Preparation of MoO2Cl2

JP7579985B2Active Publication Date: 2024-11-08SK SPECIALTY CO LTD

Patent Information

Application Number
JP2023550718
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-23
Filing Date
2021-12-02
Publication Date
2024-11-08
Estimated Expiration
2041-12-02

AI Technical Summary

Benefits of technology

【0014】 本発明は、不活性条件下でMoO2Cl2を製造する方法に関するもので、以下のステップを含む: (i) 反応容器にMoO2を充填する、 (ii) 反応容器内で、MoO2を供給されたCl2と第1の温度T1で反応させ、ガス状のMoO2Cl2に変換する、 (iii) ガス状のMoO2Cl2を受入容器に移送する、 (iv) ガス状のMoO2Cl2を受入容器内で、T1より低い第2の温度T2で固体状のMoO2Cl2に再昇華させる、および (v) ICP-OES/MSで特定した純度が99.9996wt.%以上の固体MoO2Cl2を得る。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579985000001
    Figure 0007579985000001
  • Figure 0007579985000002
    Figure 0007579985000002
  • Figure 0007579985000003
    Figure 0007579985000003
Patent Text Reader

Abstract

The present invention relates to a method for producing MoO2Cl2 under inert conditions, comprising the steps of: (i) charging the reaction vessel with MoO2; (ii) reacting MoO with the supplied Cl in a reaction vessel at a first temperature T1 to convert MoOCl into gaseous MoO; (iii) transferring the gaseous MoO2Cl2 to a receiving vessel; (iv) resublimating the gaseous MoO2Cl2 to solid MoO2Cl2 in a receiving vessel at a second temperature T2 lower than T1; and (v) Solid MoO2Cl2 is obtained with a purity of 99.9996 wt.% or more as determined by ICP-OES / MS. The present invention also relates to high purity MoO2Cl2, its use, and electronic components.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to molybdenum dioxide dichloride (MoO 2 Cl 2 ) and the MoO obtained by such a method 2 Cl 2 , its use and electronic components. [Background technology]

[0002] prior art Molybdenum-containing layers are frequently used in electronic components, for example in so-called flash memories. Such molybdenum-containing layers are often produced by vapor deposition. In such vapor deposition, MoO 2 Cl 2 In order to achieve advantageous electronic properties of the molybdenum-containing layer, in particular pure MoO 2 Cl 2 It is desirable to use MoO 2 Cl 2 It is desirable for the molybdenum-containing layer to contain as few metal impurities as possible, which may impair the electronic properties. In particular, tungsten is the impurity of interest here, since it may impair the electronic properties of the molybdenum-containing layer. Thus, MoO 2 Cl 2 is particularly desirable.

[0003] MoO 2 Cl 2 The preparation of molybdenum(IV) oxide (MoO 2 ) and chlorine gas (Cl 2 ) to MoO 2 Cl 2 The reaction in the reaction vessel is carried out at 160°C. No further active temperature setting of the test equipment is carried out. 2The gas flow rate of the generated MoO 2 Cl 2 The purity of the product is also not determined.

[0004] A method for preparing molybdenum powder is known from CN 102632245 A and is described as MoO 2 and Cl 2 By reacting with MoO 2 Cl 2 No information is given about the atmosphere in which the reaction takes place. Also, the intermediate MoO 2 Cl 2 There is no information about the purity of MoO 2 Cl 2 is then reacted with aqueous ammonia to give ammonium paramolybdate, which is then converted to molybdenum(VI) oxide (MoO 3 ), which ultimately gives molybdenum powder.

[0005] EP 3 656 741 A1 describes the reaction of molybdenum oxide and Cl under reduced pressure. 2 The method for producing molybdenum oxide chloride from MoO 2 Cl 2 In addition, molybdenum oxide trichloride (MoOCl 3 ) and molybdenum oxide tetrachloride (MoOCl 4 In an exemplary embodiment, MoO 2 Cl 2 is MoO 3 Cl 2 The produced MoO 2 Cl 2 The purity is limited to 99.9995 wt.%.

[0006] MoO 2 Cl 2 The methods used in the prior art for producing still need to be improved in some cases. Summary of the Invention [Problem to be solved by the invention]

[0007] Object of the invention The present invention overcomes, at least partially, and as completely as possible, the shortcomings of the prior art. 2 Cl 2 The present invention aims to provide a method for producing the above-mentioned compound.

[0008] A particular object of the present invention is to provide a method for the preparation of a compound comprising the steps of: 2 Cl 2 , especially MoO with low tungsten content 2 Cl 2 The present invention provides a method for producing the above-mentioned compound.

[0009] It is also an object of the present invention to provide a method for producing a molybdenum-containing layer which overcomes, at least in part, and as completely as possible, the disadvantages of the prior art.

[0010] The object of the present invention is further to provide a method for producing a MoO 2 Cl 2 In particular, the purity of MoO 2 Cl 2 The purpose of this project is to provide

[0011] The object of the present invention is also to provide a method for producing a molybdenum-containing layer comprising the steps of: (a) preparing a molybdenum-containing layer comprising: 2 Cl 2 The present invention provides for the use of

[0012] It is also an object of the present invention to provide an electronic component with a molybdenum-containing layer which overcomes, at least partially and as completely as possible, the disadvantages of the prior art. [Means for solving the problem]

[0013] Disclosure of the Invention Surprisingly, the object of the present invention is achieved by the method, product and use according to the claims.

[0014] The present invention relates to a process for producing MoO under inert conditions. 2 Cl 2 The present invention relates to a method for producing a compound comprising the steps of: (i) Add MoO 2 Filling (ii) In a reaction vessel, MoO 2 Cl was supplied 2 and the first temperature T 1 The reaction is carried out with gaseous MoO 2 Cl 2 Convert to (iii) Gaseous MoO 2 Cl 2 to a receiving vessel; (iv) Gaseous MoO 2 Cl 2 In the receiving vessel, T 1 A lower second temperature T 2 In solid state MoO 2 Cl 2 and (v) Solid MoO with a purity of 99.9996 wt.% or more as determined by ICP-OES / MS 2 Cl 2 get. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The process according to the invention is carried out under inert conditions, preferably continuously under inert conditions. The process thus comprises Cl provided in step (ii). 2 and in the absence of other reactive gases or substances. The method is therefore preferably carried out in the absence of oxygen and / or in the absence of air and / or in the absence of water. The method is particularly preferably carried out in the absence of pure Cl 2 In an atmosphere of Cl 2 -N 2 The reaction is carried out in an atmosphere of a mixture of

[0016] The process according to the invention further comprises the step of preparing a mixture of molybdenum-containing and / or oxidizable starting materials, such as MoO 2 In particular, the method according to the invention is carried out using MoO or MoO 3 Other molybdenum oxides such as MoO are not used. 2 may contain impurities, particularly metal impurities such as tungsten (W). 2 Cl 2 In addition, no other molybdenum oxide chlorides are formed in the process according to the invention, in particular MoOCl 3 and / or MoOCl 4 is preferably not generated.

[0017] The MoO obtained in step (v) 2 Cl 2 The purity of MoO is determined by combined ICP-OES / MS. Inductively coupled plasma (ICP) is used as the excitation source. 2 Cl 2 is introduced into an inert gas flow (e.g. argon flow) and radio frequency energy is transferred thereto electrodelessly by inductive coupling. The frequencies used for this purpose are usually in the range of 25-100 MHz. The power of the generator used is usually 1-10 kW. Here, the inert gas flow is heated to a temperature of usually up to 10,000 K. As a result, MoO 2 Cl 2 are atomized or ionized. The resulting liberated atoms and / or ions are analyzed optically by atomic emission spectrometry (OES, Optical Emission Spectrometry) or by mass spectrometry (MS).

[0018] Elements in solutions can generally be detected and quantified by inductively coupled plasma optical emission spectrometry (ICP-OES; or ICP-AES, ICP-atomic spectrometry). The solution to be measured is atomized as described above, and the aerosol formed is introduced into a high-frequency plasma, which atomizes and partially ionizes the solution components. The characteristic emission lines of the atoms and ions are resolved by a monochromator or polychromator, and the emission line intensity is detected by a suitable detector. The measurements can be performed in the axial and / or radial direction. According to the invention, the measurements are preferably performed in the axial direction, since axial measurements are more sensitive. For quantitative determination, a calibration can be performed with suitable standard solutions, since there is a linear correlation between the signal intensity of the emission and the concentration of the element. According to the invention, the measurement principle of ICP-OES is based on DIN EN ISO 11885(1997) / DEV E22 and / or Guidelines for chemical analysis, Determination of the elemental composition in environmental samples by ICP-OES, It is preferable to conform to TIFF0007579985000001.tif6130 [Fraunhofer Institute for Molecular Biology and Applied Ecology], Auf dem Aberg 1, D-57392 Schmallenberg, Germany.

[0019] Elements in a solution can generally be detected and quantified by inductively coupled plasma mass spectrometry (ICP-MS). The solution to be measured is atomized as described above and introduced into the high-frequency plasma, where the solution components are atomized and ionized. Ions are extracted from the high-frequency plasma by a pinhole aperture system and separated by mass-to-charge ratio. After separation, they are detected by a detector, and the resulting signal is evaluated by the instrument software. Since there is a linear correlation between the signal intensity of the ions and the concentration of the elements, quantification is possible after calibration with a standard solution. According to the present invention, the measurement principle of ICP-MS is in accordance with DIN EN ISO 17294-2:2017-01 (Water quality - Applications of inductively coupled plasma mass spectrometry (ICP-MS) - Part 2: Determination of selected elements including uranium isotopes (ISO 17294-2:2016); German version EN ISO 17294-2:2016) and / or the guidelines for chemical analysis, Determination of elemental composition in environmental samples by ICP-MS, It is preferable to conform to TIFF0007579985000002.tif6130 [Fraunhofer Institute for Molecular Biology and Applied Ecology], Auf dem Aberg 1, D-57392 Schmallenberg, Germany.

[0020] Coupling of two analytical techniques, OES and MS, allows the analysis of a wide range of elements. For example, light elements are difficult to determine by OES. However, by using MS at the same time, they can be determined. Therefore, coupling of analytical techniques is necessary. The elemental ratios determined by the two analytical techniques are consistent for the same elements, i.e., they provide consistent results within the usual measurement precision.

[0021] According to the invention, for the combined ICP-OES / MS, it is preferred to use an instrument manufactured by Thermo Fischer under the designation iCap, iCap Duo or iCap RQ.

[0022] The MoO 2 Cl 2It is possible to determine impurities, in particular metallic impurities such as tungsten, in the ppb range ("parts per billion"). The ppb values ​​or ppb limits given here correspond to the respective detection limits of the impurities.

[0023] The method according to the invention is particularly suitable for producing pure MoO 2 Cl 2 This makes it possible to produce MoO with a particularly low tungsten content. 2 Cl 2 According to the present invention, the MoO obtained in step (v) can be produced. 2 Cl 2 It is preferable that the purity of MoO be 99.99969 wt.% or more. 2 Cl 2 This makes it possible to produce molybdenum-containing layers with further improved electronic properties.

[0024] According to the present invention, the solid MoO obtained in step (v) 2 Cl 2 In the present invention, it is further preferred that the tungsten content, again measured by ICP-OES / MS, is 200 ppb or less, particularly preferably 50 ppb or less. Tungsten as an impurity can particularly impair the electronic properties of the molybdenum-containing layer. Due to the low tungsten content according to the present invention, such impairments can be avoided and the electronic properties can be further improved.

[0025] In addition to tungsten, MoO 2 Cl 2 may optionally contain very small amounts of other impurities, in particular (semi)metallic impurities such as Ag, Al, Au, B, Ba, Be, Bi, Ca, Cd, Ce, Co, Cr, Cu, Fe, Ga, Ge, Hf, In, Ir, K, La, Li, Mg, Mn, Na, Nb, Ni, Pb, Pd, Pt, Rb, Rh, Ru, Sb, Se, Sn, Sr, Te, Th, Ti, Tl, U, V, W, Zn and Zr. In this case, according to the invention, the MoO obtained in step (v) may be 2 Cl2 With respect to each one of these impurities considered independently of one another, it is preferred that the content of MoO is ≦300 ppb or less, more preferably ≦200 ppb or less, even more preferably ≦100 ppb or less, particularly preferably ≦50 ppb or less and most preferably ≦20 ppb or less. 2 Cl 2 Thanks to the inventive low content of such impurities in the molybdenum-containing layer, the electronic properties of the molybdenum-containing layer obtained therefrom can be further improved.

[0026] According to the invention, in step (ii), a first temperature T 1 Preferably, the reaction temperature is 170° C. or higher, more preferably 170 to 600° C., even more preferably 200 to 500° C., particularly preferably 350 to 450° C., and most preferably 400° C. Such a temperature makes it possible to achieve a compromise between the improvement of the reaction rate due to high temperatures on the one hand and unnecessary energy consumption due to excessively high temperatures on the other hand. Here, in a preferred embodiment, the reaction vessel is heated to a temperature T 1 It is also possible for the reaction zone to be divided into different physical and / or theoretical reaction zones, which are set differently within the aforementioned temperature ranges.

[0027] In step (ii), it is preferred to use a reaction vessel in which the temperature can be controlled or regulated. For example, a rotary kiln, a static kiln or a downpipe kiln is used. According to the invention, it is preferred to use a rotary kiln having different reaction zones which can be heated (and cooled) differently. In such a kiln, it is possible to set up one or more temperature gradients in the kiln, which allows the MoO produced in step (ii) to be heated or cooled. 2 Cl 2 This can contribute to further improving the purity of the product.

[0028] According to the invention, in step (iv), a second temperature T 2The temperature is preferably 160° C. or less, more preferably 10 to 120° C. or less, even more preferably 20 to 90° C. or less, particularly preferably 25 to 70° C. or less, and most preferably 70° C. By using such a temperature, MoO 2 Cl 2 and high yield of MoO 2 Cl 2 It is thus possible to achieve a compromise between low incorporation of impurities into the product.

[0029] According to the invention, between the start and the end of the method according to the invention, a second temperature T 2 It is particularly preferred to vary the temperature T 2 It is particularly preferred to lower the temperature from a high temperature to a low temperature, preferably from 90° C. to 20° C., more preferably from 70° C. to 25° C. Such temperature control allows the MoO 2 Cl 2 It becomes possible to set the purity of the fluorine-containing compound to a particularly high level.

[0030] In step (iv), preferably, a receiving vessel is used in which the temperature can be controlled or regulated. For example, a receiving flask is used. Alternatively, gaseous MoO 2 Cl 2 A cold trap can also be used where the resublimated MoO 2 Cl 2 can be removed from the receiving flask in the usual manner or thermally isolated from the cold trap.

[0031] According to the invention, the first temperature T 1 , the second temperature T 2 are particularly preferably set simultaneously as defined above. The following temperature pairs or temperature controls are therefore particularly preferred: T 1 ≥ 170°C, and T 2 ≦ 160°C; T 1≧ 170 ~ ≦ 600°C, and T 2 ≧ 10 ~ ≦ 120°C; T 1 ≧ 200 ~ ≦ 500°C, and T 2 ≧20 ~ ≦90°C; T 1 ≧ 350 ~ ≦ 450 ° C, and T 2 ≧25 ~ ≦70°C; T 1 = 400°C, and T 2 = 70 °C; T 1 ≧350~≦450°C, and T 2 is 90°C at the beginning of the process and is reduced to 20°C by the end of the process; T 1 = 400°C, and T 2 The temperature is 70°C at the beginning of the process and is reduced to 25°C by the end of the process.

[0032] These temperature pairs and temperature controls can simultaneously improve reaction rates, reduce energy consumption, increase yields, and reduce the inclusion of impurities.

[0033] According to the invention, it is also preferred that step (iii) is carried out at a temperature of 160° C. or higher. Such a temperature is preferred because it is possible to obtain a high molecular weight MoO 2 Cl 2 This allows preventing premature resublimation of the cation exchanger, thereby increasing the yield in the receiving vessel.

[0034] According to the present invention, in step (ii), Cl 2 It is further preferred that the gas flow rate of is 0.01-1 L / min, more preferably 0.05-0.8 L / min. Such a gas flow makes it possible to achieve a compromise between an increase in the reaction rate and yield on the one hand, and the unnecessary use of chlorine and the subsequent possible disposal problems of unused chlorine on the other hand.

[0035] According to the present invention, in step (ii), an inert gas, preferably nitrogen (N2 It is more preferable that an inert gas such as N 2 According to the invention, an inert gas, in particular N, is used to carry out the process according to the invention more safely under inert conditions. 2 It is particularly preferred that the gas flow rate of is 0.05-0.4 L / min, more preferably 0.1-0.3 L / min, particularly preferably 0.2 L / min, the choice of gas flow rate depending on the kiln size and configuration and should be adapted accordingly. Inert gas, especially N 2 Such a gas flow allows for better maintenance of inert conditions without using unnecessarily large amounts of inert gas. Moreover, such a gas flow allows for the gaseous MoO 2 Cl 2 The transfer of N from the reaction vessel to the receiving vessel can be improved. 2 In addition to MoO, other inert gases such as argon (Ar) can be used. 2 Cl 2 The purity of N can be further improved. 2 It is most preferred to use

[0036] According to the present invention, in step (ii), Cl 2 The gas flow rate is 0.01 to 1 L / min, more preferably 0.05 to 0.8 L / min, and N 2 It is also preferable to supply the gas at a flow rate of 0.05 to 0.4 L / min, more preferably 0.1 to 0.3 L / min (Cl at 0.01 to 1 L / min). 2 and 0.05-0.4 L / min N 2 ; Cl of 0.05~0.8L / min 2 and 0.05-0.4 L / min N 2 0.01~1L / min Cl 2 and 0.1-0.3 L / min N 2 or 0.05 to 0.8 L / min Cl 2 and 0.1-0.3 L / min N 2According to the present invention, in step (ii), Cl 2 was supplied at a gas flow rate of 0.8 L / min, and N 2 It is most preferable to supply a gas flow of 0.2 L / min. Such a gas flow improves the reaction rate and yield, and reduces Cl 2 The unnecessary use of inert gas and the associated disposal problems, as well as the maintenance of an inert state without excessive use of inert gas and the prevention of gaseous MoO 2 Cl 2 It is possible to achieve an even better compromise between improving the transport of

[0037] It is also preferred according to the invention that the reaction vessel, the receiving vessel and optionally the transition zone arranged between the reaction vessel and the receiving vessel are inerted before step (i) by flushing with an inert gas, preferably nitrogen. As is commonly used, "inerting" is understood to mean setting inert conditions in the apparatus. By flushing with an inert gas, the inert conditions of the method according to the invention can be set particularly quickly and efficiently. It is also preferred according to the invention that the method according to the invention does not comprise a step of depressurization, in particular does not comprise a step of reducing the pressure in the reaction vessel and / or the receiving vessel.

[0038] According to the present invention, the MoO obtained in step (v) 2 Cl 2 is preferably further purified in the subsequent step (vi) by sublimation and a new resublimation. Alternatively, in step (vi), MoO obtained in step (v) is 2 Cl 2 Other purification methods, such as recrystallization, can be used to further purify MoO. 2 Cl 2 It is possible to provide such a MoO 2 Cl 2 can be converted in a subsequent process, in particular a vapor deposition process, into a particularly pure molybdenum-containing layer having improved electronic properties. According to the invention, the process according to the invention accordingly2 Cl 2 In particular, the produced solid MoO does not have a step of wet-chemically treating the 2 Cl 2 with aqueous ammonia. In such a reaction, hydrogen chloride (HCl) is usually formed. However, the formation of HCl must be avoided according to the invention so that there are no problems with its disposal and so that there is no risk of undesirable corrosion by HCl of the equipment used, including the reaction vessel and the receiving vessel.

[0039] The present invention also relates to a method for producing a molybdenum-containing layer, which, if the method according to the invention is carried out after, i.e. after step (v) or after step (vi), comprises reacting the MoO obtained in step (v) or (vi). 2 Cl 2 as a precursor for deposition to form a molybdenum-containing layer. According to the present invention, the deposition is preferably performed by chemical vapor deposition (CVD) or atomic layer deposition (ALD).

[0040] Chemical vapor deposition (CVD) is a gas phase reaction that typically occurs at or near the surface of a substrate. The reactants involved in the reaction are simultaneously supplied in gaseous form to the substrate to be coated. The substrate is placed in a reaction chamber and heated. The gases, usually preheated, are thermally activated by the heated substrate and react with each other. In this process, the desired material is deposited and chemically bonded. Chemisorption of the desired material occurs, i.e., in the present invention, chemisorption of molybdenum occurs.

[0041] The ALD process, also known as atomic layer deposition, is an improvement over the CVD process. In the ALD process, surface reactions and sorption stop by themselves once the surface is completely covered. This self-limiting reaction takes place in several cycles, confined to intervening flushing steps. This allows very precise layer thicknesses to be achieved.

[0042] The present invention also relates to MoO obtained by the method according to the invention. 2 Cl 2 Such a MoO 2 Cl 2 is high purity MoO 2 Cl 2 and are particularly suitable as precursors for producing high-purity molybdenum-containing layers with improved electronic properties, especially storage properties, for use in flash memories, e.g. 3D-NAND. 2 Cl 2 is preferably MoO with low water content. 2 Cl 2 and particularly preferably anhydrous or dry MoO 2 Cl 2 It is.

[0043] The present invention also relates to MoO having a purity of 0.9996 wt.% or more, more preferably 0.99969 wt.% or more, as measured by ICP-OES / MS. 2 Cl 2 In this case, MoO 2 Cl 2 In particular, the tungsten content as measured by ICP-OES / MS is preferably 200 ppb or less, more preferably 100 ppb or less, and even more preferably 50 ppb or less. 2 Cl 2 is high purity MoO 2 Cl 2 and are particularly suitable as precursors for producing high-purity molybdenum-containing layers with improved electronic properties, especially memory properties, for use in flash memories, e.g. 3D-NAND. 2 Cl 2 is preferably MoO with low water content. 2 Cl 2 and particularly preferably anhydrous or dry MoO 2 Cl 2 It is.

[0044] The present invention also relates to a method for producing a molybdenum-containing layer comprising the steps of: 2 Cl 2 In particular, the use of MoO 2 Cl 2 can be useful for producing a molybdenum-containing layer by a gas phase thin film method such as CVD or ALD as described above.

[0045] The present invention also relates to an electronic component comprising a molybdenum-containing layer produced according to the present invention. 2 Cl 2 Due to the improved purity of molybdenum, the molybdenum-containing layer is likewise particularly pure, in particular substantially almost completely free of tungsten impurities, and thus the electronic component can provide improved electronic properties.

[0046] According to the invention, the electronic component is preferably what is called 3D-NAND. 3D-NAND is a non-volatile memory ("flash memory") in which a number of memory cells are stacked vertically in multiple layers. In this case, the memory cells are connected in series. For example, 16, 32, 64, 96, 128 memory cells can be connected to increase the storage density. The use of a molybdenum-containing layer produced according to the invention in such a non-volatile memory can improve its electronic properties, in particular its memory properties. EXAMPLES

[0047] Embodiment A rotary kiln with a pipe length of 1 m and a pipe diameter of 5 cm is used as a reaction vessel. The rotary kiln is connected to a product flask as a receiving vessel through a transition zone. The rotary kiln, the transition zone and the product flask can be heated separately. 400 g of MoO 2 Then, nitrogen was introduced (0.4 L / min of N 2) The entire equipment is placed in an inert gas atmosphere. Then, the rotary kiln is heated to a temperature of 400°C (T 1 ), the transition area at a temperature of 160°C, and the product flask at a temperature of 70°C (T 2 After these temperatures are reached, 2 Set the flow rate of Cl to 0.2 L / min. 2 Add 0.8 L / min of Cl to the rotary kiln. 2 ). The charged MoO 2 is the introduced Cl 2 Then, react with Cl for 2 hours (2h). 2 Shut off the introduction of N, the rotary kiln and the transition zone heating and allow the product flask to cool to 25°C. 2 Increase the flow rate to 1 L / min and continue for 30 min. Then, 2 The introduction of is terminated and the product flask is removed from the apparatus with an Ar counterflow. The product flask is placed in an inert gas atmosphere glove box where it is packaged.

[0048] Furthermore, samples are taken from the product flasks to determine the content of impurities. This measurement is carried out by ICP-OES / MS. For this purpose, Thermo Fischer instruments named iCap, iCap Duo or iCap RQ are used. The impurities shown in Table 1 below were measured (the values ​​in ppb shown correspond to the respective detection limits):

[0049] [Table 1]

[0050] Therefore, the total impurities are <3070 ppb in total. 2 Cl 2 has a purity of at least 99.9996930 wt.%.

Claims

1. A device in which a reaction vessel and a receiving vessel are connected via a transition region is used to produce MoO under inert conditions. 2 Cl 2 A method for producing a compound comprising the steps of: (i) Adding MoO to the reaction vessel 2 Filling (ii) adding MoO 2 Cl was supplied 2 and the first temperature T 1 The reaction is carried out with gaseous MoO 2 Cl 2 Convert to (iii) Gaseous MoO in the reaction vessel 2 Cl 2 through the transition region to the receiving vessel. (iv) Gaseous MoO 2 Cl 2 In the receiving vessel, T 1 A lower second temperature T 2 In solid state MoO 2 Cl 2 and (v) Solid MoO with a purity of 99.9996 wt.% or more as determined by ICP-OES / MS 2 Cl 2 get Including, the first temperature T 1 is 170 to 600° C.; The method of manufacturing, wherein the second temperature T 2 is between 10 and 90°C.

2. In step (v), solid MoO having a purity of 99.99969 wt.% or more as determined by ICP-OES / MS is added. 2 Cl 2 The method of claim 1, wherein

3. In step (v), solid MoO having a tungsten content of 200 ppb or less as determined by ICP-OES / MS is added. 2 Cl 2 The method of claim 1 , wherein

4. First temperature T 1 is between 200 and 500°C, and / or a second temperature T 2 The method of claim 1, wherein the temperature is 20 to 90°C.

5. 2. The method of claim 1, wherein step (iii) is carried out at a temperature of 160° C. or greater.

6. In step (ii), Cl 2 The method according to claim 1, wherein the gas flow rate is 0.01 to 1 L / min.

7. 2. The method of claim 1, wherein in step (ii) an inert gas is additionally supplied.

8. The method according to claim 7, wherein the flow rate of the inert gas is 0.05 to 0.4 L / min.

9. 2. The method of claim 1, wherein prior to step (i), the reaction vessel and the receiving vessel are inerted by flushing with an inert gas.

10. The MoO obtained in step (v) 2 Cl 2 is further purified in the subsequent step (vi) by sublimation and renewed resublimation.

11. A method for producing a molybdenum-containing layer, comprising the steps of: 2 Cl 2 is used in vapor deposition as a precursor to form a molybdenum-containing layer.

12. 2. The method of claim 1 for producing MoO2Cl2 which is used as a precursor for producing a molybdenum-containing layer.

13. A method for producing an electronic component comprising producing an electronic component comprising a molybdenum-containing layer produced according to claim 11.

Citation Information

Patent Citations

  • Preparation method of high-purity molybdenum powder

    CN102632245A

  • Production of high-purity tungsten or molybdenum powder

    JP1994093314A

  • Solid material pre-treatment method and solid material product filled with solid material produced by the solid material pre-treatment method

    JP2019104659A

  • Tungsten pentachloride conditioning and crystalline phase manipulation

    WO2019213115A1

  • Method for producing high-bulk-density molybdenum oxychloride

    WO2020021786A1

Cited By

  • Method for producing molybdenum dichloride dioxide, and system for producing molybdenum dichloride dioxide

    JP7935021B1