Aluminum nitride sintered body, circuit board, and laminated board
By controlling particle sizes and distributions of aluminum nitride and sintering aid particles, and employing a two-step firing process, the aluminum nitride sintered bodies achieve enhanced bending strength and connection reliability, addressing deformation and reliability issues in power modules.
Patent Information
- Application Number
- JP2023511249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-31
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Existing aluminum nitride sintered bodies used in power modules for high-power control lack sufficient bending strength and connection reliability due to variations in thermal expansion coefficients between components, leading to potential deformation and reliability issues.
The aluminum nitride sintered bodies are manufactured with controlled particle sizes and distributions of aluminum nitride and sintering aid particles, along with a two-step firing process using yttrium oxide and aluminum oxide as sintering aids, to achieve uniform structure and enhanced bending strength.
The resulting sintered bodies exhibit excellent bending strength and connection reliability, capable of withstanding thermal deformation and ensuring reliable connections in high-temperature environments.
Smart Images

Figure 0007579432000003 
Figure 0007579432000004 
Figure 0007579432000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aluminum nitride sintered body, a manufacturing method thereof, a circuit board, and a laminated board. [Background technology]
[0002] In recent years, power modules for controlling large power are used in industrial equipment such as motors and products such as electric vehicles. In such power modules, circuit boards equipped with ceramic plates are used in order to efficiently diffuse heat generated from semiconductor elements and suppress leakage current. The ceramic sintered body used in such ceramic plates is usually produced by forming a ceramic raw material powder into a predetermined shape to form a ceramic molded body, and then sintering the ceramic molded body.
[0003] Known ceramic sintered bodies are composed of nitrides, carbides, borides, silicides, etc. Among them, aluminum nitride sintered bodies have excellent thermal conductivity and electrical insulation. For this reason, they are used as heat sink materials for electronic components such as power modules. In order to improve suitability for these applications, Patent Document 1 proposes a technology for increasing the thermal conductivity and mechanical strength of aluminum nitride sintered bodies by using a nitride selected from the group of Zr and Ti in an amount of 3 to 20 parts by mass in terms of oxide as a sintering aid. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-184316 A Summary of the Invention [Problem to be solved by the invention]
[0005] As electronic components such as power modules are becoming more and more sophisticated, it is believed that the performance requirements for various products used in electronic components will continue to rise. As a result, it is expected that the amount of heat generated during use of electronic components will increase, and electronic components will require excellent bending strength to withstand the effects of differences in the thermal expansion coefficients of their constituent parts, i.e., differences in the amount of deformation between the constituent parts.
[0006] An object of the present disclosure is to provide an aluminum nitride sintered body having excellent bending strength and a manufacturing method thereof. An object of the present disclosure is to provide a laminated substrate and a circuit substrate which include the aluminum nitride sintered body and have excellent connection reliability. [Means for solving the problem]
[0007] One aspect of the present disclosure provides an aluminum nitride sintered body comprising aluminum nitride particles and sintering aid particles, the aluminum nitride particles having an average particle size of 2.0 to 10.0 μm, a BA value of 6.0 area % or less when a total amount of the sintering aid particles in a surface layer is A area % and a total amount of the sintering aid particles in an intermediate layer is B area % in a cross section horizontal to the thickness direction, and a DC value of 4.0 μm or less when an average particle size of the sintering aid particles in the surface layer is C μm and an average particle size of the sintering aid particles in the intermediate layer is D μm.
[0008] The aluminum nitride sintered body contains aluminum nitride particles having a predetermined average particle size, and the total amount and particle size distribution of the sintering aid particles satisfy the above-mentioned conditions. Therefore, the aluminum nitride sintered body has excellent uniformity of structure, suppresses stress concentration when force is applied, and can exhibit excellent bending strength.
[0009] The aluminum nitride sintered body may have a total amount of the sintering aid particles on the main surface of the body of less than 4.0% by area.
[0010] The aluminum nitride sintered body may have a cumulative frequency distribution curve of particle diameters measured by electron microscope image analysis of the aluminum nitride particles, where d90 is the particle diameter at which the integrated value from small particle diameters reaches 90% of the total, and the d90 is 13.0 μm or less.
[0011] In a cumulative frequency distribution curve of particle diameters of the aluminum nitride particles measured by electron microscope image analysis, when the particle diameter at which the integrated value from small particle diameters reaches 90% of the total is defined as d90, the difference between the d90 and the average particle diameter may be 1.0 to 3.5 μm.
[0012] One aspect of the present disclosure provides a circuit board including the above-mentioned aluminum nitride sintered body and a conductor portion attached to the aluminum nitride sintered body.
[0013] The circuit board includes the aluminum nitride sintered body described above, and therefore can withstand deformation between members even when used at high temperatures, and can exhibit excellent connection reliability.
[0014] One aspect of the present disclosure provides a laminated substrate including the above-mentioned aluminum nitride sintered body and a metal plate attached to the aluminum nitride sintered body.
[0015] The laminated substrate includes the aluminum nitride sintered body described above, and therefore can withstand deformation between members even when used at high temperatures, and can exhibit excellent connection reliability.
[0016] One aspect of the present disclosure provides a method for producing an aluminum nitride sintered body, comprising: a sintering step of sintering a molded body composed of a mixture containing aluminum nitride and a sintering aid to obtain a sintered body, wherein the sintering aid contains yttrium oxide and aluminum oxide, and a mass ratio of the aluminum oxide to the yttrium oxide is less than 0.5, the sintering step includes a step of obtaining a first sintered body from the molded body by heating at 1500 to 1700°C for 1 hour or more, and a step of obtaining the sintered body from the first sintered body by heating at more than 1700°C and not more than 1850°C for 1 hour or more, and the sintering time in the sintering step is 14.0 hours or less.
[0017] The method for producing the aluminum nitride sintered body uses sintering aids mixed in a specified ratio and sinters the material through at least two specified sintering steps, thereby producing an aluminum nitride sintered body having excellent bending strength as described above. Effect of the Invention
[0018] According to the present disclosure, it is possible to provide an aluminum nitride sintered body having excellent bending strength and a manufacturing method thereof. According to the present disclosure, it is also possible to provide a laminated substrate and a circuit substrate having excellent connection reliability, each of which includes the aluminum nitride sintered body. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a perspective view showing an example of an aluminum nitride sintered body. [Diagram 2] FIG. 2 is a perspective view showing an example of a laminated substrate. [Diagram 3] FIG. 3 is a perspective view showing an example of a circuit board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings as appropriate. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the description, the same reference numerals are used for the same elements or elements having the same functions, and redundant descriptions are omitted as the case may be. In addition, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of each element are not limited to those shown in the drawings.
[0021] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The sintering aid particles are particles containing a component derived from a sintering aid.
[0022] One embodiment of the aluminum nitride sintered body includes aluminum nitride particles and sintering aid particles. Fig. 1 is a perspective view showing an example of the aluminum nitride sintered body. The shape of the ceramic plate 100 made of the aluminum nitride sintered body may be, for example, a sheet shape, and is usually a rectangular parallelepiped shape.
[0023] The average particle diameter of the aluminum nitride particles is 2.0 to 10.0 μm. The upper limit of the average particle diameter of the aluminum nitride particles may be, for example, 9.5 μm or less, 9.0 μm or less, 8.0 μm or less, 7.0 μm or less, 6.0 μm or less, 5.0 μm or less, or 4.5 μm or less. When the upper limit of the average particle diameter is within the above range, the extension of defects in the particles due to grain growth can be suppressed, and the decrease in bending strength can be further suppressed. The lower limit of the average particle diameter of the aluminum nitride particles may be, for example, 2.5 μm or more, 3.0 μm or more, or 3.5 μm or more. When the lower limit of the average particle diameter is within the above range, an aluminum nitride sintered body having excellent bending strength and excellent thermal properties (thermal conductivity) can be obtained.
[0024] The average particle diameter of aluminum nitride particles in this specification means a value measured by the following method. First, a scanning electron microscope image (observed at 2000 times) of a cross section horizontal to the thickness direction of the aluminum nitride sintered body is obtained. The measurement target is a position at half the thickness of the aluminum nitride sintered body. At an arbitrary position in the obtained image, a region of 50 μm×50 μm is determined, and a particle size distribution of aluminum nitride particles is created using image analysis software. A particle diameter at which the cumulative frequency from the small particle diameter side in the cumulative frequency distribution curve of the particle diameter measured by the electron microscope image analysis obtained as described above is 50% is determined. In the same image, the particle diameters are determined for five regions in the same manner as described above, and the arithmetic average value is taken as the average particle diameter of aluminum nitride. Note that the shape of aluminum nitride particles is usually not constant. Therefore, the particle diameter of aluminum nitride particles is taken as the distance between the two most distant points on the periphery of the particle to be measured. For example, the image analysis software "GIMP2" (trade name) or "imageJ" (trade name), which are distributed under the GNU GPL, can be used.
[0025] In the above aluminum nitride sintered body, when the particle diameter when the integrated value from the small particle diameter reaches 90% of the total in the cumulative frequency distribution curve of the particle diameter measured by the electron microscope image analysis of the aluminum nitride particles is defined as d90, d90 may be, for example, 13.0 μm or less, 12.0 μm or less, 11.0 μm or less, 10.0 μm or less, 9.0 μm or less, 8.0 μm or less, 7.0 μm or less, 6.0 μm or less, or 5.5 μm or less. The upper limit of d90 within the above range means that the generation of coarse particles in the aluminum nitride sintered body is suppressed, and the sintered body structure is more uniform. In other words, the occurrence of stress concentration when a force is applied from the outside is suppressed, and the bending strength of the sintered body can be further improved. The lower limit of d90 may be, for example, 4.0 μm or more, or 4.5 μm or more. When the lower limit of d90 is within the above range, excellent bending strength can be exhibited and the deterioration of other properties such as thermal conductivity can be suppressed. If the lower limit of d90 is within the above range, the production of the aluminum nitride sintered body can be facilitated and an increase in costs can be suppressed. d90 may be adjusted within the above range, and may be, for example, 4.0 to 13.0 μm, or 4.0 to 6.0 μm.
[0026] The difference between the d90 and the average particle size of the aluminum nitride particles may be, for example, 1.0 to 3.5 μm. The difference between the d90 and the average particle size may be, for example, 3.0 μm or less, 2.8 μm or less, 2.6 μm or less, 2.4 μm or less, or 2.2 μm or less. When the upper limit of the difference is within the above range, the structure of the aluminum nitride sintered body can be made finer, and the size of defects and the like can be made smaller. The difference between the d90 and the average particle size may be, for example, 1.1 μm or more, or 1.2 μm or more. When the lower limit of the difference is within the above range, the production of the aluminum nitride sintered body can be made easier and an increase in costs can be suppressed.
[0027] In a cross section horizontal to the thickness direction of the aluminum nitride sintered body, when the total amount of the sintering aid particles in the surface layer is A area % and the total amount of the sintering aid particles in the intermediate layer is B area %, the BA value is 6.0 area % or less. The upper limit of the BA value may be, for example, 5.5 area % or less, 5.0 area % or less, 4.5 area % or less, or 4.0 area % or less. When the upper limit of the BA value is within the above range, the existence form and distribution of the sintering aid particles can be made more uniform, and thus the bending strength can be further improved. The lower limit of the BA value is not particularly limited, and may be, for example, 0.1 area % or more, or 0.2 area % or more. The BA value may be adjusted within the above range, and may be, for example, 0.1 to 6.0 area % or 0.1 to 5.5 area %.
[0028] In a cross section horizontal to the thickness direction of the aluminum nitride sintered body, when the average particle diameter of the sintering aid particles in the surface layer is C μm and the average particle diameter of the sintering aid particles in the intermediate layer is D μm, DC is 4.0 μm or less. The upper limit of the value of DC may be, for example, 3.5 μm or less, 3.0 μm or less, or 2.5 μm or less. The fact that the upper limit of DC is within the above range means that the variation of the sintering aid particles in the thickness direction of the aluminum nitride sintered body is suppressed, and the sintered body structure is more uniform. In other words, it is possible to suppress the occurrence of stress concentration when a force is applied from the outside, and to further improve the bending strength of the sintered body. The lower limit of the value of DC is not particularly limited, but may be, for example, 0.1 μm or more. The value of DC may be adjusted within the above range, and may be, for example, 0.1 to 4.0 μm, or 0.1 to 3.5 μm.
[0029] The total amount of sintering aid particles in this specification means a value measured by the following method. First, a scanning electron microscope image (observed at 2000 times) of a cross section horizontal to the thickness direction of the aluminum nitride sintered body is obtained. The measurement objects are a region (surface layer) from the surface layer of the aluminum nitride sintered body to 50 μm and a region (intermediate layer) from the half-thickness position to 100 μm above and below. At any position in each of the obtained images of the surface layer and intermediate layer, a region of 50 μm x 50 μm is determined, and the images are binarized (threshold: 140) using image analysis software to measure the total area of the sintering aid particles. In the same image, the total area of the sintering aid particles is determined for five regions in the same manner as described above, and the arithmetic average value is taken as the total amount of the sintering aid particles. For example, the image analysis software "GIMP2" (trade name) or "imageJ" (trade name), which are distributed under the GNU GPL, can be used. In addition, the average particle diameter of the sintering aid particles in this specification means a value obtained by measuring the circle equivalent diameters of the sintering aid particles in an image obtained by binarizing the scanning electron microscope image obtained as described above, and calculating the arithmetic mean of the obtained circle equivalent diameters.
[0030] Sintering aid particles can also be observed on the main surface of the aluminum nitride sintered body. The sintering aid particles observed on the main surface can be said to be residual sintering aids that are trying to escape from the main surface to the outside of the system during the manufacturing process of the aluminum nitride sintered body. If the amount of sintering aid particles observed on the main surface is large, the sintering aid will be insufficient inside the aluminum nitride sintered body, and the internal structure will tend to be non-uniform. In addition, if the amount of sintering aid that escapes increases and is removed outside the system without remaining on the main surface of the aluminum nitride sintered body, a recess where the auxiliary particles are missing will be formed on the main surface, which will affect the surface smoothness. In addition, if a recess where the sintering aid is missing is observed, the growth of aluminum nitride particles in the surface layer in the cross section horizontal to the thickness direction of the aluminum nitride sintered body tends to be insufficient. For this reason, the structure of the aluminum nitride sintered body may become non-uniform.
[0031] The total amount of the sintering aid particles on the main surface of the aluminum nitride sintered body may be, for example, less than 4.0 area%, 3.8 area% or less, 3.6 area% or less, 3.4 area% or less, 3.2 area% or less, or 3.0 area% or less. When the upper limit of the total amount of the sintering aid particles on the main surface is within the above range, the structure of the obtained aluminum nitride sintered body may be even denser. The lower limit of the total amount of the sintering aid particles on the main surface is not particularly limited, and may be, for example, 0.1 area% or more, 0.2 area% or more, or 0.5 area%. The total amount of the sintering aid particles on the main surface may be adjusted within the above range, and may be, for example, 0.1 area% or more and less than 4.0 area%, 0.1 to 3.8 area%, or 0.1 to 3.6 area%.
[0032] The total amount of sintering aid particles on the main surface means a value measured by the following method. First, a scanning electron microscope image (observed at 1000x) of the main surface of the aluminum nitride sintered body is obtained. A 1.2 mm x 1.2 mm region is determined at any position in the obtained image, and binarized (threshold: 140) using image analysis software to measure the total area of the sintering aid particles. In the same image, the total area of the sintering aid particles is determined for five regions in the same manner as described above, and the arithmetic average value is taken as the total amount of sintering aid particles. For example, "GIMP2" (trade name) or "imageJ" (trade name), which are distributed under the GNU GPL, can be used as the image analysis software.
[0033] The aluminum nitride sintered body is composed of aluminum nitride particles and sintering aid particles as described above, but may contain other components other than the aluminum nitride particles and the sintering aid particles within a range that does not impair the effects of the present invention. The other components may be, for example, additives for imparting desired effects, impurities, etc. The content of the other components may be, for example, 10.0 mass% or less, 5.0 mass% or less, 3.0 mass% or less, 1.0 mass% or less, or 0.5 mass% or less based on the total amount of the aluminum nitride sintered body.
[0034] The aluminum nitride sintered body has excellent bending strength. The bending strength of the aluminum nitride sintered body can be, for example, 360 MPa or more, 370 MPa or more, 390 MPa or more, 400 MPa or more, 450 MPa or more, or 500 MPa or more. The bending strength in this specification means a value measured in accordance with the method described in JIS C 2141:1992 "Testing methods for ceramic materials for electrical insulation". Specifically, it is measured according to the method described in the examples of this specification.
[0035] The aluminum nitride sintered body has a uniform structure, and therefore the distribution of the bending strength is sufficiently suppressed. The aluminum nitride sintered body has a relatively large Weibull coefficient in a Weibull statistical analysis of its bending strength. The Weibull coefficient of the bending strength of the aluminum nitride sintered body is, for example, 10.0 or more, 12.0 or more, or may be 13.0 or more, 14.0 or more, 15.0 or more, or 16.0 or more.
[0036] Weibull statistics are used to evaluate the distribution of bending strength. When a Weibull plot is created for an aluminum nitride sintered body, with the fracture probability F(σ) on the vertical axis and the bending strength σ (strength at fracture, flexural strength) on the horizontal axis, the slope m is the Weibull coefficient. The fracture probability F(σ) in the Weibull plot is given by the following formula (1). F(σ)=1-exp[-(σ / η) m ]···(1) In the above formula (1), η is a fitting parameter.
[0037] The above-mentioned aluminum nitride sintered body can be manufactured, for example, by the following method. One embodiment of the manufacturing method for an aluminum nitride sintered body includes a sintering step of sintering a molded body made of a mixture containing aluminum nitride and a sintering aid to obtain a sintered body.
[0038] First, raw materials are prepared. Examples of the raw materials include aluminum nitride, a sintering aid, and additives as necessary. Examples of the additives include binders, plasticizers, dispersion media, and release agents. Examples of the binders include methylcellulose-based binders having plasticity or surface activity, and acrylic ester-based binders having excellent thermal decomposition properties. Examples of the plasticizers include glycerin. Examples of the dispersion media include ion-exchanged water and ethanol.
[0039] The aluminum nitride is not particularly limited, and aluminum nitride powder produced by known methods such as a direct nitridation method in which metallic aluminum is nitrided in a nitrogen atmosphere, and a reduction nitridation method in which aluminum oxide is reduced with carbon can be used.
[0040] The sintering aid contains yttrium oxide and aluminum oxide. The sintering aid may be granular. The mass ratio of aluminum oxide to yttrium oxide (aluminum oxide content / yttrium oxide content) is less than 0.5. This can suppress the agglomeration of oxides in the aluminum nitride sintered body. The blending ratio of yttrium oxide and aluminum oxide can be adjusted within the above-mentioned range, and this can also adjust the composition of oxides in the aluminum nitride sintered body. Aluminum oxide and yttrium oxide form a liquid phase of a composite oxide during sintering to promote sintering. This can make the aluminum nitride sintered body sufficiently dense.
[0041] The content of the sintering aid may be, for example, 1 to 10.0 parts by mass relative to 100 parts by mass of aluminum nitride. By setting the content of the sintering agent within the above range, the density of the resulting aluminum nitride sintered body can be improved, and the bending strength can be further improved. By setting the content of the sintering aid within the above range, the thermal conductivity of the resulting aluminum nitride sintered body can also be improved. The content of the sintering aid is a value calculated based on the amount of the sintering aid converted into oxide.
[0042] The content of aluminum oxide may be, for example, 0.1 to 5.0 parts by mass relative to 100 parts by mass of aluminum nitride. By making the content of aluminum oxide 0.1 parts by mass or more, the density of the obtained sintered body can be further improved. By making the content of aluminum oxide 5.0 parts by mass or less, the relative content ratio of aluminum nitride can be increased, and the decrease in the thermal conductivity of the obtained sintered body can be further suppressed.
[0043] Aluminum nitride, a sintering aid, and additives added as necessary may be blended and mixed to be used as a molding raw material. The molding raw material is molded into, for example, a sheet shape by a known method such as a doctor blade method. The obtained molded body may be degreased. The degreasing method is not particularly limited, and for example, the molded body may be heated to 300 to 700°C in air or a non-oxidizing atmosphere such as nitrogen. The heating time may be, for example, 1 to 10 hours.
[0044] The aluminum nitride sintered body can be obtained by firing the above-mentioned molded body. The firing step (hereinafter also referred to as the firing step) may be carried out in an inert gas atmosphere. The inert gas may be, for example, nitrogen. The firing step may be carried out under atmospheric pressure.
[0045] The firing process includes a process of obtaining a first fired body from the molded body by heating at 1500 to 1700°C for 1 hour or more (hereinafter also referred to as the first firing process), and a process of obtaining the sintered body from the first fired body by heating at a temperature higher than 1700°C and not higher than 1850°C for 1 hour or more (hereinafter also referred to as the second firing process).
[0046] The firing temperature in the first firing step can be selected depending on the composition of the sintering aid, and may be, for example, 1650°C or higher, or 1680°C or higher. The heating rate until the firing temperature in the first firing step is reached may be relatively high, for example, 20°C / min or higher, or 30°C / min or higher. In the first firing step, the firing temperature is preferably maintained for a predetermined time. The firing time in the first firing step may be, for example, 1.0 hour or more, 2.0 hours or more, or 2.5 hours or more.
[0047] The firing temperature in the second firing step may be, for example, less than 1850°C, less than 1840°C, or 1830°C or less, from the viewpoint of improving the texture density of the obtained sintered body and suppressing the loss of the auxiliary agent in the surface layer. The heating rate until the above firing temperature in the second firing step is reached may be, for example, 0.5°C / min or more, or 1.0°C / min or more. In the second firing step, the above firing temperature is preferably maintained for a predetermined time. The firing time in the second firing step may be, for example, 1.0 hour or more, 1.5 hours or more, or 2.0 hours or more.
[0048] The firing time in this specification means the time during which the temperature of the atmosphere in which the object to be fired, such as the molded body, is placed is maintained at the firing temperature after it has reached the firing temperature.
[0049] The total firing time of the first firing step and the second firing step in the firing step is 14.0 hours or less, but may be, for example, 10.0 hours or less, 8.0 hours or less, or 7.0 hours or less. By setting the total firing time within the above range, it is possible to reduce the sintering aid in the surface layer of the molded body or aluminum nitride sintered body from passing through to the surface of the molded body or aluminum nitride sintered body, and to reduce surface roughness. The total firing time of the first firing step and the second firing step in the firing step may be, for example, 4.5 hours or more, or 5.0 hours or more. By setting the total firing time within the above range, the sintering aid is melted, the aluminum nitride particles are sufficiently dissolved, and the aluminum nitride particles can grow in a more uniform environment, so that an aluminum nitride sintered body having a more uniform particle size distribution and a more dense structure can be prepared. The firing time of the firing step can be adjusted within the above range, and may be, for example, 5.0 to 8.0 hours.
[0050] The aluminum nitride sintered body obtained by the above-mentioned manufacturing method may be processed into a desired shape as necessary. The aluminum nitride sintered body may be processed into a plate shape to be an aluminum nitride plate. A metal part such as a metal circuit or a metal plate may be attached to the aluminum nitride plate to form a substrate. The substrate may be, for example, a laminated substrate in which the main surface of an aluminum nitride plate and the main surface of a metal plate such as a copper plate are joined. Also, the substrate may be a circuit board in which a circuit pattern serving as a conductor part is formed by removing a part of the metal plate by etching or the like. Thus, the substrate of the present disclosure may be a laminated substrate or a circuit board. In the case of a plate shape, the lower limit of the thickness of the aluminum nitride sintered body may be, for example, 0.10 mm or more, 0.20 mm or more, or 0.25 mm or more. In the case of a plate shape, the upper limit of the thickness of the aluminum nitride sintered body may be, for example, 3.00 mm or less, 1.50 mm or less, or 1.00 mm or less. The thickness of the aluminum nitride sintered body can be adjusted within the above range, and may be, for example, 0.10 to 3.00 mm, or 0.25 to 1.00 mm. By setting the thickness of the aluminum nitride sintered body within the above range, the heat dissipation characteristics and thermal resistivity of the entire circuit board can be simultaneously achieved at higher levels.
[0051] One embodiment of the laminated substrate includes the aluminum nitride sintered body and a metal plate attached to the aluminum nitride sintered body. FIG. 2 is a perspective view showing an example of the laminated substrate. The laminated substrate 200 includes a pair of metal plates 110 arranged to face each other, and a ceramic plate 100 composed of an aluminum nitride sintered body between the pair of metal plates 110. The metal plate 110 may be, for example, a copper plate. The ceramic plate 100 and the metal plate 110 may have the same shape and size or may have different shapes and sizes. The metal plate 110 and the ceramic plate 100 may be joined by, for example, a brazing material. One of the pair of metal plates 110 may be a heat dissipation material, and the other may be processed into a circuit pattern. The circuit pattern may be formed by etching the metal plate 110 using a resist. This makes it possible to form a circuit board that can sufficiently suppress leakage current, etc., or a heat dissipation board.
[0052] One embodiment of the circuit board includes the aluminum nitride sintered body described above and a conductor portion attached to the aluminum nitride sintered body. Fig. 3 is a perspective view showing an example of the circuit board. The circuit board 300 includes a ceramic plate 100, a plurality of conductor portions 20, and a metal plate 110. The conductor portions 20 are provided on one surface 100A of the ceramic plate 100, and the metal plate 110 is provided on the other surface of the ceramic plate 100. When the circuit board 300 is used in a power module, the metal plate 110 may function as a heat dissipation material.
[0053] The ceramic plate 100 in the laminated substrate 200 and the circuit substrate 300 is made of an aluminum nitride sintered body having excellent electrical insulation and thermal conductivity, and therefore has excellent reliability when used in various products such as power modules.
[0054] Although several embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. For example, the shape and structure of the substrate of the present disclosure are not limited to those shown in Figs. 2 and 3. For example, a circuit pattern may be formed on both main surfaces of the ceramic plate 100. Also, instead of forming the conductor portion 20 by etching the metal plate 110, the conductor portion 20 may be formed by spraying metal powder and subjecting it to heat treatment. Also, the contents of the description of the above-mentioned embodiments can be mutually applied. EXAMPLES
[0055] The present disclosure will be described in more detail below using examples and comparative examples. Note that the present disclosure is not limited to the following examples.
[0056] Example 1 (Preparation of sintered aluminum nitride) 100 parts by mass of aluminum nitride powder were mixed with 6.0 parts by mass of yttrium oxide powder as a sintering aid and 0.3 parts by mass of α-aluminum oxide, and mixed using a ball mill to obtain a mixed powder. 6 parts by mass of cellulose ether binder (manufactured by Shin-Etsu Chemical Co., Ltd., product name: Metrose), 5 parts by mass of glycerin (manufactured by Kao Corporation, product name: Exepar), and 10 parts by mass of ion-exchanged water were added to 100 parts by mass of the mixed powder, and mixed for 1 minute using a Henschel mixer to obtain a molding raw material.
[0057] This molding raw material was molded by a screw-type extrusion molding machine to produce a sheet-like molded body (width: 80 mm, thickness: 0.8 mm), which was dried at 100°C for 1 hour and then cut to obtain a molded body with a length: 60 mm x width: 60 mm shape. After applying boron nitride powder as a release agent to this molded body, a stacking test was performed on multiple of the above laminates, and the mass of the laminate was adjusted to 95 kg. The obtained laminate was degreased by heating at 570°C for 10 hours in air, and a degreased body was obtained.
[0058] Next, the degreased body was placed in a heating furnace, and in a nitrogen gas atmosphere, the temperature was increased from 25°C to 1700°C at a rate of 20°C / min under atmospheric pressure, and held at 1700°C for 2.0 hours (first firing step). Next, the temperature was increased to 1830°C at a rate of 5°C / min, and held at 1830°C for 8 hours (second firing step). After that, the heating was stopped, and the body was allowed to cool in the heating furnace to obtain an aluminum nitride sintered body.
[0059] <Measurement of physical properties of sintered aluminum nitride> For the obtained aluminum nitride sintered body, the d50 (average particle size) and d90 of the aluminum nitride particles, the total amount of the sintering aid particles, and the average particle size of the sintering aid particles were measured. The results are shown in Table 1.
[0060] <Evaluation of Aluminum Nitride Sintered Body> The flexural strength and flexural strength distribution (Weibull coefficient) of the obtained aluminum nitride sintered body were measured. The flexural strength of the aluminum nitride sintered body was measured in accordance with the method described in JIS C 2141:1992 "Testing methods for ceramic materials for electrical insulation". In addition, a Weibull plot was created based on the obtained flexural strength results, and the Weibull coefficient was determined. The results are shown in Table 1.
[0061] Example 2 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that the heating rate in the first firing step was changed to 30°C / min and the firing time was changed to 1.0 hour, and that the firing temperature in the second firing step was changed to 1800°C and the firing time was changed to 1 hour.
[0062] Example 3 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that the firing time in the first firing step was changed to 8.0 hours, and that the firing temperature in the second firing step was changed to 1850°C and the firing time was changed to 4 hours.
[0063] Example 4 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that in the second firing step, the firing temperature was changed to 1820° C. and the firing time was changed to 4 hours.
[0064] Example 5 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that in the first firing step, the firing temperature was changed to 1500°C and the firing time was changed to 3 hours, and in the second firing step, the firing temperature was changed to 1800°C and the firing time was changed to 4 hours.
[0065] Example 6 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that in the second firing step, the heating rate was changed to 1° C. / min, the firing temperature was changed to 1840° C., and the firing time was changed to 2 hours.
[0066] Example 7 An aluminum nitride sintered body was prepared in the same manner as in Example 1, except that in the second firing step, the heating rate was changed to 1° C. / min, the firing temperature was changed to 1830° C., and the firing time was changed to 2 hours.
[0067] <Measurement and evaluation of physical properties of aluminum nitride sintered body> For the aluminum nitride sintered bodies obtained in Examples 2 to 7, the d50 (average particle size) and d90 of the aluminum nitride particles, the total amount of the sintering aid particles, and the average particle size of the sintering aid particles were measured in the same manner as in Example 1. The results are shown in Table 1.
[0068] <Evaluation of sintered aluminum nitride> For the aluminum nitride sintered bodies obtained in Examples 2 to 7, the bending strength and bending strength distribution (Weibull coefficient) were measured in the same manner as in Example 1. The results are shown in Table 1.
[0069] [Table 1]
[0070] Comparative Example 1 An aluminum nitride sintered body was obtained in the same manner as in Example 1, except that in the first firing step, the heating rate was changed to 30°C / min, the firing temperature was changed to 1450°C, and in the second firing step, the heating rate was changed to 0.3°C / min, the firing temperature was changed to 1900°C, and the firing time was changed to 2 hours.
[0071] Comparative Example 2 An aluminum nitride sintered body was prepared in the same manner as in Comparative Example 1, except that in the second firing step, the heating rate was changed to 5° C. / min, the firing temperature was changed to 1870° C., and the firing time was changed to 10 hours.
[0072] Comparative Example 3 An aluminum nitride sintered body was prepared in the same manner as in Comparative Example 1, except that in the first firing step, the heating rate was changed to 10°C / min, the firing temperature was changed to 1750°C, and the firing time was changed to 8 hours, and in the second firing step, the heating rate was changed to 5.0°C / min, and the firing temperature was changed to 1870°C.
[0073] Comparative Example 4 An aluminum nitride sintered body was prepared in the same manner as in Comparative Example 1, except that in the first firing step, the heating rate was changed to 40°C / min, the firing temperature was changed to 1750°C, and the firing time was changed to 0.5 hours, and in the second firing step, the heating rate was changed to 10°C / min, and the firing temperature was changed to 1800°C.
[0074] <Measurement and evaluation of physical properties of aluminum nitride sintered body> For the aluminum nitride sintered bodies obtained in Comparative Examples 2 to 4, the d50 (average particle size) and d90 of the aluminum nitride particles, as well as the total amount of sintering aid particles and the average particle size of the sintering aid particles, were measured in the same manner as in Example 1. The results are shown in Table 2.
[0075] <Evaluation of sintered aluminum nitride> For the aluminum nitride sintered bodies obtained in Comparative Examples 2 to 4, the bending strength and bending strength distribution (Weibull coefficient) were measured in the same manner as in Example 1. The results are shown in Table 2.
[0076] [Table 2] [Industrial Applicability]
[0077] According to the present disclosure, it is possible to provide an aluminum nitride sintered body having excellent bending strength and a manufacturing method thereof. According to the present disclosure, it is also possible to provide a laminated substrate and a circuit substrate having excellent connection reliability, each of which includes the aluminum nitride sintered body. [Explanation of symbols]
[0078] 20... conductor portion, 100... ceramic plate (aluminum nitride sintered body), 110... metal plate, 200... laminated substrate, 300... circuit board.
Claims
1. Aluminum nitride particles and sintering aid particles are included, The average particle size of the aluminum nitride particles is 2.0 to 10.0 μm, In a cross section horizontal to the thickness direction, When the total amount of the sintering aid particles in the surface layer is A area % and the total amount of the sintering aid particles in the intermediate layer is B area %, the value of B-A is 6.0 area % or less, An aluminum nitride sintered body, in which, when the average particle diameter of the sintering aid particles in the surface layer is C μm and the average particle diameter of the sintering aid particles in the intermediate layer is D μm, D - C is 4.0 μm or less.
2. 2. The aluminum nitride sintered body according to claim 1, wherein a total amount of said sintering aid particles on the main surface is less than 4.0 area %.
3. 3. The aluminum nitride sintered body according to claim 1, wherein, in a cumulative frequency distribution curve of particle diameters measured by electron microscope image analysis of the aluminum nitride particles, d90 is the particle diameter at which an integrated value from small particle diameters reaches 90% of the total, and d90 is 13.0 μm or less.
4. The aluminum nitride sintered body according to any one of claims 1 to 3, wherein, in a cumulative frequency distribution curve of particle diameters measured by electron microscope image analysis of the aluminum nitride particles, the particle diameter at which an integrated value from small particle diameters reaches 90% of the total is defined as d90, and the difference between the d90 and the average particle diameter is 1.0 to 3.5 μm.
5. A circuit board comprising the aluminum nitride sintered body according to any one of claims 1 to 4, and a conductor portion attached to the aluminum nitride sintered body.
6. A laminated substrate comprising the aluminum nitride sintered body according to any one of claims 1 to 4, and a metal plate attached to the aluminum nitride sintered body.
Citation Information
Patent Citations
Aln sintered compact and production thereof
JP1993024930A
Manufacture of aluminum nitride substrate
JP1993226795A
Aluminum nitride sintered compact and method of manufacturing the same
JP2005075695A
Ceramic copper circuit board and semiconductor device
JP2010183096A
Aluminum nitride sintered body and manufacturing method thereof
JP2018184316A