reading of the following detailed description when taken in conjunction with the drawings and the claims. [Brief description of the drawings]
[0032] [Figure 1] 1 is a schematic diagram of a manufacturing process of a SiC substrate, a SiC epitaxial substrate, and a SiC ingot according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a conceptual diagram showing a preferred embodiment of the heat treatment step of the present invention. [Diagram 3] FIG. 2 is an explanatory diagram showing an outline of an etching mechanism in a heat treatment step of the present invention. [Figure 4] FIG. 2 is an explanatory diagram showing an overview of the growth mechanism in the heat treatment process of the present invention. [Diagram 5] FIG. 2 is a schematic diagram of a main container and a high melting point container according to an embodiment. [Figure 6] FIG. 2 is an explanatory diagram of an apparatus for producing a SiC seed crystal according to one embodiment. [Figure 7] FIG. 2 is a schematic diagram showing a vessel configuration in a preferred embodiment of the heat treatment step of the present invention. [Figure 8] FIG. 13 is a diagram showing an outline of a strained layer removing step. [Figure 9] FIG. 1 is a diagram showing an apparatus configuration for implementing a strained layer removal step. [Figure 10] FIG. 1 is a diagram showing an outline of an etching bunching removal process. [Figure 11] FIG. 1 is a diagram showing an apparatus configuration for implementing an etching bunching removal process. [Figure 12] FIG. 13 is an explanatory diagram showing an overview of a growth bunching removal process. [Figure 13] FIG. 1 is a diagram showing an apparatus configuration and overview for implementing a growth bunching removal process. [Figure 14] FIG. 1 is an explanatory diagram showing an overview of a basal plane dislocation reduction process. [Figure 15] FIG. 1 is a diagram showing an apparatus configuration and overview for implementing a basal plane dislocation reduction process. [Figure 16]A preferred embodiment of the process for producing a SiC substrate, a SiC epitaxial substrate, and a SiC ingot of the present invention will be described. [Figure 17] 2 is an explanatory diagram of a SiC substrate obtained in the strained layer removing step of the present invention. FIG. [Figure 18] FIG. 2 is an explanatory diagram of a SiC substrate obtained in the etching bunching removal step of the present invention. [Figure 19] FIG. 2 is an explanatory diagram of a SiC substrate obtained in the growth bunching removal step of the present invention. [Figure 20] FIG. 2 is an explanatory diagram of a method for determining the BPD conversion rate in the basal plane dislocation reduction process of the present invention. [Figure 21] FIG. 2 is an explanatory diagram of a growth layer formed in the crystal growth process of the present invention. [Figure 22] 1 is an Arrhenius plot of the etching process and the crystal growth process of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] <1> Summary of the Invention The preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The technical scope of the present invention is not limited to the embodiments shown in the accompanying drawings, and may be modified as appropriate within the scope of the claims.
[0034] First, with reference to FIG. 1, an overview of the production of a SiC substrate 11, a SiC epitaxial substrate 12, and a SiC ingot 13 by the method of the present invention will be described.
[0035] A feature of the present invention is to obtain a high-quality SiC substrate 11 by performing a heat treatment step S1 on the original SiC substrate 10. By performing the heat treatment step S1 on the original SiC substrate 10, a high-quality SiC substrate 11 can be obtained in which at least one of distortion (strained layer 101), basal plane dislocations (BPD), and macro step bunching (MSB) is removed or reduced. When the heat treatment step S1 includes a crystal growth step for forming growth layer 105 that serves as a voltage-resistant layer, a high-quality SiC epitaxial substrate can be obtained.
[0036] Moreover, since the strained layer 101, BPDs, and MSBs are removed or reduced from the SiC substrate 11 after the heat treatment step S1, the SiC substrate 11 is suitable for growing a high-quality SiC epitaxial substrate 12 or a SiC ingot 13. That is, in the present invention, by performing the epitaxial growth step S2 and the ingot growth step S3 for growing single crystal SiC on the SiC substrate 11, a high-quality SiC epitaxial substrate 12 or a SiC ingot 13 can be manufactured. Each of the configurations of the present invention will be described in further detail below.
[0037] <2> SiC substrate 10 The SiC base substrate 10 may be, for example, a single crystal SiC processed into a thin plate. Specifically, it may be a SiC wafer sliced into a disk shape from a SiC ingot produced by a sublimation method or the like. Note that any polytype may be used as the crystal polytype of the single crystal SiC.
[0038] Typically, a SiC substrate 10 that has been subjected to mechanical processing (e.g., slicing, grinding, and polishing) or laser processing has a strained layer 101 in which processing damage such as scratches 1011, latent scratches 1012, and distortions 1013 has been introduced, and a bulk layer 102 in which such processing damage has not been introduced (see FIG. 8).
[0039] The presence or absence and depth of this strained layer 101 can be confirmed by SEM-EBSD, TEM, μXRD, Raman spectroscopy, etc. In order to manufacture a high-quality SiC epitaxial substrate 12 or SiC ingot 13, it is preferable to remove the strained layer 101 and expose the bulk layer 102 that is not damaged by processing.
[0040] A step-terrace structure is confirmed on the surface of the atomically flattened SiC substrate 10. This step-terrace structure is a staircase structure in which steps 103, which are step portions of one molecular layer or more, and terraces 104, which are flat portions where the {0001} plane is exposed, are arranged alternately (see FIGS. 10 and 12).
[0041] The step 103 has a minimum height (minimum unit) of one molecular layer (0.25 nm), and various step heights are formed by stacking multiple monolayers. In the description in this specification, the step 103 bunches up and becomes huge, and has a height exceeding one unit cell of each polytype, and is called an MSB.
[0042] That is, the MSB refers to a step 103 bunched beyond four molecular layers (five molecular layers or more) in the case of 4H-SiC, and refers to a step 103 bunched beyond six molecular layers (seven molecular layers or more) in the case of 6H-SiC.
[0043] It is desirable that the MSB is not formed on the surface of the SiC substrate 10 because the MSB causes defects during epitaxial growth and is one of the factors that impair the reliability of the oxide film of a MOSFET.
[0044] In addition, BPDs are found in the commercially available SiC substrate at a density of several hundred to several thousand particles per cm. 2 It is known that many of these BPDs are converted to TEDs during epitaxial growth. However, some of the BPDs are present at a density of 0.1 to several particles / cm. 2 Since the BPDs deteriorate the reliability of the SiC semiconductor device, it is desirable that the BPDs are not exposed on the surface of the SiC substrate 11.
[0045] The dopant may be any element that is generally doped into the SiC base substrate 10. Specifically, nitrogen (N), phosphorus (P), aluminum (Al), boron (B), etc. are preferable.
[0046] The doping concentration of the SiC substrate 10 is preferably 1×10 17 cm -3 Higher concentrations, preferably 1×10 18 cm -3 More preferably, it is 1×10 19 cm -3 That's all.
[0047] The dopants and doping concentrations can be confirmed by Raman spectroscopy or secondary ion mass spectrometry (SIMS).
[0048] In the SiC substrate 10 and the SiC substrate 11, the surface on which the semiconductor element is to be formed (specifically, the surface on which the epitaxial layer is to be deposited) is referred to as the main surface. The surface opposite to the main surface is referred to as the back surface. The main surface and the back surface are collectively referred to as the front surface.
[0049] The main surface may be, for example, a surface having an off angle of several degrees (e.g., 0.4 to 8°) from the (0001) or (000-1) plane (in this specification, in the notation of Miller indices, "-" refers to a bar attached to the index immediately following it).
[0050] <3> Heat treatment process S1 The heat treatment process S1 includes two or more steps selected from the following steps: a strained layer removal process S11 for removing the strained layer 101 of the SiC original substrate 10; a bunching removal process S12 for removing the MSBs on the SiC original substrate 10; and a basal plane dislocation reduction process S13 for forming a growth layer 105 with reduced BPDs on the SiC original substrate 10.
[0051] The SiC substrate 11 that has been subjected to this heat treatment step S1 has a surface from which at least one of the distortion (strained layer 101), BPDs, and MSBs has been removed or reduced. Therefore, in the subsequent steps of the epitaxial growth step S2 and the ingot growth step S3, it is possible to suppress the occurrence of defects due to the distortion, BPDs, and MSBs of the SiC substrate 11, or the inheritance of the defects. In other words, it is possible to manufacture a high-quality SiC epitaxial substrate 12 and a SiC ingot 13.
[0052] Specifically, the heat treatment step S1 may be exemplified by heating the SiC original substrate 10 and the SiC material while facing each other. That is, the heat treatment step S1 may include an etching step of transporting Si and C elements from the SiC original substrate 10 to the SiC material to etch the SiC original substrate 10, and a crystal growth step of transporting Si and C elements from the SiC material to the SiC original substrate 10 to grow the SiC original substrate 10 as a crystal. The specific form of the heat treatment step S1 is not particularly limited as long as it is a step that can remove or reduce the strained layer 101, BPDs, and MSBs contained in the SiC base substrate 10.
[0053] As a driving force for transporting the Si element and the C element in the etching process and the crystal growth process, a temperature gradient or a chemical potential difference provided between the SiC substrate 10 and the SiC material can be used.
[0054] The SiC material is made of SiC that can receive or transfer Si and C elements between the SiC original substrate 10 and the SiC original substrate 10 by heating the SiC material against the SiC original substrate 10. For example, a container (main container 20) made of SiC or a substrate (SiC member) made of SiC can be used. Note that any polytype can be used as the crystal polymorph of this SiC material, and polycrystalline SiC may also be used.
[0055] The dopant may be the same element as that of the SiC base substrate 10. Specifically, nitrogen (N), phosphorus (P), aluminum (Al), boron (B), etc. are preferable.
[0056] The doping concentration of the SiC material is preferably set to be lower than the doping concentration of the SiC base substrate 10. The value of this doping concentration is preferably 1×10 17 cm -3 More preferably, it is 1×10 16 cm -3 More preferably, it is 1×10 15 cm -3 The following is the result.
[0057] The dopants and doping concentrations can be confirmed by Raman spectroscopy or secondary ion mass spectrometry (SIMS).
[0058] The original SiC substrate 10 and the SiC material are preferably placed in a semi-closed space and heated. By receiving or transferring the Si element and the C element in the semi-closed space, the surface of the original SiC substrate 10 can be etched and grown to form a surface in which at least one of the strained layer 101, the BPD, and the MSB is removed or reduced. In this specification, the term "semi-closed space" refers to a space in which it is possible to evacuate the inside of the container, but which is capable of containing at least a portion of the steam generated within the container.
[0059] A preferred embodiment of the heat treatment step S1 will be described in detail below with reference to FIGS. A preferred embodiment of the heat treatment step S1 can be roughly divided into an etching step for etching the surface of the SiC base substrate 10 and a crystal growth step for growing crystals on the surface of the SiC base substrate 10 (see FIG. 2).
[0060] (Etching process) According to the etching step (the step located on the left side of FIG. 2), the strained layer 101 and MSB present on the surface of the SiC original substrate 10 can be removed or reduced.
[0061] 3 is an explanatory diagram showing an outline of the etching process. In this etching process, the SiC substrate 10 is placed in a semi-closed space where the SiC material is exposed, and heated at a temperature range of 1400° C. to 2300° C., whereby the following reactions 1) to 5) are continuously carried out, and as a result, etching proceeds.
[0062] 1) SiC(s) → Si(v) + C(s) 2) 2C(s)+Si(v)→SiC2(v) 3) C(s)+2Si(v) → Si2C(v) 4) Si(v) + SiC2(v) → 2SiC(s) 5) Si2C(v) → Si(v) + SiC(s)
[0063] Description of 1): When the SiC substrate 10 (SiC(s)) is heated, Si atoms (Si(v)) are desorbed from the surface of the SiC substrate 10 by thermal decomposition (Si atom sublimation process). Explanation of 2) and 3): The C (C(s)) remaining on the surface of the SiC substrate 10 due to the desorption of Si atoms (Si(v)) reacts with the Si vapor (Si(v)) in the semi-closed space. As a result, the C (C(s)) becomes Si2C or SiC2, etc., and sublimes from the surface of the SiC substrate 10 (C atom sublimation process). Explanation of 4) and 5): Sublimated Si2C or SiC2, etc., reach the SiC material in the semi-closed space due to the temperature gradient and grow.
[0064] Thus, the etching process includes a Si atom sublimation process in which Si atoms are thermally sublimated from the surface of the SiC original substrate 10, and a C atom sublimation process in which C atoms remaining on the surface of the SiC original substrate 10 are sublimated from the surface of the SiC original substrate 10 by reacting with Si vapor in the quasi-closed space.
[0065] Preferably, in the etching process, the SiC substrate 10 is heated to be located on the high temperature side of the temperature gradient, and the SiC material is heated to be located on the low temperature side of the temperature gradient, so that an etching space X is formed between the SiC substrate 10 and the SiC material, and the surface of the SiC substrate 10 can be etched using the temperature gradient as a driving force.
[0066] (Crystal growth process) According to the crystal growth process (the process located on the right side of FIG. 2), the BPDs on the surface of the original SiC substrate 10 can be converted into other dislocations, and the BPDs exposed on the surface of the SiC substrate 11 can be removed or reduced. Moreover, the MSB formed on the surface of the SiC substrate 11 can be removed or reduced.
[0067] 4 is an explanatory diagram showing an overview of the crystal growth process. In this crystal growth process, the SiC substrate 10 is placed in a semi-closed space where the SiC material is exposed, and is heated at a temperature range of 1400° C. to 2300° C., whereby the following reactions 1) to 5) are continuously carried out, which is considered to result in the progress of crystal growth.
[0068] 1) Poly-SiC(s) → Si(v) + C(s) 2) 2C(s)+Si(v)→SiC2(v) 3) C(s)+2Si(v) → Si2C(v) 4) Si(v) + SiC2(v) → 2SiC(s) 5) Si2C(v) → Si(v) + SiC(s)
[0069] Explanation of 1): When SiC material (Poly-SiC(s)) is heated, Si atoms (Si(v)) are released from the SiC through thermal decomposition. Explanation of 2) and 3): The remaining C (C(s)) reacts with the Si vapor (Si(v)) in the semi-closed space after the Si atom (Si(v)) is removed. As a result, the C (C(s)) becomes Si2C or SiC2, etc., and sublimes into the semi-closed space. Explanation of 4) and 5): The sublimated Si2C or SiC2, etc., reaches and diffuses onto the terraces of the SiC original substrate 10 due to the temperature gradient (or chemical potential difference), and when it reaches the steps, it grows while inheriting the polytype of the underlying SiC original substrate 10 (step-flow growth).
[0070] Thus, the crystal growth process includes a Si atom sublimation process in which Si atoms are thermally sublimated from the surface of the SiC material, a C atom sublimation process in which C atoms remaining on the surface of the SiC material are reacted with Si vapor in the quasi-closed space to be sublimated from the surface of the SiC material, a raw material transport process in which raw materials (Si atoms and C atoms) are transported to the surface of the SiC original substrate 10 using a temperature gradient or a chemical potential difference as a driving force, and a step-flow growth process in which the raw materials reach the steps of the SiC substrate 10 and grow.
[0071] The raw materials referred to here include Si element, C element, and dopant. Therefore, the dopant of the SiC material is transported together with the Si element and C element, so that the growth layer 105 grows with the doping concentration of the SiC material. Therefore, by adopting a SiC material with a doping concentration suitable for the voltage-resistant layer (epilayer), the SiC epitaxial substrate 12 can be manufactured in the heat treatment step S1.
[0072] Preferably, in the crystal growth step, the SiC material is heated to be located on the high temperature side of the temperature gradient, and the SiC base substrate 10 is heated to be located on the low temperature side of the temperature gradient. This forms a source supply space Y between the SiC base substrate 10 and the SiC material, and the SiC base substrate 10 can be crystal-grown using the temperature gradient as a driving force.
[0073] When single crystal SiC is used for the SiC substrate 10 and polycrystalline SiC is used for the SiC material, the partial pressure difference (chemical potential difference) generated on the surfaces of the polycrystalline SiC and single crystal SiC can be used as the driving force for transporting the raw materials to grow the crystals. In this case, a temperature gradient may or may not be provided.
[0074] Up to this point, the heat treatment step S1 has been roughly divided into an etching step and a crystal growth step, but the heat treatment step S1 can also be divided into two steps from the viewpoint of the environment in which the SiC substrate 10 is heated.
[0075] That is, as shown in the vertical direction of FIG. 2, the heat treatment step S1 can be classified into a form in which the SiC base substrate 10 is heated in a SiC-Si equilibrium vapor pressure environment and a form in which the SiC-C equilibrium vapor pressure environment is heated.
[0076] Here, the SiC-Si equilibrium vapor pressure environment refers to a vapor pressure environment in which SiC (solid) and Si (liquid phase) are in phase equilibrium via the gas phase. In addition, the SiC-C equilibrium vapor pressure environment refers to a vapor pressure environment when SiC (solid phase) and C (solid phase) are in phase equilibrium via the gas phase.
[0077] In this specification, the SiC-Si equilibrium vapor pressure environment and the SiC-C equilibrium vapor pressure environment include a near-thermal equilibrium vapor pressure environment that satisfies the relationship between growth rate and growth temperature derived from a theoretical thermal equilibrium environment.
[0078] The atomic ratio Si / C in the gas phase of the SiC-Si equilibrium vapor pressure environment is greater than the atomic ratio Si / C in the gas phase of the SiC-C equilibrium vapor pressure environment.
[0079] The SiC-Si equilibrium vapor pressure environment can be formed by placing and heating the original SiC substrate 10 in a semi-closed space in which the atomic ratio Si / C exceeds 1. For example, when the original SiC substrate 10 satisfying a stoichiometric ratio of 1:1, a SiC material satisfying a stoichiometric ratio of 1:1, and a Si vapor supply source (Si pellets, etc.) are placed in a SiC container (main container 20) that satisfies a stoichiometric ratio of 1:1, the atomic ratio Si / C in the semi-closed space exceeds 1.
[0080] The SiC-C equilibrium vapor pressure environment can be formed by placing and heating the original SiC substrate in a semi-closed space in which the atomic ratio Si / C is equal to or less than 1. For example, when an original SiC substrate 10 having a stoichiometric ratio of 1:1 and an SiC material having a stoichiometric ratio of 1:1 are placed in a SiC container (main container 20) having a stoichiometric ratio of 1:1, the atomic ratio Si / C in the main container 20 is 1. Alternatively, the atomic ratio Si / C may be set to 1 or less by placing a C vapor supply source (C pellets, etc.).
[0081] As described above, the heat treatment process S1 can be classified according to whether it is an etching process or a crystal growth process, and whether it is a heat treatment in a SiC-Si equilibrium vapor pressure environment or a SiC-C equilibrium vapor pressure environment. By linking the combination of these classifications with the effects, it can be classified into the following four types.
[0082] In the case where the etching process is performed under a SiC-C equilibrium vapor pressure environment, the strained layer 101 of the SiC substrate 10 can be removed by etching, and MSBs are formed on the surface after etching. Therefore, this process is classified as an etching bunching process S111 (lower left of FIG. 2).
[0083] In the embodiment where the etching step is performed under a SiC-Si equilibrium vapor pressure environment, the strained layer 101 of the SiC original substrate 10 can be removed by etching, and no MSB is formed on the surface after etching. Therefore, this step is classified as an etching bunching removal step S121 (upper left in FIG. 2).
[0084] In addition, since the etching bunching step S111 and the etching bunching removing step S121 can remove or reduce the strained layer 101 of the SiC original substrate 10, they are collectively classified as the strained layer removing step S11 (left side of FIG. 2).
[0085] In the case where the crystal growth process is performed under a SiC-Si equilibrium vapor pressure environment, it is possible to form a growth layer 105 on the SiC original substrate 10, and no MSB is formed on the surface of the growth layer 105. Therefore, this is classified as a growth bunching removal process S122 (upper right in FIG. 2).
[0086] In addition, the etching bunching removal step S121 and the growth bunching removal step S122 can remove or reduce MSBs, so they are collectively classified as the bunching removal step S12 (upper side of FIG. 2).
[0087] In the case where the crystal growth step is performed under a SiC-C equilibrium vapor pressure environment, it is possible to remove or reduce BPDs in the growth layer 105. Therefore, this is classified as a basal plane dislocation reduction step S13 (lower right of FIG. 2).
[0088] In addition, in the embodiment in which the crystal growth process (growth bunching removal process S122 and basal plane dislocation reduction process S13) is performed, it is possible to manufacture the SiC epitaxial substrate 12. That is, the heat treatment process S1 includes a crystal growth process using a SiC material having a lower doping concentration than the SiC original substrate 10, so that the growth layer 105 that becomes the voltage-resistant layer can be formed.
[0089] (manufacturing equipment) Next, the configuration of a manufacturing apparatus capable of realizing the above-mentioned four types of classification will be described. Hereinafter, as a preferred embodiment, a form using a main body container 20 capable of heat-treating a SiC base substrate 10 in an atmosphere containing Si and C elements will be described. Naturally, any device configuration that forms an environment similar to that of the main body container 20 can be adopted. Specifically, any device configuration that can form an atmosphere of Si and C elements in a semi-closed space can be adopted.
[0090] The main container 20 is preferably configured such that the SiC material is exposed in the internal space. In this embodiment, the entire main container 20 is made of a SiC material (polycrystalline SiC). By heating the main container 20 made of such a material, an atmosphere containing Si elements and C elements can be generated inside (semi-closed space).
[0091] The environment in the heated main container 20 is preferably a vapor pressure environment of a mixture of gaseous species containing Si element and gaseous species containing C element. Examples of the gaseous species containing Si element include Si, Si2, Si3, Si2C, SiC2, and SiC. Examples of the gaseous species containing C element include Si2C, SiC2, SiC, and C. That is, the SiC-based gas is present in the main container 20.
[0092] Any configuration can be adopted so long as it generates vapor pressure of a gaseous species containing Si element and a gaseous species containing C element in the internal space during heat treatment of main container 20. For example, a configuration in which a SiC material is exposed on a part of the inner surface, or a configuration in which a separate SiC material (such as a substrate made of SiC) is disposed inside main container 20 can be shown.
[0093] The heat treatment step S1 is preferably performed by accommodating the SiC base substrate 10 inside the main container 20 and heating the main container 20 so as to form a temperature gradient inside. Below, the device configuration (main container 20, heating furnace 30, high melting point container 40) when the main container 20 is heated so as to form a temperature gradient inside will be described with reference to Figs. 5 and 6.
[0094] 5, the main container 20 is a fitting container having an upper container 21 and a lower container 22 that can fit together. A minute gap 23 is formed at the fitting portion between the upper container 21 and the lower container 22, and the main container 20 is configured so that the inside of the main container 20 can be evacuated (vacuumed) through this gap 23. In other words, the inside of the main container 20 is a semi-closed space.
[0095] The heating furnace 30 has a configuration capable of heating the main container 20 with a temperature gradient in an atmosphere containing Si elements. Specifically, as shown in Fig. 6, the heating furnace 30 includes a main heating chamber 31 capable of heating the workpiece (such as the SiC base substrate 10) to a temperature of 1000°C to 2300°C, a preheating chamber 32 capable of preheating the workpiece to a temperature of 500°C or higher, a high-melting-point container 40 capable of accommodating the main container 20, and a moving means 33 (moving stage) capable of moving the high-melting-point container 40 from the preheating chamber 32 to the main heating chamber 31.
[0096] The main heating chamber 31 is formed into a regular hexagon in a planar cross-sectional view, and a high-melting point container 40 is placed inside the main heating chamber 31. A heater 34 (mesh heater) is provided inside the main heating chamber 31. A multi-layer heat reflecting metal plate (not shown) is fixed to the side walls and ceiling of the main heating chamber 31. This multi-layer heat reflecting metal plate is configured to reflect heat from the heater 34 toward approximately the center of the main heating chamber 31.
[0097] As a result, within the main heating chamber 31, a heater 34 is arranged to surround the high-melting point container 40 in which the workpiece is housed, and a multi-layer heat-reflecting metal plate is further arranged on the outside of that, thereby making it possible to raise the temperature to a temperature of 1000°C or higher and 2300°C or lower. As the heater 34, for example, a resistance heating type heater or a high-frequency induction heating type heater can be used.
[0098] The heater 34 may be configured to form a temperature gradient in the high melting point container 40. For example, the heater 34 may be configured so that more heaters are arranged on the upper side (or lower side). The heater 34 may be configured so that its width increases toward the upper side (or lower side). Alternatively, the heater 34 may be configured so that the power supplied to it can be increased toward the upper side (or lower side).
[0099] In addition, connected to the main heating chamber 31 are a vacuum forming valve 35 for evacuating the inside of the main heating chamber 31, an inert gas injection valve 36 for introducing an inert gas into the main heating chamber 31, and a vacuum gauge 37 for measuring the degree of vacuum within the main heating chamber 31.
[0100] The vacuum forming valve 35 is connected to a vacuum pump (not shown) that evacuates the inside of the main heating chamber 31 to create a vacuum. By using the vacuum forming valve 35 and the vacuum pump, the degree of vacuum in the main heating chamber 31 is set to, for example, 10 Pa or less, more preferably 1 Pa or less, and further preferably 10 -3 The pressure can be adjusted to be equal to or less than Pa. An example of the vacuum pump is a turbo molecular pump.
[0101] The inert gas injection valve 36 is connected to an inert gas supply source (not shown). The inert gas is injected into the heating chamber 31 by the inert gas injection valve 36 and the inert gas supply source. -5 It can be introduced at a pressure in the range of up to 10,000 Pa. As the inert gas, Ar, He, N2, etc. can be selected.
[0102] The preheating chamber 32 is connected to the main heating chamber 31, and is configured to be able to move the high-melting point container 40 by a moving means 33. The preheating chamber 32 in this embodiment is configured to be able to be heated by the residual heat of the heater 34 of the main heating chamber 31. For example, when the main heating chamber 31 is heated to 2000°C, the preheating chamber 32 is heated to about 1000°C, and degassing of the workpieces (SiC base substrate 10, main container 20, high-melting point container 40, etc.) can be performed.
[0103] The moving means 33 is configured to be capable of placing the high melting point container 40 thereon and moving it between the main heating chamber 31 and the preheating chamber 32. The transfer between the main heating chamber 31 and the preheating chamber 32 by this moving means 33 can be completed in as little as one minute, making it possible to realize a temperature increase / decrease rate of 1 to 1000° C. / min. In this way, since the present manufacturing apparatus can rapidly increase and decrease the temperature, it is possible to observe the surface shape that does not have a history of low-temperature growth during the temperature increase and decrease, which was difficult with conventional apparatus. In addition, in FIG. 6, the preheating chamber 32 is disposed below the main heating chamber 31, but this is not limiting and the chamber may be disposed in any direction.
[0104] Moreover, the moving means 33 according to this embodiment is a moving stage on which the high melting point container 40 is placed. A small amount of heat is released from the contact portion between the moving stage and the high melting point container 40. This allows a temperature gradient to be formed in the high melting point container 40.
[0105] In the heating furnace 30 of this embodiment, since the bottom of the high melting point container 40 is in contact with the moving stage, a temperature gradient is provided such that the temperature decreases from the upper container 41 to the lower container 42 of the high melting point container 40 . The direction of this temperature gradient can be set to any direction by changing the position of the contact part between the moving stage and the high-melting-point container 40. For example, if a hanging type moving stage is used and the contact part is provided on the ceiling of the high-melting-point container 40, heat escapes upward. Therefore, the temperature gradient is set so that the temperature increases from the upper container 41 to the lower container 42 of the high-melting-point container 40. It is preferable that this temperature gradient is formed along the front-to-back direction of the SiC base substrate 10. As described above, the heater 34 may be configured to create a temperature gradient.
[0106] The atmosphere containing Si elements in heating furnace 30 is formed using high melting point container 40 and Si vapor supply source 44. For example, any method capable of forming an atmosphere containing Si elements around main body container 20 can be adopted in the manufacturing apparatus for SiC substrate 11.
[0107] The high-melting-point container 40 is configured to include a high-melting-point material, such as C, which is a general-purpose heat-resistant member, W, Re, Os, Ta, and Mo, which are high-melting-point metals, Ta9C8, HfC, TaC, NbC, ZrC, Ta2C, TiC, WC, and MoC, which are carbides, HfN, TaN, BN, Ta2N, ZrN, and TiN, and HfB2, TaB2, ZrB2, NB2, TiB2, and polycrystalline SiC, which are borides.
[0108] Like the main container 20, the high melting point container 40 is a fitting container including an upper container 41 and a lower container 42 that can fit together, and is configured to be able to house the main container 20. A minute gap 43 is formed at the fitting portion between the upper container 41 and the lower container 42, and it is configured so that the inside of the high melting point container 40 can be evacuated (vacuumed) through this gap 43. That is, like the main container 20, the inside of the high melting point container 40 is preferably a semi-closed space.
[0109] The high-melting-point container 40 has a Si vapor supply source 44 capable of supplying Si vapor into the high-melting-point container 40. The Si vapor supply source 44 may be configured to generate Si vapor in the high-melting-point container 40 during heat treatment. Examples of the Si vapor supply source 44 include solid Si (single crystal Si pieces, Si pellets such as Si powder, etc.) and a Si compound.
[0110] In the manufacturing apparatus for the SiC substrate 11 according to this embodiment, TaC is used as the material of the high-melting-point container 40, and tantalum silicide is used as the Si vapor supply source 44. That is, as shown in Fig. 5, a tantalum silicide layer is formed on the inside of the high-melting-point container 40, and Si vapor is supplied from the tantalum silicide layer into the container during heat treatment. As a result, a Si vapor pressure environment is formed in the high-melting-point container 40, and the main container 20 can be heated in an atmosphere containing Si elements. In addition, any other configuration may be used as long as an atmosphere containing Si elements is formed in the high melting point container 40 during the heat treatment.
[0111] According to the manufacturing apparatus for SiC substrate 11 of this embodiment, main body container 20 is heated in an atmosphere containing Si element (e.g., Si vapor pressure environment), thereby making it possible to prevent gaseous species containing Si element from being exhausted from inside main body container 20. That is, by balancing the vapor pressure of the gaseous species containing Si element inside main body container 20 and the vapor pressure of the gaseous species containing Si element outside main body container 20, the environment inside main body container 20 can be maintained.
[0112] Moreover, in the manufacturing apparatus for SiC substrate 11 according to the present embodiment, main container 20 is made of polycrystalline SiC. With such a configuration, when main container 20 is heated using heating furnace 30, vapor of a gas phase species containing Si element and a gas phase species containing C element can be generated in main container 20.
[0113] (Equipment configuration for implementing heat treatment process S1) The outline of the apparatus configuration for realizing the above-mentioned four types of classification (etching under a SiC-C equilibrium vapor pressure environment (lower left in Fig. 2), etching under a SiC-Si equilibrium vapor pressure environment (upper left in Fig. 2), crystal growth under a SiC-C equilibrium vapor pressure environment (lower right in Fig. 2), and crystal growth under a SiC-Si equilibrium vapor pressure environment (upper right in Fig. 2)) will be described in detail with reference to Fig. 7.
[0114] An outline of the apparatus configuration for implementing the etching process is shown on the left side of Fig. 7. As shown on the left side of Fig. 7, the main body container 20 has an etching space X in which the SiC original substrate 10 is located on the high temperature side of the temperature gradient, and the SiC material (part of the main body container 20) is located on the low temperature side of the temperature gradient. That is, the etching space X is formed by arranging the SiC original substrate 10 at a position where it is hotter than the SiC material (e.g., the bottom surface of the lower container 22) due to the temperature gradient formed by the heating furnace 30.
[0115] The etching space X is a space in which the Si atoms and C atoms on the surface of the SiC substrate 10 are transported to the main container 20 by using the temperature difference between the SiC substrate 10 and the main container 20 as a driving force. For example, the main container 20 is heated so that the temperature of one side of the SiC substrate 10 is higher than that of the lower container 22 when comparing the temperature of the bottom surface of the lower container 22 facing the one side (see the left side of FIG. 7). In this way, by forming a space (etching space X) with a temperature difference between the SiC substrate 10 and the lower container 22, it is possible to transport Si atoms and C atoms using the temperature difference as a driving force and etch one side of the SiC substrate 10 (the open arrow on the right side of FIG. 7 indicates the direction of transport).
[0116] The main container 20 may have a substrate holder 24 provided between the SiC substrate 10 and the main container 20 .
[0117] The heating furnace 30 according to this embodiment is configured to be capable of heating by forming a temperature gradient such that the temperature decreases from the upper container 21 to the lower container 22 of the main container 20. For this reason, a substrate holder 24 capable of holding the SiC substrate 10 may be provided between the SiC substrate 10 and the lower container 22 to form an etching space X between the SiC substrate 10 and the lower container 22.
[0118] The substrate holder 24 may have any configuration as long as it can hold at least a portion of the SiC substrate 10 in the hollow of the main body container 20. For example, any conventional supporting means may be used, such as one-point support, three-point support, a configuration that supports the outer periphery, or a configuration that clamps a portion. The substrate holder 24 may be made of SiC or a high-melting point metal material.
[0119] The substrate holder 24 may not be provided depending on the direction of the temperature gradient of the heating furnace 30. For example, when the heating furnace 30 forms a temperature gradient such that the temperature decreases from the lower vessel 22 to the upper vessel 21, the SiC original substrate 10 may be placed on the bottom surface of the lower vessel 22 (without providing the substrate holder 24).
[0120] Next, an outline of the apparatus configuration for realizing the crystal growth process is shown on the right side of Fig. 7. As shown on the right side of Fig. 7, the main body container 20 has a raw material supply space Y in which the SiC base substrate 10 is located on the low temperature side of the temperature gradient, and the SiC material (part of the main body container 20) is located on the high temperature side of the temperature gradient. That is, the raw material supply space Y is formed by arranging the SiC base substrate 10 at a position where the temperature is lower than that of the SiC material (for example, the bottom surface of the lower container 22) due to the temperature gradient formed by the heating furnace 30.
[0121] That is, in addition to the SiC original substrate 10, a Si atom supply source and a C atom supply source, which are the raw materials, exist in the raw material supply space Y. These are heated to supply Si atoms and C atoms, which are the raw materials for the SiC original substrate 10, into the raw material supply space Y. These Si atoms and C atoms are transported to the surface of the SiC original substrate 10 and recrystallized to form a growth layer 105 (the black arrow on the right side of FIG. 7 indicates the direction of transport).
[0122] In this embodiment, at least a portion of main container 20 is made of polycrystalline SiC (Poly-SiC), so that main container 20 itself serves as a Si atom supply source and a C atom supply source. As the Si atom source and the C atom source, a material capable of supplying Si atoms, such as a Si substrate, a material capable of supplying C atoms, such as graphite, and a material capable of supplying Si atoms and C atoms, such as a SiC substrate, can be used. Moreover, by using a SiC material with a lower doping concentration than the SiC base substrate 10, the growth layer 105 that serves as a voltage-resistant layer can be formed.
[0123] The arrangement of the Si atom supply source and the C atom supply source is not limited to this form, and may be any form capable of supplying Si atoms and C atoms into the raw material supply space Y. When polycrystalline SiC is used as the source material, the vapor pressure difference (chemical potential difference) between polycrystalline SiC (source material) and single-crystalline SiC (SiC base substrate 10) can be used as the growth driving force.
[0124] In addition, a temperature gradient is provided in the source supply space Y such that the temperature decreases toward the SiC substrate 10. This temperature gradient serves as a growth driving force to transport Si atoms and C atoms to the SiC substrate 10, thereby increasing the growth rate of the growth layer (the black arrow on the right side of FIG. 7 indicates the direction of transport).
[0125] Furthermore, in order to allow the Si atoms and the C atoms to efficiently reach the SiC original substrate 10, the Si atom source and the C atom source may be placed close to the SiC original substrate 10. In the configuration on the right side of Fig. 7, an upper vessel 21 made of polycrystalline SiC, which serves as the Si atom source and the C atom source, may be placed close to and parallel to the SiC original substrate 10.
[0126] The distance between the surface of the SiC substrate 10 and the top surface of the upper container 21 is preferably set to 100 mm or less, more preferably 10 mm or less, and even more preferably 2.7 mm or less, and is preferably set to 0.7 mm or more, more preferably 1.2 mm or more, and even more preferably 1.7 mm or more.
[0127] It is preferable that the etching space X and the raw material supply space Y are evacuated (evacuated) via the Si vapor pressure space Z. That is, it is preferable that a main body container 20 having the etching space X and / or the raw material supply space Y is placed in a high-melting point container 40 having the Si vapor pressure space Z, and further, a SiC base substrate 10 is placed in this main body container 20.
[0128] Next, an outline of the apparatus configuration for realizing the SiC-Si equilibrium vapor pressure environment is shown in the upper part of Fig. 7. The SiC-Si equilibrium vapor pressure environment can be created by placing and heating the SiC original substrate 10 in a semi-closed space in which the atomic ratio Si / C exceeds 1, as shown in the upper part of Fig. 7.
[0129] 7, when an SiC original substrate 10 satisfying a stoichiometric ratio of 1:1, a SiC substrate holder 24 satisfying a stoichiometric ratio of 1:1, and a Si vapor supply source 25 (Si pellets, etc.) are placed in a main container 20 made of polycrystalline SiC satisfying a stoichiometric ratio of 1:1, the atomic ratio Si / C in main container 20 exceeds 1. By heating this main container 20, the inside of main container 20 approaches a SiC-Si equilibrium vapor pressure environment.
[0130] The outline of the apparatus configuration for realizing the SiC-C equilibrium vapor pressure environment is shown in the lower part of Fig. 7. The SiC-C equilibrium vapor pressure environment can be created by placing and heating the SiC original substrate 10 in a semi-closed space with an atomic ratio Si / C of 1 or less, as shown in the lower part of Fig. 7.
[0131] 7, when an SiC base substrate 10 satisfying a stoichiometric ratio of 1:1 and a SiC substrate holder 24 satisfying a stoichiometric ratio of 1:1 are placed in a main container 20 made of polycrystalline SiC satisfying a stoichiometric ratio of 1:1, the atomic ratio Si / C in the main container 20 becomes 1 or less than 1. By heating this main container 20, the inside of the main container 20 approaches a SiC-C equilibrium vapor pressure environment.
[0132] Furthermore, in order to reduce the atomic ratio Si / C in main vessel 20, a C vapor supply source may be separately arranged, or main vessel 20 or substrate holder 24 including a C vapor supply source may be employed. Examples of this C vapor supply source include solid C (C substrate or C pellets such as C powder) and C compounds.
[0133] If the heat treatment step S1 in which etching is performed in a SiC--C equilibrium vapor pressure environment is performed, then it is possible to obtain a SiC substrate 11 from which the strained layer 101 has been removed. Furthermore, if the heat treatment step S1 for growing a crystal in a SiC--C equilibrium vapor pressure environment is performed, a high-quality SiC substrate 11 having a growth layer 105 in which BPDs are eliminated or reduced can be obtained.
[0134] This can prevent defects caused by the distortion (strained layer 101) of the SiC original substrate 10 and the inheritance of the BPD of the SiC original substrate 10 in the subsequent epitaxial growth process S2 and ingot growth process S3.
[0135] On the other hand, if the heat treatment step S1 in which etching or crystal growth is performed in a SiC-Si equilibrium vapor pressure environment is performed, it is possible to obtain a SiC substrate 11 in which MSBs are removed or reduced, thereby making it possible to suppress the occurrence of defects due to MSBs in the subsequent epitaxial growth step S2 and ingot growth step S3.
[0136] Next, the strained layer removing step S11, bunching removing step S12, and basal plane dislocation reducing step S13, which are performed using the manufacturing apparatus according to this embodiment, will be described in detail with reference to FIGS.
[0137] <3-1> Strained layer removal process S11 8, the strained layer removal step S11 is a step of removing the strained layer 101 introduced in the SiC original substrate 10. The strained layer removal step S11 will be explained below, but the explanation overlapping with the general explanation of the heat treatment step S1 described above will be omitted.
[0138] As shown in FIG. 9, the strained layer removal process S11 is a process in which an SiC original substrate 10 and a SiC material (upper container 21 made of polycrystalline SiC) are arranged opposite each other in a semi-closed space in which the atomic ratio Si / C is 1 or less, and heated so that the SiC original substrate 10 is on the high temperature side and the SiC material is on the low temperature side (etching bunching process S111).
[0139] Alternatively, the strained layer removal process S11 is a process in which the SiC original substrate 10 and a SiC material (upper container 21 made of polycrystalline SiC) are arranged opposite each other in a quasi-closed space in which the atomic ratio Si / C exceeds 1, and heated so that the SiC original substrate 10 is on the high temperature side and the SiC material is on the low temperature side (etching bunching removal process S121).
[0140] In other words, this is a process in which the SiC original substrate 10 and the SiC material are arranged opposite to each other and heated in a SiC-Si equilibrium vapor pressure environment or a SiC-C equilibrium vapor pressure environment so that the SiC original substrate 10 is on the high temperature side and the SiC material is on the low temperature side.
[0141] In this way, by subjecting the SiC base substrate 10, which is located on the high temperature side of the temperature gradient, to a heat treatment in opposition to a part of the main body container 20, which is located on the low temperature side of the temperature gradient, atoms are transported from the SiC base substrate 10 to the main body container 20, thereby achieving etching of the SiC base substrate 10.
[0142] That is, one side of the SiC base substrate 10 and the bottom surface of the main body container 20, which has a lower temperature than the one side, are arranged opposite to each other to form an etching space X. In this etching space X, atomic transport occurs with the temperature gradient formed by the heating furnace 30 as a driving force, and as a result, the SiC base substrate 10 can be etched.
[0143] On the other hand, the other surface (rear surface) of the SiC original substrate 10 to be etched may be provided with a raw material supply space Y between the rear surface of the SiC original substrate 10 and the top surface of the main body container 20, which has a higher temperature than the rear surface, by arranging them facing each other. In the raw material supply space Y, the raw material is transported by using the temperature gradient formed by the heating furnace 30 as a driving force, and as a result, a growth layer 105 can be formed on the other surface of the SiC original substrate 10. Note that in the strained layer removal step S11, a configuration may be adopted in which the raw material supply space Y is not formed, for example, by bringing the other surface of the SiC original substrate 10 into contact with the top surface of the main body container 20.
[0144] Furthermore, main body container 20 is disposed in Si vapor pressure space Z in which an atmosphere containing Si elements is formed. In this manner, main body container 20 is disposed in Si vapor pressure space Z, and the inside of main body container 20 is evacuated (evacuated) through the space of the Si vapor pressure environment, thereby making it possible to suppress a decrease in Si atoms from within main body container 20. This makes it possible to maintain a preferable atomic ratio Si / C within main body container 20 for a long period of time.
[0145] That is, when exhausting directly from the etching space X or the raw material supply space Y without passing through the Si vapor pressure space Z, Si atoms are exhausted from the gap 23. In this case, the atomic ratio Si / C in the etching space X or the raw material supply space Y is significantly reduced. On the other hand, when exhausting the inside of the main body container through the Si vapor pressure space Z of the Si vapor pressure environment, exhaust of Si atoms from the etching space X and the raw material supply space Y can be suppressed, and the atomic ratio Si / C in the main body container 20 can be maintained.
[0146] The etching temperature in the strained layer removing step S11 is preferably set in the range of 1400 to 2300°C, and more preferably in the range of 1600 to 2000°C. The etching rate in the strained layer removing step S11 can be controlled by the above temperature range, and can be selected within the range of 0.001 to 2 μm / min. The etching amount in the strained layer removal step S11 can be any amount that can remove the strained layer 101 of the SiC base substrate 10. The etching amount can be, for example, 0.1 μm or more and 20 μm or less, but can be adapted as necessary. The etching time in the strained layer removal step S11 can be set to any time so as to obtain a desired etching amount. For example, when the etching rate is 1 μm / min and the etching amount is desired to be 1 μm, the etching time is 1 minute. The temperature gradient in the strained layer removing step S11 is set in the etching space X in the range of 0.1 to 5° C. / mm.
[0147] The case where the SiC base substrate 10 and the SiC material are placed opposite each other in a semi-closed space in which the atomic ratio Si / C is 1 or less and etched (etching bunching step S111) has been described above with reference to FIG. Even when etching is performed by placing the SiC substrate 10 and the SiC material opposite each other in a quasi-closed space in which the atomic ratio Si / C exceeds 1 (etching bunching removal step S121), the strained layer 101 can be removed in a similar manner.
[0148] By carrying out the strained layer removing step S11 described above, it is possible to manufacture a SiC substrate 11 in which the strained layer 101 is reduced or removed, as shown in FIG.
[0149] <3-2> Bunching removal process S12 10 and 12, the bunching removal step S12 is a step of decomposing and removing MSBs formed on the surface of the SiC substrate 11. As described above, preferred examples of the bunching removal step S12 include an etching bunching removal step S121 and a growth bunching removal step S122. The bunching removal step S12 will be explained below, but explanations that overlap with the general explanation of the heat treatment step S1 described above will be omitted.
[0150] <3-2-1> Etching bunching removal process S121 The etching bunching removal step S121 is a step of removing or reducing the MSBs by etching the surface of the SiC substrate 10 on which the MSBs are formed, as shown in FIG.
[0151] The etching bunching removal process S121 is a process in which, as shown in FIG. 11, a SiC original substrate 10 and a SiC material (a lower container 22 made of polycrystalline SiC) are arranged opposite each other in a quasi-closed space in which the atomic ratio Si / C exceeds 1, and heated so that the SiC original substrate 10 is on the high temperature side and the SiC material is on the low temperature side. In other words, this is a process in which the original SiC substrate 10 and the SiC material are arranged opposite to each other and heated in a SiC-Si equilibrium vapor pressure environment so that the original SiC substrate 10 is on the high temperature side and the SiC material is on the low temperature side.
[0152] The apparatus configuration for implementing this etching bunching removal step S121 is configured such that a Si vapor supply source 25 is further disposed in the main body container 20 of the strained layer removal step S11. By disposing this Si vapor supply source 25, it is possible to heat the SiC original substrate 10 in a SiC-Si equilibrium vapor pressure environment. The explanation of the parts that overlap with the general explanation of the strained layer removing step S11 will be omitted as appropriate.
[0153] The etching temperature in the etching bunching removing step S121 is preferably set in the range of 1400 to 2300°C, and more preferably in the range of 1600 to 2000°C. The etching rate in the etching bunching removing step S121 can be controlled by the above temperature range, and can be selected within the range of 0.001 to 2 μm / min. The etching amount in the etching bunching removal step S121 can be any amount that can decompose the MSB of the SiC base substrate 10. An example of this etching amount is 0.1 μm or more and 20 μm or less. The etching time in the etching bunching removal step S121 can be set to any time so as to obtain a desired etching amount. For example, when the etching rate is 1 μm / min and the etching amount is desired to be 1 μm, the etching time is 1 minute. The temperature gradient in the etching bunching removing step S121 is set in the etching space X in the range of 0.1 to 5° C. / mm.
[0154] According to the etching bunching removal step S121, as shown in FIG. 10, by etching the surface of the SiC original substrate 10, it is possible to manufacture a SiC substrate 11 in which MSBs have been removed or reduced.
[0155] <3-2-2> Growth bunching removal process S122 The growth bunching removal step S122 is a step of forming a growth layer 105 in which the MSBs have been removed or reduced by growing a crystal on the surface of the SiC base substrate 10 on which the MSBs have been formed, as shown in FIG.
[0156] The growth bunching removal process S122 is a process in which, as shown in FIG. 13, a SiC original substrate 10 and a SiC material (upper container 21 made of polycrystalline SiC) are arranged opposite each other in a quasi-closed space in which the atomic ratio Si / C exceeds 1, and heated so that the SiC original substrate 10 is on the low temperature side and the SiC material is on the high temperature side. In other words, this is a process in which the original SiC substrate 10 and the SiC material are arranged opposite to each other and heated in a SiC-Si equilibrium vapor pressure environment so that the original SiC substrate 10 is on the low temperature side and the SiC material is on the high temperature side.
[0157] In this manner, the SiC base substrate 10 arranged on the low temperature side of the temperature gradient and a part of the main body container 20 arranged on the high temperature side of the temperature gradient are placed opposite each other and subjected to heat treatment, whereby the raw material is transported from the main body container 20 to the SiC base substrate 10 to form the growth layer 105.
[0158] That is, the surface of the SiC substrate 10 and the top surface of the main container 20, which has a higher temperature than the surface, are arranged opposite to each other to form a raw material supply space Y. In the raw material supply space Y, the raw material is transported by the driving forces of the temperature gradient formed by the heating furnace 30 and the chemical potential difference between the SiC substrate 10 and the SiC material, and as a result, a growth layer 105 can be formed on the surface of the SiC substrate 10.
[0159] Moreover, the apparatus configuration for realizing this growth bunching removal step S122 is the same as the etching bunching removal step S121, in which a Si vapor supply source 25 is further arranged in the main body vessel 20. Note that explanations of points that overlap with the general explanation of the etching bunching removal step S121 described above will be omitted.
[0160] The heating temperature in the growth bunching removing step S122 is preferably set in the range of 1400 to 2200°C, and more preferably in the range of 1600 to 2000°C. The growth rate in the growth bunching removal step S122 can be controlled by the above-mentioned temperature range, and can be selected within the range of 0.001 to 1 μm / min. The amount of growth in the growth bunching removal step S122 is preferably 5 μm or more, and more preferably 8 μm or more. The growth time in the growth bunching removal step S122 can be set to any time so as to obtain a desired growth amount. For example, when the growth rate is 10 nm / min and the growth amount is desired to be 10 μm, the growth time is 100 minutes. The degree of vacuum (main heating chamber 31) in the growth bunching removal step S122 is 10 -5 ~10 Pa, more preferably 10 -3 ~1 Pa. In the growth bunching removal step S122, it is also possible to introduce an inert gas during growth. The inert gas may be selected from Ar and the like. -5 By introducing a pressure in the range of 10,000 Pa or less, the degree of vacuum in the heating furnace 30 (main heating chamber 31) can be adjusted.
[0161] According to the growth bunching removal step S122, as shown in FIG. 12, a growth layer 105 having no MSBs is grown on the surface of the SiC original substrate 10, thereby making it possible to manufacture a SiC substrate 11 in which the MSBs have been removed or reduced.
[0162] <3-3> Basal plane dislocation reduction process S13 The basal plane dislocation reduction step S13 is a step of forming a growth layer 105 in which BPDs are removed or reduced by growing a crystal under conditions that increase the terrace width W of the SiC base substrate 10, as shown in Fig. 14. Explanations that overlap with the general explanation of the heat treatment step S1 described above will be omitted.
[0163] The basal plane dislocation reduction process S13 is a process in which, as shown in FIG. 15, a SiC original substrate 10 and a SiC material (upper container 21 made of polycrystalline SiC) are arranged opposite each other in a quasi-closed space in which the atomic ratio Si / C is 1 or less, and heated so that the SiC original substrate 10 is on the low temperature side and the SiC material is on the high temperature side. In other words, this is a process in which the original SiC substrate 10 and the SiC material are arranged opposite to each other and heated in a SiC-C equilibrium vapor pressure environment so that the original SiC substrate 10 is on the low temperature side and the SiC material is on the high temperature side.
[0164] The apparatus configuration for realizing this basal plane dislocation reduction step S13 is similar to that of the growth bunching removal step S122, in that the SiC original substrate 10, placed on the low temperature side of the temperature gradient, and a part of the main body container 20, placed on the high temperature side of the temperature gradient, are placed opposite each other and heat-treated, thereby transporting raw material from the main body container 20 to the SiC original substrate 10 to form the growth layer 105.
[0165] On the other hand, unlike the growth bunching removal step S122, the basal plane dislocation reduction step S13 does not include the Si vapor supply source 25. Note that a description of parts that overlap with the general description of the growth bunching removal step S122 described above will be omitted.
[0166] The heating temperature in the basal plane dislocation reducing step S13 is set preferably in the range of 1400 to 2200°C, and more preferably in the range of 1600 to 2000°C. The growth rate in the basal plane dislocation reducing step S13 can be controlled by the above-mentioned temperature range and growth environment, and can be selected from the range of 0.001 to 1 μm / min. The amount of growth in the basal plane dislocation reducing step S13 is preferably 5 μm or more, and more preferably 8 μm or more. The growth time in the basal plane dislocation reduction step S13 can be set to any time so as to obtain a desired growth amount. For example, when the growth rate is 10 nm / min and the growth amount is desired to be 10 μm, the growth time is 100 minutes. The degree of vacuum in the basal plane dislocation reduction step S13 (main heating chamber 31) is 10 -5 ~10 Pa, more preferably 10 -3 ~1 Pa. In the basal plane dislocation reduction step S13, it is also possible to introduce an inert gas during growth. The inert gas may be selected from Ar and the like. -5 By introducing a pressure in the range of 10,000 Pa or less, the degree of vacuum in the heating furnace 30 (main heating chamber 31) can be adjusted.
[0167] According to the basal plane dislocation reduction step S13, by growing under conditions that increase the width (terrace width W) of the terraces 104, the conversion rate (BPD conversion rate) of BPDs to other defects / dislocations can be improved, and the BPDs in the growth layer 105 can be removed or reduced. The conditions that increase the terrace width W are conditions that increase the terrace width W2 after growth compared to the terrace width W1 before growth, and can be realized, for example, by growing in a SiC-C equilibrium vapor pressure environment or a C-rich environment.
[0168] The value of the terrace width W (including terrace width W1 and terrace width W2) may be, for example, an average value of the terrace width obtained by drawing a line perpendicular to the steps 103 in the captured SEM image and counting the number of steps 103 present on this line (terrace width W = line length / number of steps on the line).
[0169] Preferably, the bunching removal step S12 is followed by the basal plane dislocation reduction step S13. That is, when comparing the width of terrace 104 on a surface where MSBs are not formed with the width of terrace 104 on a surface where MSBs are formed, the width of terrace 104 on the surface where MSBs are not formed is narrower. Therefore, by growing growth layer 105 under conditions where MSBs are formed after decomposition of MSBs, the BPD conversion rate can be improved.
[0170] <3-4> Preferred form of heat treatment step S1 FIG. 16 shows a preferred embodiment of a process for manufacturing a SiC substrate 11 or a SiC epitaxial substrate 12 by subjecting an original SiC substrate 10 to a heat treatment process S1. FIG. 16( a ) shows a preferred embodiment for producing a SiC substrate 11 , and FIG. 16( b ) shows a preferred embodiment for producing a SiC epitaxial substrate 12 .
[0171] As the strained layer removing step S11 in the embodiment shown in FIG. 16, either the etching bunching step S111 or the etching bunching removing step S121 can be adopted. When the etching bunching removing step S121 is employed, the MSB can be removed or reduced at the same time as the strained layer 101 is removed.
[0172] 16 shows a form in which the bunching removal step S12 is performed after the strained layer removal step S11. According to this form, it is possible to manufacture a SiC substrate 11 or a SiC epitaxial substrate 12 that does not include a strained layer 101 or an MSB on the surface.
[0173] 16 shows an embodiment in which the basal plane dislocation reducing step S13 is performed following the strained layer removing step S11 and bunching removing step S12. By performing the strained layer removing step S11 and bunching removing step S12 in advance as in this embodiment, the conversion rate at which BPDs are converted to other defects / dislocations (BPD conversion rate) can be improved in the subsequent basal plane dislocation reducing step S13, and a growth layer 105 with a reduced BPD density can be formed.
[0174] 16 shows an embodiment in which the bunching removal step S12 is further performed after the basal plane dislocation reduction step S13. By performing the bunching removal step S12 after the basal plane dislocation reduction step S13 in this manner, it is possible to manufacture a SiC substrate 11 or a SiC epitaxial substrate 12 that is free of not only strained layer 101 and BPDs but also MSBs on the surface.
[0175] As the bunching removing step S12 in the embodiment shown in FIG. 16, either the etching bunching removing step S121 or the growth bunching removing step S122 can be adopted.
[0176] FIG. 16(b) shows a form in which a SiC material with a lower doping concentration than the SiC substrate 10 is used in the crystal growth process (the basal plane dislocation reducing step S13 and / or the growth bunching removing step S122).
[0177] When the heat treatment process S1 includes two or more steps selected from the strained layer removal process S11 (etching bunching process S111 or etching bunching removal process S121), the bunching removal process S12 (etching bunching removal process S121 or growth bunching removal process S122), and the basal plane dislocation reduction process S13, the two or more steps can be heat treated using the same apparatus configuration.
[0178] An example of a container in which the multiple heat treatment steps S1 are performed is a container that generates an atmosphere containing Si elements and C elements in its internal space, specifically, main container 20. In this way, by using the main vessel 20, etc., even if the heat treatment process S1 includes multiple processes, all of the processes can be completed in the same vessel, so that the work can be simplified. Also, since etching and crystal growth can be performed in the same equipment system, there is no need to introduce multiple devices, which is extremely advantageous industrially.
[0179] <4> SiC substrate 11 The present invention also relates to a SiC substrate 11 manufactured through a heat treatment step S1. The SiC substrate 11 of the present invention does not contain factors such as distortion (strained layer 101), BPD, MSB, etc., which adversely affect epitaxial growth and ingot growth due to the heat treatment step S1, on the surface. Therefore, the SiC substrate 11 of the present invention allows a higher quality SiC epitaxial substrate 12 and SiC ingot 13 to be grown.
[0180] SiC substrate 11 is characterized by having a growth layer 105 that does not contain BPDs on the surface. The thickness of BPD-free growth layer 105 is preferably 0.001 μm or more, more preferably 0.01 μm or more, and even more preferably 0.1 μm or more. If the thickness of the layer that does not contain BPDs is within the above range, it may be possible to suppress the propagation of BPDs present in SiC substrate 11 in epitaxial growth step S2 and ingot growth step S3 in which SiC is grown on SiC substrate 11.
[0181] Furthermore, when the heat treatment step S1 includes a crystal growth step using a SiC material with a lower doping concentration than the original SiC substrate 10, it is possible to obtain the SiC epitaxial substrate 12. In this case, the SiC epitaxial substrate 12 can be manufactured without going through the epitaxial growth step S2 described later.
[0182] The diameter of the SiC substrate 11 of the present invention is not particularly limited, and is preferably 6 inches or more, more preferably 8 inches or more, and further preferably 12 inches or more. By growing the SiC substrate 11 of such a size, it is possible to obtain a SiC epitaxial substrate 12 or a SiC ingot 13 that is large in diameter but high quality.
[0183] <5> Epitaxial growth process S2 The epitaxial growth step S2 is a step of forming an epitaxial layer by epitaxial growth on the main surface of the SiC substrate 11 to form a SiC epitaxial substrate 12 to be used for applications such as power devices.
[0184] As the epitaxial growth means in the epitaxial growth step S2, any known method can be used without limitation, such as chemical vapor deposition (CVD), physical vapor transport (PVT), metastable solvent epitaxy (MSE), etc.
[0185] <6> SiC epitaxial substrate 12 The present invention also relates to a SiC epitaxial substrate 12 produced by the above-described process. The SiC epitaxial substrate 12 of the present invention is derived from the SiC substrate 11 in which distortion, BPD, and MSB are suppressed as described above, and therefore the propagation of defects to the epitaxial layer is suppressed. Therefore, the SiC epitaxial substrate 12 of the present invention can provide a high-performance SiC semiconductor device.
[0186] <7> Ingot growth process S3 The ingot growth step S3 is a step of producing a SiC ingot 13 by growing single crystal SiC on the SiC substrate 11. Any known growth method may be adopted for the ingot growth step S3, and examples of the method include a sublimation method and a CVD method.
[0187] <8> SiC ingot 13 The present invention also relates to a SiC ingot 13 produced by the ingot growing step S3 described above. The SiC ingot 13 of the present invention contains almost no BPDs and is of high quality. EXAMPLES
[0188] The present invention will be described more specifically below with reference to Examples 1, 2, 3, 4 and 5. Example 1 is an example that specifically describes the etching bunching step S111. Example 2 is an example that specifically describes the etching bunching removal step S121. Example 3 is an example that specifically describes the growth bunching removal step S122. Example 4 is an example that specifically describes the basal plane dislocation reduction step S13. Example 5 is an example that specifically describes the crystal growth step of forming a pressure-resistant layer.
[0189] <Example 1: Etching bunching process> The original SiC substrate 10 was placed in the main container 20 and the high melting point container 40 (see FIG. 9), and was heat-treated under the following heat treatment conditions to remove the strained layer 101 of the original SiC substrate 10.
[0190] [SiC substrate 10] Polymorphism: 4H-SiC Board size: width 10mm x height 10mm x thickness 0.45mm Off direction and off angle: 4° off in the <11-20> direction Etching surface: (0001) surface Depth of strain layer 101: 5 μm The depth of the strained layer 101 was confirmed by SEM-EBSD. The strained layer 101 can also be confirmed by TEM, μXRD, or Raman spectroscopy.
[0191] [Main container 20] Material: Polycrystalline SiC Container size: diameter 60mm x height 4mm Material of the substrate holder 24: Single crystal SiC Distance between the bottom surface of the SiC substrate 10 and the main container 20: 2 mm Atomic ratio inside the container: Si / C: 1 or less
[0192] [High melting point container 40] Material: TaC Container size: diameter 160mm x height 60mm Si vapor source 44 (Si compound): TaSi2
[0193] [Heat treatment conditions] The SiC substrate 10 arranged under the above conditions was subjected to a heat treatment under the following conditions. Heating temperature: 1800℃ Heating time: 20min Etching amount: 5μm Temperature gradient: 1℃ / mm Etching speed: 0.25μm / min Main heating chamber vacuum degree: 10 -5 Pa
[0194] [Measurement of strained layer by SEM-EBSD method] The lattice strain of the SiC substrate 10 can be obtained by comparing it with a reference crystal lattice. For example, the SEM-EBSD method can be used as a means for measuring this lattice strain. The SEM-EBSD method is a method (Electron Back Scattering Diffraction: EBSD) that can measure strain in a microscopic area based on a Kikuchi line diffraction pattern obtained by backscattering electron beams in a scanning electron microscope (SEM). In this method, the amount of lattice strain can be obtained by comparing the diffraction pattern of the reference crystal lattice and the diffraction pattern of the measured crystal lattice.
[0195] For the reference crystal lattice, for example, a reference point is set in a region where it is considered that no lattice distortion occurs. In other words, it is desirable to place the reference point in the region of the bulk layer 102 in FIG. 8. Normally, it is generally accepted that the depth of the strained layer 101 is about 10 μm. Therefore, it is sufficient to set the reference point at a position about 20 to 35 μm deep, which is considered to be sufficiently deeper than the strained layer 101.
[0196] The diffraction pattern of the crystal lattice at this reference point is then compared with the diffraction patterns of the crystal lattice in each measurement area measured at a pitch on the order of nanometers, allowing the amount of lattice strain in each measurement area relative to the reference point to be calculated.
[0197] In addition, although the case where a reference point where no lattice distortion is considered to occur is set as the reference crystal lattice has been shown, it is of course also possible to use an ideal crystal lattice of single crystal SiC as the reference, or a crystal lattice that occupies the majority (e.g., more than half) of the surface of the measurement area as the reference.
[0198] By measuring whether or not lattice strain exists by this SEM-EBSD method, it is possible to determine the presence or absence of the strained layer 101. That is, when processing damage such as scratches 1011, latent scratches 1012, and strains 1013 is introduced, lattice strain occurs in the SiC original substrate 10, and therefore stress is observed by the SEM-EBSD method.
[0199] The strained layer 101 present in the SiC substrate 10 before the heat treatment step S1 and the strained layer 101 present in the SiC substrate 10 after the heat treatment step S1 were observed by the SEM-EBSD method. The results are shown in Figures 17(a) and 17(b).
[0200] In this measurement, the cross sections of the cleaved SiC substrate 10 before and after the heat treatment step S1 were measured using a scanning electron microscope under the following conditions. SEM equipment: Zeiss Merline EBSD analysis: TSL Solutions OIM crystal orientation analysis device Acceleration voltage: 15 kV Probe current: 15nA Step size: 200nm Reference point R depth: 20μm
[0201] FIG. 17(a) is a cross-sectional SEM-EBSD image of the original SiC substrate 10 before the heat treatment step S1. As shown in Fig. 17(a), before the heat treatment step S1, lattice distortion of a depth of 5 µm was observed in the SiC original substrate 10. This is lattice distortion introduced during machining, and it is understood that there is a strained layer 101. In addition, compressive stress is observed in Fig. 17(a).
[0202] FIG. 17(b) is a cross-sectional SEM-EBSD image of the original SiC substrate 10 after the heat treatment step S1. 17(b), after the heat treatment step S1, no lattice distortion was observed in the SiC base substrate 10. That is, it is understood that the heat treatment step S1 removed the strained layer 101. After the heat treatment step S1, MSBs were formed on the surface of the SiC substrate 10.
[0203] Thus, according to the etching bunching step S111, the strained layer 101 can be removed or reduced by etching the SiC original substrate 10 in a semi-closed space in which the atomic ratio Si / C is 1 or less. This makes it possible to manufacture the SiC substrate 11 in which the strained layer 101 is reduced or removed.
[0204] <Example 2: Etching bunching removal process> The original SiC substrate 10 was placed in a main container 20 and a high-melting-point container 40 (see FIG. 11), and was heat-treated under the following heat treatment conditions to remove the MSB from the surface of the original SiC substrate 10.
[0205] [SiC substrate 10] Polymorphism: 4H-SiC Board size: width 10mm x length 10mm x thickness 0.3mm Off direction and off angle: 4° off in the <11-20> direction Etching surface: (0001) surface MSB: Yes
[0206] The step height, terrace width, and the presence or absence of MSB can be confirmed by an atomic force microscope (AFM) or a method for evaluating the contrast of a scanning electron microscope (SEM) image described in JP 2015-179082 A.
[0207] [Main container 20] Material: Polycrystalline SiC Container size: diameter 60mm x height 4mm Material of the substrate holder 24: Single crystal SiC Distance between the SiC substrate 10 and the bottom of the main container 20: 2 mm Si vapor source 25: single crystal Si piece The atomic ratio of Si / C in the container exceeds 1.
[0208] In this manner, by accommodating the Si pieces together with the SiC base substrate 10 in the main container 20, the atomic ratio Si / C in the container exceeds 1.0.
[0209] [High melting point container 40] Material: TaC Container size: diameter 160mm x height 60mm Si vapor source 44 (Si compound): TaSi2
[0210] [Heat treatment conditions] The SiC substrate 10 arranged under the above conditions was subjected to a heat treatment under the following conditions. Heating temperature: 1900℃ Heating time: 60min Temperature gradient: 1℃ / mm Etching speed: 300nm / min Main heating chamber vacuum degree: 10 -5 Pa
[0211] The steps 103 of the SiC substrate 10 before the heat treatment step S1 and the steps 103 of the SiC substrate 10 after the heat treatment step S1 were observed by SEM. The results are shown in Figures 18(a) and 18(b). The height of the steps 103 was measured by an atomic force microscope (AFM). The width of the terraces 104 was also measured by SEM.
[0212] 18(a) is an SEM image of the SiC substrate 10 before the heat treatment step S1. MSBs with a height of 3 nm or more are formed on the surface of the SiC substrate 10 before the heat treatment step S1. The step height was measured by AFM.
[0213] 18(b) is an SEM image of the SiC substrate 10 after the heat treatment step S1. It can be seen that no MSB is formed on the surface of the SiC substrate 10 after the heat treatment step S1, and steps of 1.0 nm (full unit cell) are regularly arranged.
[0214] Thus, according to the etching bunching removal step S121, it is possible to remove or reduce the MSBs by etching the original SiC substrate 10 in a semi-closed space in which the atomic ratio Si / C exceeds 1. This makes it possible to manufacture a SiC substrate 11 in which the MSBs are reduced or removed.
[0215] Moreover, when the SiC substrate 10 after the heat treatment step S1 was observed by the SEM-EBSD method, the strained layer 101 was not observed, similar to Example 1. That is, the strained layer 101 can also be removed in the etching bunching removal step S121.
[0216] <Example 3: Growth bunching removal process> The original SiC substrate 10 was placed in a main container 20 and a high-melting-point container 40 (see FIG. 13), and heat-treated under the following heat treatment conditions to remove the MSB from the surface of the original SiC substrate 10.
[0217] [SiC substrate 10] Polymorphism: 4H-SiC Board size: width 10mm x length 10mm x thickness 0.3mm Off direction and off angle: 4° off in the <11-20> direction Etching surface: (0001) surface MSB: Yes
[0218] [Main container 20] Material: Polycrystalline SiC Container size: diameter 60mm x height 4mm Distance between the SiC substrate 10 and the bottom of the main container 20: 2 mm Si vapor source 25: single crystal Si piece The atomic ratio of Si / C in the container exceeds 1.
[0219] In this manner, by accommodating the Si pieces together with the SiC base substrate 10 in the main container 20, the atomic ratio Si / C in the container exceeds 1.0.
[0220] [High melting point container 40] Material: TaC Container size: diameter 160mm x height 60mm Si vapor source 44 (Si compound): TaSi2
[0221] [Heat treatment conditions] The SiC substrate 10 arranged under the above conditions was subjected to a heat treatment under the following conditions. Heating temperature: 1800℃ Heating time: 60min Temperature gradient: 1℃ / mm Growth rate: 68nm / min Main heating chamber 31 degree of vacuum: 10 -5 Pa
[0222] The steps 103 on the surface of the SiC substrate 10 after the heat treatment step S1 were observed by SEM. The results are shown in Fig. 19. The height of the steps 103 was measured by an atomic force microscope (AFM), and the width of the terraces 104 was measured by SEM.
[0223] Fig. 19 is an SEM image of the surface of the SiC original substrate 10 after the heat treatment step S1. Similar to Fig. 18(a), MSBs with a height of 3 nm or more were formed on the surface of the SiC original substrate 10 before the heat treatment step S1. As shown in Fig. 19, no MSBs were formed on the surface of the SiC original substrate 10 after the heat treatment step S1, and steps of 1.0 nm (full unit cell) were found to be regularly arranged.
[0224] Thus, according to the growth bunching removal step S122, it is possible to form a growth layer 105 in which no MSBs are formed by growing the crystal of the SiC original substrate 10 in a semi-closed space in which the atomic ratio Si / C exceeds 1. This makes it possible to manufacture a SiC substrate 11 in which the MSBs are reduced or removed.
[0225] <Example 4: Basal Plane Dislocation Reduction Process> The SiC substrate 10 is housed in a main container 20 and a high-melting-point container 40 (see FIG. 15), and is heat-treated under the following heat treatment conditions, thereby making it possible to remove or reduce BPDs.
[0226] [SiC substrate 10] Polymorphism: 4H-SiC Board size: width 10mm x length 10mm x thickness 0.3mm Off direction and off angle: 4° off in the <11-20> direction Growth plane: (0001) plane MSB: None Presence or absence of strain layer 101: None
[0227] [Main container 20] Material: Polycrystalline SiC Container size: diameter 60mm x height 4mm Distance between SiC substrate 10 and SiC material: 2 mm Atomic ratio inside the container: Si / C: 1 or less
[0228] [High melting point container 40] Material: TaC Container size: diameter 160mm x height 60mm Si vapor source 44 (Si compound): TaSi2
[0229] [Heat treatment conditions] The SiC substrate 10 arranged under the above conditions was subjected to a heat treatment under the following conditions. Heating temperature: 1700℃ Heating time: 300min Temperature gradient: 1℃ / mm Growth rate: 5nm / min Main heating chamber 31 degree of vacuum: 10 -5 Pa
[0230] [BPD conversion rate in the growing layer] FIG. 20 is an explanatory diagram of a method for determining the conversion rate of BPDs into other defects / dislocations (TEDs, etc.) in the growth layer 105. In FIG. 20(a) shows the state where the growth layer 105 is grown by the heat treatment step S1. In this heating step, the BPDs present in the SiC base substrate 10 are converted to TEDs with a certain probability. Therefore, unless 100% is converted, TEDs and BPDs will be mixed on the surface of the growth layer 105. 20(b) shows the state where defects in the growth layer 105 were confirmed using the KOH dissolution etching method. This KOH dissolution etching method is a method in which the SiC substrate is immersed in molten salt (KOH, etc.) heated to about 500°C, etch pits are formed at the dislocation or defect parts, and the type of dislocation is identified based on the size and shape of the etch pits. By this method, the number of BPDs present on the surface of the growth layer 105 is obtained. 20(c) shows the state in which the growth layer 105 is removed after the KOH dissolution etching. In this method, after planarization to the etch pit depth by mechanical polishing, CMP, or the like, the growth layer 105 is removed by thermal etching to expose the surface of the SiC base substrate 10. 20(d) shows the state in which the defects in the SiC original substrate 10 are confirmed by using a KOH dissolution etching method for the SiC original substrate 10 from which the growth layer 105 has been removed. By this method, the number of BPDs present on the surface of the SiC original substrate 10 is obtained.
[0231] By comparing the number of BPDs present on the surface of the growth layer 105 (see FIG. 20(b)) with the number of BPDs present on the surface of the SiC substrate 10 (see FIG. 20(d)) using the sequence shown in FIG. 20, the BPD conversion rate of BPDs converted to other defects and dislocations during the heat treatment step S1 can be obtained.
[0232] The number of BPDs present on the surface of the growth layer 105 in Example 4 was 0 cm -2The number of BPDs present on the surface of the SiC substrate 10 is approximately 1000 cm -2 It was. That is, it can be understood that by placing the original SiC substrate 10 having no MSB on the surface in a semi-closed space with an atomic ratio Si / C of 1 or less and growing the crystal, BPDs can be reduced or eliminated.
[0233] Thus, according to the basal plane dislocation reduction step S13, it is possible to form a grown layer 105 on the surface in which BPDs are reduced or removed by growing the crystal of the original SiC substrate 10 in a quasi-closed space in which the atomic ratio Si / C is equal to or less than 1. This makes it possible to manufacture a SiC substrate 11 having a grown layer 105 in which BPDs are reduced or removed.
[0234] <Example 5: Formation of pressure-resistant layer> The original SiC substrate 10 is housed in a main container 20 and a high-melting-point container 40 (see FIG. 15), and is heat-treated under the following heat treatment conditions, thereby forming a voltage-resistant layer on the original SiC substrate 10.
[0235] [SiC substrate 10] Polymorphism: 4H-SiC Board size: width 10mm x length 10mm x thickness 0.3mm Off direction and off angle: 4° off in the <11-20> direction Growth plane: (0001) plane Dopant: N Doping concentration: 3×10 18 cm -3 MSB: None Presence or absence of strain layer 101: None
[0236] The dopants and doping concentrations of the SiC substrate 10 were confirmed by Raman spectroscopy.
[0237] [Main container 20] Material: Polycrystalline SiC Container size: diameter 60mm x height 4mm Distance between SiC substrate 10 and SiC material: 2 mm Dopant: N Doping concentration: 1×10 17 cm -3 Below the detection limit of Raman spectroscopy Atomic ratio inside the container: Si / C: 1 or less
[0238] [High melting point container 40] Material: TaC Container size: diameter 160mm x height 60mm Si vapor source 44 (Si compound): TaSi2
[0239] [Heat treatment conditions] The SiC substrate 10 arranged under the above conditions was subjected to a heat treatment under the following conditions. Heating temperature: 1700℃ Heating time: 300min Temperature gradient: 1℃ / mm Growth rate: 5nm / min Main heating chamber 31 degree of vacuum: 10 -5 Pa
[0240] 21 is an SEM image of the cross section of the SiC substrate 10 grown under the above conditions, observed at a magnification of ×10000. The thickness of this grown layer 105 was 1.5 μm.
[0241] The doping concentration of this growth layer 105 is 1×10 17 cm -3 The doping concentration of the SiC substrate 10 is 3×10 18 cm -3 21, the doping concentration of the growth layer 105 is brighter than that of the SiC substrate 10 in the SEM image, which indicates that the doping concentration of the growth layer 105 is lower than that of the SiC substrate 10.
[0242] Thus, according to the crystal growth process of the present invention, the SiC original substrate 10 and a SiC material having a lower doping concentration than the SiC original substrate 10 are placed opposite each other and heated, and the raw material is transported from the SiC material to the SiC original substrate 10 to form the growth layer 105. This makes it possible to grow the growth layer 105 with a doping concentration capable of functioning as a voltage-resistant layer for a SiC semiconductor device, and to manufacture a SiC substrate having a voltage-resistant layer.
[0243] In the fifth embodiment, the SiC substrate 10 is grown in a semi-closed space in which the atomic ratio Si / C is equal to or less than 1. Similarly, when the substrate is grown in a semi-closed space in which the atomic ratio Si / C is greater than 1, the grown layer 105 can be formed while retaining the doping density of the SiC material.
[0244] [Thermodynamic calculation] 22(a) is a graph showing the relationship between the heating temperature and the etching rate in the etching process of the present invention, where the horizontal axis of the graph is the reciprocal of the temperature, and the vertical axis of the graph shows the etching rate in logarithm. 22(b) is a graph showing the relationship between the heating temperature and the growth rate in the crystal growth process of the present invention. The horizontal axis of this graph is the reciprocal of the temperature, and the vertical axis of this graph shows the logarithmic growth rate.
[0245] 22, the results of heat treatment of the SiC original substrate 10 placed in a space (inside the main container 20) where the atomic ratio Si / C exceeds 1 are indicated by circles, and the results of heat treatment of the SiC original substrate 10 placed in a space (inside the main container 20) where the atomic ratio Si / C is 1 or less are indicated by crosses.
[0246] In addition, no MSB was formed on any of the areas marked with a circle on the surface of the original SiC substrate 10, and the steps 103 had a height of one unit cell. On the other hand, MSBs were formed on any of the areas marked with a cross on the surface of the original SiC substrate 10.
[0247] In addition, in the graph of FIG. 22, the results of thermodynamic calculations in a SiC-Si equilibrium vapor pressure environment are shown by a dashed line (Arrhenius plot), and the results of thermodynamic calculations in a SiC-C equilibrium vapor pressure environment are shown by a two-dot chain line (Arrhenius plot). Hereinafter, the thermodynamic calculation of the etching process and the thermodynamic calculation of the crystal growth process will be separately explained in detail.
[0248] (Thermodynamic calculation of the etching process) In the thermodynamic calculation of the etching process, the amount of steam (vapor phase species containing Si element and vapor phase species containing C element) generated from the SiC base substrate 10 when the main container 20 is heated can be converted into an etching amount. In this case, the etching rate of the SiC base substrate 10 can be calculated by the following formula 1.
[0249]
number
[0250] Here, T is the temperature of the SiC substrate 10, m i is a gas phase species (Si x C y ) and k is the Boltzmann constant. Also, P i is the sum of the vapor pressures generated in the main container 20 by heating the SiC substrate 10. i The gas phase species are expected to be SiC-Si2C, SiC2, etc.
[0251] The dashed line in Fig. 22(a) is the result of a thermodynamic calculation when etching single crystal SiC in a vapor pressure environment where SiC (solid) and Si (liquid phase) are in phase equilibrium via the gas phase. Specifically, using Equation 1, the thermodynamic calculation was performed under the following conditions (i) to (iv): (i) a SiC-Si equilibrium vapor pressure environment with a constant volume, (ii) the etching driving force is the temperature gradient inside the main container 20, (iii) the source gas is SiC, Si2C, and SiC2, and (iv) the desorption coefficient when the source material sublimes from step 103 is 0.001.
[0252] The two-dot chain line in Fig. 22(a) is the result of a thermodynamic calculation when etching single crystal SiC in a vapor pressure environment where SiC (solid phase) and C (solid phase) are in phase equilibrium via the gas phase. Specifically, using Equation 1, the thermodynamic calculation was performed under the following conditions (i) to (iv): (i) a constant volume SiC-C equilibrium vapor pressure environment, (ii) the etching driving force is the temperature gradient inside the main body container 20, (iii) the source gas is SiC, Si2C, and SiC2, and (iv) the desorption coefficient of the source material sublimating from step 103 is 0.001. The data for each chemical species used in the thermodynamic calculations were taken from the JANAF Thermochemical Tables.
[0253] According to the graph in FIG. 22(a), when the SiC base substrate 10 is placed in a space (inside the main container 20) where the atomic ratio Si / C exceeds 1, the result of etching the SiC base substrate 10 (marked with circles) shows a tendency consistent with the result of thermodynamic calculation of single crystal SiC etching in a SiC-Si equilibrium vapor pressure environment. In addition, the SiC base substrate 10 was placed in a space (inside the main container 20) where the atomic ratio Si / C was 1 or less, and the results of etching the SiC base substrate 10 (marked with x) showed a tendency consistent with the results of thermodynamic calculations of single crystal SiC etching in a SiC-C equilibrium vapor pressure environment.
[0254] It can be seen that under the conditions of the circled areas etched under a SiC-Si equilibrium vapor pressure environment, the formation of MSBs is decomposed and suppressed, and steps 103 with a height of 1 nm (1 unit cell) are aligned on the surface of the original SiC substrate 10. On the other hand, it is clear that MSBs are formed under the conditions of the x marks, which are etched under the SiC-C equilibrium vapor pressure environment.
[0255] (Thermodynamic calculation of the crystal growth process) Next, in the thermodynamic calculation of the crystal growth process, the partial pressure difference between the SiC raw material and the steam generated from the SiC substrate when the inside of the main container 20 is heated can be converted into the growth amount. At this time, the growth driving force can be assumed to be a chemical potential difference or a temperature gradient. Note that this chemical potential difference can be assumed to be the partial pressure difference between the gas phase species generated on the surfaces of the polycrystalline SiC (SiC material) and the single-crystalline SiC (SiC substrate 10). In this case, the growth rate of SiC can be calculated by the following equation 2.
[0256]
number
[0257] Here, T is the temperature of the SiC raw material side, m i is a gas phase species (Si x C y ) and k is the Boltzmann constant. Also, P 原料 -P 基板 is the amount of SiC deposited when the source gas becomes supersaturated, and the source gas is assumed to be SiC, Si2C, or SiC2.
[0258] That is, the dashed line in Figure 22(b) is the result of a thermodynamic calculation when single crystal SiC is grown using polycrystalline SiC as a raw material in a vapor pressure environment when SiC (solid) and Si (liquid phase) are in phase equilibrium via the gas phase. Specifically, using Equation 2, thermodynamic calculations were performed under the following conditions (i) to (iv): (i) a constant volume SiC-Si equilibrium vapor pressure environment, (ii) the growth driving force was the temperature gradient in the main body container 20 and the vapor pressure difference (chemical potential difference) between polycrystalline SiC and single crystal SiC, (iii) the source gases were SiC, Si2C, and SiC2, and (iv) the adsorption coefficient of the source material adsorbed to the steps of the SiC base substrate 10 was 0.001.
[0259] Moreover, the two-dot chain line in Figure 22(b) is the result of a thermodynamic calculation when single crystal SiC is grown using polycrystalline SiC as a raw material in a vapor pressure environment when SiC (solid phase) and C (solid phase) are in phase equilibrium via the gas phase. Specifically, using Equation 2, thermodynamic calculations were performed under the following conditions (i) to (iv): (i) a SiC-C equilibrium vapor pressure environment with constant volume, (ii) the growth driving force was the temperature gradient in the main container 20 and the vapor pressure difference (chemical potential difference) between polycrystalline SiC and single-crystalline SiC, (iii) the source gases were SiC, Si2C, and SiC2, and (iv) the adsorption coefficient of the source material adsorbed to the steps of the SiC base substrate 10 was 0.001. The data for each chemical species used in the thermodynamic calculations were taken from the JANAF Thermochemical Tables.
[0260] According to the graph in FIG. 22(b), it can be seen that the result (marked with an open circle) of placing the SiC base substrate 10 in a space (inside the main body container 20) where the atomic ratio Si / C exceeds 1 and growing a growth layer 105 on the SiC base substrate 10 coincides with the trend of the thermodynamic calculation result of SiC growth in a SiC-Si equilibrium vapor pressure environment. In addition, the SiC base substrate 10 was placed in a space (inside the main container 20) where the atomic ratio Si / C was 1 or less, and a growth layer 105 was grown on the SiC base substrate 10 (marked with an x). It can be seen that the results show a trend consistent with the results of thermodynamic calculations of SiC growth in a SiC-C equilibrium vapor pressure environment.
[0261] In a SiC-Si equilibrium vapor pressure environment, it is estimated that a growth rate of 1.0 μm / min or more can be achieved at a heating temperature of 1960°C, and a growth rate of 2.0 μm / min or more can be achieved at a heating temperature of 2000°C or higher. On the other hand, in a SiC-C equilibrium vapor pressure environment, it is estimated that a growth rate of 1.0 μm / min or more can be achieved at a heating temperature of 2000°C, and a growth rate of 2.0 μm / min or more can be achieved at a heating temperature of 2030°C or higher. [Explanation of symbols]
[0262] 10 SiC substrate 101 Strain layer 1011 Scratch 1012 Latent injury 1013 Distortion 102 Bulk layer 103 Steps 104 Terrace 105 Growth layer 11 SiC substrate 12 SiC epitaxial substrate 13 SiC ingot 20 Main container 21 Upper container 22 Lower container 23 Gap 24 Board holder 25 Si vapor source 30 Furnace 31 main heating chamber 32 Pre-heating chamber 33 Transportation 34 Heater 35 Vacuum forming valve 36 Inert gas injection valve 37 Vacuum gauge 40 High melting point container 41 Upper container 42 Lower container 43 Gap 44 Si vapor source X Etching Space Y Raw material supply space Z Si vapor pressure space S1 Heat treatment process S11 Strained layer removal process S111 Etching bunching process S12 Bunching removal process S121 Etching bunching removal process S122 Growth bunching removal process S13 Basal plane dislocation reduction process S2 Epitaxial growth process S3 Ingot growth process
Claims
1. A heat treatment process for heat-treating the SiC substrate is provided. the heat treatment step is a step of heat treating the original SiC substrate in a semi-closed space in which a SiC material is exposed, The heat treatment step includes two or more steps of the following steps (a), (b), and (c): (a) a strained layer removing step of removing the strained layer of the SiC base substrate; (b) a bunching removal step for removing macrostep bunching on the original SiC substrate; (c) a basal plane dislocation reduction step of forming a growth layer having reduced basal plane dislocations on the original SiC substrate.
2. 2. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step is a step of heat treating the original SiC substrate in a main body container made of a SiC material.
3. 3. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step is a step of disposing the SiC substrate and the SiC material so as to face each other and heating the SiC substrate and the SiC material so as to form a temperature gradient between the SiC substrate and the SiC material.
4. 4. The method for manufacturing a SiC substrate according to claim 1, wherein the strained layer removing step is a step of disposing the SiC original substrate and the SiC material opposite to each other and heating the SiC original substrate to a high temperature side and the SiC material to a low temperature side.
5. 5. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step is a step of arranging the SiC original substrate and the SiC material so as to face each other, and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so as to form a temperature gradient between the SiC original substrate and the SiC material.
6. 6. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step includes a step of arranging the SiC original substrate and the SiC material so as to face each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate and the SiC material so as to form a temperature gradient between the SiC original substrate and the SiC material.
7. 7. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step includes a step of: arranging the SiC original substrate and the SiC material so as to face each other; and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so that the SiC original substrate is on a high temperature side and the SiC material is on a low temperature side.
8. 8. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step includes a step of arranging the SiC original substrate and the SiC material so as to face each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate to a high temperature side and the SiC material to a low temperature side.
9. 9. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step includes a step of: arranging the SiC original substrate and the SiC material so as to face each other; and heating the SiC original substrate and the SiC material in a SiC-Si equilibrium vapor pressure environment so that the SiC original substrate is on a low temperature side and the SiC material is on a high temperature side.
10. 10. The method for manufacturing a SiC substrate according to claim 1, wherein the bunching removal step includes a step of arranging the SiC original substrate and the SiC material so as to face each other in a quasi-closed space in which an atomic ratio Si / C exceeds 1, and heating the SiC original substrate to a low temperature side and the SiC material to a high temperature side.
11. 11. The method for manufacturing a SiC substrate according to claim 1, wherein the basal plane dislocation reduction step includes a step of disposing the SiC original substrate and the SiC material opposite to each other, and heating the SiC original substrate to a low temperature side and the SiC material to a high temperature side in a SiC-C equilibrium vapor pressure environment.
12. 12. The method for manufacturing a SiC substrate according to claim 1, wherein the basal plane dislocation reduction step includes a step of arranging the SiC original substrate and the SiC material opposite each other in a quasi-closed space in which an atomic ratio Si / C is 1 or less, and heating the SiC original substrate to a low temperature side and the SiC material to a high temperature side.
13. 13. The method for manufacturing a SiC substrate according to claim 1, wherein a doping concentration of the SiC material is lower than a doping concentration of the original SiC substrate.
14. The doping concentration of the SiC material is 1×10 17 cm -3 The method for manufacturing a SiC substrate according to any one of claims 1 to 13, wherein:
15. 15. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step includes the bunching removal step after the strained layer removal step.
16. 16. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step includes the basal plane dislocation reduction step after the bunching removal step.
17. 17. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step includes the bunching removal step after the basal plane dislocation reduction step.
18. 18. The method for manufacturing a SiC substrate according to claim 1, wherein the heat treatment step includes the basal plane dislocation reduction step after the strained layer removal step.
19. The method for manufacturing a SiC substrate according to any one of claims 1 to 18, wherein the heat treatment step includes the strained layer removal step, the bunching removal step, the basal plane dislocation reduction step, and the bunching removal step in this order.
20. A method for producing a SiC epitaxial substrate, comprising: an epitaxial growth step of growing a SiC epitaxial layer on a SiC substrate produced by the method according to any one of claims 1 to 19.
21. A method for producing a SiC ingot, comprising: an ingot growing step of growing a SiC ingot on a SiC substrate produced by the method according to any one of claims 1 to 19.
Citation Information
Patent Citations
Method of manufacturing silicon carbide single crystal wafer and silicon carbide single crystal wafer
JP2004131328A
How to Reduce Stacking Fault Nucleation Sites to Reduce vf Drift in Bipolar Devices
JP2007506289A
Method of reforming surface of single crystal silicon carbide substrate, method of forming single crystal silicon carbide thin film, ion implantation and annealing method, and single crystal silicon carbide substrate and single crystal silicon carbide semiconductor substrate
JP2008016691A
Annealing method of silicon carbide single crystal
JP2016050141A
Method of manufacturing semiconductor laminate
JP2017071525A