WC-based cemented carbide and cutting tools using said alloy

A WC-based cemented carbide with optimized Co, V, Cr, and Ta ratios and a hard coating addresses wear resistance issues in cutting tools, ensuring durability during high-hardness steel machining.

JP7580027B2Active Publication Date: 2024-11-11MOLDINO TOOL ENG LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021004826
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-15
Publication Date
2024-11-11
Estimated Expiration
2041-01-15

AI Technical Summary

Technical Problem

Conventional WC-based cemented carbides used for cutting tools face insufficient wear resistance when machining high-hardness steel, despite attempts to enhance toughness through grain size reduction with additives like V, Cr, and Ta.

Method used

A WC-based cemented carbide composition with specific mass ratios of Co, V, Cr, and Ta, along with a hard coating, ensuring a Vickers hardness of 2000 or more, and controlled Ta content at the interface between the hard and binder phases to prevent coarse precipitates, thereby enhancing wear resistance.

Benefits of technology

The cemented carbide exhibits improved wear resistance and durability when cutting high-hardness steel, minimizing tool damage and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580027000005
    Figure 0007580027000005
  • Figure 0007580027000006
    Figure 0007580027000006
  • Figure 0007580027000001
    Figure 0007580027000001
Patent Text Reader

Abstract

To provide a cemented carbide that has excellent wear resistance and durability even in the cutting of high hardness steel, and a cutting tool including the cemented carbide.SOLUTION: A cemented carbide has a hard phase and a binder phase and contains Co: 3.0-6.0 mass%, V: 0.024-0.180 mass%, Cr: 0.150-1.200 mass%, Ta: 0.030-0.120 mass%, with the balance being WC and unavoidable impurities, with, in a mass ratio, V / Co: 0.8-3.0%, Cr / Co: 5.0-20.0%, Ta / Co: 1.0-2.0%. At an interface between the (0001) plane of the WC constituting the hard phase and the binder phase, Ta is 2 atom% or less. The Vickers hardness (Hv30) is 2000 or more. There is also provided a cutting tool with a hard coat deposited on the cemented carbide.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a WC-based cemented carbide. [Background technology]

[0002] WC-based cemented carbide is used as a cutting tool because of its excellent mechanical strength and thermal fatigue resistance. Generally, the cemented carbide used for machining high-hardness steel is a WC-based cemented carbide with grain growth inhibitors such as V, Cr, and Ta added to reduce the average WC grain size and improve wear resistance. However, adding too much grain growth inhibitor reduces toughness, so various proposals have been made.

[0003] For example, Patent Document 1 describes a WC-based cemented carbide having high toughness, in which the addition ratios of the metals Cr, V, and Ta are controlled to make the WC particles small. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-183760 A Summary of the Invention [Problem to be solved by the invention]

[0005] According to the investigations of the present inventors, it has been recognized that cutting tools using conventional WC-based cemented carbide including the WC-based cemented carbide described in Patent Document 1 (cutting tools having a surface coating layer on the surface of a WC-based cemented carbide) may not have sufficient wear resistance when cutting high-hardness steel.

[0006] An object of the present invention is to provide a cemented carbide which provides a cutting tool having excellent wear resistance and durability even when used for cutting high-hardness steel. [Means for solving the problem]

[0007] The cemented carbide according to the embodiment of the present invention is It has a hard phase and a binder phase, Co: 3.0 to 6.0 mass%, V: 0.024 to 0.180 mass%, Cr: 0.150 to 1.200 mass%, Ta: 0.030 to 0.120 mass%, and the remainder being WC and unavoidable impurities; The mass ratios are V / Co: 0.8-3.0%, Cr / Co: 5.0-20.0%, and Ta / Co: 1.0-2.0%, respectively. Ta is 2 atomic % or less at the interface between the (0001) plane of WC constituting the hard phase and the binder phase, Vickers hardness (Hv30) is 2000 or more.

[0008] The cutting tool according to this embodiment is formed by forming a hard film on the cemented carbide. Effect of the Invention

[0009] According to the above, it is possible to obtain a WC-based cemented carbide which has excellent wear resistance when used as a cutting tool. [Brief description of the drawings]

[0010] [Figure 1] 1 is a photograph showing an interface between a (0001) plane of a WC particle forming a hard phase in Example 1 and a binder phase. [Diagram 2] FIG. 2 is a diagram showing the distribution of elements including Ta at the interface of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present inventors have conducted extensive research to improve the wear resistance of WC-based cemented carbide containing Co, which forms a binder phase, and the metals Cr, V, and Ta, which act as WC grain growth inhibitors. As a result, they have found that the wear resistance of WC-based cemented carbide can be improved by reducing the content of Co and preventing the V and Ta concentrated phases from becoming coarse.

[0012] Hereinafter, an embodiment of the present invention will be described in detail. In this specification and claims, when a numerical range is expressed as "L to M" (where L and M are both numerical values), the range includes an upper limit value (M) and a lower limit value (L), and the upper limit value (M) and the lower limit value (L) have the same units.

[0013] 1.Composition The metallic elements contained in WC-based cemented carbide are explained below.

[0014] (1)Co Co is the main component of the binder phase that holds together the WC particles that mainly constitute the hard phase, and is a metallic element that imparts high toughness to WC-based cemented carbide.

[0015] If the Co content is less than necessary, it becomes difficult to obtain a healthy structure without the precipitation of decarburized phases or free carbon, making it difficult to adjust the carbon content appropriately for mass production. Furthermore, the toughness and strength of the WC-based cemented carbide are reduced, which causes early chipping during milling of high-hardness steel. In addition, the sinterability of the WC-based cemented carbide is deteriorated, which makes it easy for voids and Co pools to occur, making it difficult to maintain high levels of toughness and strength.

[0016] On the other hand, if the Co content is higher than necessary, the hardness decreases and the surface area of ​​the WC in the structure decreases, so that the V-enriched phase, which tends to precipitate on the surface of the WC particles, tends to precipitate coarsely.

[0017] In view of the above, the WC-based cemented carbide of this embodiment preferably contains 3.0 to 6.0 mass% Co, which is the main component of the binder phase. When the Co content is in this range, the toughness and strength of the WC-based cemented carbide are both high, and the V-enriched phase is less likely to coarsen. The Co content is more preferably 3.5 to 5.0 mass %, and even more preferably 3.0 to 4.5 mass %.

[0018] V is the element with the strongest effect of inhibiting the grain growth of WC, and is an essential element for refining the structure of a WC-based cemented carbide.4 ~0.18 0 It is preferable that the content is % by mass. Furthermore, according to the findings of the present inventors, it was found that there is an appropriate range for the mass ratio of the V content to the Co content, V / Co.

[0019] If the V / Co ratio is smaller than this appropriate range, the average WC grain size of the WC-based cemented carbide becomes coarse, which reduces the hardness and wear resistance. On the other hand, if the V / Co ratio is larger than the appropriate range, a coarse V-enriched phase precipitates, which deteriorates the sinterability of the WC-based cemented carbide and makes it easier for voids and Co pools to occur. For example, when a cutting tool using a WC-based cemented carbide with a ratio larger than this appropriate range is used for milling high-hardness steel, the coarse precipitation of the brittle V-enriched phase will cause significant damage to the cutting tool.

[0020] In view of the above, the WC-based cemented carbide of this embodiment has a V / Co mass ratio of 0.8 to 3.0%. With V / Co in this range, the structure of the WC-based cemented carbide becomes finer and the hardness increases, and the V-enriched phase is less likely to precipitate coarsely, so that cutting tools using the cemented carbide of this embodiment are more likely to suppress tool damage during milling of high-hardness steel. The appropriate range of V / Co is more preferably 1.0 to 2.5%.

[0021] (3)Cr Cr is a grain growth inhibitor, and when added together with V, it refines the structure of the WC-based cemented carbide. In the cemented carbide of this embodiment, 0.15 0 ~1.20 0 It is preferable that the content is % by mass. Furthermore, according to the findings of the present inventors, it was found that there is also an appropriate range for the mass ratio of the Co content to the Cr content, Cr / Co.

[0022] The appropriate range of Cr / Co is preferably 5.0 to 20.0%. With Cr / Co in this range, the structure becomes finer and the hardness of the cemented carbide increases, and the Cr-enriched phase is less likely to precipitate coarsely, so that in a cutting tool using the cemented carbide of this embodiment, tool damage is more likely to be suppressed during milling of high-hardness steel.

[0023] In other words, if the content is smaller than the appropriate range, the structure of the WC-based cemented carbide becomes coarse, and the wear resistance of a cutting tool using this cemented carbide decreases. On the other hand, if the content is larger than the appropriate range, a coarse Cr-enriched phase precipitates. In addition, the sinterability of the WC-based cemented carbide deteriorates, making it easier for voids and Co pools to occur. The appropriate range is more preferably 8.0 to 20.0%.

[0024] (4)Ta Ta is a grain growth inhibitor, and when added together with V and Cr, it refines the structure of the WC-based cemented carbide. 0 ~0.12 0 It is preferable that the content is % by mass. Furthermore, according to the findings of the present inventors, it was found that there is also an appropriate range for the mass ratio of the Co content to the Ta content, Ta / Co.

[0025] The appropriate range of Ta / Co is preferably 1.0 to 2.0%. With Ta / Co in this range, the structure of the cemented carbide becomes fine and the hardness is increased, and the Ta-enriched phase is less likely to precipitate coarsely, so that in a cutting tool using the cemented carbide of this embodiment, tool damage is more likely to be suppressed during milling of high-hardness steel. The appropriate range is more preferably 1.0 to 1.5%.

[0026] 2. Ta content at the interface between the hard phase and the binder phase In the WC-based cemented carbide of this embodiment, it is preferable that the Ta content at the interface between the (0001) of the WC grains constituting the hard phase and the binder phase is 2 atomic % or less. The reason for this is that the low Ta content at the interface can increase the interfacial strength between the hard phase and the binder phase.

[0027] In addition, at the interface between the WC(0001) surface of the hard phase and the binder phase, the atomic percentage of V>the atomic percentage of Cr>the atomic percentage of Ta is preferable. At the interface between the surface and the binder phase, the atomic percentage of V is preferably 10.0 atomic percent or less. Note that ">" is an inequality sign.

[0028] 3. Vickers hardness The WC-based cemented carbide of this embodiment preferably has a Vickers hardness of 2000 or more. To mill high-hardness steel, it is preferable that the hardness of the WC-based cemented carbide substrate is high. Therefore, the WC-based cemented carbide of this embodiment has a Vickers hardness of 2000 or more. It is more preferable that the hardness of the WC-based cemented carbide is 2100 or more. The hardness and toughness of the WC-based cemented carbide are in a trade-off relationship, and as the hardness increases, the toughness tends to decrease, and as the hardness decreases, the toughness tends to increase. If the hardness is too high, the toughness decreases, so the WC-based cemented carbide of this embodiment has a Vickers hardness of 2000 or more. Vickers The hardness is preferably 2500 or less.

[0029] The hardness of the WC-based cemented carbide depends on the Co content and the average WC grain size. In order to achieve a Vickers hardness of 2000 or more with the Co content of the WC-based cemented carbide of this embodiment, the average grain size of the WC grains equivalent to a circle is more preferably 0.6 μm or less. Furthermore, the average grain size of the WC grains equivalent to a circle is even more preferably 0.4 μm or less. EXAMPLES

[0030] 1. Preparation of WC-based cemented carbide The WC raw powder used had an average particle size of 0.4 μm. The Co raw powder had an average particle size of 1.5 μm, the VC raw powder had an average particle size of 1 μm, and the Cr raw powder had an average particle size of 1.5 μm. 3 C 2 The raw material powder used had an average particle size of 1 μm, and the TaC raw material powder used had an average particle size of 1 μm.

[0031] These raw powders were weighed to obtain a predetermined composition and wet mixed in an attritor. When mixing, a small amount of C powder and molding binder powder were added to compensate for the carbon consumed in the sintering process. After mixing, the mixture was dried in a spray dryer to produce granulated powder of each composition, and a round bar was formed. Thereafter, the sintering temperature was 1450°C for Examples 1 to 7 and 1430°C for Comparative Example 1, and the sintering temperature was held for 1 hour, and then sintered at a pressure of 5 MPa to form a round bar made of a WC-based cemented carbide alloy that is a medium carbon alloy in which no decarburized phase or free carbon is precipitated.

[0032] These round bars were then machined into a ball end mill shape for cutting evaluation. In addition, the round bars were machined for physical property evaluation, and hardness measurements and structure observations were performed. Table 1 shows the composition and hardness measurement results. In the structure observation, a V surface analysis was performed at 1500x magnification on the mirror-polished cross section of the sintered body using a field emission electron probe microanalyzer (EPMA, JEOL JXA-8530F model). In the surface analysis, if V was measured at 2 mass% or more / pixel, it was determined that a coarse V-enriched phase was present. As a result, a coarse V-enriched phase was confirmed only in the substrate of Comparative Example 1, which had a large amount of Co and V.

[0033] The Vickers hardness was measured at two points on a mirror-polished substrate using a Vickers hardness tester (AVK type manufactured by Akashi Seisakusho) under conditions of a test force of HV30 (294.2 N) and a holding time of 15 seconds, and the average value was calculated.

[0034] 2. Hard coating The hard coating was formed using an arc ion plating type film forming device. The surface of the base material was coated with AlCrSiN of about 2 μm, and then coated with TiSiN of about 1 μm to obtain cutting tools of Examples 1 to 7 and Comparative Example 1.

[0035] [Table 1]

[0036] 3.Cutting test The following cutting tests 1 to 3 were carried out for the examples and comparative examples, and the wear resistance of the coated cutting tools was evaluated based on the exposed area of ​​the substrate after the cutting tests. The test conditions for each of the cutting tests 1 to 3 are shown below. In both cutting tests 1 to 3, the substrate exposed area ratio, which is an evaluation method, was evaluated by observing the substrate at a specified magnification using a scanning electron microscope after cutting, and calculating the ratio of the substrate's exposed cemented carbide to the entire substrate. Commercially available image analysis software was used to calculate the substrate exposed area ratio.

[0037] (1) Cutting conditions for cutting test 1 Tool: 2-blade carbide ball end mill (ball radius 0.3 mm) Cutting method: Pocket processing (25mm x 25mm x depth 0.08mm) ·Work material: ASP23(64HRC) Depth of cut: Axial, 0.04mm, Radial, 0.12mm ·Cutting speed: 75m / min Feed per blade: 0.015mm / blade Cutting oil: Mist blow (oil-based) Number of processed pockets: 4 Magnification of exposed substrate area: 300x The results of the exposed area ratio of the substrate (=area of ​​exposed part of the substrate / total area of ​​the substrate×100) are shown in Table 2.

[0038] [Table 2]

[0039] (2) Cutting conditions for cutting test 2 Tool: 2-blade carbide ball end mill (ball radius 0.15 mm) Cutting method: Pocket processing (1mm x 3mm x depth 0.4mm) ·Work material: ASP23(64HRC) Depth of cut: Axial, 0.013mm, Radial, 0.013mm ·Cutting speed: 37.7m / min Feed per blade: 0.0045mm / blade Cutting oil: Mist blow (oil-based) Number of pockets: 20 Magnification of exposed substrate area: 600x The results of the substrate exposed area ratio are shown in Table 3.

[0040] [Table 3]

[0041] (3) Cutting conditions for cutting test 3 Tool: 2-blade carbide ball end mill (ball radius 0.15 mm) Cutting method: Pocket processing (1mm x 3mm x depth 0.4mm) ·Work material: ASP23(64HRC) Depth of cut: Axial, 0.006mm, Radial, 0.006mm ·Cutting speed: 37.7m / min Feed per blade: 0.0045mm / blade Cutting oil: Mist blow (oil-based) Number of pockets: 7 Magnification of exposed substrate area: 600x The results of the substrate exposed area ratio are shown in Table 4.

[0042] [Table 4]

[0043] As is clear from Tables 2 to 4, the substrate exposed area ratio was small in all machining operations, and the examples showed excellent durability in cutting hardened steel. The reason for this is believed to be that the examples maintained high hardness with low Co and did not have a coarse concentrated phase of the grain growth inhibitor.

[0044] Here, Fig. 1 is a photograph of the structure of Example 1, and the distribution of Ta was measured at the interface between the hard phase (shown as the WC phase in Fig. 2) WC(0001) plane in this photograph and the binder phase (shown as the Co phase in Fig. 2). The results are shown in Fig. 2, and it is presumed that the excellent durability was exhibited because the interface strength was increased due to the small amount of Ta at the interface.

Claims

1. It has a hard phase and a binder phase, Co: 3.0 to 6.0 mass%, V: 0.024 to 0.180 mass%, Cr: 0.150 to 1.200 mass%, Ta: 0.030 to 0.120 mass%, with the balance being WC and unavoidable impurities; The mass ratios are V / Co: 0.8 to 3.0%, Cr / Co: 5.0 to 20.0%, and Ta / Co: 1.0 to 2.0%, respectively. Ta is 2 atomic % or less at the interface between the (0001) plane of WC constituting the hard phase and the binder phase, Vickers hardness (Hv30) is 2000 or more. The present invention relates to a hard alloy.

2. A cutting tool comprising the cemented carbide according to claim 1 and a hard coating formed thereon.

Citation Information

Patent Citations

  • Tungsten carbide-based hard metal

    JP2003183760A

  • Fine-grained cemented carbide for fine tool and production method

    JP2007162067A