Non-aqueous electrolyte and non-aqueous electrolyte battery

By adding specific metal ions to lithium fluorosulfonate-containing non-aqueous electrolytes, the charge storage characteristics of non-aqueous electrolyte batteries are improved in high-temperature environments, addressing the issue of insufficient performance.

JP7579784B2Active Publication Date: 2024-11-08MITSUBISHI CHEM CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021524899
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-15
Filing Date
2020-06-04
Publication Date
2024-11-08
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

Lithium fluorosulfonate-containing non-aqueous electrolytes exhibit insufficient charge storage characteristics in high-temperature environments.

Method used

Incorporating specific amounts of metal ions such as nickel, cobalt, copper, manganese, or aluminum ions within a non-aqueous electrolyte, along with lithium fluorosulfonate, to improve charge storage characteristics in high-temperature environments.

Benefits of technology

Enhances the charge storage performance of non-aqueous electrolyte batteries in high-temperature conditions by reducing negative electrode reduction reactions and increasing reduction resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579784000001
    Figure 0007579784000001
  • Figure 0007579784000002
    Figure 0007579784000002
  • Figure 0007579784000003
    Figure 0007579784000003
Patent Text Reader

Abstract

Provided are: a non-aqueous electrolyte which contains FSO3Li and by which the charging preservation characteristics of a non-aqueous electrolyte battery in a high-temperature environment can be improved; and a non-aqueous electrolyte battery having excellent charging preservation characteristics in a high-temperature environment. This non-aqueous electrolyte contains FSO3Li, and a specific amount of specific metal element ions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nonaqueous electrolyte and a nonaqueous electrolyte battery, and more particularly to a nonaqueous electrolyte containing a specific compound and a specific amount of a specific metal element ion, and a nonaqueous electrolyte battery using this nonaqueous electrolyte. [Background technology]

[0002] 2. Description of the Related Art In recent years, non-aqueous electrolyte batteries such as lithium secondary batteries have been put to practical use as on-board power sources for driving electric vehicles and the like.

[0003] As a means for improving the battery characteristics of non-aqueous electrolyte batteries, many studies have been conducted in the fields of positive and negative electrode active materials and additives for non-aqueous electrolytes.

[0004] For example, in Patent Document 1, M(FSO3) is used to improve the initial charge capacity and input / output characteristics of non-aqueous electrolyte secondary batteries. x The present invention discloses a nonaqueous electrolyte and a nonaqueous electrolyte secondary battery, which further contains LiPF6 in addition to a nonaqueous electrolyte containing at least one fluorosulfonate represented by the following formula: Patent Document 2 aims to provide a nonaqueous electrolyte solution capable of improving electrochemical characteristics over a wide temperature range, and an electricity storage device using the same. The nonaqueous electrolyte solution is characterized in that the nonaqueous electrolyte solution contains an electrolyte salt dissolved in a nonaqueous solvent and contains 0.001 to 5 mass % of a specific noncyclic lithium salt, and the electricity storage device using the same is disclosed. Patent Document 3 describes a nonaqueous electrolyte secondary battery having an electrode assembly including a positive electrode and a negative electrode, and a nonaqueous electrolyte, with the aim of providing a nonaqueous electrolyte secondary battery capable of exhibiting higher battery performance by forming a stable coating on the surface of a negative electrode active material (graphite material); the negative electrode has a negative electrode active material layer mainly made of graphite material, and the amount of acidic functional groups of the graphite material is 1 μeq / m 2The nonaqueous electrolyte secondary battery is disclosed, which is characterized in that a coating containing sulfur (S) atoms and charge carriers is formed on the surface of the graphite material. Patent Document 4 discloses a lithium ion secondary battery having excellent durability, the battery comprising a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, and a non-aqueous electrolyte, in which tungsten is present on the surface of the positive electrode active material, and lithium fluorosulfonate is added to the non-aqueous electrolyte, with the aim of providing a lithium ion secondary battery having excellent durability. This document describes that the above-mentioned configuration makes it possible to provide a lithium ion battery having excellent durability, which can maintain low reaction resistance for a long period of time even when the battery is used for a long period of time, without the metal element attached to the surface of the positive electrode being eluted into the non-aqueous electrolyte. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2011 / 099585 [Patent Document 2] International Publication No. 2013 / 168821 [Patent Document 3] JP 2014-127313 A [Patent Document 4] JP 2015-037012 A Summary of the Invention [Problem to be solved by the invention]

[0006] The durability of non-aqueous electrolyte batteries tends to improve by adding lithium fluorosulfonate (FSO3Li) to the non-aqueous electrolyte. On the other hand, according to the study by the present inventors, it was found that batteries containing a non-aqueous electrolyte containing FSO3Li have insufficient charged storage characteristics in a high-temperature environment. Therefore, the present invention provides a non-aqueous electrolyte containing FSO3Li that can improve the charged storage characteristics of non-aqueous electrolyte batteries in a high-temperature environment, and a non-aqueous electrolyte battery having excellent charged storage characteristics in a high-temperature environment. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that the charged storage characteristics of a nonaqueous electrolyte battery in a high temperature environment can be improved by further adding at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e) to a nonaqueous electrolyte solution containing FSO3Li, and by setting the content of any one of the metal ions (a) to (e) within a specific range, the present inventors have arrived at the present invention.

[0008] That is, the present invention provides specific embodiments as shown in [1] to [9] below. [1] (1a) Contains FSO3Li, (1b) containing at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e); and (1c) A non-aqueous electrolyte solution that satisfies at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) The concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less. (iii) The concentration of (c) is 1 ppm by mass or more and 500 ppm by mass or less. (iv) The concentration of (d) is 1 ppm by mass or more and 100 ppm by mass or less. (v) The concentration of (e) is 1 ppm by mass or more and 100 ppm by mass or less. [2] The nonaqueous electrolyte according to [1], which contains at least nickel ions (a). [3] The nonaqueous electrolyte solution according to [2], containing nickel ions in an amount of 40 mass% or more based on the total amount of the metal ions (a) to (e). [4] The nonaqueous electrolyte solution according to [3], wherein the total concentration of (a) to (e) is 1 ppm by mass or more and 120 ppm by mass or less. [5] The content of FSO3Li is 0.001% by mass or more and 10.0% by mass or less; [1] The nonaqueous electrolyte solution according to any one of items [1] to [4]. [6] A non-aqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a non-aqueous electrolyte, (1a) Contains FSO3Li, (1b) containing at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e); and (1c) A nonaqueous electrolyte battery, the nonaqueous electrolyte satisfying at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) The concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less. (iii) The concentration of (c) is 1 ppm by mass or more and 500 ppm by mass or less. (iv) The concentration of (d) is 1 ppm by mass or more and 100 ppm by mass or less. (v) The concentration of (e) is 1 ppm by mass or more and 100 ppm by mass or less. [7] The nonaqueous electrolyte battery according to [6], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following composition formula (1): Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≦ a1 ≦ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [8] The positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (2). [6] The non-aqueous electrolyte battery according to Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90 ≦ a2 ≦ 1.10, 0.4 ≦ b2 < 1.0, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [9] The non-aqueous electrolyte battery according to any one of [6] to [8], wherein the positive electrode is an NMC positive electrode and the content of nickel element in the NMC positive electrode is 40 mol% or more.

[0009] As a result of intensive studies to solve the above problems, the present inventors have found that by using a non-aqueous electrolyte containing FSO3Li, further containing nickel ions, and having a nickel ion content within a specific range, the charge storage characteristics of the non-aqueous electrolyte battery under a high-temperature environment can be improved, and aspect A of the present invention has been reached.

[0010] That is, aspect A of the present invention provides the following specific aspects [A1] to [A8]. [A1] A non-aqueous electrolyte containing FSO3Li and containing 1 mass ppm or more and 500 mass ppm or less of nickel ions. [A2] The non-aqueous electrolyte according to [A1], wherein the content of FSO3Li is 0.001 mass% or more and 10.0 mass% or less. [A3] A non-aqueous electrolyte battery comprising a positive electrode and a negative electrode capable of occluding and releasing metal ions, and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains FSO3Li and contains nickel ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. [A4] The non-aqueous electrolyte battery according to [A3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (1). Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≦ a1 ≦ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [A5] The non-aqueous electrolyte battery according to [A3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (2). Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90 ≦ a2 ≦ 1.10, 0.4 ≦ b2 < 1.0, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [A6] The non-aqueous electrolyte battery according to any one of [A3] to [A5], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 30 mol% or more. [A7] The non-aqueous electrolyte battery according to [A3], [A5], or [A6], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 40 mol% or more. [A8] The non-aqueous electrolyte battery according to any one of [A3] to [A7], wherein the content of FSO3Li in the non-aqueous electrolyte is 0.001% by mass or more and 10.0% by mass or less.

[0011] As a result of intensive studies to solve the above problems, the present inventors have found that, for a non-aqueous electrolyte containing FSO3Li, by using a non-aqueous electrolyte further containing cobalt ions and having a cobalt ion content within a specific range, the charge storage characteristics of a non-aqueous electrolyte battery under a high-temperature environment can be improved, and aspect B of the present invention has been reached.

[0012] That is, aspect B of the present invention provides the following specific aspects [B1] to [B8]. [B1] A non-aqueous electrolyte containing FSO3Li and containing cobalt ions in an amount of 1 mass ppm or more and 500 mass ppm or less. [B2] The non-aqueous electrolyte according to [B1], wherein the content of FSO3Li is 0.001 mass% or more and 10.0 mass% or less. [B3] A non-aqueous electrolyte battery including a positive electrode and a negative electrode capable of occluding and releasing metal ions and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains FSO3Li and contains cobalt ions in an amount of 1 mass ppm or more and 500 mass ppm or less. [B4] The non-aqueous electrolyte battery according to [B3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (1). Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≤ a1 ≤ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [B5] The non-aqueous electrolyte battery according to [B3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (2). Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90≦a2≦1.10, 0.4≦b2<1.0, and b2+c2+d2=1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [B6] The nonaqueous electrolyte battery according to any one of [B3] to [B5], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 30 mol % or more. [B7] The nonaqueous electrolyte battery according to [B3], [B5] or [B6], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 40 mol % or more. [B8] The nonaqueous electrolyte battery according to any one of [B3] to [B7], wherein the content of FSO3Li in the nonaqueous electrolyte is 0.001% by mass or more and 10.0% by mass or less.

[0013] As a result of intensive research aimed at solving the above problems, the present inventors have found that the charged storage characteristics of a nonaqueous electrolyte battery in a high temperature environment can be improved by using a nonaqueous electrolyte solution that further contains copper ions in addition to a nonaqueous electrolyte solution containing FSO3Li, and that has a copper ion content within a specific range, and have arrived at aspect C of the present invention.

[0014] That is, aspect C of the present invention provides specific aspects shown in [C1] to [C8] below. [C1] A non-aqueous electrolyte containing FSO3Li and copper ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. [C2] The nonaqueous electrolyte solution according to [C1], wherein the content of FSO3Li is 0.001% by mass or more and 10.0% by mass or less. [C3] A nonaqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a nonaqueous electrolyte, the nonaqueous electrolyte containing FSO3Li and containing copper ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. [C4] The nonaqueous electrolyte battery according to [C3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following composition formula (1): Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≤ a1 ≤ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [C5] The positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the non-aqueous electrolyte battery according to [C3], wherein the positive electrode active material is a metal oxide represented by the following compositional formula (2). Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90 ≤ a2 ≤ 1.10, 0.4 ≤ b2 < 1.0, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [C6] The non-aqueous electrolyte battery according to any one of [C3] to [C5], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 30 mol% or more. [C7] The non-aqueous electrolyte battery according to [C3], [C5], or [C6], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 40 mol% or more. [C8] The non-aqueous electrolyte battery according to any one of [C3] to [C7], wherein the content of LiFSO3 in the non-aqueous electrolyte is 0.001% by mass or more and 10.0% by mass or less.

[0015] As a result of intensive studies to solve the above problems, the present inventors have found that by using a non-aqueous electrolyte containing LiFSO3 and further containing manganese ions and having the content of manganese ions within a specific range, the charge storage characteristics of the non-aqueous electrolyte battery under high-temperature environments can be improved, and aspect D of the present invention has been achieved.

[0016] That is, Aspect D of the present invention provides the following specific aspects and the like shown in [D1] to [D8]. [D1] A non-aqueous electrolyte containing FSO3Li and containing manganese ions in an amount of 1 mass ppm or more and 100 mass ppm or less. [D2] The non-aqueous electrolyte according to [D1], wherein the content of FSO3Li is 0.001 mass % or more and 10.0 mass % or less. [D3] A non-aqueous electrolyte battery including a positive electrode and a negative electrode capable of occluding and releasing metal ions and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains FSO3Li and contains manganese ions in an amount of 1 mass ppm or more and 100 mass ppm or less. [D4] The non-aqueous electrolyte battery according to [D3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (1). Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≦ a1 ≦ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [D5] The non-aqueous electrolyte battery according to [D3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (2). Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90 ≦ a2 ≦ 1.10, 0.4 ≦ b2 < 1.0, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [D6] The non-aqueous electrolyte battery according to any one of [D3] to [D5], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 30 mol % or more. [D7] The non-aqueous electrolyte battery according to [D3], [D5] or [D6], wherein the positive electrode is an NMC positive electrode and the content of nickel element in the NMC positive electrode is 40 mol% or more. [D8] The non-aqueous electrolyte battery according to any one of [D3] to [D7], wherein the content of LiFSO3 in the non-aqueous electrolyte is 0.001% by mass or more and 10.0% by mass or less.

[0017] As a result of intensive studies to solve the above problems, the present inventors have found that by further containing aluminum ions in a non-aqueous electrolyte containing LiFSO3 and setting the content of aluminum ions within a specific range, the charge storage characteristics of the non-aqueous electrolyte battery under a high-temperature environment can be improved, and aspect E of the present invention has been reached.

[0018] That is, aspect E of the present invention provides the following specific aspects [E1] to [E8]. [E1] A non-aqueous electrolyte containing LiFSO3 and containing 1 mass ppm or more and 100 mass ppm or less of aluminum ions. [E2] The non-aqueous electrolyte according to [E1], wherein the content of LiFSO3 is 0.001% by mass or more and 10.0% by mass or less. [E3] A non-aqueous electrolyte battery including a positive electrode and a negative electrode capable of occluding and releasing metal ions and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains LiFSO3 and contains 1 mass ppm or more and 100 mass ppm or less of aluminum ions. [E4] The non-aqueous electrolyte battery according to [E3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following compositional formula (1). Li a1 Ni b1 Co c1 M d1 O2···(1) (In the above formula (1), a1, b1, c1 and d1 satisfy 0.90 ≤ a1 ≤ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti and Er.) [E5] The nonaqueous electrolyte battery according to [E3], wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following composition formula (2): Li a2 Ni b2 Co c2 M d2 O2···(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90≦a2≦1.10, 0.4≦b2<1.0, and b2+c2+d2=1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) [E6] The nonaqueous electrolyte battery according to any one of [E3] to [E5], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 30 mol % or more. [E7] The nonaqueous electrolyte battery according to [E3], [E5] or [E6], wherein the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is 40 mol % or more. [E8] The nonaqueous electrolyte battery according to any one of [E3] to [E7], wherein the content of FSO3Li in the nonaqueous electrolyte is 0.001% by mass or more and 10.0% by mass or less. Effect of the Invention

[0019] By using the nonaqueous electrolyte of the present invention, it is possible to obtain a nonaqueous electrolyte battery having improved charged storage characteristics in a high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the embodiments of the present invention will be described in detail. The following embodiments are examples (representative examples) of the present invention, and the present invention is not limited to these. Furthermore, the present invention can be modified and carried out as desired without departing from the scope of the present invention.

[0021] <1.Non-aqueous electrolyte> A nonaqueous electrolyte according to one embodiment of the present invention contains FSO3Li and contains ions of specific metal elements in a specific range of amounts. Hereinafter, a non-aqueous electrolyte according to an embodiment of the present invention will be described in detail. The explanations in each section of this specification are applicable to all aspects except for the explanations regarding ions of specific metal elements.

[0022] <1-1.FSO3Li> The nonaqueous electrolyte of this embodiment contains FSO3Li. The content of FSO3Li in the nonaqueous electrolyte is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, even more preferably 0.010% by mass or more, and particularly preferably 0.10% by mass or more. On the other hand, although there is no particular upper limit, it is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, even more preferably 5.0% by mass or less, especially preferably 4.0% by mass or less, and particularly preferably 3.0% by mass or less. When the content of FSO3Li in the nonaqueous electrolyte is 10.0% by mass or less, it is preferable in that the negative electrode reduction reaction does not increase to such an extent that the internal resistance of the nonaqueous electrolyte battery increases, and when it is 0.001% by mass or more, it is preferable in that the effect of the present application of containing FSO3Li is obtained. Therefore, within the above range, the negative electrode reduction reaction in a high-temperature environment is suppressed, and thus the charged storage characteristics in a high-temperature environment can be improved. FSO3Li may be synthesized by a known method or may be a commercially available product. When measuring the amount of FSO3Li in the electrolyte of a nonaqueous electrolyte battery, a member containing the nonaqueous electrolyte may be removed from the nonaqueous electrolyte battery, and the nonaqueous electrolyte may be extracted and measured. For example, extraction may be performed using a centrifuge, or the nonaqueous electrolyte may be extracted using an organic solvent. Ice-cooled pure water is added to the extracted nonaqueous electrolyte, and the mixture is quickly mixed, and the SO4 separated by anion ion chromatography (e.g., Thermo Fisher Scientific, ICS-2000, column: AS23, eluent: 5.0 mM Na2CO3 / 0.9 mM NaHCO3, detection method: suppressor-equipped electrical conductivity detection method (12.5 mM H2SO4)) is immediately measured. 2- ions and FSO3 - ions to SO42- From the calibration curve of the ions, the molar sensitivity ratio [k(SO4 2- ) / k(FSO3 - )] = 2.0 and converting it to FSO3 - Ions can be quantified. Usually, in non-aqueous electrolytes, FSO3 - The amount of ions can be regarded as the amount of FSO3Li. On the other hand, as described later, FSO3 - For example, Al(FSO3)3 may be used as the aluminum ion source. In this case, the FSO3 in the non-aqueous electrolyte solution - From the total amount of ions, FSO3 derived from Al(FSO3)3 - If it is unclear whether Al(FSO3)3 was used as the aluminum ion source, the amount of FSO3Li in the non-aqueous electrolyte can be calculated by subtracting the amount of ions. - The amount of ions may be considered as the amount of FSO3Li.

[0023] <1-2. Metal ions> A nonaqueous electrolyte according to one embodiment of the present invention contains at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d), and aluminum ions (e), and satisfies at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) The concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less. (iii) (c) The concentration is 1 ppm by mass or more and 500 ppm by mass or less. (iv) (d) concentration is 1 ppm by mass or more and 100 ppm by mass or less (v) (e) concentration is 1 ppm by mass or more and 100 ppm by mass or less In this specification, the content of the specific ions (a) to (e) in the non-aqueous electrolyte refers to the concentration of the ions of the specific metal elements in the non-aqueous electrolyte (100 mass%). The valence of the ions of the specific metal elements may be any number, and may be a combination of metal ions with different valences. In addition, the non-aqueous electrolyte may contain multiple types of metal ions. When measuring the amount of metal ions contained in the electrolyte of a nonaqueous electrolyte battery, a member containing the nonaqueous electrolyte is removed from the nonaqueous electrolyte battery, and the nonaqueous electrolyte is extracted and measured. For example, the nonaqueous electrolyte can be extracted using a centrifuge, or the nonaqueous electrolyte can be extracted using an organic solvent. The extracted nonaqueous electrolyte is used to quantify the metal elements, i.e., metal ions, using an inductively coupled plasma atomic emission spectrometry (ICP-AES, for example Thermo Fischer Scientific, iCAP 7600duo) with Li and an acid concentration matching calibration curve method. Each ion will be described below.

[0024] <1-2-1. Nickel ion> The non-aqueous electrolyte according to one embodiment of the present invention contains nickel ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. In this specification, the content of nickel ions in the non-aqueous electrolyte refers to the concentration of nickel element ions in the non-aqueous electrolyte. The valence of the nickel ions contained in the non-aqueous electrolyte is not particularly limited, and may be divalent or trivalent. In addition, the non-aqueous electrolyte according to one embodiment of the present invention contains divalent nickel ions (Ni 2+ ) and trivalent nickel ions (Ni 3+ ) in any ratio. The content of nickel ions in the nonaqueous electrolyte is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, especially preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 500 ppm by mass or less, preferably 400 ppm by mass or less, more preferably 350 ppm by mass or less, even more preferably 300 ppm by mass or less, especially preferably 220 ppm by mass or less, and particularly preferably 150 ppm by mass or less. If the nickel ion content is higher than 500 ppm by mass, the negative electrode reduction reaction increases, causing the internal resistance of the nonaqueous electrolyte battery to rise. On the other hand, if the nickel ion content is lower than 1 ppm by mass, the difference from when no nickel ions are contained becomes small, causing the effect as an auxiliary agent to decrease. The nickel ion source compound may be used alone or in any combination and ratio of two or more. The nickel ion source compound is, for example, Ni(EC) n Examples of the ligand include Ni complexes such as (PF6)2 (EC=ethylene carbonate ligand, n=0 to 6). As the ligand, preferred examples include elements constituting a battery, such as cyclic carbonates such as ethylene carbonate, propylene carbonate, and fluoroethylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, carboxylic acid esters such as methyl acetate, ether compounds, and organic solvents such as sulfone compounds, which are used as non-aqueous solvents. Examples of the ligand include nickel halides such as Ni(CH3COO)2, Ni(OH)2, NiO, NiCO3, NiSO4, and nickel chloride. The nickel ions may be eluted from battery components such as a positive electrode active material, a negative electrode active material, a positive electrode current collector, a negative electrode current collector, or an exterior body, which may contain nickel element. In a non-aqueous electrolyte, nickel ions usually form salts with counter anions. In this embodiment, FSO3 - A counter anion other than the nickel ion may be coordinated with the nickel ion to form a complex, or may form a salt with one or more counter anions. As the counter anion, a preferable example is an element constituting a battery, for example, PF6 derived from LiPF6. - Ion, PO2F2 derived from LiPO2F2 - Fluorophosphate ions such as FSO3Li derived FSO3 - ion, fluoride ion, carbonate ion, carboxylate ion, sulfonate ion, sulfonylimide ion, (oxalato)borate ion, etc. are preferred. PF6 - Ion, FSO3 -ions or fluoride ions. Among them, FSO3 - Ion is PF6 - It is particularly preferred because it has a higher coordinating power for nickel ions than for silver ions. In this embodiment, by containing a specific amount of nickel ions and FSO3Li in the non-aqueous electrolyte solution, FSO3 - It is presumed that the coordination or interaction of the ions with the nickel ions increases the reduction resistance of the nickel ions, suppresses the negative electrode reduction reaction in high-temperature environments, and improves the charged storage characteristics in high-temperature environments.

[0025] <1-2-2. Cobalt ion> The non-aqueous electrolyte according to one embodiment of the present invention contains cobalt ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. In this specification, the content of cobalt ions in the non-aqueous electrolyte refers to the concentration of ions of the cobalt element in the non-aqueous electrolyte. The valence of the cobalt ions contained in the non-aqueous electrolyte is not particularly limited, and may be divalent or trivalent. In addition, the non-aqueous electrolyte according to one embodiment of the present invention contains divalent cobalt ions (Co 2+ ) and trivalent cobalt ion (Co 3+ ) in any ratio. The content of cobalt ions in the nonaqueous electrolyte is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, especially preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 500 ppm by mass or less, preferably 400 ppm by mass or less, more preferably 350 ppm by mass or less, even more preferably 300 ppm by mass or less, especially preferably 220 ppm by mass or less, and particularly preferably 150 ppm by mass or less. If the cobalt ion content is higher than 500 ppm by mass, the negative electrode reduction reaction increases, causing the internal resistance of the nonaqueous electrolyte battery to rise. On the other hand, if the cobalt ion content is lower than 1 ppm by mass, the difference from when no cobalt ion is contained becomes small, causing a decrease in the effect as an auxiliary agent. The cobalt ion source compound may be used alone or in any combination and ratio of two or more kinds. The cobalt ion source compound may be Co(EC) n (PF6)2 (EC = ethylene carbonate ligand, n = 0-6), Co(EC) n Examples of the ligand include Co complexes such as (PF6)3 (n = 0 to 6). Examples of the ligand include elements constituting a battery, such as cyclic carbonates such as ethylene carbonate, propylene carbonate, and fluoroethylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, carboxylic acid esters such as methyl acetate, ether compounds, and sulfone compounds, which are used as non-aqueous solvents. Examples of the ligand include cobalt oxides such as Co(CH3COO)2, Co(HCOO)2, Co(OH)2, CoO, and Co3O4, CoLiO2, CoCO3, CoSO4, Co(NO3)2, and cobalt halides such as cobalt fluoride (II), cobalt fluoride (III), cobalt bromide (II), and cobalt chloride (II). The cobalt ions may also be ions eluted from battery components that may contain elemental cobalt, such as a positive electrode active material, a negative electrode active material, a positive electrode current collector, a negative electrode current collector, or an exterior body. In a non-aqueous electrolyte, cobalt ions usually form salts with counter anions. In this embodiment, FSO3 - A counter anion other than the cobalt ion may be coordinated with the cobalt ion to form a complex, or may form a salt with one or more counter anions. As the counter anion, a preferable example is an element constituting a battery, for example, PF6 derived from LiPF6. - Ion, PO2F2 derived from LiPO2F2 - Fluorophosphate ions such as FSO3Li derived FSO3 - ion, fluoride ion, carbonate ion, carboxylate ion, sulfonate ion, sulfonylimide ion, (oxalato)borate ion, etc. are preferred. PF6 - Ion, FSO3 - ions or fluoride ions. Among them, FSO3- Ion is PF6 - It is particularly preferred since it has a higher coordinating power to cobalt ions than to cations. In this embodiment, a specific amount of cobalt ions and FSO3Li are contained in the non-aqueous electrolyte solution, thereby - It is presumed that the coordination or interaction of the ions with the cobalt ions increases the reduction resistance of the cobalt ions, suppressing the negative electrode reduction reaction in high-temperature environments, and thereby improving the charged storage characteristics in high-temperature environments.

[0026] <1-2-3. Copper ions> The non-aqueous electrolyte according to one embodiment of the present invention contains copper ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. In this specification, the content of copper ions in the non-aqueous electrolyte refers to the concentration of copper ions in the non-aqueous electrolyte. The valence of the copper ions contained in the non-aqueous electrolyte is not particularly limited, and may be monovalent or divalent. In addition, the non-aqueous electrolyte according to one embodiment of the present invention contains monovalent copper ions (Cu + ) and divalent copper ions (Cu 2+ ) in any ratio. The content of copper ions in the nonaqueous electrolyte is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, especially preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 500 ppm by mass or less, preferably 400 ppm by mass or less, more preferably 350 ppm by mass or less, even more preferably 300 ppm by mass or less, especially preferably 220 ppm by mass or less, and particularly preferably 150 ppm by mass or less. If the copper ion content is higher than 500 ppm by mass, the negative electrode reduction reaction increases, causing the internal resistance of the nonaqueous electrolyte battery to rise. On the other hand, if the copper ion content is lower than 1 ppm by mass, the difference from when no copper ions are contained becomes small, causing the effect as an auxiliary agent to decrease. The copper ion source compound may be used alone or in any combination and ratio of two or more. The copper ion source compound is, for example, Cu(EC) nExamples of the ligand include Cu complexes such as (PF6)2 (EC=ethylene carbonate ligand, n=0 to 6). As the ligand, preferred examples include elements constituting a battery, such as cyclic carbonates such as ethylene carbonate, propylene carbonate, and fluoroethylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, carboxylic acid esters such as methyl acetate, ether compounds, and sulfone compounds, which are used as non-aqueous solvents. Examples of the ligand include Cu(CH3COO)2; Cu(HCOO)2; Cu(OH)2; copper oxides such as CuO and Cu2O; CuCO3; CuSO4, Cu(NO3)2; copper halides such as copper chloride (I) and copper chloride (II). The copper ions may be eluted from battery components such as a positive electrode active material, a negative electrode active material, a positive electrode current collector, a negative electrode current collector, or an exterior body, which may contain copper element. In a non-aqueous electrolyte, copper ions usually form salts with counter anions. In this embodiment, FSO3 - A counter anion other than the copper ion may be coordinated with the copper ion to form a complex, or may form a salt with one or more counter anions. As the counter anion, a preferable example is an element constituting a battery, for example, PF6 derived from LiPF6. - Ion, PO2F2 derived from LiPO2F2 - Fluorophosphate ions such as FSO3Li derived FSO3 - ion, fluoride ion, carbonate ion, carboxylate ion, sulfonate ion, sulfonylimide ion, (oxalato)borate ion, etc. are preferred. PF6 - Ion, FSO3 - ions or fluoride ions. Among them, FSO3 - Ion is PF6 - It is particularly preferred because it has a higher coordinating power for copper ions than for copper ions. In this embodiment, by containing a specific amount of copper ions and FSO3Li in the non-aqueous electrolyte, FSO3 -It is presumed that the coordination or interaction of the ions (fluorosulfonate ions) with the copper ions increases the reduction resistance of the copper ions, suppresses the negative electrode reduction reaction in high-temperature environments, and thereby improves the charged storage characteristics in high-temperature environments.

[0027] <1-2-4. Manganese ion> The non-aqueous electrolyte according to one embodiment of the present invention contains manganese ions in an amount of 1 ppm by mass or more and 100 ppm by mass or less. In this specification, the content of manganese ions in the non-aqueous electrolyte refers to the concentration of manganese ions in the non-aqueous electrolyte. The valence of the manganese ions contained in the non-aqueous electrolyte is not particularly limited, and may be divalent or trivalent. In addition, the non-aqueous electrolyte according to one embodiment of the present invention contains divalent manganese ions (Mn 2+ ) and trivalent manganese ion (Mn 3+ ) in any ratio. The content of manganese ions in the nonaqueous electrolyte is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, especially preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 100 ppm by mass or less, preferably 95 ppm by mass or less, more preferably 90 ppm by mass or less, even more preferably 85 ppm by mass or less, especially preferably 80 ppm by mass or less, and particularly preferably 75 ppm by mass or less. If the manganese ion content is higher than 100 ppm by mass, the negative electrode reduction reaction increases, causing the internal resistance of the nonaqueous electrolyte battery to rise. On the other hand, if the manganese ion content is lower than 1 ppm by mass, the difference from when no manganese ion is contained becomes small, causing a decrease in the effect as an auxiliary agent. The manganese ion source compound may be used alone or in any combination and ratio of two or more kinds. The manganese ion source compound may be Mn(EC) nExamples of the ligand include Mn complexes such as (PF6)2 (EC=ethylene carbonate ligand, n=0-6). Examples of the ligand include elements constituting a battery, such as cyclic carbonates such as ethylene carbonate, propylene carbonate, and fluoroethylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, carboxylic acid esters such as methyl acetate, ether compounds, and sulfone compounds, which are used as non-aqueous solvents. Examples of the ligand include manganese acetate hydrates such as Mn(CH3COO)2·2H2O, Mn(CH3COO)2·4H2O, and Mn(CH3COO)3·2H2O; manganese oxides such as MnO2 and Mn3O4; and manganese halides such as MnCO3, MnSO4, KMnO4, MnB4O7·8H2O, and manganese chloride (II). The manganese ions may also be eluted from battery components that may contain elemental manganese, such as a positive electrode active material, a negative electrode active material, a positive electrode current collector, a negative electrode current collector, or an exterior body. In a non-aqueous electrolyte, manganese ions usually form a salt with a counter anion. In this embodiment, FSO3 - A counter anion other than the manganese ion may be coordinated with the manganese ion to form a complex, or may form a salt with one or more counter anions. As the counter anion, a preferable example is an element constituting a battery, for example, PF6 derived from LiPF6. - Ion, PO2F2 derived from LiPO2F2 - Fluorophosphate ions such as FSO3Li derived FSO3 - ion, fluoride ion, carbonate ion, carboxylate ion, sulfonate ion, sulfonylimide ion, (oxalato)borate ion, etc. are preferred. PF6 - Ion, FSO3 - ions or fluoride ions. Among them, FSO3 - Ion is PF6 - It is particularly preferred because it has a higher coordinating power to manganese ions than manganese ions. In this embodiment, a specific amount of manganese ions and FSO3Li are contained in the non-aqueous electrolyte solution, thereby - It is presumed that the coordination or interaction of the ions with the manganese ions increases the reduction resistance of the manganese ions, thereby suppressing the negative electrode reduction reaction in high-temperature environments, thereby improving the charged storage characteristics in high-temperature environments.

[0028] <1-2-5. Aluminum ion> The non-aqueous electrolyte according to one embodiment of the present invention contains aluminum ions in an amount of 1 ppm by mass to 100 ppm by mass. In this specification, the content of aluminum ions in the non-aqueous electrolyte refers to the concentration of aluminum ions in the non-aqueous electrolyte. The content of aluminum ions in the nonaqueous electrolyte solution is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, particularly preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 100 ppm by mass or less, preferably 90 ppm by mass or less, more preferably 80 ppm by mass or less, even more preferably 70 ppm by mass or less, and particularly preferably 60 ppm by mass or less. If the aluminum ion content is higher than 100 ppm by mass, the negative electrode reduction reaction increases, causing the internal resistance of the nonaqueous electrolyte battery to rise. On the other hand, if the aluminum ion content is lower than 1 ppm by mass, the difference from when no aluminum ions are contained becomes small, resulting in a reduced effect. The aluminum ion source compound may be used alone or in any combination and ratio of two or more. The aluminum ion source compound may be Al(EC), nExamples of the ligand include Al complexes such as (PF6)3 (EC=ethylene carbonate ligand, n=0 to 6). Examples of the ligand include elements constituting a battery, such as organic solvents used as non-aqueous solvents, such as cyclic carbonates such as ethylene carbonate, propylene carbonate, and fluoroethylene carbonate; chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; carboxylic acid esters such as methyl acetate; ether compounds; and sulfone compounds. Examples of compounds serving as aluminum ion sources include aluminum salts such as Al(FSO3)3; Al(CH3COO)3; Al(CF3COO)3; Al(CF3SO3)3; aluminum alkoxides such as tris(2,4-pentanedionato)aluminum, aluminum ethoxide, aluminum isopropoxide, and aluminum-n-butoxide; alkyl aluminum such as trimethylaluminum; and Al halides such as aluminum chloride. The aluminum ions may be eluted from components of the battery, such as a positive electrode active material, a negative electrode active material, a positive electrode current collector, a negative electrode current collector, or an exterior body, which may contain elemental aluminum. In a non-aqueous electrolyte, aluminum ions usually form salts with counter anions. In this embodiment, FSO3 - A counter anion other than the aluminum ion may be coordinated to the aluminum ion to form a complex, or the aluminum ion and one or more counter anions may form a salt. As the counter anion, elements constituting a battery are also preferably mentioned, for example, PF6 derived from LiPF6. - Ion, PO2F2 derived from LiPO2F2 - Fluorophosphate ions such as FSO3Li ions, which may be derived from FSO3 - ion, fluoride ion, carbonate ion, carboxylate ion, sulfonate ion, sulfonylimide ion, (oxalato)borate ion, etc. are preferred. PF6 - Ion, FSO3 - ions or fluoride ions. Among them, FSO3 - Ion is PF6 -It is particularly preferred since it has a higher coordinating power to aluminum ions than to cations. In this embodiment, by containing a specific amount of aluminum ions and FSO3Li in the non-aqueous electrolyte, FSO3 - It is presumed that the aluminum ion is coordinated or interacted with the aluminum ion, which increases the reduction resistance of the aluminum ion and suppresses the negative electrode reduction reaction in a high-temperature environment, thereby improving the charge storage characteristics in a high-temperature environment. When measuring the amount of aluminum ions in the electrolyte in a nonaqueous electrolyte battery, a member containing the nonaqueous electrolyte may be removed from the nonaqueous electrolyte battery, and the nonaqueous electrolyte may be extracted and measured. For example, the nonaqueous electrolyte may be extracted by a centrifuge, or the nonaqueous electrolyte may be extracted using an organic solvent. The extracted nonaqueous electrolyte is used to quantify the aluminum element, i.e., aluminum ion, by inductively coupled plasma atomic emission spectroscopy (ICP-AES, for example Thermo Fischer Scientific, iCAP 7600duo) using Li and an acid concentration matching calibration curve method.

[0029] When the nonaqueous electrolyte solution according to one embodiment of the present invention contains at least one metal ion selected from the group consisting of nickel ions, cobalt ions, copper ions, manganese ions, and aluminum ions, the total content of the metal ions in the nonaqueous electrolyte solution is usually 1 ppm by mass or more, preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, even more preferably 5 ppm by mass or more, particularly preferably 10 ppm by mass or more, and particularly preferably 25 ppm by mass or more, while the upper limit is usually 500 ppm by mass or less, preferably 400 ppm by mass or less, more preferably 300 ppm by mass or less, even more preferably 200 ppm by mass or less, and particularly preferably 120 ppm by mass or less. Furthermore, the nonaqueous electrolyte according to one embodiment of the present invention contains at least nickel ions, and preferably contains 30% by mass or more, and more preferably 40% by mass or more, of nickel ions based on the total amount of the five metal ions. In addition, in the case where the nonaqueous electrolyte solution according to one embodiment of the present invention contains a plurality of metal ions selected from the group consisting of nickel ions, cobalt ions, copper ions, manganese ions, and aluminum ions, it is preferable that the electrolyte solution contains at least a combination of the metal ions shown below. Combinations of nickel ions and cobalt ions; nickel ions and copper ions; nickel ions and manganese ions; cobalt ions and copper ions; cobalt ions and manganese ions; copper ions and manganese ions; nickel ions, cobalt ions and copper ions; nickel ions, cobalt ions and manganese ions; nickel ions, copper ions and manganese ions; cobalt ions, copper ions and manganese ions; nickel ions, cobalt ions, copper ions and manganese ions, and particularly preferred are combinations of nickel ions and cobalt ions; nickel ions and copper ions; nickel ions and manganese ions; nickel ions, cobalt ions and manganese ions; nickel ions, copper ions and manganese ions; nickel ions, cobalt ions, copper ions and manganese ions; nickel ions, cobalt ions, copper ions and manganese ions. The preferred contents of each metal ion in the particularly preferred combination are as follows: Nickel ions and cobalt ions: Nickel ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, more preferably 20 ppm by mass or more, and even more preferably 25 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, and more preferably 150 ppm by mass or less; cobalt ions are usually 1 ppm by mass or more, preferably 5 ppm by mass or more, and more preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, and more preferably 150 ppm by mass or less. Nickel ions and copper ions: Nickel ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, more preferably 20 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less, and copper ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, more preferably 25 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less. Nickel ions and manganese ions: Nickel ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, preferably 25 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less, and manganese ions are usually 1 ppm by mass or more, preferably 2 ppm by mass or more, and usually 100 ppm by mass or less, preferably 80 ppm by mass or less, more preferably 75 ppm by mass or less. Nickel ions, cobalt ions and manganese ions; nickel ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, more preferably 25 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less; cobalt ions are usually 1 ppm by mass or more, preferably 5 ppm by mass or more, more preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less; and manganese ions are preferably 1 ppm by mass or more, and usually 100 ppm by mass or less, preferably 80 ppm by mass or less, more preferably 75 ppm by mass or less. Nickel ions, copper ions and manganese ions; nickel ions are usually 1 ppm by mass or more, preferably 5 ppm by mass or more, more preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, more preferably 150 ppm by mass or less; copper ions are usually 1 ppm by mass or more, preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, preferably 150 ppm by mass or less; and manganese ions are preferably 1 ppm by mass or more, and usually 100 ppm by mass or less, preferably 80 ppm by mass or less, more preferably 75 ppm by mass or less. Nickel ions, cobalt ions, copper ions and manganese ions; nickel ions are usually 1 ppm by mass or more, preferably 5 ppm by mass or more, preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, and more preferably 150 ppm by mass or less; cobalt ions are usually 1 ppm by mass or more, preferably 2 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, and preferably 150 ppm by mass or less; copper ions are usually 1 ppm by mass or more, preferably 5 ppm by mass or more, more preferably 10 ppm by mass or more, and usually 300 ppm by mass or less, preferably 220 ppm by mass or less, and preferably 150 ppm by mass or less; and manganese ions are preferably 1 ppm by mass or more, and usually 100 ppm by mass or less, preferably 80 ppm by mass or less, and more preferably 75 ppm by mass or less.

[0030] <1-3. Electrolytes> The non-aqueous electrolyte of the present embodiment, like a general non-aqueous electrolyte, usually contains an electrolyte as a component. There is no particular limitation on the electrolyte used in the non-aqueous electrolyte of the present embodiment, and any known electrolyte can be used. Specific examples of the electrolyte will be described in detail below. <1-3-1. Lithium salts> As the electrolyte in the non-aqueous electrolyte solution of the present embodiment, a lithium salt is usually used. The lithium salt is not particularly limited as long as it is known to be used for this purpose, and one or more of any lithium salts can be used. Specifically, the following can be mentioned:

[0031] For example, lithium fluoroborates such as LiBF4; Lithium fluorophosphates such as LiPF6 and LiPO2F2; Lithium tungstate salts such as LiWOF5; Lithium carboxylates such as CF3CO2Li; Lithium sulfonate salts such as CH3SO3Li; Lithium imide salts such as LiN(FSO2)2, LiN(CF3SO2)2; Lithium methide salts such as LiC(FSO2)3; Lithium oxalate salts such as lithium difluorooxalatoborate; Other fluorine-containing organic lithium salts such as LiPF4(CF3)2; etc.

[0032] In order to further enhance the effect of improving the charge / discharge rate characteristics and the impedance characteristics in addition to the effect of improving the charge storage characteristics under high temperature environments obtained by the present invention, the lithium fluoroborate salts are preferably selected from lithium fluorophosphate salts, lithium sulfonate salts, lithium imide salts, and lithium oxalate salts, and more preferably selected from lithium fluoroborate salts, lithium fluorophosphate salts, lithium imide salts, and lithium oxalate salts.

[0033] The total concentration of these electrolytes in the non-aqueous electrolyte is not particularly limited, but is usually 8% by mass or more, preferably 8.5% by mass or more, more preferably 9% by mass or more, based on the total amount of the non-aqueous electrolyte.The upper limit is usually 18% by mass or less, preferably 17% by mass or less, more preferably 16% by mass or less.When the total concentration of the electrolytes is within the above range, the electrical conductivity is appropriate for the battery operation, so that sufficient output characteristics tend to be obtained.

[0034] <1-4.Non-aqueous solvents> The nonaqueous electrolyte of the present embodiment, like a general nonaqueous electrolyte, usually contains a nonaqueous solvent that dissolves the above-mentioned electrolyte as its main component. There is no particular limitation on the nonaqueous solvent used here, and a known organic solvent can be used. Examples of the organic solvent include saturated cyclic carbonates, chain carbonates, carboxylate esters, ether compounds, and sulfone compounds. Although not particularly limited to these, saturated cyclic carbonates, chain carbonates, and carboxylate esters are preferred, and saturated cyclic carbonates and chain carbonates are more preferred. These can be used alone or in combination of two or more. As a combination of two or more nonaqueous solvents, a combination of two or more selected from the group consisting of saturated cyclic carbonates, chain carbonates, and carboxylate esters is preferred, and a combination of saturated cyclic carbonates or chain carbonates is more preferred.

[0035] <1-4-1. Saturated cyclic carbonates> Examples of the saturated cyclic carbonate include those having an alkylene group having 2 to 4 carbon atoms, and from the viewpoint of improving the battery characteristics resulting from the improvement of the degree of dissociation of lithium ions, saturated cyclic carbonates having 2 to 3 carbon atoms are preferably used. The saturated cyclic carbonate may be a cyclic carbonate having a fluorine atom, such as monofluoroethylene carbonate.

[0036] Examples of the saturated cyclic carbonate include ethylene carbonate, propylene carbonate, butylene carbonate, etc. Among them, ethylene carbonate and propylene carbonate are preferred, and ethylene carbonate, which is less susceptible to oxidation and reduction, is more preferred. The saturated cyclic carbonate may be used alone or in any combination and ratio of two or more.

[0037] The content of the saturated cyclic carbonate is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but the lower limit is usually 3% by volume or more, preferably 5% by volume or more, based on the total amount of the solvent in the nonaqueous electrolyte. By setting it in this range, the decrease in electrical conductivity due to the decrease in the dielectric constant of the nonaqueous electrolyte can be avoided, and the large current discharge characteristics, stability to the negative electrode, and cycle characteristics of the nonaqueous electrolyte battery can be easily set in a good range. The upper limit is usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less. By setting it in this range, the oxidation / reduction resistance of the nonaqueous electrolyte tends to be improved, and the stability during high-temperature storage tends to be improved. In the present invention, the volume % means the volume at 25° C. and 1 atmospheric pressure.

[0038] <1-4-2. Chain carbonate> As the chain carbonate, one having 3 to 7 carbon atoms is usually used, and in order to adjust the viscosity of the electrolyte solution within an appropriate range, a chain carbonate having 3 to 5 carbon atoms is preferably used.

[0039] Specific examples of chain carbonates include dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, methyl-n-propyl carbonate, n-butyl methyl carbonate, isobutyl methyl carbonate, t-butyl methyl carbonate, ethyl-n-propyl carbonate, n-butyl ethyl carbonate, isobutyl ethyl carbonate, and t-butyl ethyl carbonate.

[0040] Of these, dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate are preferred, and dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are particularly preferred.

[0041] In addition, chain carbonates having fluorine atoms (hereinafter, sometimes abbreviated as "fluorinated chain carbonate") can also be suitably used. The number of fluorine atoms in the fluorinated chain carbonate is not particularly limited as long as it is 1 or more, but is usually 6 or less, and preferably 4 or less. When the fluorinated chain carbonate has multiple fluorine atoms, they may be bonded to the same carbon or different carbons. Examples of the fluorinated chain carbonate include fluorinated dimethyl carbonate derivatives, fluorinated ethyl methyl carbonate derivatives, and fluorinated diethyl carbonate derivatives.

[0042] Examples of the fluorinated dimethyl carbonate derivative include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, trifluoromethyl methyl carbonate, bis(fluoromethyl)carbonate, bis(difluoro)methyl carbonate, and bis(trifluoromethyl)carbonate.

[0043] Examples of fluorinated ethyl methyl carbonate derivatives include 2-fluoroethyl methyl carbonate, ethyl fluoromethyl carbonate, 2,2-difluoroethyl methyl carbonate, 2-fluoroethyl fluoromethyl carbonate, ethyl difluoromethyl carbonate, 2,2,2-trifluoroethyl methyl carbonate, 2,2-difluoroethyl fluoromethyl carbonate, 2-fluoroethyl difluoromethyl carbonate, and ethyl trifluoromethyl carbonate.

[0044] Examples of fluorinated diethyl carbonate derivatives include ethyl-(2-fluoroethyl)carbonate, ethyl-(2,2-difluoroethyl)carbonate, bis(2-fluoroethyl)carbonate, ethyl-(2,2,2-trifluoroethyl)carbonate, 2,2-difluoroethyl-2'-fluoroethyl carbonate, bis(2,2-difluoroethyl)carbonate, 2,2,2-trifluoroethyl-2'-fluoroethyl carbonate, 2,2,2-trifluoroethyl-2',2'-difluoroethyl carbonate, and bis(2,2,2-trifluoroethyl)carbonate.

[0045] The chain carbonate may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0046] The content of the chain carbonate is not particularly limited, but is usually 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, based on the total amount of the solvent in the nonaqueous electrolyte. Also, it is usually 90% by volume or less, preferably 85% by volume or less, more preferably 80% by volume or less. By setting the content of the chain carbonate within the above range, the viscosity of the nonaqueous electrolyte can be set to an appropriate range, the decrease in ion conductivity can be suppressed, and the output characteristics of the nonaqueous electrolyte battery can be easily set to a good range. When two or more types of chain carbonates are used in combination, the total amount of the chain carbonates can be set to satisfy the above range.

[0047] Furthermore, by combining a specific chain carbonate with ethylene carbonate in a specific content, the battery performance can be significantly improved.

[0048] For example, when dimethyl carbonate and ethyl methyl carbonate are selected as the specific chain carbonate, the content of ethylene carbonate is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but is usually 15% by volume or more, preferably 20% by volume, based on the total amount of the solvent in the nonaqueous electrolyte solution. EndThe content of dimethyl carbonate is usually 20% by volume or more, preferably 30% by volume or more, and usually 50% by volume or less, preferably 45% by volume or less, based on the total amount of the solvent in the nonaqueous electrolyte solution, and the content of ethyl methyl carbonate is usually 20% by volume or more, preferably 30% by volume or more, and usually 50% by volume or less, preferably 45% by volume or less. The contents of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate are within the above ranges. By setting the temperature within the range, the composition tends to have excellent high-temperature stability and suppress gas generation.

[0049] <1-4-3. Ether compounds> As the ether-based compound, a chain ether having 3 to 10 carbon atoms and a cyclic ether having 3 to 6 carbon atoms are preferred.

[0050] The ether-based compounds may be used alone or as a mixture of two or more kinds in any combination and in any ratio. The content of the ether-based compound is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but is usually 1% by volume or more, preferably 2% by volume or more, more preferably 3% by volume or more, and usually 30% by volume or less, preferably 25% by volume or less, more preferably 20% by volume or less, in 100% by volume of the non-aqueous solvent. When two or more ether-based compounds are used in combination, the total amount of the ether-based compounds should satisfy the above range. If the content of the ether-based compound is within the above preferred range, it is easy to ensure the effect of improving the lithium ion dissociation degree of the chain ether and improving the ion conductivity due to the viscosity reduction. In addition, when the negative electrode active material is a carbonaceous material, the phenomenon in which the chain ether is co-inserted with the lithium ion can be suppressed, so that the input / output characteristics and the charge / discharge rate characteristics can be set to an appropriate range.

[0051] <1-4-4. Sulfone compounds> The sulfone compound is not particularly limited, whether it is a cyclic sulfone or a chain sulfone, but in the case of a cyclic sulfone, the carbon number is usually 3 to 6, preferably 3 to 5, and in the case of a chain sulfone, the carbon number is usually 2 to 6, preferably 2 to 5. The number of sulfonyl groups in one molecule of the sulfone compound is not particularly limited, but is usually 1 or 2.

[0052] Examples of cyclic sulfones include monosulfone compounds such as trimethylene sulfones, tetramethylene sulfones, and hexamethylene sulfones; and disulfone compounds such as trimethylene disulfones, tetramethylene disulfones, and hexamethylene disulfones. Among these, from the viewpoint of dielectric constant and viscosity, tetramethylene sulfones, tetramethylene disulfones, hexamethylene sulfones, and hexamethylene disulfones are more preferred, and tetramethylene sulfones (sulfolanes) are particularly preferred.

[0053] The sulfolane is preferably sulfolane or a sulfolane derivative (hereinafter, sulfolane may be abbreviated as "sulfolane") The sulfolane derivative is preferably one in which one or more hydrogen atoms bonded to the carbon atom constituting the sulfolane ring are substituted with a fluorine atom or an alkyl group.

[0054] The sulfone-based compounds may be used alone or as a mixture of two or more kinds in any combination and in any ratio. The content of the sulfone-based compound is not particularly limited, and is arbitrary as long as it does not significantly impair the effects of the present invention, but is usually 0.3% by volume or more, preferably 0.5% by volume or more, more preferably 1% by volume or more, and is usually 40% by volume or less, preferably 35% by volume or less, more preferably 30% by volume or less, based on the total amount of the solvent in the non-aqueous electrolyte. When two or more sulfone-based compounds are used in combination, the total amount of the sulfone-based compounds should be set to satisfy the above range. If the content of the sulfone-based compound is within the above range, an electrolyte with excellent high-temperature storage stability tends to be obtained.

[0055] <1-4-5. Carboxylic acid esters> The carboxylate is preferably a chain carboxylate, more preferably a saturated chain carboxylate. The total number of carbon atoms in the carboxylate is usually 3 to 7, and from the viewpoint of improving the battery characteristics resulting from the improvement of the output characteristics, a carboxylate having 3 to 5 carbon atoms is preferably used.

[0056] Examples of the carboxylate include saturated chain carboxylates such as methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, methyl pivalate, and ethyl pivalate, and unsaturated chain carboxylates such as methyl acrylate, ethyl acrylate, methyl methacrylate, and ethyl methacrylate. Among them, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, methyl pivalate, and ethyl pivalate are preferred, and from the viewpoint of improving output characteristics, methyl acetate, ethyl acetate, methyl propionate, and ethyl propionate are more preferred. The carboxylate may be used alone or in any combination and ratio of two or more.

[0057] The content of the carboxylate is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but the lower limit is usually 3% by volume or more, preferably 5% by volume or more, based on the total amount of the solvent in the nonaqueous electrolyte. By setting the content in this range, the decrease in electrical conductivity due to the decrease in the dielectric constant of the nonaqueous electrolyte can be avoided, and the large current discharge characteristics, stability to the negative electrode, and cycle characteristics of the nonaqueous electrolyte battery can be easily set in a good range. The upper limit is usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less. By setting the content in this range, the oxidation / reduction resistance of the nonaqueous electrolyte tends to be improved, and the stability during high-temperature storage tends to be improved. In the present invention, the volume % means the volume at 25° C. and 1 atmospheric pressure.

[0058] <1-5. Fluorosulfonates other than FSO3Li> The counter cation of fluorosulfonates other than FSO3Li (hereinafter simply referred to as "fluorosulfonates") is not particularly limited, but may be sodium, potassium, rubidium, cesium, magnesium, calcium, barium, or NR 13 R 14 R 15 R 16 (In the formula, R 13 ~R 16 each independently represents a hydrogen atom or an organic group having 1 to 12 carbon atoms.

[0059] Specific examples of fluorosulfonates include: Examples of the fluorosulfonate include sodium fluorosulfonate, potassium fluorosulfonate, rubidium fluorosulfonate, and cesium fluorosulfonate.

[0060] The fluorosulfonate may be used alone or in any combination and ratio of two or more. The total content of the fluorosulfonate and FSO3Li in the non-aqueous electrolyte of the present embodiment is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and usually 15% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, particularly preferably 2% by mass or less, and particularly preferably 1% by mass or less, in the case of using two or more fluorosulfonates in combination, the total amount of FSO3Li and the fluorosulfonate may be set to satisfy the above range. Within this range, swelling of the nonaqueous electrolyte battery due to charging and discharging can be suitably suppressed.

[0061] <1-6. Auxiliaries> The nonaqueous electrolyte solution of the present embodiment may contain the following auxiliary agents within the range in which the effects of the present invention are achieved. Unsaturated cyclic carbonates such as vinylene carbonate, vinyl ethylene carbonate, or ethynyl ethylene carbonate; Carbonate compounds such as methoxyethyl-methyl carbonate; Spiro compounds such as methyl-2-propynyl oxalate; Sulfur-containing compounds such as ethylene sulfite; Isocyanate compounds such as diisocyanates having a cycloalkylene group, such as 1,3-bis(isocyanatomethyl)cyclohexane; Nitrogen-containing compounds such as 1-methyl-2-pyrrolidinone; Hydrocarbon compounds such as cycloheptane; Fluorinated aromatic compounds such as fluorobenzene; Silane compounds such as tris(trimethylsilyl) borate; 2-(methanesulfonyloxy)propionic acid 2-propynyl ester compounds; Lithium salts such as lithium ethylmethyloxycarbonylphosphonate; Isocyanate esters such as triallyl isocyanurate; These may be used alone or in combination of two or more. By adding these auxiliary agents, it is possible to improve the capacity retention characteristics and cycle characteristics after high-temperature storage.

[0062] The content of the auxiliary is not particularly limited, and is arbitrary as long as it does not significantly impair the effects of the present invention. The content of the auxiliary is usually 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 0.2 mass% or more, and is usually 5 mass% or less, preferably 3 mass% or less, more preferably 1 mass% or less, based on the total amount of the non-aqueous electrolyte. Within this range, the effect of the auxiliary is easily exerted, and high-temperature storage stability tends to be improved. When two or more auxiliary agents are used in combination, the total amount of the auxiliary agents should be set to satisfy the above range.

[0063] <2.Nonaqueous electrolyte battery> A nonaqueous electrolyte battery according to one embodiment of the present invention is a nonaqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a nonaqueous electrolyte, and is equipped with the nonaqueous electrolyte according to one embodiment of the present invention described above. More specifically, the nonaqueous electrolyte battery according to one embodiment of the present invention comprises a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and at least one kind of metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e), and satisfying at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) The concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less. (iii) The concentration of (c) is 1 ppm by mass or more and 500 ppm by mass or less. (iv) The concentration of (d) is 1 ppm by mass or more and 100 ppm by mass or less. (v) The concentration of (e) is 1 ppm by mass or more and 100 ppm by mass or less. In particular, the nonaqueous electrolyte battery according to aspect A of the present invention comprises a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and containing nickel ions in an amount of 1 ppm by mass or more and 500 ppm by mass or less. Furthermore, a nonaqueous electrolyte battery according to aspect B of the present invention includes a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and containing 1 ppm by mass or more and 500 ppm by mass or less of cobalt ions. Furthermore, a nonaqueous electrolyte battery according to aspect C of the present invention includes a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and containing 1 ppm by mass or more and 500 ppm by mass or less of copper ions. Furthermore, a nonaqueous electrolyte battery according to aspect D of the present invention includes a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and containing manganese ions in an amount of 1 ppm by mass or more and 100 ppm by mass or less. Furthermore, a nonaqueous electrolyte battery according to aspect E of the present invention includes a positive electrode having a current collector and a positive electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, a negative electrode having a current collector and a negative electrode active material layer provided on the current collector and capable of absorbing and releasing metal ions, and a nonaqueous electrolyte containing FSO3Li and containing 1 ppm by mass or more and 100 ppm by mass or less of aluminum ions.

[0064] <2-1. Battery configuration> The nonaqueous electrolyte battery of this embodiment is the same as the conventional nonaqueous electrolyte battery except for the nonaqueous electrolyte. Usually, the positive electrode and the negative electrode are laminated through a porous membrane (separator) impregnated with the nonaqueous electrolyte, and these are housed in a case (exterior body). Therefore, the shape of the nonaqueous electrolyte battery of this embodiment is not particularly limited, and may be any of a cylindrical type, a square type, a laminate type, a coin type, a large type, etc.

[0065] <2-2. Non-aqueous electrolyte> As the non-aqueous electrolyte solution, the non-aqueous electrolyte solution according to the embodiment of the present invention is used. Note that, within the scope of the present invention, it is also possible to mix other non-aqueous electrolyte solutions with the non-aqueous electrolyte solution.

[0066] <2-3. Positive electrode> In one embodiment of the present invention, the positive electrode has a current collector and a positive electrode active material layer provided on the current collector. The positive electrode used in the nonaqueous electrolyte battery of this embodiment will be described in detail below.

[0067] <2-3-1. Positive electrode active material> The positive electrode active material used in the positive electrode will be described below. (1) Composition The positive electrode active material is not particularly limited as long as it is a lithium cobalt oxide or a transition metal oxide containing at least Ni and Co, with 50 mol % or more of the transition metals being Ni and Co, and capable of electrochemically absorbing and releasing metal ions, but for example, a material capable of electrochemically absorbing and releasing lithium ions is preferred, and a transition metal oxide containing lithium, at least Ni and Co, with 60 mol % or more of the transition metals being Ni and Co is preferred. This is because Ni and Co have oxidation-reduction potentials suitable for use as positive electrode materials for secondary batteries, and are suitable for high capacity applications.

[0068] The metal components of the lithium transition metal oxide include at least Ni or Co as essential transition metal elements, and other metal elements include Mn, V, Ti, Cr, Fe, Cu, Al, Mg, Zr, Er, etc., with Mn, Ti, Fe, Al, Mg, Zr, etc. being preferred. Specific examples of lithium transition metal oxides include LiCoO2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, Li 1.05 Ni 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.50 Mn 0.29 Co 0.21 O2, LiNi 0.6Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 Examples include O2 and the like.

[0069] In particular, an embodiment in which the positive electrode active material is a transition metal oxide represented by the following compositional formula (1) is preferable. Li a1 Ni b1 Co c1 M d1 O2 ··· (1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90 ≤ a1 ≤ 1.10, 0 < b1 < 0.4, and b1 + c1 + d1 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In the compositional formula (1), it is preferable to show a numerical value of 0.1 ≤ d1 < 0.5. This is because when the composition ratios of Ni and Co and the composition ratios of other metal species are within specific ranges, transition metals are less likely to elute from the positive electrode, and even if they elute, Ni and Co have little adverse effect in the non-aqueous secondary battery.

[0070] In particular, an embodiment in which the positive electrode active material is a transition metal oxide represented by the following compositional formula (2) is preferable. Li a2 Ni b2 Co c2 M d2 O2 ··· (2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90 ≤ a2 ≤ 1.10, 0.4 ≤ b2 < 1.0, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In the compositional formula (2), it is preferable to show a numerical value of 0.10 ≤ d2 < 0.40. Also, it is preferable to show a numerical value of 0.50 ≤ b2 ≤ 0.96. This is because when Ni and Co are the main components and the composition ratio of Ni is larger than the composition ratio of Co, it becomes stable and can extract a high capacity when used as the positive electrode of a non-aqueous electrolyte battery.

[0071] In a particularly preferred embodiment, the positive electrode active material is a transition metal oxide represented by the following composition formula (3). Li a3 Ni b3 Co c3 M d3 O2···(3) (In formula (3), the numerical values ​​are 0.90≦a3≦1.10, 0.50≦b3≦0.94, 0.05≦c3≦0.2, and 0.01≦d3≦0.3, and b3+c3+d3=1 is satisfied. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In the composition formula (3), it is preferable that the value 0.10≦d3≦0.3 is satisfied. When the positive electrode active material has the above composition, it becomes possible to obtain a particularly high capacity when used as a positive electrode for a non-aqueous secondary battery.

[0072] In addition, two or more of the above positive electrode active materials may be mixed and used. Similarly, at least one of the above positive electrode active materials may be mixed and used with another positive electrode active material. Examples of the other positive electrode active materials include transition metal oxides, transition metal phosphate compounds, transition metal silicate compounds, and transition metal borate compounds that are not listed above. Among them, lithium manganese composite oxides having a spinel structure and lithium-containing transition metal phosphate compounds having an olivine structure are preferred. Specifically, lithium manganese composite oxides having a spinel structure include LiMn2O4, LiMn 1.8 Al 0.2 O4, LiMn 1.5 Ni 0.5 O4, etc. These lithium manganese composite oxides have the most stable structure, are less likely to release oxygen even when the non-aqueous electrolyte battery is abnormal, and are therefore excellent in safety. In addition, the transition metal of the lithium-containing transition metal phosphate compound is preferably V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc., and specific examples include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7, cobalt phosphates such as LiCoPO4, manganese phosphates such as LiMnPO4, and lithium transition metal phosphate compounds in which a part of the transition metal atoms that constitute the main part of these lithium transition metal phosphate compounds has been replaced with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Si, Nb, Mo, Sn, W, etc. Among the lithium-containing transition metal phosphate compounds, lithium iron phosphate compounds are preferred. This is because iron is a metal that is abundant in resources, is extremely inexpensive, and has little harmfulness. In other words, among the above specific examples, LiFePO4 can be cited as a more preferred specific example.

[0073] In one embodiment of the present invention, the positive electrode is an NMC positive electrode, and the content of nickel element in the NMC positive electrode is preferably 30 mol % or more, and more preferably 40 mol % or more from the viewpoint of increasing the capacity of the nonaqueous electrolyte battery. In this specification, the NMC positive electrode refers to a positive electrode in which the positive electrode active material contains nickel-manganese-cobalt (NMC) and is a material represented by the following formula (I). Li a Ni b Co c Mn d O2···(I) (In the above formula (I), a, b, c, and d satisfy 0.90≦a≦1.10 and b+c+d=1.)

[0074] (2) Surface coating The above-mentioned positive electrode active material may have a surface to which a substance (hereinafter, appropriately referred to as a "surface-attached substance") having a different composition from the substance constituting the main positive electrode active material is attached. Examples of the surface-attached substance include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; and carbon.

[0075] These surface-attaching substances can be attached to the surface of the positive electrode active material by, for example, a method of dissolving or suspending the substance in a solvent, impregnating the positive electrode active material with the substance, and then drying the substance, a method of dissolving or suspending a surface-attaching substance precursor in a solvent, impregnating the positive electrode active material with the substance, and then reacting the substance by heating or the like, a method of adding the substance to a positive electrode active material precursor and simultaneously baking the substance, etc. When carbon is attached, a method of mechanically attaching the carbonaceous material, for example, in the form of activated carbon, etc., after the surface-attaching substance is attached can also be used.

[0076] The mass of the surface-attached substance attached to the surface of the positive electrode active material is preferably 0.1 ppm or more, more preferably 1 ppm or more, and even more preferably 10 ppm or more, relative to the mass of the positive electrode active material, and is preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less. The surface-attached substance can suppress the oxidation reaction of the non-aqueous electrolyte on the surface of the positive electrode active material, thereby improving the battery life. In addition, when the amount of the attached substance is within the above range, the effect can be fully exerted, and the inflow and outflow of lithium ions is not hindered, and the resistance is not likely to increase.

[0077] (3) Shape The positive electrode active material may have a particulate form. The positive electrode active material particles may have a conventional shape such as a block, a polyhedron, a sphere, an oval sphere, a plate, a needle, a column, etc. Also, primary particles may be aggregated to form secondary particles, and the secondary particles may have a spherical or oval sphere shape.

[0078] (4) Manufacturing method of positive electrode active material The method for producing the positive electrode active material is not particularly limited as long as it does not deviate from the gist of the present invention. Several methods can be mentioned, and a general method for producing an inorganic compound can be used. In particular, various methods can be considered for producing spherical or ellipsoidal active materials. One example is a method in which transition metal raw materials such as transition metal nitrates or sulfates, and, if necessary, raw materials of other elements, are dissolved or crushed and dispersed in a solvent such as water, and the pH is adjusted while stirring to produce and recover a spherical precursor, which is then dried if necessary, and a Li source such as LiOH, Li2CO3, or LiNO3 is added and the mixture is fired at high temperature to obtain the active material.

[0079] Another example of the method is to dissolve or pulverize and disperse transition metal raw materials such as transition metal nitrates, sulfates, hydroxides, and oxides, and, if necessary, raw materials of other elements, in a solvent such as water, and then dry and mold the resulting mixture using a spray dryer or the like to form a spherical or ellipsoidal precursor. To this, a Li source such as LiOH, Li2CO3, or LiNO3 is added, and the mixture is fired at high temperature to obtain an active material.

[0080] As yet another example of the method, a transition metal raw material such as a transition metal nitrate, sulfate, hydroxide, or oxide, a Li source such as LiOH, Li2CO3, or LiNO3, and, if necessary, raw materials of other elements are dissolved or pulverized and dispersed in a solvent such as water, and then dried and molded using a spray dryer or the like to form a spherical or ellipsoidal precursor, which is then fired at a high temperature to obtain the active material.

[0081] <2-3-2. Positive electrode structure and manufacturing method> The configuration of the positive electrode used in the present invention and the method for producing the same will be described below. (Method of making positive electrode) The positive electrode is prepared by forming a positive electrode active material layer containing positive electrode active material particles and a binder on a current collector. The positive electrode using the positive electrode active material may be manufactured by any known method. For example, the positive electrode active material and the binder, and if necessary, a conductive material and a thickener, etc. are mixed in a dry state to form a sheet, which is then pressed onto the positive electrode current collector, or these materials are dissolved or dispersed in a liquid medium to form a slurry, which is then applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode.

[0082] The content of the positive electrode active material in the positive electrode active material layer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and preferably 99.9% by mass or less, more preferably 99% by mass or less. When the content of the positive electrode active material is within the above range, the electric capacity of the nonaqueous electrolyte battery can be sufficiently ensured. Furthermore, the strength of the positive electrode is also sufficient. In this embodiment, the positive electrode active material powder (particle) may be used alone, or two or more types of different compositions or different powder properties may be used in any combination and ratio. When two or more types of active materials are used in combination, it is preferable to use the composite oxide containing lithium and manganese as a component of the powder. Cobalt or nickel is an expensive metal with a small amount of resources, and the amount of active material used is large in large batteries that require high capacity for automobile applications, etc., which is not preferable in terms of cost. Therefore, in large batteries, it is desirable to use manganese as a cheaper transition metal as the main component of the positive electrode active material.

[0083] <Conductive material> Any known conductive material can be used as the conductive material. Specific examples include metal materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; and carbonaceous materials such as amorphous carbon such as needle coke. These materials may be used alone or in any combination and ratio of two or more.

[0084] The content of the conductive material in the positive electrode active material layer is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 1% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 15% by mass or less. When the content is within the above range, sufficient conductivity can be ensured. Furthermore, the decrease in battery capacity is easily prevented.

[0085] <Binding agent> The binder used in producing the positive electrode active material layer is not particularly limited as long as it is a material that is stable to the nonaqueous electrolyte solution and the solvent used in producing the electrode. In the case of the coating method, there is no particular limitation as long as the material is dissolved or dispersed in the liquid medium used in the production of the electrode. Specific examples include resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, aromatic polyamide, cellulose, and nitrocellulose; rubber-like polymers such as SBR (styrene-butadiene rubber), NBR (acrylonitrile-butadiene rubber), fluororubber, isoprene rubber, butadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or hydrogenated products thereof, and EPDM (ethylene-propylene-diene ternary copolymers). Examples of such materials include thermoplastic elastomer-like polymers such as styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers, and hydrogenated products thereof; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, and propylene-α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and tetrafluoroethylene-ethylene copolymers; and polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions). These substances may be used alone or in any combination and ratio of two or more.

[0086] The content of the binder in the positive electrode active material layer is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and also preferably 80% by mass or less, more preferably 60% by mass or less, even more preferably 40% by mass or less, and particularly preferably 10% by mass or less. When the proportion of the binder is within the above range, the positive electrode active material can be sufficiently held, and the mechanical strength of the positive electrode can be secured, so that the battery performance such as cycle characteristics is improved. Furthermore, it also leads to avoiding a decrease in battery capacity and conductivity.

[0087] <Liquid medium> The liquid medium used in preparing the slurry for forming the positive electrode active material layer is not particularly limited in type, and either an aqueous solvent or an organic solvent may be used, so long as it is a solvent capable of dissolving or dispersing the positive electrode active material, the conductive material, the binder, and the thickener used as needed. Examples of aqueous solvents include water and mixed solvents of alcohol and water. Examples of organic solvents include aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphatamide and dimethylsulfoxide. These may be used alone or in any combination and ratio of two or more.

[0088] <Thickener> When using an aqueous solvent as the liquid medium for forming the slurry, it is preferable to use a thickener and a latex such as styrene butadiene rubber (SBR) to form the slurry. The thickener usually increases the viscosity of the slurry. adjustment is used to. There are no limitations on the thickener as long as it does not significantly limit the effects of the present invention, and specific examples include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof, etc. These may be used alone or in any combination and ratio of two or more.

[0089] When a thickener is used, the ratio of the thickener to the positive electrode active material is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.6% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. Within the above range, the coating property is good, and furthermore, the ratio of the active material in the positive electrode active material layer is sufficient, so that the problem of the battery capacity decreasing and the problem of the resistance between the positive electrode active materials increasing can be easily avoided.

[0090] <Consolidation> The positive electrode active material layer obtained by applying the above slurry to the current collector and drying it is preferably compacted by a hand press, roller press, or the like in order to increase the packing density of the positive electrode active material. The density of the positive electrode active material layer is 1 g cm -3 More than 1.5g cm is preferable. -3 More preferably, 2 g cm -3 More than 4g cm is particularly preferable. -3 Less than 3.5 g cm is preferable. -3 Less than 3g cm is more preferable. -3 The following are particularly preferred: When the density of the positive electrode active material layer is within the above range, the permeability of the non-aqueous electrolyte solution to the vicinity of the current collector / active material interface is not reduced, and the charge / discharge characteristics are good, particularly at high current densities. Furthermore, the conductivity between the active materials is less likely to decrease, and the battery resistance is less likely to increase.

[0091] <Current collector> The material of the positive electrode current collector is not particularly limited, and any known material can be used. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; and carbonaceous materials such as carbon cloth and carbon paper. Among them, metal materials, especially aluminum, are preferred.

[0092] The shape of the current collector may be, for example, a metal foil, a metal cylinder, a metal coil, a metal plate, a metal thin film, an expanded metal, a punched metal, or a foamed metal, for example, when it is a metal material, or a carbonaceous material, a carbon plate, a carbon thin film, or a carbon cylinder, for example. Among these, a metal thin film is preferred. The thin film may be appropriately formed into a mesh shape. The thickness of the current collector is arbitrary, but is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, and is preferably 1 mm or less, more preferably 100 μm or less, even more preferably 50 μm or less. When the thickness of the current collector is within the above range, the strength required as a current collector can be sufficiently ensured. Furthermore, the handling property is also good.

[0093] The thickness ratio between the current collector and the positive electrode active material layer is not particularly limited, but (thickness of the active material layer on one side immediately before the injection of the nonaqueous electrolyte solution) / (thickness of the current collector) is preferably 150 or less, more preferably 20 or less, and particularly preferably 10 or less, and is also preferably 0.1 or more, more preferably 0.4 or more, and particularly preferably 1 or more. When the thickness ratio of the current collector to the positive electrode active material layer is within the above range, the current collector is less likely to generate heat due to Joule heat during high current density charge / discharge, and the volume ratio of the current collector to the positive electrode active material is less likely to increase, preventing a decrease in battery capacity.

[0094] <Electrode area> From the viewpoint of increasing the stability at high output and high temperature, the area of ​​the positive electrode active material layer is preferably made larger than the outer surface area of ​​the battery outer case. Specifically, the sum of the electrode areas of the positive electrodes relative to the surface area of ​​the outer case of the nonaqueous electrolyte battery is preferably 20 times or more in area ratio, and more preferably 40 times or more. In the case of a bottomed rectangular shape, the outer surface area of ​​the outer case refers to the total area calculated from the length, width, and thickness dimensions of the case part filled with the power generating element excluding the protruding part of the terminal. In the case of a bottomed cylindrical shape, it is the geometric surface area of ​​the case part filled with the power generating element excluding the protruding part of the terminal as a cylinder. The sum of the electrode areas of the positive electrodes refers to the geometric surface area of ​​the positive electrode composite layer facing the composite layer containing the negative electrode active material, and in a structure in which a positive electrode composite layer is formed on both sides via a collector foil, it refers to the sum of the areas calculated separately for each side.

[0095] <Discharge capacity> When the non-aqueous electrolyte is used, the electric capacity of the battery element housed in one battery exterior of the non-aqueous electrolyte battery (electric capacity when the battery is discharged from a fully charged state to a discharged state) is preferably 1 ampere hour (Ah) or more, since this increases the effect of improving low-temperature discharge characteristics. Therefore, the positive electrode plate is designed so that the discharge capacity at full charge is preferably 3 Ah (ampere hour) or more, more preferably 4 Ah or more, and also preferably 100 Ah or less, more preferably 70 Ah or less, and particularly preferably 50 Ah or less.

[0096] Within the above range, the voltage drop due to electrode reaction resistance during drawing of a large current is not too large, and deterioration of power efficiency can be prevented. Furthermore, the temperature distribution due to heat generation inside the battery during pulse charging and discharging is not too large, and the durability of the battery during repeated charging and discharging is deteriorated, and the heat dissipation efficiency is also deteriorated against sudden heat generation during abnormality such as overcharging or internal short circuit.

[0097] <Thickness of positive electrode plate> The thickness of the positive electrode plate is not particularly limited, but from the viewpoint of high capacity, high output, and high rate characteristics, the thickness of the positive electrode active material layer minus the thickness of the current collector is preferably 10 μm or more, more preferably 20 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, on one side of the current collector.

[0098] <2-4. Negative electrode> In one embodiment of the present invention, the negative electrode has a current collector and a negative electrode active material layer provided on the current collector. The negative electrode active material used in the negative electrode will be described below. There are no particular limitations on the negative electrode active material as long as it is capable of electrochemically absorbing and releasing metal ions. Specific examples include carbonaceous materials and other materials having carbon as a constituent element, alloy-based materials, and the like. These materials may be used alone or in any combination of two or more.

[0099] <2-4-1. Negative electrode active material> As mentioned above, examples of the negative electrode active material include carbonaceous materials and alloy-based materials.

[0100] Examples of the carbonaceous material include (1) natural graphite, (2) artificial graphite, (3) amorphous carbon, (4) carbon-coated graphite, (5) graphite-coated graphite, and (6) resin-coated graphite.

[0101] (1) Examples of natural graphite include scaly graphite, scaly graphite, soil graphite, and / or graphite particles obtained by subjecting these graphites to treatments such as spheroidization and densification. Among these, from the viewpoints of particle packing and charge / discharge rate characteristics, spherical or ellipsoidal graphite that has been subjected to a spheroidization treatment is particularly preferred.

[0102] The spheronization treatment can be carried out using a device that repeatedly applies mechanical actions to particles, such as compression, friction, shear force, and particle interactions, mainly impact force.

[0103] Specifically, a device having a rotor with many blades installed inside a casing, which rotates at high speed to apply mechanical actions such as impact compression, friction, shear force, etc. to the raw material natural graphite (1) introduced inside, thereby carrying out spheroidization is preferred. Also, a device having a mechanism for repeatedly applying mechanical actions by circulating the raw material is preferred.

[0104] For example, when the spheronization treatment is performed using the above-mentioned device, the peripheral speed of the rotating rotor is preferably set to 30 to 100 m / sec, more preferably 40 to 100 m / sec, and even more preferably 50 to 100 m / sec. Although the spheronization treatment can be performed by simply passing the raw material through the device, it is preferable to circulate or retain the raw material in the device for 30 seconds or more, and more preferably to circulate or retain the raw material in the device for 1 minute or more.

[0105] (2) Examples of artificial graphite include those produced by graphitizing organic compounds such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene silicide, polyphenylene oxide, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin at a temperature usually in the range of 2500°C or higher and usually 3200°C or lower, and then pulverizing and / or classifying as necessary.

[0106] In this case, a silicon-containing compound or a boron-containing compound can be used as a graphitization catalyst. In addition, an artificial graphite obtained by graphitizing mesocarbon microbeads separated during the heat treatment of pitch can be used. Furthermore, an artificial graphite of granulated particles consisting of primary particles can be used. For example, mesocarbon microbeads and graphite particles obtained by mixing graphitizable carbonaceous material powder such as coke with a graphitizable binder such as tar or pitch and a graphitization catalyst, graphitizing the mixture, and pulverizing the mixture as necessary can be used. The graphite particles are obtained by assembling or bonding a plurality of flat particles so that the oriented planes are non-parallel.

[0107] (3) Examples of amorphous carbon include amorphous carbon particles obtained by using graphitizable carbon precursors such as tar and pitch as raw materials and heat-treating them at least once in a temperature range in which graphitization does not occur (400 to 2200°C), and amorphous carbon particles obtained by using non-graphitizable carbon precursors such as resin as raw materials and heat-treating them.

[0108] (4) Carbon-coated graphite can be obtained as follows. Natural graphite and / or artificial graphite are mixed with a carbon precursor, which is an organic compound such as tar, pitch, or resin, and the mixture is heat-treated at least once in the range of 400 to 2300°C. The natural graphite and / or artificial graphite after the heat treatment is used as core graphite, which is then coated with amorphous carbon to obtain a carbon-graphite composite. This carbon-graphite composite can be referred to as carbon-coated graphite (4).

[0109] The composite may be in the form of a core graphite whose surface is entirely or partially covered with amorphous carbon, or a plurality of primary particles may be composited with carbon originating from the carbon precursor as a binder. The carbon-graphite composite may also be obtained by reacting natural graphite and / or artificial graphite with a hydrocarbon gas such as benzene, toluene, methane, propane, or aromatic volatile matter at high temperature to deposit carbon on the graphite surface (CVD).

[0110] (5) Graphite-coated graphite can be obtained as follows: Natural graphite and / or artificial graphite are mixed with a carbon precursor of an easily graphitizable organic compound such as tar, pitch, or resin, and the mixture is heat-treated at least once in a temperature range of about 2400 to 3200° C. The natural graphite and / or artificial graphite after the heat treatment is used as core graphite, and the surface of the core graphite is entirely or partially coated with a graphitized material to obtain graphite-coated graphite (5).

[0111] (6) Resin-coated graphite can be obtained, for example, by mixing natural graphite and / or artificial graphite with a resin or the like, drying the mixture at a temperature of less than 400°C to obtain natural graphite and / or artificial graphite as core graphite, and then coating the core graphite with a resin or the like.

[0112] In addition, the carbonaceous materials (1) to (6) described above may be used alone, or two or more thereof may be used in combination in any combination and ratio.

[0113] Examples of the organic compounds such as tar, pitch, and resin used in the carbonaceous materials (2) to (5) above include carbonizable organic compounds selected from the group consisting of coal-based heavy oil, straight-run heavy oil, cracked petroleum heavy oil, aromatic hydrocarbons, N-ring compounds, S-ring compounds, polyphenylene, organic synthetic polymers, natural polymers, thermoplastic resins, and thermosetting resins. Further, the raw material organic compound may be dissolved in a low molecular weight organic solvent for adjusting the viscosity during mixing and used.

[0114] In addition, as the natural graphite and / or artificial graphite used as the raw material of the nuclear graphite, spherical natural graphite is preferable.

[0115] Next, the above alloy-based material used as the negative electrode active material may be any of lithium metal, simple metals and alloys that form a lithium alloy, or compounds such as their oxides, carbides, nitrides, silicides, sulfides or phosphides, as long as it can occlude and release lithium ions, and is not particularly limited. The simple metals and alloys that form a lithium alloy are preferably materials containing group 13 and group 14 metal and metalloid elements (i.e., excluding carbon), more preferably simple metals of aluminum, silicon and tin and alloys or compounds containing these atoms, and still more preferably those having silicon or tin as a constituent element, such as simple metals of silicon and tin and alloys or compounds containing these atoms. These may be used alone or in combination of two or more in any combination and ratio.

[0116] <Metal particles capable of alloying with Li> When a single metal or alloy that forms a lithium alloy, or a compound such as an oxide, carbide, nitride, silicide, sulfide, or phosphide thereof is used as a negative electrode active material, the metal that can be alloyed with Li is in a particulate form. Methods for confirming that the metal particles are metal particles that can be alloyed with Li include identification of the metal particle phase by X-ray diffraction, observation of the particle structure by an electron microscope and EDX elemental analysis, and elemental analysis by fluorescent X-rays.

[0117] Any conventionally known metal particles can be used as the metal particles capable of being alloyed with Li, but from the viewpoint of the capacity and cycle life of the non-aqueous electrolyte battery, the metal particles are preferably, for example, a metal selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Ag, Si, Sn, Al, Zr, Cr, P, S, V, Mn, As, Nb, Mo, Cu, Zn, Ge, In, Ti and W, or a compound thereof. The metal particles may also be alloy particles formed from two or more metal elements. Among these, a metal selected from the group consisting of Si, Sn, As, Sb, Al, Zn and W, or a metal compound thereof, is preferred.

[0118] The metal compound includes metal oxides, metal nitrides, metal carbides, etc. Furthermore, an alloy consisting of two or more kinds of metals may be used.

[0119] Among metal particles that can be alloyed with Li, Si or a Si metal compound is preferred from the viewpoint of increasing the capacity of the battery. The Si metal compound is preferably a Si metal oxide. In this specification, Si or a Si metal compound is collectively referred to as a Si compound. Specifically, the Si compound is SiO x ,SiN x ,SiC x , SiZ x O y (Z=C, N), etc. The Si compound is preferably a Si metal oxide, which can be represented by the general formula SiO x This general formula is SiO x is obtained from silicon dioxide (SiO2) and metallic silicon (Si), and the value of x is usually 0 <x<2である。SiOx Compared with graphite, it has a larger theoretical capacity. Moreover, amorphous Si or nano-sized Si crystals allow alkali ions such as lithium ions to easily enter and exit, making it possible to obtain a high-capacity battery.

[0120] The Si metal oxide is specifically represented as SiO x where x satisfies 0 ≦ x < 2, more preferably 0.2 or more and 1.8 or less, still more preferably 0.4 or more and 1.6 or less, and particularly preferably 0.6 or more and 1.4 or less. Within this range, the battery has a high capacity, and at the same time, it is possible to reduce the irreversible capacity due to the bond between Li and oxygen.

[0121] <Oxygen content of metal particles alloyable with Li> The oxygen content of the metal particles alloyable with Li is not particularly limited, but is usually 0.01% by mass or more and 8% by mass or less, preferably 0.05% by mass or more and 5% by mass or less. The oxygen distribution state within the particles may be present near the surface, inside the particles, or uniformly within the particles, but it is particularly preferably present near the surface. When the oxygen content of the metal particles alloyable with Li is within the above range, the strong bond between the metal particles and O (oxygen atoms) suppresses the volume expansion associated with the secondary charge and discharge of the non-aqueous electrolyte battery, and it is possible to obtain a non-aqueous electrolyte battery with excellent cycle characteristics, which is preferable.

[0122] <Negative electrode active material containing metal particles alloyable with Li and graphite particles> The negative electrode active material may contain metal particles alloyable with Li and graphite particles. The negative electrode active material may be a mixture in which the metal particles alloyable with Li and the graphite particles are mixed in a state of independent particles, or a composite in which the metal particles alloyable with Li are present on the surface and / or inside of the graphite particles.

[0123] The composite of metal particles capable of alloying with Li and graphite particles (also referred to as composite particles) is not particularly limited as long as it contains metal particles capable of alloying with Li and graphite particles. Preferably, it is a particle in which metal particles capable of alloying with Li and graphite particles are integrated by physical and / or chemical bonds. A more preferable form is that the metal particles capable of alloying with Li and the graphite particles are in a state where each solid component is dispersed in the particle to such an extent that they exist in at least both the surface and the bulk interior of the composite particle, and in a form where graphite particles are present in order to integrate them by physical and / or chemical bonds. A more specific preferable form is a composite material composed of at least metal particles capable of alloying with Li and graphite particles, and a composite material (negative electrode active material) characterized in that metal particles capable of alloying with Li are present in the gaps within the structure of particles having a folded structure with curved surfaces, preferably natural graphite. The gaps may be voids, or substances such as amorphous carbon, graphite-like substances, and resins that buffer the expansion and contraction of metal particles capable of alloying with Li may be present in the gaps.

[0124] <Content ratio of metal particles capable of alloying with Li> The content ratio of metal particles capable of alloying with Li to the total of metal particles capable of alloying with Li and graphite particles is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, still more preferably 2.0% by mass or more. Also, it is usually 99% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less, still more preferably 30% by mass or less, even more preferably 25% by mass or less, even more preferably 20% by mass or less, particularly preferably 15% by mass or less, and most preferably 10% by mass or less. When the content ratio of metal particles capable of alloying with Li is within this range, it is preferable in that side reactions on the Si surface can be controlled and sufficient capacity can be obtained in a non-aqueous electrolyte battery.

[0125] <Coating rate> In this embodiment, the negative electrode active material may be coated with a carbonaceous material or a graphite material. Among these, it is preferable to coat with an amorphous carbonaceous material from the viewpoint of lithium ion acceptance. The coating rate is usually 0.5% to 30%, preferably 1% to 25%, more preferably 2% to 20%. The upper limit of the coating rate is preferably within the above range from the viewpoint of reversible capacity when assembled into a battery, and the lower limit of the coating rate is preferably within the above range from the viewpoint of the core carbonaceous material being uniformly coated with amorphous carbon to be firmly granulated, and from the viewpoint of the particle size of the particles obtained when pulverized after firing.

[0126] The coverage (content) of the organic compound-derived carbonized material in the final negative electrode active material can be calculated by the following formula using the amount of the negative electrode active material, the amount of the organic compound, and the carbon residue rate measured by a micro method in accordance with JIS K 2270.

[0127] Formula: Coverage rate of carbon derived from organic compound (%) = (mass of organic compound × carbon remaining rate × 100) / {mass of negative electrode active material + (mass of organic compound × carbon remaining rate)}

[0128] <Internal porosity> The internal porosity of the negative electrode active material is usually 1% or more, preferably 3% or more, more preferably 5% or more, and even more preferably 7% or more. It is usually less than 50%, preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. If the internal porosity is too small, the amount of liquid in the particles of the negative electrode active material tends to be small in a nonaqueous electrolyte battery. On the other hand, if the internal porosity is too large, the gap between particles tends to be small when the material is used as an electrode. The lower limit of the internal porosity is preferably set to the above range from the viewpoint of charge / discharge characteristics, and the upper limit is preferably set to the above range from the viewpoint of diffusion of the nonaqueous electrolyte. In addition, as described above, the gap may be a void, or a substance that buffers the expansion and contraction of metal particles that can be alloyed with Li, such as amorphous carbon, graphite, or resin, may be present in the gap or the gap may be filled with these substances.

[0129] <2-4-2. Negative electrode structure and manufacturing method> The negative electrode can be manufactured by any known method as long as it does not significantly impair the effects of the present invention. For example, the negative electrode can be formed by adding a binder, a solvent, and, if necessary, a thickener, a conductive material, a filler, etc. to the negative electrode active material to form a slurry, applying the slurry to a current collector, drying it, and pressing it.

[0130] In addition, the alloy-based material negative electrode can be manufactured by any known method. Specifically, the manufacturing method of the negative electrode includes, for example, a method of adding a binder, a conductive material, etc. to the above-mentioned negative electrode active material, and then rolling the material to form a sheet electrode, or a method of compressing the material to form a pellet electrode. Usually, a method of forming a thin film layer (negative electrode active material layer) containing the above-mentioned negative electrode active material on a current collector for a negative electrode (hereinafter sometimes referred to as "negative electrode current collector") by a coating method, a vapor deposition method, a sputtering method, a plating method, or the like is used. In this case, a binder, a thickener, a conductive material, a solvent, etc. are added to the above-mentioned negative electrode active material to form a slurry, which is applied to a negative electrode current collector, dried, and then pressed to densify, thereby forming a negative electrode active material layer on the negative electrode current collector.

[0131] Examples of the material for the negative electrode current collector include steel, copper, copper alloy, nickel, nickel alloy, stainless steel, etc. Among these, copper is preferred from the viewpoints of ease of processing into a thin film and cost, and copper foil is more preferred.

[0132] The thickness of the negative electrode current collector is usually 1 μm or more, preferably 5 μm or more, and usually 100 μm or less, preferably 50 μm or less. If the thickness of the negative electrode current collector is too thick, the capacity of the entire nonaqueous electrolyte battery may be too low, and conversely, if it is too thin, handling may be difficult.

[0133] In order to improve the bonding effect with the negative electrode active material layer formed on the surface, it is preferable to roughen the surface of the negative electrode current collector in advance. Examples of the surface roughening method include blasting, rolling with a rough-surface roll, mechanical polishing in which the current collector surface is polished with an abrasive cloth with abrasive particles fixed thereto, a grindstone, an emery buff, a wire brush equipped with a steel wire, or the like, electrolytic polishing, chemical polishing, and the like.

[0134] In addition, in order to reduce the mass of the negative electrode collector and improve the energy density per unit mass of the battery, a perforated type negative electrode collector such as an expanded metal or a punched metal can be used. The mass of this type of negative electrode collector can be freely changed by changing the aperture ratio. In addition, when a negative electrode active material layer is formed on both sides of this type of negative electrode collector, the rivet effect through the holes makes it even more difficult for the negative electrode active material layer to peel off. However, if the aperture ratio is too high, the contact area between the negative electrode active material layer and the negative electrode collector becomes small, and the adhesive strength may be reduced.

[0135] The slurry for forming the negative electrode active material layer is usually prepared by adding a binder, a thickener, etc. to the negative electrode material. In this specification, the term "negative electrode material" refers to a material in which the negative electrode active material and the conductive material are combined.

[0136] The content of the negative electrode active material in the negative electrode material is usually 70% by mass or more, particularly 75% by mass or more, and usually 97% by mass or less, particularly 95% by mass or less. If the content of the negative electrode active material is too small, the capacity of the secondary battery using the obtained negative electrode tends to be insufficient, and if it is too large, the content of the conductive material is relatively insufficient, making it difficult to ensure the electrical conductivity of the negative electrode. When two or more negative electrode active materials are used in combination, the total amount of the negative electrode active materials should be set to satisfy the above range.

[0137] Examples of the conductive material used in the negative electrode include metal materials such as copper and nickel; and carbon materials such as graphite and carbon black. These may be used alone or in any combination and ratio of two or more. In particular, it is preferable to use a carbon material as the conductive material, since the carbon material also acts as an active material. The content of the conductive material in the negative electrode material is usually 3% by mass or more, preferably 5% by mass or more, and usually 30% by mass or less, preferably 25% by mass or less. If the content of the conductive material is too small, the conductivity tends to be insufficient, and if it is too large, the content of the negative electrode active material, etc. is relatively insufficient, which tends to reduce the battery capacity and strength. When two or more conductive materials are used in combination, the total amount of the conductive materials should be set to satisfy the above range.

[0138] Any binder can be used for the negative electrode as long as it is stable against the solvent and electrolyte used in the manufacture of the electrode. Examples include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, styrene-butadiene rubber, isoprene rubber, butadiene rubber, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, etc. These may be used alone or in any combination and ratio of two or more. The content of the binder is usually 0.5 parts by mass or more, preferably 1 part by mass or more, and usually 10 parts by mass or less, preferably 8 parts by mass or less, per 100 parts by mass of the negative electrode material. If the content of the binder is too small, the strength of the resulting negative electrode tends to be insufficient, and if it is too large, the content of the negative electrode active material, etc. will be relatively insufficient, which will result in insufficient battery capacity and conductivity. When two or more binders are used in combination, the total amount of the binders should be set to satisfy the above range.

[0139] Examples of thickeners used in the negative electrode include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, etc. These may be used alone or in any combination and ratio of two or more. A thickener may be used as needed, but when used, it is preferable that the content of the thickener in the negative electrode active material layer is usually in the range of 0.5 mass% or more and 5 mass% or less.

[0140] The slurry for forming the negative electrode active material layer is prepared by mixing the negative electrode active material with a conductive material, a binder, and a thickener as necessary, and using an aqueous solvent or an organic solvent as a dispersion medium. As the aqueous solvent, water is usually used, but it is also possible to use an organic solvent such as alcohols such as ethanol and cyclic amides such as N-methylpyrrolidone in a range of 30 mass% or less with respect to water. In addition, examples of the organic solvent include cyclic amides such as N-methylpyrrolidone; linear amides such as N,N-dimethylformamide and N,N-dimethylacetamide; aromatic hydrocarbons such as anisole, toluene, and xylene; and alcohols such as butanol and cyclohexanol; among them, cyclic amides such as N-methylpyrrolidone; and linear amides such as N,N-dimethylformamide and N,N-dimethylacetamide are preferred. Note that any one of these may be used alone, or two or more may be used in any combination and ratio.

[0141] The obtained slurry is applied onto the above-mentioned negative electrode current collector, dried, and then pressed to form a negative electrode active material layer, thereby obtaining a negative electrode. The application method is not particularly limited, and a method known per se can be used. The drying method is also not particularly limited, and a known method such as natural drying, heat drying, and reduced pressure drying can be used.

[0142] <Electrode density> There are no particular restrictions on the structure of the electrode when the negative active material is made into an electrode, but the density of the negative active material present on the current collector must be less than 1 g cm -3 More than 1.2 g cm is preferable.-3 More preferably, 1.3 g cm -3 More than 2.2 g cm is particularly preferable. -3 Less than 2.1 g cm is preferable. -3 Less than 2.0 g cm is preferable. -3 Less than 1.9 g cm is more preferable. -3 The following is particularly preferred. If the density of the negative electrode active material present on the current collector exceeds the above range, the negative electrode active material particles are destroyed, which may lead to an increase in the initial irreversible capacity of the non-aqueous electrolyte battery and a deterioration in high current density charge / discharge characteristics due to a decrease in the permeability of the non-aqueous electrolyte near the current collector / negative electrode active material interface. If the density of the negative electrode active material is below the above range, the conductivity between the negative electrode active materials may decrease, the battery resistance may increase, and the capacity per unit volume may decrease.

[0143] <2-5. Separator> A separator is usually interposed between the positive electrode and the negative electrode to prevent short circuiting. In this case, the nonaqueous electrolyte of the present invention is usually impregnated into the separator before use.

[0144] There is no particular restriction on the material or shape of the separator, and any known material can be used as long as it does not significantly impair the effects of the present invention. Among them, resins, glass fibers, inorganic materials, etc., which are formed of materials stable to the nonaqueous electrolyte of the present invention, are preferably used, and it is preferable to use a porous sheet or nonwoven fabric-like material with excellent liquid retention.

[0145] Examples of materials that can be used for the resin and glass fiber separator include polyolefins such as polyethylene and polypropylene, polytetrafluoroethylene, polyethersulfone, and glass filters. Among these, glass filters and polyolefins are preferred, and polyolefins are more preferred. These materials may be used alone or in any combination and ratio of two or more.

[0146] The thickness of the separator is arbitrary, but is usually 1 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and is usually 50 μm or less, preferably 40 μm or less, more preferably 30 μm or less. If the separator is thinner than the above range, the insulating properties and mechanical strength may be reduced. If the separator is thicker than the above range, not only may the battery performance such as rate characteristics be reduced, but also the energy density of the nonaqueous electrolyte battery as a whole may be reduced.

[0147] Furthermore, when a porous material such as a porous sheet or nonwoven fabric is used as the separator, the porosity of the separator is optional, but is usually 20% or more, preferably 35% or more, more preferably 45% or more, and is usually 90% or less, preferably 85% or less, more preferably 75% or less. If the porosity is too small, the membrane resistance tends to increase and the rate characteristics tend to deteriorate. If the porosity is too large, the mechanical strength of the separator tends to decrease and the insulating properties tend to decrease.

[0148] The average pore size of the separator is also optional, but is usually 0.5 μm or less, preferably 0.2 μm or less, and usually 0.05 μm or more. If the average pore size exceeds the above range, short circuits are likely to occur. If the average pore size is below the above range, the membrane resistance increases and the rate characteristics may deteriorate.

[0149] On the other hand, examples of inorganic materials that can be used include oxides such as alumina and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates such as barium sulfate and calcium sulfate.

[0150] As for the form, a thin film such as a nonwoven fabric, a woven fabric, or a microporous film is used. In the thin film form, a film with a pore size of 0.01 to 1 μm and a thickness of 5 to 50 μm is preferably used. In addition to the above-mentioned independent thin film form, a separator formed by forming a composite porous layer containing a particulate or fibrous inorganic material using a resin binder on the surface layer of a positive electrode and / or a negative electrode can be used. For example, a porous layer containing alumina particles with a 90% particle size of less than 1 μm and using a fluororesin as a binder can be formed on both sides of a positive electrode.

[0151] <2-6.Battery design> [Electrode group] The electrode group may be either a laminated structure of the positive electrode plate and the negative electrode plate with the separator interposed therebetween, or a structure in which the positive electrode plate and the negative electrode plate are spirally wound with the separator interposed therebetween. The ratio of the volume of the electrode group to the internal volume of the battery (hereinafter referred to as the electrode group occupancy rate) is usually 40% or more, preferably 50% or more, and usually 90% or less, preferably 80% or less. The lower limit of the electrode group occupancy rate is preferably set to the above range from the viewpoint of the battery capacity. Also, the upper limit of the electrode group occupancy rate is preferably set to the above range in order to secure a gap space from the viewpoint of various characteristics such as the charge / discharge repeatability and high-temperature storage characteristics of the battery, and from the viewpoint of avoiding the operation of a gas release valve that releases internal pressure to the outside. If the gap space is too small, the battery will become hot, causing the components to expand or the vapor pressure of the electrolyte liquid components to increase, resulting in an increase in internal pressure, which will degrade the battery's characteristics such as repeated charge / discharge performance and high-temperature storage characteristics, and may even cause the gas release valve, which releases internal pressure to the outside, to operate.

[0152] [Current collection structure] Although the current collecting structure is not particularly limited, in order to more effectively realize the improvement of the discharge characteristics by the non-aqueous electrolyte, it is preferable to adopt a structure that reduces the resistance of the wiring parts and the joint parts. When the internal resistance is reduced in this way, the effect of using the non-aqueous electrolyte is particularly well exhibited.

[0153] In the case where the electrode group has the aforementioned laminated structure, a structure formed by bundling the metal core parts of each electrode layer and welding them to a terminal is preferably used. When the area of ​​one electrode becomes large, the internal resistance increases, so it is also preferably used to reduce the resistance by providing multiple terminals in the electrode. In the case where the electrode group has the aforementioned wound structure, the internal resistance can be reduced by providing multiple lead structures on each of the positive electrode and the negative electrode and bundling them to a terminal.

[0154] [Protection element] Examples of protective elements include a PTC (Positive Temperature Coefficient) element whose resistance increases when abnormal heat is generated or an excessive current flows, a temperature fuse, a thermistor, a valve (current cutoff valve) that cuts off the current flowing in the circuit due to a sudden increase in the internal pressure or temperature of the battery when abnormal heat is generated, etc. It is preferable to select a protective element that does not operate under normal use at high current, and from the viewpoint of high output, it is more preferable to design the battery so that abnormal heat generation or thermal runaway does not occur even without a protective element.

[0155] [Exterior body] The nonaqueous electrolyte battery of this embodiment is usually configured by housing the above-mentioned nonaqueous electrolyte, negative electrode, positive electrode, separator, etc. in an exterior body (exterior case). There are no limitations on this exterior body, and any known exterior body can be used as long as it does not significantly impair the effects of the present invention.

[0156] The material of the exterior case is not particularly limited as long as it is a substance that is stable against the non-aqueous electrolyte used. Specifically, metals such as nickel-plated steel sheet, stainless steel, aluminum or aluminum alloy, magnesium alloy, nickel, titanium, etc., or a laminate film of resin and aluminum foil are preferably used.

[0157] The exterior case using the above metals includes a sealed and sealed structure formed by welding the metals together by laser welding, resistance welding, or ultrasonic welding, or a crimped structure formed by using the above metals via a resin gasket. The exterior case using the above laminate film includes a sealed and sealed structure formed by heat fusing the resin layers together. In order to improve the sealing property, a resin different from the resin used in the laminate film may be interposed between the resin layers. In particular, when the resin layer is heat-sealed via the current collecting terminal to form a sealed structure, the joining between the metal and the resin is performed, so that a resin having a polar group or a modified resin into which a polar group has been introduced is preferably used as the interposed resin.

[0158] The shape of the exterior body may also be arbitrary, and may be, for example, cylindrical, rectangular, laminated, coin-shaped, large, or the like. EXAMPLES

[0159] [Experiment A] Hereinafter, one embodiment of the present invention will be described in more detail with reference to Examples and Reference Examples. However, the present invention is not limited to these Examples as long as it does not depart from the gist of the present invention.

[0160] <Examples A1-1 to A1-4 and Comparative Examples A1-1 to A1-7> [Preparation of EC solution containing Ni(PF6)2] In an argon glove box, 20.5 g (3.9 mmol) of NiCl was weighed into a 50 mL beaker and suspended in acetonitrile (AN). While stirring, 61.95 g (7.7 mmol) of AgPF was added slowly in small portions, and the mixture was then stirred at room temperature for 3 hours. As the reaction proceeded, a white solid of AgCl was produced. After leaving the mixture overnight, the AgCl was filtered off, and the filtrate was concentrated under reduced pressure using a rotary evaporator to obtain [Ni(AN) nA blue solid of Ni(PF6)2 (n = 0-6) was obtained. 5.0 g (56.8 mmol) of ethylene carbonate (EC) melted at 45°C was added to dissolve the solid, and the solution was evacuated at 35°C for 6 hours to remove the coordinating solvent AN, yielding an EC solution containing Ni(PF6)2.

[0161] [Preparation of positive electrode] Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 85 parts by mass of 102O2, 10 parts by mass of acetylene black as a conductive material, and 5 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone solvent with a disperser to form a slurry. This was evenly applied to one side of an aluminum foil with a thickness of 15 μm, dried, and pressed to form a positive electrode.

[0162] [Preparation of negative electrode] 98 parts by mass of natural graphite was mixed with 1 part by mass of an aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose: 1% by mass) and 1 part by mass of an aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber: 50% by mass) as a thickener and binder, and the mixture was mixed in a disperser to form a slurry. The obtained slurry was applied to one side of a copper foil having a thickness of 10 μm, dried, and pressed to form a negative electrode.

[0163] [Preparation of non-aqueous electrolyte] Under a dry argon atmosphere, an EC solution containing Ni(PF6)2 was diluted with EC, EMC, and DMC so that the nickel ion concentration in the mixed solvent was as shown in Table 1, and the solvent composition was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:4:3, and LiPF6 that had been thoroughly dried was dissolved at 1 mol / L (as the concentration in the non-aqueous electrolyte). The non-aqueous electrolyte that does not contain Ni(PF6)2 is called reference electrolyte A1. FSO3Li was added to the Ni(PF6)2-containing non-aqueous electrolyte or reference electrolyte A1 prepared above to prepare the non-aqueous electrolyte described in Table 1 below. However, Comparative Example A1-1 is the reference electrolyte A1 itself. In the table, the content of FSO3Li indicates the amount added, and the content of nickel element (nickel ion) is a value obtained based on the measurement results of inductively coupled plasma atomic emission spectroscopy (ICP-AES) described later. In addition, the "content (mass %)" and "content (mass ppm)" in the table are the contents when the reference electrolyte A1 is taken as 100 mass %.

[0164] <Measurement of nickel content in non-aqueous electrolyte> 100 μL (approximately 130 mg) of the non-aqueous electrolyte was taken out. The taken non-aqueous electrolyte was weighed into a PTFE beaker, and an appropriate amount of concentrated nitric acid was added and wet decomposed on a hot plate, after which the volume was adjusted to 50 mL. The content of Li and nickel elements was measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES, Thermo Fischer Scientific, iCAP 7600duo) with an acid concentration matching calibration curve method.

[0165] [Manufacture of non-aqueous electrolyte secondary batteries] The above positive electrode, negative electrode, and polyethylene separator were laminated in the order of negative electrode, separator, and positive electrode to prepare a battery element. This battery element was inserted into a bag made of a laminate film of aluminum (thickness 40 μm) coated on both sides with a resin layer while the positive and negative terminals were protruding, and the above prepared nonaqueous electrolyte was then injected into the bag and vacuum sealed to prepare a laminate type nonaqueous electrolyte secondary battery.

[0166] <Evaluation of non-aqueous electrolyte secondary batteries> [Initial conditioning] In a thermostatic bath at 25°C, the non-aqueous electrolyte secondary battery was charged at a constant current and constant voltage (hereinafter referred to as CC-CV charging) to 4.2V at a current equivalent to 1 / 6C (1C refers to a current value that requires one hour for charging or discharging. The same applies below.) and then discharged to 2.5V at 1 / 6C. CC-CV charging was performed at 1 / 6C to 4.1V. Then, aging was performed under conditions of 60°C and 12 hours. Then, the non-aqueous electrolyte secondary battery was discharged to 2.5V at 1 / 6C to stabilize it. Furthermore, CC-CV charging was performed at 1 / 6C to 4.2V, and then discharged to 2.5V at 1 / 6C to perform initial conditioning.

[0167] [Charged storage test] The non-aqueous electrolyte secondary battery after the initial conditioning was again subjected to CC-CV charging at 1 / 6C to 4.2V, and then stored at high temperature at 60°C for 168 hours. After high temperature storage, the battery was cooled, and the non-aqueous electrolyte secondary battery was discharged at 1 / 6C at 25°C to 2.5V to determine the discharge capacity, which was recorded as the "remaining capacity (1 week)". Table 1 below shows the remaining capacity (1 week) values ​​when the remaining capacity (1 week) of Comparative Example A1-1 is set to 100. The nonaqueous electrolyte secondary battery after the charged storage test was again subjected to CC-CV charging at 1 / 6C to 4.2V, and then subjected to high-temperature storage at 60°C for 336 hours. The nonaqueous electrolyte secondary battery was discharged at 1 / 6C to 2.5V at 25°C to determine the discharge capacity, which was recorded as the "remaining capacity (2 weeks)". Table 1 below shows the remaining capacity values ​​when the remaining capacity (2 weeks) of Comparative Example A1-1 is taken as 100.

[0168] [Table 1]

[0169] A comparison between Comparative Example A1-1 and Comparative Example A1-2 shows that the remaining capacity of the battery is increased by the electrolyte containing FSO3Li. On the other hand, Comparative Examples A1-1 to A1-3 show that even if the electrolyte contains FSO3Li, if the electrolyte contains more than a predetermined amount of nickel ions, the remaining capacity decreases. In addition, Comparative Examples A1-4 to A1-7 show that the remaining capacity is improved when the electrolyte contains about 50 mass ppm of nickel ions (Comparative Example A1-6), but the remaining capacity is decreased when the electrolyte contains less or more nickel ions than that. On the other hand, Examples A1-2 to A1-4 show that when the electrolyte contains FSO3Li, even if it contains the same amount of nickel ions as Comparative Examples A1-4, A1-5, and A1-7, the remaining capacity is improved compared to when FSO3Li is contained alone. That is, it is shown that the nonaqueous electrolyte contains FSO3Li and a predetermined amount of nickel ions, and thus the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high temperature environment are improved.

[0170] <Examples A2-1 to A2-3, Comparative Examples A2-1 to A2-3> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A1-1.

[0171] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A1-1.

[0172] [Preparation of non-aqueous electrolyte] As in Example A1-1, etc., FSO3Li was added to the Ni(PF6)2-containing nonaqueous electrolyte solution or the reference electrolyte solution A1 to prepare the nonaqueous electrolyte solutions shown in Table 2 below.

[0173] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above nonaqueous electrolyte was used.

[0174] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and charged storage tests were performed in the same manner as in Example A1-1. The remaining capacity was determined in the same manner as in Example A1-1. In Table 2 below, the remaining capacity (1 week) values ​​of Examples A2-1 to A2-3 and Comparative Examples A2-1 to A2-3, when the remaining capacity (1 week) of Comparative Example A1-1 is set to 100, are shown together with the results of Comparative Examples A1-1 and A1-5.

[0175] [Table 2]

[0176] Comparison between Comparative Example A1-1 and Comparative Example A1-5 shows that an electrolyte containing 103 mass ppm of nickel ions reduces the remaining capacity of the battery more than an electrolyte containing no nickel ions. Comparative Examples A2-1 and A2-2 show that even if the electrolyte contains FSO3Li, if the content is too small, the remaining capacity of the battery is not improved but rather reduced. From these results, it is expected that the remaining capacity of the battery of Example A2-1 will be lower than that of Comparative Example A1-5 and Comparative Example A2-1. However, Example A2-1 showed a remarkable effect of improving the remaining capacity more than Comparative Example A1-5 and Comparative Example A2-1, and further improving the remaining capacity more than Comparative Example A1-1. Furthermore, a comparison between Example A2-2 and Comparative Example A2-2, and a comparison between Example A2-3 and Comparative Example A2-3 also showed that the electrolyte containing FSO3Li and a predetermined amount of nickel ions improved the remaining capacity of the nonaqueous electrolyte secondary battery, that is, improved the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment.

[0177] <Examples A3-1 to A3-2, Comparative Examples A3-1 to A3-5> [Preparation of positive electrode] Li(Ni 0.5 Mn 0.3 Co 0.290 parts by mass of 100% ethylene oxide, 7 parts by mass of acetylene black as a conductive material, and 3 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone solvent using a disperser to form a slurry. This was evenly applied to one side of an aluminum foil with a thickness of 15 μm, dried, and pressed to form a positive electrode.

[0178] [Preparation of negative electrode] A negative electrode was produced in the same manner as in Example A1-1, except that the slurry containing the negative electrode active material was applied to both sides of the copper foil.

[0179] [Preparation of non-aqueous electrolyte] As in Example A1-1, FSO3Li was added to the Ni(PF6)2-containing nonaqueous electrolyte or the reference electrolyte A1 to prepare the nonaqueous electrolytes shown in Table 3 below. However, Comparative Example A3-1 is the reference electrolyte A1 itself. In addition, the "content (mass%)" and "content (mass ppm)" in the table are the contents when the reference electrolyte A1 is taken as 100 mass%.

[0180] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above positive electrode, negative electrode, and nonaqueous electrolyte were used.

[0181] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were carried out in the same manner as in Example A1-1. The remaining capacity (1 week) and the remaining capacity (2 weeks) were obtained in the same manner as in Example A1-1. The remaining capacity value when the remaining capacity (1 week) of Comparative Example A3-1 is set to 100, and the remaining capacity value (2 weeks) when the remaining capacity (2 weeks) of Comparative Example A3-1 is set to 100 are shown in Table 3 below.

[0182] [Table 3]

[0183] From Comparative Example A3-1, Comparative Example A3-4, and Comparative Example A3-5, it can be seen that an electrolyte containing 5 ppm by mass of nickel ions improves the remaining capacity of a nonaqueous electrolyte battery, while a nickel ion amount as large as 515 ppm by mass reduces the remaining capacity. On the other hand, from Example A3-1, Example A3-2, and Comparative Example A3-2, it was shown that when the electrolyte contains a predetermined amount of nickel ions and also contains FSO3Li, the remaining capacity is increased compared to when FSO3Li is contained alone. Furthermore, from the remaining capacity after storage for 2 weeks, it was shown that the deterioration of the nonaqueous electrolyte battery due to the change over time is suppressed by the electrolyte containing a predetermined amount of nickel ions and also contains FSO3Li, that is, the charge storage characteristics of the nonaqueous electrolyte secondary battery in a high temperature environment are improved. Moreover, from the comparison between Comparative Example A3-3 and Comparative Example A3-2, it can be seen that when the amount of nickel ions contained in the electrolyte is outside the predetermined range, the effect of adding FSO3Li is impaired, and the remaining capacity of the nonaqueous electrolyte battery is reduced.

[0184] For example, the storage period of a battery for a vehicle manufacturer is usually about 200 days. Since the difference in remaining capacity after storage for one week and two weeks increases over time, it can be said that the longer the storage period, the more remarkable the effect of the present invention becomes.

[0185] [Experiment B] Hereinafter, one embodiment of the present invention will be described in more detail with reference to Examples and Reference Examples. However, the present invention is not limited to these Examples as long as it does not depart from the gist of the present invention.

[0186] <Examples B1-1 to B1- 3 , Comparative Examples B1-1~B1- 5 > [Preparation of EC solution containing Co(PF6)2] In an argon glove box, 0.30 g (2.3 mmol) of CoCl2 was weighed into a 50 mL beaker and suspended in acetonitrile (AN). While stirring, 1.168 g (4.6 mmol) of AgPF6 was added slowly in small portions, and the mixture was then stirred at room temperature for 3 hours. As the reaction proceeded, a white solid of AgCl was produced. After leaving the mixture overnight, the AgCl was filtered off, and the filtrate was concentrated under reduced pressure using a rotary evaporator to obtain [Co(AN) n An orange solid of ](PF6)2 (n = 0-6) was obtained. 0.5 g of the obtained orange solid was dissolved in 2.0 g (22.7 mmol) of ethylene carbonate (EC) melted at 45°C, and the solution was evacuated at 35°C for 6 hours to remove AN, which was the coordination solvent, and an EC solution containing Co(PF6)2 was obtained.

[0187] [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A1-1.

[0188] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A1-1.

[0189] [Preparation of non-aqueous electrolyte] Under a dry argon atmosphere, the EC solution containing Co(PF6)2 was diluted with EC, EMC, and DMC so that the cobalt ion concentration in the mixed solvent was as shown in Table 4, and the solvent composition was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:4:3, and LiPF6 that had been thoroughly dried was dissolved at 1 mol / L (as the concentration in the non-aqueous electrolyte). The non-aqueous electrolyte that does not contain Co(PF6)2 is called reference electrolyte B1. FSO3Li was added to the non-aqueous electrolyte containing Co(PF6)2 or reference electrolyte B1 prepared above to prepare the non-aqueous electrolyte shown in Table 4 below. However, Comparative Example B1-1 is the reference electrolyte B1 itself. In the table, the content of FSO3Li indicates the amount added, and the content of cobalt element (cobalt ion) is a value obtained based on the measurement results of inductively coupled plasma atomic emission spectroscopy (ICP-AES) described later. In addition, the "content (mass %)" and "content (mass ppm)" in the table are the contents when the reference electrolyte B1 is taken as 100 mass %.

[0190] <Measurement of the content of cobalt element in non-aqueous electrolyte> 100 μL (approximately 130 mg) of the non-aqueous electrolyte was taken out. The taken non-aqueous electrolyte was weighed into a PTFE beaker, and an appropriate amount of concentrated nitric acid was added and wet decomposed on a hot plate, and the volume was adjusted to 50 mL. The content of Li and cobalt elements was measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES, Thermo Fischer Scientific, iCAP 7600duo) by the acid concentration matching calibration curve method.

[0191] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above nonaqueous electrolyte was used.

[0192] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were performed in the same manner as in Example A1-1. The remaining capacity was determined in the same manner as in Example A1-1. The remaining capacity value when the remaining capacity (1 week) of Comparative Example B1-1 is set to 100 is shown in Table 4 below. The remaining capacity value when the remaining capacity (2 weeks) of Comparative Example B1-1 is set to 100 is shown in Table 4 below.

[0193] [Table 4]

[0194] A comparison between Comparative Example B1-1 and Comparative Example B1-2 shows that the remaining capacity of the nonaqueous electrolyte secondary battery increases when the nonaqueous electrolyte contains FSO3Li. Also, Comparative Examples B1-3 to B1-5 show that when the nonaqueous electrolyte does not contain FSO3Li and contains only cobalt ions at 4 to 190 mass ppm, the nonaqueous electrolyte secondary battery can be used without any problem. battery On the other hand, in Examples B1-1 to B1-3, when the electrolyte solution contained FSO3Li, Comparative Example B1-3 Even when the same amount of cobalt ions as in B1-1 to B1-5 are contained, contrary to expectation, the effect of improving the remaining capacity compared to the case where FSO3Li is contained alone is shown. Furthermore, a comparison between Comparative Example B1-2 and Example B1-2 shows that the difference between the remaining capacity after 168 hours (1 week) high-temperature storage and the remaining capacity after 336 hours (2 weeks) high-temperature storage is even greater depending on whether or not cobalt ions are contained. In other words, it was shown that by the non-aqueous electrolyte containing FSO3Li and a predetermined amount of cobalt ions, the change over time during high-temperature storage is significantly suppressed, and the charged storage characteristics of the non-aqueous electrolyte secondary battery in a high-temperature environment are improved.

[0195] <Examples B2-1 to B2-3 and Comparative Examples B2-1 to B2-3> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example B1-1.

[0196] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example B1-1.

[0197] [Preparation of non-aqueous electrolyte] As in Example B1-1, FSO3Li was added to the Co(PF6)2-containing nonaqueous electrolyte solution or the reference electrolyte solution B1 to prepare the nonaqueous electrolyte solutions shown in Table 5 below.

[0198] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example B1-1, except that the above nonaqueous electrolyte was used.

[0199] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and a charged storage test were performed in the same manner as in Example B1-1. The remaining capacity was determined in the same manner as in Example B1-1. In Table 5 below, the remaining capacity (1 week) values ​​of Examples B2-1 to B2-3 and Comparative Examples B2-1 to B2-3, when the remaining capacity (1 week) of Comparative Example B1-1 is set to 100, are shown together with the results of Comparative Examples B1-1 and B1-4.

[0200] [Table 5]

[0201] Comparison between Comparative Example B1-1 and Comparative Example B1-4 shows that a non-aqueous electrolyte solution containing 78 mass ppm of cobalt ions without FSO3Li reduces the remaining capacity of a non-aqueous electrolyte secondary battery more than a non-aqueous electrolyte solution not containing cobalt ions. Comparative Examples B2-1 and B2-2 show that even if the non-aqueous electrolyte solution contains FSO3Li, if the content is too small, the remaining capacity of the non-aqueous electrolyte secondary battery is not improved, but rather reduced. From these results, the non-aqueous electrolyte secondary battery of Example B2-1 is predicted to have a lower remaining capacity than Comparative Example B1-4 and Comparative Example B2-1. However, Example B2-1 showed a remarkable effect of improving the remaining capacity more than Comparative Example B1-4 and Comparative Example B2-1, and further improving the remaining capacity more than Comparative Example B1-1. Furthermore, a comparison between Example B2-2 and Comparative Example B2-2, and a comparison between Example B2-3 and Comparative Example B2-3 also showed that the nonaqueous electrolyte solution containing FSO3Li and a predetermined amount of cobalt ions improved the remaining capacity of the nonaqueous electrolyte secondary battery, that is, improved the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment.

[0202] <Examples B3-1 to B3-3 and Comparative Examples B3-1 to B3-6> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A3-1.

[0203] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A3-1.

[0204] [Preparation of non-aqueous electrolyte] As in Example B1-1, FSO3Li was added to the non-aqueous electrolyte solution containing Co(PF6)2 or the reference electrolyte solution B1 to prepare the non-aqueous electrolyte solutions shown in Table 6 below. However, Comparative Example B3-1 is the reference electrolyte solution B1 itself. In addition, the "content (mass%)" and "content (mass ppm)" in the table are the contents when the reference electrolyte solution B1 is taken as 100 mass%.

[0205] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example B1-1, except that the above positive electrode, negative electrode, and nonaqueous electrolyte were used.

[0206] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were carried out in the same manner as in Example B1-1. The remaining capacity (1 week) and the remaining capacity (2 weeks) were obtained in the same manner as in Example B1-1. The remaining capacity (1 week) value when the remaining capacity (1 week) of Comparative Example B3-1 is set to 100, and the remaining capacity (2 weeks) value when the remaining capacity (2 weeks) of Comparative Example B3-1 is set to 100 are shown in Table 6 below.

[0207] [Table 6]

[0208] Comparative Example B3-1, Comparative Example B3-4, and Comparative Example B3-6 show that a non-aqueous electrolyte containing 4 ppm by mass of cobalt ions improves the remaining capacity of a non-aqueous electrolyte secondary battery, while when the amount of cobalt ions is as high as 476 ppm by mass, the remaining capacity after 168 hours (1 week) of high-temperature storage is reduced, and the remaining capacity after 336 hours (2 weeks) of high-temperature storage is equivalent to that without cobalt ions. Also, a comparison between Comparative Example B3-3 and Comparative Example B3-2 shows that even if the non-aqueous electrolyte contains FSO3Li, when it contains 760 ppm by mass of cobalt ions, the effect of adding FSO3Li is impaired, and the remaining capacity of the non-aqueous electrolyte secondary battery after 168 hours (1 week) of high-temperature storage is reduced. Furthermore, from Examples B3-1 to B3-3 and Comparative Examples B3-1 to B3-6, it was shown that when the nonaqueous electrolyte contains a predetermined amount of cobalt ions and also contains FSO3Li, the remaining capacity of the nonaqueous electrolyte secondary battery after high-temperature storage is increased compared to when the nonaqueous electrolyte contains FSO3Li or cobalt ions alone, and in particular, from a comparison of the ratio of the remaining capacity after 168 hours (1 week) of high-temperature storage to that after 336 hours (2 weeks) of high-temperature storage, deterioration of the nonaqueous electrolyte secondary battery due to changes over time is significantly suppressed, and the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment are improved.

[0209] For example, the storage period of a battery for a vehicle manufacturer is usually about 200 days. Since the difference in remaining capacity after storage for one week and two weeks increases over time, it can be said that the longer the storage period, the more remarkable the effect of the present invention becomes.

[0210] [Experiment C] Hereinafter, one embodiment of the present invention will be described in more detail with reference to Examples and Reference Examples. However, the present invention is not limited to these Examples as long as it does not depart from the gist of the present invention.

[0211] <Examples C1-1 to C1-4 and Comparative Examples C1-1 to C1-7> [Preparation of EC solution containing Cu(PF6)2] In an argon glove box, 0.50 g (3.7 mmol) of CuCl2 was weighed into a 50 mL beaker and suspended in acetonitrile (AN). While stirring, 1.88 g (7.4 mmol) of AgPF6 was added slowly in small portions, and then stirred at room temperature for 3 hours. As the reaction proceeded, a white solid of AgCl was produced. After leaving it overnight, AgCl was filtered off, and the obtained filtrate was concentrated under reduced pressure using a rotary evaporator to obtain [Cu(AN) n A blue solid of ](PF6)2 (n = 0-6) was obtained. 5.0 g (56.8 mmol) of ethylene carbonate (EC) melted at 45°C was added to dissolve the solid, and the solution was evacuated at 35°C for 6 hours to remove the coordination solvent AN, yielding an EC solution containing Cu(PF6)2.

[0212] [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A1-1.

[0213] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A1-1.

[0214] [Preparation of non-aqueous electrolyte] Under a dry argon atmosphere, the EC solution containing Cu(PF6)2 was diluted with EC, EMC, and DMC so that the copper ion concentration in the mixed solvent was as shown in Table 7, and the solvent composition was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:4:3, and LiPF6 that had been thoroughly dried was dissolved at 1 mol / L (as the concentration in the non-aqueous electrolyte). The non-aqueous electrolyte that does not contain Cu(PF6)2 is called reference electrolyte C1. FSO3Li was added to the non-aqueous electrolyte containing Cu(PF6)2 or reference electrolyte C1 prepared above to prepare the non-aqueous electrolyte shown in Table 7 below. However, Comparative Example C1-1 is the reference electrolyte C1 itself. In the table, the content of FSO3Li indicates the amount added, and the content of copper element (copper ion) is a value obtained based on the measurement results of inductively coupled plasma atomic emission spectroscopy (ICP-AES) described later. In addition, the "content (mass %)" and "content (mass ppm)" in the table are the contents when the reference electrolyte C1 is taken as 100 mass %.

[0215] <Measurement of copper content in non-aqueous electrolyte> 100 μL (approximately 130 mg) of the non-aqueous electrolyte was taken out. The taken non-aqueous electrolyte was weighed into a PTFE beaker, and an appropriate amount of concentrated nitric acid was added and wet decomposed on a hot plate, after which the volume was adjusted to 50 mL. The content of Li and copper elements was measured by the acid concentration matching calibration curve method using inductively coupled plasma atomic emission spectroscopy (ICP-AES, Thermo Fischer Scientific, iCAP 7600duo).

[0216] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above nonaqueous electrolyte was used.

[0217] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were performed in the same manner as in Example A1-1. The remaining capacity was determined in the same manner as in Example A1-1. The following Table 7 shows the remaining capacity (1 week) when the remaining capacity of Comparative Example C1-1 is set to 100. The following Table 7 shows the remaining capacity when the remaining capacity of Comparative Example C1-1 is set to 100 (2 weeks).

[0218] [Table 7]

[0219] Comparison between Comparative Example C1-1 and Comparative Example C1-2 shows that the remaining capacity of the battery increases when the electrolyte contains FSO3Li. On the other hand, Comparative Examples C1-1 to C1-3 show that even if the electrolyte contains FSO3Li, if it contains more than a certain amount of copper ions, the remaining capacity does not change and the effect of containing FSO3Li is not exhibited. Furthermore, Comparative Examples C1-4 to C1-7 show that when the electrolyte contains 5 ppm by mass of copper ions, the remaining capacity is the same as when it does not contain copper ions, and when it contains about 60 ppm by mass, the remaining capacity is improved, but when it contains more copper ions than that, the remaining capacity is reduced (Comparative Examples C1-4, C1-5). On the other hand, Examples C1-1 to C1-4 show that when the electrolyte contains FSO3Li, even when it contains the same amount of copper ions as Comparative Examples C1-5 to C1-7, the effect of improving the remaining capacity is shown to be higher than when FSO3Li is contained alone. That is, it was shown that the non-aqueous electrolyte contains FSO3Li and a predetermined amount of copper ions, and thus the charge storage characteristics of the non-aqueous electrolyte secondary battery in a high temperature environment are improved. In addition, in Comparative Example C1-5, the remaining capacity decreased after high temperature storage at 60°C for 168 hours, and the remaining capacity value further decreased after high temperature storage at 60°C for 336 hours, whereas in Example C1-2 of the non-aqueous electrolyte battery containing the same amount of copper ions and FSO3Li, the remaining capacity ratio improved after high temperature storage at 60°C for 168 hours, and the remaining capacity ratio further improved after high temperature storage at 60°C for 336 hours. That is, it was shown that the non-aqueous electrolyte contains a predetermined amount of copper ions and contains FSO3Li, and thus the deterioration of the non-aqueous electrolyte battery due to aging is significantly suppressed.

[0220] <Examples C2-1 to C2-3 and Comparative Examples C2-1 to C2-3> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example C1-1.

[0221] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example C1-1.

[0222] [Preparation of non-aqueous electrolyte] As in Example C1-1, FSO3Li was added to the Cu(PF6)2-containing nonaqueous electrolyte solution or the reference electrolyte solution C1 to prepare the nonaqueous electrolyte solutions shown in Table 8 below.

[0223] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example C1-1, except that the above nonaqueous electrolyte was used.

[0224] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and charged storage tests were performed in the same manner as in Example C1-1. The remaining capacity (1 week) was determined in the same manner as in Example C1-1. In Table 8 below, the remaining capacity (1 week) values ​​of Examples C2-1 to C2-3 and Comparative Examples C2-1 to C2-3, when the remaining capacity (1 week) of Comparative Example C1-1 is set to 100, are shown together with the results of Comparative Examples C1-1 and C1-5.

[0225] [Table 8]

[0226] Comparison between Comparative Example C1-1 and Comparative Example C1-5 shows that a non-aqueous electrolyte solution that does not contain FSO3Li and contains 123 mass ppm of copper ions reduces the remaining capacity of the battery more than a non-aqueous electrolyte solution that does not contain copper ions. In addition, Comparative Examples C2-1 to C2-3 show that even if the non-aqueous electrolyte solution contains FSO3Li, if the content is too small, the remaining capacity of the battery is not improved, but rather reduced. From these results, the non-aqueous electrolyte batteries of Examples C2-1 and C2-2 are expected to have a lower remaining capacity than Comparative Example C1-5 and Comparative Example C2-1 or Comparative Example C2-2. However, the non-aqueous electrolyte battery of Example C2-1 showed a remarkable effect of improving the remaining capacity more than Comparative Example C1-5 and Comparative Example C2-1, and further improving the remaining capacity more than Comparative Example C1-1. Moreover, the nonaqueous electrolyte battery of Example C2-2 showed a remarkable effect of improving the remaining capacity compared to Comparative Examples C1-5 and C2-2, and furthermore improving the remaining capacity compared to Comparative Example C1-1. Moreover, Examples C2-1 to C2-3 showed a remarkable effect of improving the remaining capacity of the nonaqueous electrolyte secondary battery by containing FSO3Li and a predetermined amount of copper ions in the electrolyte, that is, improving the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high temperature environment.

[0227] <Examples C3-1 to C3-2, Comparative Examples C3-1 to C3-5> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A3-1.

[0228] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A3-1.

[0229] [Preparation of non-aqueous electrolyte] As in Example C1-1, FSO3Li was added to the Cu(PF6)2-containing nonaqueous electrolyte or the reference electrolyte D1 to prepare the nonaqueous electrolytes shown in Table 9 below. However, Comparative Example C3-1 is the reference electrolyte C1 itself. In addition, the "content (mass%)" and "content (mass ppm)" in the table are the contents when the reference electrolyte C1 is taken as 100 mass%.

[0230] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example C1-1, except that the above positive electrode, negative electrode, and nonaqueous electrolyte were used.

[0231] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were carried out in the same manner as in Example C1-1. The remaining capacity (1 week) and the remaining capacity (2 weeks) were obtained in the same manner as in Example C1-1. The remaining capacity (1 week) value when the remaining capacity (1 week) of Comparative Example C3-1 is set to 100, and the remaining capacity (2 weeks) value when the remaining capacity (2 weeks) of Comparative Example C3-1 is set to 100 are shown in Table 9 below.

[0232] [Table 9]

[0233] From Comparative Examples C3-1 and C3-4, it can be seen that a non-aqueous electrolyte solution that does not contain FSO3Li and contains 308 mass ppm of copper ions reduces the remaining capacity of a non-aqueous electrolyte secondary battery. Also, from Comparative Example C3-5, it can be seen that when FSO3Li is not contained and the amount of copper ions is as small as 5 mass ppm, the ratio of remaining capacity decreases after high-temperature storage at 60°C for 168 hours, but the ratio of remaining capacity improves after high-temperature storage at 60°C for 336 hours. Also, from a comparison between Comparative Examples C3-3 and C3-2, it can be seen that if the amount of copper ions contained in the non-aqueous electrolyte solution is outside the specified range, the effect of adding FSO3Li is impaired, and the remaining capacity of the non-aqueous electrolyte battery decreases. Furthermore, from Examples C3-1 and C3-2 and Comparative Examples C3-1 to C3-5, it was shown that when the nonaqueous electrolyte contains a predetermined amount of copper ions and also contains FSO3Li, the remaining capacity after 168 hours (1 week) of high-temperature storage is increased compared to when FSO3Li or copper ions are contained alone, and further, a comparison of the remaining capacity after 168 hours (1 week) of high-temperature storage and after 336 hours (2 weeks) of high-temperature storage shows that deterioration of the nonaqueous electrolyte secondary battery due to changes over time is significantly suppressed. In other words, it was shown that when the nonaqueous electrolyte contains FSO3Li and a predetermined amount of copper ions, the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment are improved.

[0234] For example, the storage period of a battery for a vehicle manufacturer is usually about 200 days. Since the difference in remaining capacity after storage for one week and two weeks increases over time, it can be said that the longer the storage period, the more remarkable the effect of the present invention becomes.

[0235] [Experiment D] Hereinafter, one embodiment of the present invention will be described in more detail with reference to Examples and Reference Examples. However, the present invention is not limited to these Examples as long as it does not depart from the gist of the present invention.

[0236] <Examples D1-1 to D1-2, Comparative Examples D1-1 to D1-5> [Preparation of EC solution containing Mn(PF6)2] In an argon glove box, 0.10 g (0.8 mmol) of MnCl2 was weighed into a 50 mL beaker and suspended in acetonitrile (AN). While stirring, 0.402 g (1.6 mmol) of AgPF6 was added slowly in small portions, and then stirred at room temperature for 3 hours. As the reaction proceeded, a white solid of AgCl was produced. After leaving it overnight, the AgCl was filtered off, and the obtained filtrate was concentrated under reduced pressure using a rotary evaporator to obtain [Mn(AN) n A white solid of Mn(PF6)2 (n = 0-6) was obtained. 5.0 g (56.8 mmol) of ethylene carbonate (EC) melted at 45°C was added to dissolve the solid, and the solution was evacuated at 35°C for 6 hours to remove the coordination solvent AN, yielding an EC solution containing Mn(PF6)2.

[0237] [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A1-1.

[0238] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A1-1.

[0239] [Preparation of non-aqueous electrolyte] Under a dry argon atmosphere, the EC solution containing Mn(PF6)2 was diluted with EC, EMC, and DMC so that the manganese ion concentration in the mixed solvent was as shown in Table 10, and the solvent composition was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:4:3, and LiPF6 that had been thoroughly dried was dissolved at 1 mol / L (as the concentration in the non-aqueous electrolyte). The non-aqueous electrolyte that does not contain Mn(PF6)2 is called reference electrolyte D1. FSO3Li was added to the non-aqueous electrolyte containing Mn(PF6)2 or reference electrolyte D1 prepared above to prepare the non-aqueous electrolytes listed in Table 10 below. However, Comparative Example D1-1 is the reference electrolyte D1 itself. In the table, the content of FSO3Li indicates the amount added, and the content of manganese element (manganese ion) is a value obtained based on the measurement results of inductively coupled plasma atomic emission spectroscopy (ICP-AES) described later. In addition, the "content (mass %)" and "content (mass ppm)" in the table are the contents when the reference electrolyte D1 is taken as 100 mass %.

[0240] <Measurement of manganese element content in non-aqueous electrolyte> 100 μL (approximately 130 mg) of the non-aqueous electrolyte was taken out. The taken non-aqueous electrolyte was weighed into a PTFE beaker, and an appropriate amount of concentrated nitric acid was added and the solution was wet-decomposed on a hot plate, and then the volume was adjusted to 50 mL. The content of Li and manganese elements was measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES, Thermo Fischer Scientific, iCAP 7600duo) with an acid concentration matching calibration curve method.

[0241] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above nonaqueous electrolyte was used.

[0242] <Evaluation of non-aqueous electrolyte secondary batteries> [Initial conditioning] The initial conditioning and the charged storage test were performed in the same manner as in Example A1-1. The remaining capacity was determined in the same manner as in Example A1-1. The remaining capacity (1 week) is shown in Table 10 below, taking the remaining capacity (1 week) of Comparative Example D1-1 as 100. Table 10 below shows the remaining capacity values ​​when the remaining capacity (2 weeks) of Comparative Example D1-1 is taken as 100.

[0243] [Table 10]

[0244] Comparison between Comparative Example D1-1 and Comparative Example D1-2 shows that the nonaqueous electrolyte solution containing FSO3Li increases the remaining capacity of the nonaqueous electrolyte secondary battery after high-temperature storage. On the other hand, Comparative Examples D1-1 to D1-3 show that even if the nonaqueous electrolyte solution contains FSO3Li, if it contains more than a predetermined amount of manganese ions, the remaining capacity after high-temperature storage decreases. In addition, Comparative Example D1-4 shows that when the nonaqueous electrolyte solution does not contain FSO3Li but contains 26 mass ppm of manganese ions, the remaining capacity after high-temperature storage at 60°C for 168 hours (1 week) is the same as when the nonaqueous electrolyte solution does not contain manganese ions, but the ratio of the remaining capacity after high-temperature storage for 336 hours (2 weeks) is lowered, which shows that the charge storage characteristics of the nonaqueous electrolyte secondary battery containing manganese ions tend to deteriorate over time. In addition, a comparison between Comparative Example D1-1 and Comparative Example D1-5 shows that when the non-aqueous electrolyte does not contain FSO3Li and contains 7 ppm by mass of manganese ions, the remaining capacity after high-temperature storage at 60°C for 168 hours (1 week) is improved, but after high-temperature storage for 336 hours (2 weeks), the remaining capacity is significantly lower than when the electrolyte does not contain manganese ions. On the other hand, Examples D1-1 and D1-2 show that when the non-aqueous electrolyte contains FSO3Li, even when the electrolyte contains the same amount of manganese ions as Comparative Examples D1-4 and D1-5, the remaining capacity after high-temperature storage is improved compared to when the electrolyte contains FSO3Li alone. That is, it was shown that the deterioration of the non-aqueous electrolyte secondary battery due to aging is significantly suppressed by the non-aqueous electrolyte containing FSO3Li and a predetermined amount of manganese ions, and the charge storage characteristics of the non-aqueous electrolyte secondary battery in a high-temperature environment are improved.

[0245] <Examples D2-1 to D2-3, Comparative Examples D2-1 to D2-3> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example D1-1.

[0246] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example D1-1.

[0247] [Preparation of non-aqueous electrolyte] As in Example D1-1, FSO3Li was added to the Mn(PF6)2-containing nonaqueous electrolyte solution or the reference electrolyte solution D1 to prepare the nonaqueous electrolyte solutions shown in Table 11 below.

[0248] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example D1-1, except that the above nonaqueous electrolyte was used.

[0249] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and charged storage test were performed in the same manner as in Example D1-1. The remaining capacity was determined in the same manner as in Example D1-1. In Table 11 below, the remaining capacity (1 week) values ​​of Examples D2-1 to D2-3 and Comparative Examples D2-1 to D2-3, when the remaining capacity (1 week) of Comparative Example D1-1 is set to 100, are shown together with the results of Comparative Examples D1-1 and D1-4.

[0250] [Table 11]

[0251] Comparison between Comparative Example D1-1 and Comparative Example D1-4 shows that the remaining capacity of the non-aqueous electrolyte solution not containing FSO3Li and containing 26 mass ppm of manganese ions after high-temperature storage at 60°C for 168 hours (1 week) is equivalent to that of the non-aqueous electrolyte solution not containing manganese ions. Comparative Example D2-1 shows that even if the non-aqueous electrolyte solution contains FSO3Li, if the content is too small, the remaining capacity of the non-aqueous electrolyte secondary battery is not improved, but rather reduced. From these results, the non-aqueous electrolyte secondary battery of Example D2-1 is predicted to have a lower remaining capacity than Comparative Example D1-4 and Comparative Example D2-1. However, Example D2-1 showed a remarkable effect that the remaining capacity was improved compared to Comparative Example D1-4 and Comparative Example D2-1, and furthermore, the remaining capacity was improved compared to Comparative Example D1-1. Furthermore, a comparison between Example D2-2 and Comparative Example D2-2, and a comparison between Example D2-3 and Comparative Example D2-3 also showed that the nonaqueous electrolyte solution containing FSO3Li and a predetermined amount of manganese ions improves the remaining capacity of the nonaqueous electrolyte secondary battery after high-temperature storage, that is, improves the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment.

[0252] <Examples D3-1 to D3-3 and Comparative Examples D3-1 to D3-6> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A3-1.

[0253] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A3-1.

[0254] [Preparation of non-aqueous electrolyte] As in Example D1-1, FSO3Li was added to the Mn(PF6)2-containing non-aqueous electrolyte or the reference electrolyte D1 to prepare the non-aqueous electrolytes shown in Table 12 below. However, Comparative Example D3-1 is the reference electrolyte D1 itself. In addition, the "content (mass%)" and "content (mass ppm)" in the table are the contents when the reference electrolyte D1 is taken as 100 mass%.

[0255] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example D1-1, except that the above positive electrode, negative electrode, and nonaqueous electrolyte were used.

[0256] <Evaluation of non-aqueous electrolyte secondary batteries> The initial conditioning and the charge storage test were performed in the same manner as in Example D1-1. The remaining capacity (1 week) and the remaining capacity (2 weeks) were obtained in the same manner as in Example D1-1. The remaining capacity value when the remaining capacity of Comparative Example D3-1 is set to 100, and the remaining capacity value (2 weeks) when the remaining capacity of Comparative Example D3-1 is set to 100 are shown in Table 12 below.

[0257] [Table 12]

[0258] A comparison between Comparative Example D3-1 and Comparative Example D3-2 shows that the nonaqueous electrolyte solution containing FSO3Li improves the charge storage characteristics of the nonaqueous electrolyte secondary battery after high-temperature storage. On the other hand, Comparative Examples D3-1 to D3-3 and Examples D3-1 to D3-3 show that even if the nonaqueous electrolyte solution contains FSO3Li, if it contains more than a predetermined amount of manganese ions, the remaining capacity of the nonaqueous electrolyte secondary battery after high-temperature storage decreases. In addition, Comparative Examples D3-1, D3-4, and D3-5 show that a nonaqueous electrolyte solution containing 10 mass ppm or more of manganese ions reduces the remaining capacity of a nonaqueous electrolyte secondary battery after 168 hours (1 week) of high-temperature storage, but improves the remaining capacity after 336 hours (2 weeks) of high-temperature storage compared to a case without manganese ions. Furthermore, from Examples D3-1 to D3-3, it was shown that when the nonaqueous electrolyte contains a predetermined amount of manganese ions and also contains FSO3Li, the remaining capacity after 168 hours (1 week) of high-temperature storage is greater than when FSO3Li or manganese ions are contained alone, and further, from a comparison of the ratio of the remaining capacity after 168 hours (1 week) of high-temperature storage to that after 336 hours (2 weeks) of high-temperature storage, deterioration of the nonaqueous electrolyte secondary battery due to changes over time is significantly suppressed, and the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment are improved.

[0259] For example, the storage period of a battery for a vehicle manufacturer is usually about 200 days. Since the difference in remaining capacity after storage for one week and two weeks increases over time, it can be said that the longer the storage period, the more remarkable the effect of the present invention becomes.

[0260] [Experiment E] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and reference examples. However, this embodiment is not limited to these examples as long as it does not depart from the gist of the present invention.

[0261] <Examples E1-1 to E1-7 and Comparative Examples E1-1 to E1-10> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A3-1.

[0262] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A3-1.

[0263] [Preparation of non-aqueous electrolyte] Under a dry argon atmosphere, tris(2,4-pentanedionato)aluminum (Al(acac)3) or aluminum fluorosulfonate (Al(FSO3)3) was dissolved in ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) so that the aluminum ion concentration in the mixed solvent was as shown in Table 13, and the solvent composition was such that the volume ratio of EC, EMC, and DMC was 3:4:3. LiPF6 was then dissolved at 1 mol / L (12.3 mass%, as the concentration in the non-aqueous electrolyte) after sufficient drying. A non-aqueous electrolyte that does not contain either Al(acac)3 or Al(FSO3)3 is called reference electrolyte E1. FSO3Li was added to the non-aqueous electrolyte or reference electrolyte E1 prepared above to prepare the non-aqueous electrolytes of Examples E1-1 to E1-7 and the non-aqueous electrolytes of Comparative Examples E1-2 to E1-3 shown in Table 13 below. Comparative Example E1-1 is the standard electrolyte E1 itself. In addition, the non-aqueous electrolytes of Comparative Examples E1-4 to E1-10 were made without adding FSO3Li. In the table, the content of FSO3Li indicates the amount added, and the content of aluminum element (aluminum ion) is a value obtained based on the measurement results of inductively coupled plasma atomic emission spectrometry (ICP-AES) described later. In addition, the "content (mass%)" and "content (mass ppm)" in the table are the contents when the standard electrolyte E1 is taken as 100 mass%. Al(FSO3)3 was synthesized according to the method described in Polyhedron, 1983, Volume 2, Issue 11, Pages 1209-1210.

[0264] <Measurement of aluminum element content in non-aqueous electrolyte> 100 μL (approximately 130 mg) of the non-aqueous electrolyte was taken. The taken non-aqueous electrolyte was weighed into a PTFE beaker, and an appropriate amount of concentrated nitric acid was added and wet decomposed on a hot plate, after which the volume was adjusted to 50 mL. The content of Li and aluminum element (aluminum ion) was measured using an inductively coupled plasma atomic emission spectrometry (ICP-AES, Thermo Fischer Scientific, iCAP 7600duo) with an acid concentration matching calibration curve method.

[0265] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A1-1, except that the above nonaqueous electrolyte was used.

[0266] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and a charge storage test were performed in the same manner as in Example A1-1. The remaining capacity was determined in the same manner as in Example A1-1. Table 13 below shows the remaining capacity (1 week) values ​​of Examples E1-1 to E1-7 and Comparative Examples E1-1 to E1-10 when the remaining capacity (1 week) of Comparative Example E1-1 is set to 100. Table 13 below shows the remaining capacity (2 weeks) values ​​of Examples E1-1 to E1-7 and Comparative Examples E1-1 to E1-10 when the remaining capacity (2 weeks) of Comparative Example E1-1 is set to 100.

[0267] [Table 13]

[0268] Comparison between Comparative Example E1-1 and Comparative Example E1-2 showed that the remaining capacity of the battery was increased by the electrolyte containing FSO3Li. On the other hand, Comparative Examples E1-1 to E1-3 showed that even if the electrolyte contains FSO3Li, if it contains more than a specific amount of aluminum ions, the remaining capacity is reduced. Examples E1-1 to E1-7 showed that when the electrolyte contains FSO3Li, even if it contains the same amount of aluminum ions as Comparative Examples E1-4 to E1-10, the remaining capacity is improved compared to when FSO3Li is contained alone (Comparative Example E1-2). Furthermore, the remaining capacity after storage for 2 weeks also showed that the deterioration of the nonaqueous electrolyte battery due to aging is suppressed by the electrolyte containing a specific amount of aluminum ions and FSO3Li, that is, the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high temperature environment are improved. From Examples E1-1 to E1-7, it was shown that the non-aqueous electrolyte secondary battery has improved charging storage characteristics in a high temperature environment when the non-aqueous electrolyte contains FSO3Li and a specific amount of aluminum ions, regardless of the type of counter anion of the aluminum ion. For example, the storage period of a battery is usually about 200 days for a vehicle manufacturer. Since the difference in remaining capacity after storage for one week and two weeks increases over time, it can be said that the effect of the present invention becomes more pronounced as the storage period becomes longer.

[0269] <Examples E2-1 to E2-3, Comparative Examples E2-1 to E2-3> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example E1-1.

[0270] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example E1-1.

[0271] [Preparation of non-aqueous electrolyte] The Al(FSO3)3-containing nonaqueous electrolyte solutions of Examples E2-1 to E2-3 were prepared in the same manner as in Example E1-4, except that the content of FSO3Li was changed as shown in the following Table 14. In addition, FSO3Li was added to the reference electrolyte E1 as shown in the following Table 14 to prepare the nonaqueous electrolyte solutions of Comparative Examples E2-1 to E2-3.

[0272] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example E1-4, except that the above nonaqueous electrolyte was used.

[0273] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and a charged storage test were performed in the same manner as in Example E1-4. The remaining capacity (1 week) was determined in the same manner as in Example E1-4. Table 14 below shows the remaining capacities of Examples E2-1 to E2-3 and Comparative Examples E2-1 to E2-3 when the remaining capacity (1 week) of Comparative Example E1-1 is set to 100. (1 week) The values ​​are shown together with the results of Comparative Example E1-1 and Comparative Example E1-7.

[0274] [Table 14]

[0275] Comparison between Comparative Example E1-1 and Comparative Example E1-7 shows that the electrolyte solution not containing FSO3Li and containing a specific amount of aluminum ions (Comparative Example E1-7) reduces the remaining capacity of the non-aqueous electrolyte battery more than the electrolyte solution not containing aluminum ions (Comparative Example E1-1). In addition, Comparative Examples E2-1 and E2-2 show that even if the electrolyte solution contains FSO3Li, if the content is too small, the remaining capacity of the battery is not improved, but rather reduced. From these results, it is expected that the remaining capacity of the battery of Example E2-1 will be lower than that of Comparative Examples E1-7 and E2-1. However, Example E2-1 showed a remarkable effect of improving the remaining capacity more than Comparative Examples E1-7 and E2-1, and further improving the remaining capacity more than Comparative Example E1-1. Furthermore, a comparison between Example E2-2 and Comparative Example E2-2, and a comparison between Example E2-3 and Comparative Example E2-3 also showed that the nonaqueous electrolyte solution containing FSO3Li and a specific amount of aluminum ions improves the remaining capacity of the nonaqueous electrolyte secondary battery, that is, improves the charged storage characteristics of the nonaqueous electrolyte secondary battery in a high-temperature environment.

[0276] [Experiment F] Hereinafter, one embodiment of the present invention will be described in more detail with reference to Examples and Reference Examples. However, the present invention is not limited to these Examples as long as it does not depart from the gist of the present invention.

[0277] <Examples F1-1 to F1-17 and Comparative Examples F1-1 to F1-19> [Preparation of positive electrode] A positive electrode was prepared in the same manner as in Example A3-1.

[0278] [Preparation of negative electrode] A negative electrode was prepared in the same manner as in Example A3-1.

[0279] [Preparation of non-aqueous electrolyte] The metal ion-containing nonaqueous electrolyte solutions of Examples F1-1 to F1-17 were prepared in the same manner as in Example A3, except that the content of FSO3Li and metal ions was changed as shown in Table 15 below. The reference electrolyte solution F1 is an electrolyte solution obtained by dissolving LiPF6 at 1 mol / L (as the concentration in the nonaqueous electrolyte solution) in a mixture of EC:EMC:DMC with a volume ratio of 3:4:3, as in the reference electrolyte solution A1. In addition, FSO3Li was added to the reference electrolyte solution F1 as shown in the table below to prepare the nonaqueous electrolyte solution of Comparative Example F1-2. In addition, the nonaqueous electrolyte solutions of Comparative Examples F1-3 to F1-19 were prepared by adding specific metal ions but not adding FSO3Li.

[0280] [Manufacture of non-aqueous electrolyte secondary batteries] A laminate-type nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example A3-1, except that the above nonaqueous electrolyte was used.

[0281] <Evaluation of non-aqueous electrolyte secondary batteries> Initial conditioning and a charged storage test were performed in the same manner as in Example A3-1. The remaining capacity (1 week) was determined in the same manner as in Example A3-1. The remaining capacity (1 week) of Comparative Example F1-1 is set to 100 in the table below. (1 week) Indicates the value of. The following table shows the remaining capacity (2 weeks) of Examples F1-1 to F1-17 and Comparative Examples F1-1 to F1-19, assuming that the remaining capacity (2 weeks) of Comparative Example F1-1 is 100.

[0282] [Table 15]

[0283] Comparative Examples F1-3 to F1-19 used electrolytes containing specific metal ions and not containing FSO3Li. Comparative Examples F1-3, F1-5, F1-7, F1-8, F1-12, F1-14, and F1-16 showed a tendency for the remaining capacity of the battery to be lower than that of Comparative Example F1-1, which does not contain specific metal ions or FSO3Li. In addition, Comparative Examples F1-4, F1-9, F1-10, and F1-15, the remaining capacity after one week was equivalent to that of Comparative Example F1-1, but the remaining capacity after two weeks was lower. Comparative Examples F1-6, F1-11, F1-13, F1-17, F1-18, and F1-19 showed an increase in the remaining capacity after one week compared to Comparative Example F1-1, but some of them had a remaining capacity after two weeks that was inferior to that of Comparative Example F1-1. These results show that the use of a non-aqueous electrolyte containing multiple specific metal ions does not necessarily improve the remaining capacity of the battery, and in most cases the remaining capacity deteriorates over time. On the other hand, from Examples F1-1 to F1-17, when the electrolyte contains both a specific metal ion and FSO3Li, even if it contains the same amount of metal ions as Comparative Examples F1-3 to F1-19, the effect of improving the remaining capacity was shown to be greater than when FSO3Li is contained alone (Comparative Example F1-2). Furthermore, from the remaining capacity after storage for 2 weeks, it was shown that the electrolyte contains a specific amount of metal ions and FSO3Li, thereby suppressing the deterioration of the nonaqueous electrolyte battery due to changes over time, that is, the charging storage characteristics of the nonaqueous electrolyte secondary battery in a high temperature environment are improved. For example, the storage period of the battery is usually about 200 days for a vehicle manufacturer. Since the difference between the remaining capacity after storage for 1 week and 2 weeks increases over time, it can be said that the effect of the present invention becomes more pronounced as the storage period becomes longer.

[0284] This application is based on Japanese patent applications filed on June 4, 2019 (Patent Application No. 2019-104306), June 26, 2019 (Patent Application No. 2019-118148), June 26, 2019 (Patent Application No. 2019-118074), June 26, 2019 (Patent Application No. 2019-118145), and April 15, 2020 (Patent Application No. 2020-073075), the contents of which are incorporated herein by reference. [Industrial Applicability]

[0285] INDUSTRIAL APPLICABILITY The present invention is useful in that it realizes a nonaqueous electrolyte battery that has excellent charged storage characteristics in a high-temperature environment. In addition, the nonaqueous electrolyte and nonaqueous electrolyte battery of the present invention can be used in various known applications using nonaqueous electrolyte or nonaqueous electrolyte battery.Specific examples include notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, mobile fax machines, mobile copiers, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, handheld cleaners, portable CDs, minidiscs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, motorcycles, motorized bicycles, bicycles, lighting equipment, toys, game equipment, watches, power tools, strobes, cameras, home backup power sources, business backup power sources, load leveling power sources, natural energy storage power sources, and lithium ion capacitors.

Claims

1. (1a) FSO 3 Contains Li, (1b) containing at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e); and (1c) A non-aqueous electrolyte solution that satisfies at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) the concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less (iii) The concentration of the (c) is 1 ppm by mass or more and 500 ppm by mass or less. (iv) The concentration of (d) is 1 ppm by mass or more and 100 ppm by mass or less. (v) The concentration of (e) is 1 ppm by mass or more and 100 ppm by mass or less.

2. The non-aqueous electrolyte solution according to claim 1 , comprising at least nickel ions (a).

3. 3. The nonaqueous electrolyte solution according to claim 2, comprising nickel ions in an amount of 40 mass% or more based on the total amount of the metal ions (a) to (e).

4. The nonaqueous electrolyte solution according to claim 3, wherein the total concentration of (a) to (e) is 1 ppm by mass or more and 120 ppm by mass or less.

5. FSO 3 The nonaqueous electrolyte according to any one of claims 1 to 4, wherein the Li content is 0.001% by mass or more and 10.0% by mass or less.

6. A non-aqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a non-aqueous electrolyte, (1a) FSO 3 Contains Li, (1b) containing at least one metal ion selected from the group consisting of nickel ions (a), cobalt ions (b), copper ions (c), manganese ions (d) and aluminum ions (e); and (1c) A nonaqueous electrolyte battery, the nonaqueous electrolyte satisfying at least one of the following conditions (i) to (v): (i) The concentration of (a) is 1 ppm by mass or more and 500 ppm by mass or less. (ii) the concentration of (b) is 1 ppm by mass or more and 500 ppm by mass or less (iii) The concentration of the (c) is 1 ppm by mass or more and 500 ppm by mass or less. (iv) The concentration of (d) is 1 ppm by mass or more and 100 ppm by mass or less. (v) The concentration of (e) is 1 ppm by mass or more and 100 ppm by mass or less.

7. 7. The nonaqueous electrolyte battery according to claim 6, wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following composition formula (1): Li a1 Ni b1 Co c1 M d1 O 2 ・・・(1) (In the above formula (1), a1, b1, c1, and d1 satisfy 0.90≦a1≦1.10, 0<b1<0.4, and b1+c1+d1=1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.)

8. 7. The nonaqueous electrolyte battery according to claim 6, wherein the positive electrode has a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material is a metal oxide represented by the following composition formula (2): Li a2 Ni b2 Co c2 M d2 O 2 ・・・(2) (In the above formula (2), a2, b2, c2, and d2 satisfy 0.90≦a2≦1.10, 0.4≦b2<1.0, and b2+c2+d2=1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.)

9. 9. The nonaqueous electrolyte battery according to claim 6, wherein the positive electrode is an NMC positive electrode, and the content of the nickel element in the NMC positive electrode relative to the total amount of the nickel element, the manganese element, and the cobalt element is 40 mol % or more.

Citation Information

Patent Citations

  • Battery

    JP2003346900A

  • Nonaqueous electrolytic solution and nonaqueous electrolyte secondary battery using it

    JP2008269978A

  • Nonaqueous electrolyte secondary battery and nonaqueous electrolyte

    JP2013239426A

  • Nonaqueous electrolyte secondary battery and manufacturing method of the battery

    JP2014127313A

  • Lithium ion secondary battery

    JP2015037012A