Manufacturing method of silicon nitride ceramic sintered substrate and manufacturing method of circuit board
By incorporating scribe holes and positioning through holes in silicon nitride ceramic substrates, the method addresses the misalignment issue, enhancing the production efficiency and thermal performance of circuit boards.
Patent Information
- Application Number
- JP2019170848
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-09-19
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2039-09-19
AI Technical Summary
The existing methods for manufacturing circuit boards using silicon nitride ceramic substrates face challenges in aligning the centers of metal plates on the front and back sides, leading to potential misalignment and increased thermal resistance.
A silicon nitride ceramic sintered substrate with scribe holes and positioning through holes is used, where the through holes are formed at specific corners to serve as common references for aligning metal plates on both sides, ensuring precise alignment.
This approach prevents misalignment between metal plates on the front and back sides, improving the acceptance rate of circuit boards by ensuring accurate positioning and reducing thermal resistance.
Smart Images

Figure 0007580188000001 
Figure 0007580188000002 
Figure 0007580188000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon nitride ceramic sintered substrate for producing a large number of circuit boards and a manufacturing method thereof, a silicon nitride ceramic aggregate substrate, and a manufacturing method for circuit boards. [Background technology]
[0002] Circuit boards used in semiconductor modules, power modules, etc. use ceramic circuit boards because of their thermal conductivity, insulation, strength, etc., and are made by bonding metal circuit plates or metal heat sinks made of Cu, Al, etc. to these ceramic circuit boards. Alumina materials have been widely used as ceramic circuit boards, but recently silicon nitride, which has high strength and improved thermal conductivity, has come to be used so that it can be used in harsher environments.
[0003] In addition, a technique for mass-producing circuit boards includes joining a metal plate such as a Cu plate by active metal brazing or direct bonding to a single ceramics assembly board of a size from which a large number of ceramic circuit boards can be cut out, forming a metal circuit plate and a metal heat sink by etching or the like, and dividing the ceramics assembly board into pieces of a specified size to obtain individual circuit boards.
[0004] As a method for dividing the individual circuit boards, for example, a method is adopted in which recesses or grooves are formed in the ceramic assembly board by laser processing before bonding the Cu plate or the like, and after bonding the Cu plate or the like, the ceramic assembly board is bent and divided at the recesses or grooves.
[0005] The inventors of the present invention have produced a ceramics assembly substrate by forming scribe holes (non-through holes) for division in an as-sintered sintered plate by laser processing, and dividing (cutting) the sintered plate along the division lines of the scribe holes to remove the four sides of the sintered plate, but have found that burrs are likely to occur on the edges of the ceramics assembly substrate. In the process of producing a circuit substrate, even if the substrate is aligned based on the edges, it is difficult to produce the substrate so that the center of a metal plate such as a Cu plate is located at the center of the circuit substrate, and there is a problem that the center of the metal plate on the front side and the center of the metal plate on the back side are misaligned, resulting in a decrease in the pass rate of the circuit substrate.
[0006] Note that a technique for separating a circuit board from a ceramic assembly substrate using scribed holes or separation grooves is disclosed in Patent Document 1 (JP 2008-198905 A) and Patent Document 2 (JP 2017-28192 A). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-198905 A [Patent Document 2] JP 2017-28192 A Summary of the Invention [Problem to be solved by the invention]
[0008] The conventional technology has not been able to solve the problem that the center of the metal plate on the front side may be misaligned with the center of the metal plate on the back side. If the center of the metal plate on the front side is significantly misaligned with the center of the metal plate on the back side, there is a risk that the thermal resistance of the circuit board will increase.
[0009] The object of the present invention is to provide a silicon nitride ceramic sintered substrate and a method for manufacturing the same, a silicon nitride ceramic aggregate substrate, and a method for manufacturing a circuit board, in order to prevent misalignment between the center of a metal plate on the front side and the center of a metal plate on the back side. [Means for solving the problem]
[0010] The silicon nitride ceramics sintered substrate of the present invention is a silicon nitride ceramics sintered substrate for producing a silicon nitride ceramics aggregate substrate having a circuit formation portion and an edge portion for obtaining a large number of circuit boards from a rectangular silicon nitride ceramics sintered substrate having ear portions around the periphery of the silicon nitride ceramics aggregate substrate, a scribe hole for dividing the silicon nitride ceramics aggregate substrate and the ear portion, and a positioning through hole; The scribe hole forms an edge break line along an outer edge of the silicon nitride ceramic sintered substrate at a position inward from the outer edge of the substrate, The positioning through hole is formed inside the side break line and in one of the four corners of the silicon nitride ceramic aggregate substrate.
[0011] The silicon nitride ceramics aggregate substrate of the present invention is a silicon nitride ceramics aggregate substrate having a circuit formation portion and an edge portion for producing a large number of circuit boards, and is characterized in that a positioning through hole is formed in one of the four corners on the inside of the side of the silicon nitride ceramics aggregate substrate.
[0012] The method for producing a silicon nitride ceramic sintered substrate of the present invention is a method for producing a silicon nitride ceramic aggregate substrate having a circuit formation portion and an edge portion for obtaining a large number of circuit boards from a rectangular silicon nitride ceramic sintered substrate having ear portions around the periphery of the silicon nitride ceramic aggregate substrate, comprising the steps of: a step of forming scribe holes for dividing the silicon nitride ceramics aggregate substrate and the ear portions, and a step of forming through holes for positioning; The scribe hole forming step forms an edge break line by a scribe hole along an outer edge of the silicon nitride ceramic sintered substrate at a position inward from the outer edge of the substrate, The positioning through-hole forming step is characterized in that a through-hole is formed in one of the four corners of the silicon nitride ceramic aggregate substrate, on the inside of the side break line.
[0013] In the silicon nitride ceramic sintered substrate, it is preferable that at least one of the through holes is formed in one of the four corners of the silicon nitride ceramic aggregate substrate. The through hole can be used as a common positioning reference for the front surface (circuit side) and the back surface (heat dissipation side) of the silicon nitride ceramic sintered substrate.
[0014] In the silicon nitride ceramic sintered substrate, it is preferable that the center point determined from at least one through hole formed in one of the four corners of the silicon nitride ceramic aggregate substrate coincides with the center point of the silicon nitride ceramic aggregate substrate. Moreover, the silicon nitride ceramic aggregate substrate can be obtained by removing the edge portion from this silicon nitride ceramic sintered substrate (having positioning through holes). Moreover, it is preferable that the center point of the front surface determined from at least one through hole formed in one of the four corners of the silicon nitride ceramic aggregate substrate coincides with the center point of the back surface determined from the through hole. Moreover, it is preferable that the center point of the front surface determined from at least one through hole formed in one of the four corners of the silicon nitride ceramic aggregate substrate coincides with the center point of the back surface determined from the through hole.
[0015] In the silicon nitride ceramics sintered substrate and the silicon nitride ceramics aggregate substrate, the through holes preferably have a circular opening.
[0016] In the silicon nitride ceramics sintered substrate, the distance between the side break line and the through hole is preferably 0.1 to 4.0 mm.In the silicon nitride ceramics aggregate substrate, the distance between the side of the silicon nitride ceramics aggregate substrate (corresponding to the side break line) and the through hole is preferably 0.1 to 4.0 mm.
[0017] The method for producing a circuit board of the present invention is a method for producing a circuit board by adding a step of providing a metal plate on a circuit side and a step of providing a metal plate on a heat dissipation side to the method for producing a silicon nitride ceramic sintered substrate, The present invention is characterized in that one opening of the through hole and its position information are used when positioning the metal plate on the circuit side, and the other opening of the through hole and its position information are used when positioning the metal plate on the heat dissipation side.
[0018] A method for producing a circuit board of the present invention includes the steps of: preparing a silicon nitride ceramics aggregate substrate having a circuit formation portion and an edge portion for producing a large number of circuit boards; and forming a positioning through hole at one of four corners of the silicon nitride ceramics aggregate substrate, inside a side of the silicon nitride ceramics aggregate substrate; The method includes providing a metal plate on a circuit side and a metal plate on a heat dissipation side on the silicon nitride ceramics assembly substrate, The present invention is characterized in that one opening of the through hole and its position information are used when positioning the metal plate on the circuit side, and the other opening of the through hole and its position information are used when positioning the metal plate on the heat dissipation side.
[0019] In the method for producing a circuit board, when providing a first pattern of resist on the metal plate for the circuit side, a center point of the first pattern is determined based on a center of one opening of the through hole and its position information; When a second pattern of resist is provided on the metal plate for heat dissipation, the center point of the second pattern is determined by the center of the other opening of the through hole and its position information. Effect of the Invention
[0020] The silicon nitride ceramic sintered substrate and its manufacturing method, silicon nitride ceramic aggregate substrate, and circuit board manufacturing method of the present invention suppress misalignment between the metal plate on the front side and the metal plate on the back side, thereby improving the pass rate of circuit boards. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic diagram illustrating a silicon nitride ceramic sintered substrate according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a silicon nitride ceramics aggregate substrate obtained from the substrate of FIG. [Diagram 3] FIG. 3 is a schematic diagram showing a second break line formed in the substrate of FIG. 2. [Figure 4] 4 is a schematic diagram of the substrate in FIG. 3 to which brazing material has been applied, where (4a) shows the front surface and (4b) shows the back surface. [Diagram 5] 5 is a schematic diagram of an original Cu plate placed and brazed on the substrate in FIG. 4, where (5a) shows the front surface and (5b) shows the back surface. [Figure 6] 6A and 6B are schematic diagrams showing the state where the master Cu plate is patterned using the substrate of FIG. 5 and the excess brazing layer is removed, where (6a) shows the front surface and (6b) shows the back surface. [Figure 7] FIG. 7 is a schematic diagram of a circuit board derived from the substrate of FIG. 6. [Figure 8] FIG. 2A is a cross-sectional view of the through hole in FIG. 1 etc., and FIG. 2B is a cross-sectional view of another embodiment of the through hole. [Figure 9] FIG. 2 is a schematic diagram illustrating another (a) silicon nitride ceramic sintered substrate and (b) silicon nitride ceramic aggregate substrate according to the present invention. [Figure 10] FIG. 4 is a schematic diagram illustrating a main portion of another silicon nitride ceramic aggregate substrate according to the present invention. [Figure 11] FIG. 4 is a schematic diagram illustrating a main portion of another silicon nitride ceramic aggregate substrate according to the present invention. [Figure 12] FIG. 4 is a schematic diagram illustrating a main portion of another silicon nitride ceramic aggregate substrate according to the present invention. [Figure 13] FIG. 4 is a schematic diagram illustrating a main portion of another silicon nitride ceramic aggregate substrate according to the present invention. [Figure 14] FIG. 3 is a schematic diagram showing the substrate of FIG. 2 to which a brazing material has been applied. [Figure 15] FIG. 15 is a schematic diagram showing an original Cu plate placed and brazed on the substrate in FIG. 14. [Figure 16]FIG. 16 is a schematic diagram showing a master Cu plate patterned with the substrate of FIG. [Figure 17] FIG. 17 is a schematic diagram showing a state in which the exposed brazing material layer is removed from the substrate in FIG. 16. [Figure 18] FIG. 18 is a schematic diagram showing a second break line formed in the substrate of FIG. 17. [Figure 19] FIG. 4 is a schematic diagram illustrating another silicon nitride ceramic sintered substrate according to the present invention. [Figure 20] FIG. 2 is a schematic diagram illustrating another (a) silicon nitride ceramic sintered substrate and (b) silicon nitride ceramic aggregate substrate according to the present invention. [Figure 21] FIG. 4 is a schematic diagram illustrating a main portion of another silicon nitride ceramic aggregate substrate according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The embodiments of the present invention will be described in detail below, but the present invention is not necessarily limited thereto. The description of each embodiment can also be applied to other embodiments unless otherwise specified.
[0023] The inventors conducted extensive research into silicon nitride ceramics sintered substrates obtained by sintering in order to prevent misalignment when a metal plate such as a Cu plate is formed on a silicon nitride ceramics aggregate substrate portion, and arrived at the present invention of providing positioning through holes in the silicon nitride ceramics sintered substrate or the silicon nitride ceramics aggregate substrate.
[0024] (Embodiment 1) A silicon nitride ceramic sintered substrate according to the present invention is shown in Fig. 1, and a manufacturing method thereof and a manufacturing method of a circuit board will be described with reference to Figs. 1 to 7. First, as shown in Fig. 1, a carbon dioxide gas laser (CO2 laser) or the like is used to form a plurality of scribe holes 13a (non-through holes) along an outer edge 10 of the silicon nitride ceramic sintered substrate 1 obtained by sintering, from the outer edge 10 to a position inward, to form break lines 13 (hereinafter referred to as side break lines) by dividing lines connecting the centers of the scribe holes (scribe hole forming step). Hereinafter, "scribe holes" refers to holes (non-through holes) that do not penetrate the substrate.
[0025] Then, a slit 14 is formed in the thickness direction of the silicon nitride ceramic sintered substrate 1 at the corner where the side break line 13 intersects, in a direction inclined to the side break line 13, so as to chamfer the corner (a through hole forming process for chamfering (more specifically, a slit forming process)). Hereinafter, a "slit" refers to a long and thin cut that penetrates the substrate from one surface to the other surface. A "through hole for chamfering" refers to a hole that penetrates the substrate from one surface to the other surface. The slit 14 is formed by connecting a plurality of through holes, and forms a break line 15 (hereinafter, referred to as a corner break line) by a dividing line that connects the centers of the through holes. The corner break line 15 may intersect with the side break line and protrude from the side break line by a length L2. It is preferable that the length L2 is greater than the beam spot diameter of the laser used to form the slit and less than 3.5 mm. Although the corner break line is formed in the first embodiment, it is also possible to adopt a form in which the corner break line is not provided.
[0026] Among the four sides constituting the outer edge 10 of the silicon nitride ceramic sintered substrate, the longer side is defined as the long side, and one positioning through hole 5 is formed at a predetermined distance L1 on the inside (opposite side from the outer edge 10) of the side break line 13 formed along one of the long sides (positioning through hole forming step). By forming one through hole 5 at the corner of the silicon nitride ceramic aggregate substrate 12, i.e., near the corner break line 15, the silicon nitride ceramic sintered substrate of embodiment 1 is obtained. The diameter of the positioning through hole 5 is preferably 100 to 500 μm, more preferably 150 to 300 μm. The distance L1 is preferably 0.1 to 4.0 mm, more preferably 0.2 to 3.0 mm, and more preferably 0.5 mm to 2.0 mm. The reason for specifying the numerical range in this way is that if L1 is too small, the positioning through hole 5 may come into contact with the edge break line, and if a through hole is provided near the edge break line, this may lead to a decrease in the strength of the board. Also, if L1 is too large, the width of the machining allowance (corresponding to the second ear) for providing the positioning through hole becomes large, the area of the ceramic part in the circuit board becomes relatively small, and the number of circuit boards that can be produced decreases.
[0027] Next, the ears of the four sides of the silicon nitride ceramics sintered substrate 1 are bent in order, and tensile stress is applied by bending in a direction perpendicular to the side break line 13 to separate the ears 11 on the four sides from the silicon nitride ceramics sintered substrate (earl dividing process). The obtained silicon nitride ceramics aggregate substrate 12a has one positioning through hole 5 near one of the four chamfered corners (the lower right corner in FIG. 2) and at a predetermined distance L1 from the side break line 13, as shown in FIG.
[0028] Next, as shown in FIG. 3, second break lines 18, 18' are formed on the surface of silicon nitride ceramics aggregate substrate 12a by the second scribed holes. Second break line 18 is formed along side break line 13, and the distance between side break line 13 and second break line 18 is greater than distance L1. Through hole 5 is located at a location corresponding to the second ear portion. For example, two second break lines 18' are formed so as to intersect with the midpoints of, for example, four second break lines 18. In the silicon nitride ceramics aggregate substrate, diagonal lines can be drawn and the intersection of the diagonal lines can be determined as the center point of the silicon nitride ceramics aggregate substrate.
[0029] Next, as shown in Fig. 4(a), brazing material 16a is arranged by applying brazing material paste by screen printing to the regions separated by the second break lines 18, 18' on the front surface (surface) of the substrate in Fig. 3 (four regions in Fig. 4). Furthermore, the substrate is turned over, and brazing material 16a' is arranged on the back surface by applying brazing material paste by screen printing.
[0030] Next, as shown in Fig. 5 (5a), an original Cu plate 16b is provided on the front surface (surface) of the substrate in Fig. 4 so as to cover the brazing material 16a in four places. Furthermore, the substrate is turned over, and another original Cu plate 16b' is provided on the back surface so as to cover the brazing material 16a' in four places. Next, the laminate in which the Cu plate 16b' / brazing material 16a' / silicon nitride ceramics aggregate substrate (12a) / brazing material 16a / Cu plate 16b is laminated in this order is heat-treated, and the brazing materials 16a, 16a' are turned into a brazing material layer, and brazing is performed.
[0031] In addition, when providing the Cu plate 16b and the Cu plate 16b', their positions are adjusted so as not to cover at least the through-hole 5. If the positioning through-hole 5 is covered and cannot be seen, it cannot be used to position the resist pattern in a later process. To adjust the positions of the Cu plate 16b and the Cu plate 16b', for example, a method is used in which a pair of pins or stoppers are prepared as jigs, and one pin or stopper is abutted against one side of the Cu plate 16b and the other pin or stopper is abutted against the adjacent side of the Cu plate 16b.
[0032] Next, using an image analyzer or the like, the center (corresponding to the center of the opening on the entrance side) and radius of the positioning through hole 5 on the front surface are calculated, and the distance L1 between the positioning through hole 5 and the long side edge break line 13 and the distance L3 between the positioning through hole 5 and the short side edge break line 13 are measured as shown in FIG. 1. The direction of L1 is the y-axis, and the direction of L3 is the x-axis. Based on the vertical dimension (L11) and horizontal dimension (L13) of the size of the silicon nitride ceramics aggregate substrate determined by design, L11 / 2-L1=L5 and L13 / 2-L3=L7 are calculated, and the position away from the through hole 5 toward the center of the substrate at a distance of L5 on the y-axis and a distance of L7 on the x-axis is set as the position for setting the first center point 200 (the circle of the through hole 5 and the circle drawn virtually as shown in FIG. 1 with the first center point 200 as the center are assumed to have the same diameter). Four resist patterns are formed on Cu plate 16b using a method for forming a photoresist or a method for attaching a resist film based on the first coordinates of the silicon nitride ceramics aggregate substrate obtained by the center of first center point 200, the y-axis, and the x-axis. The center, outline, and position of the resist patterns can be determined by the first coordinates.
[0033] Furthermore, the substrate is turned over, and the center (corresponding to the center of the opening on the through side) and radius are calculated at the positioning through hole 5 on the back side, and the distance L1 between the positioning through hole 5 and the long side edge break line 13, and the distance L3 between the positioning through hole 5 and the short side edge break line 13 are measured. The direction of L1 is the y axis, and the direction of L3 is the x axis. Based on the vertical dimension (L11) and horizontal dimension (L13) determined by the design of the size of the silicon nitride ceramics aggregate substrate, L11 / 2-L1=L5 and L13 / 2-L3=L7 are calculated, and the position away from the through hole 5 toward the center of the substrate by a distance of L5 on the y axis and a distance of L7 on the x axis is set as the position for setting the second center point 200' (the circle of the through hole 5 and the circle drawn virtually with the second center point 200' as the center (for example, as in FIG. (5b)) have the same diameter). Based on the second coordinates of the silicon nitride ceramics aggregate substrate obtained by the second center point 200' and the y-axis and x-axis, four resist patterns are formed on the Cu plate 16b' using a method of forming a photoresist or a method of attaching a resist film. The center, outline and position of the resist patterns can be determined by the second coordinates. By using the same through hole 5 on the front and back surfaces (using it as a common reference for positioning), the first and second coordinates can be made common, or the first center point and the second center point can be made to coincide with each other, and the centers and positions of the resist patterns facing each other across the silicon nitride ceramics aggregate substrate can be accurately aligned so that they overlap when viewed through a see-through view. In addition, if the diameters of the circle of through hole 5 and the circle drawn virtually about the first center point 200 or the second center point 200' are different, calculations are made as L11 / 2-(L1+radius of through hole 5)=L5' and L13 / 2-(L3+radius of through hole 5)=L7', and the position away from the center of through hole 5 toward the center of the substrate, a distance of L5' on the y-axis and a distance of L7' on the x-axis, is determined to be the first center point 200 or the second center point 200'.
[0034] Next, the Cu plate 16b and the Cu plate 16b' are patterned by etching, and the brazing layer protruding from the edge of the Cu plate is selectively removed by etching, so that four copper circuit plates 16 are formed from the Cu plate 16b as shown in Fig. 6(6a), and four copper heat sink plates 16' are formed from the Cu plate 16b' as shown in Fig. 6(6b). Since they are patterned into shapes according to the areas covered with the resist pattern, the positions of the copper circuit plates 16 and the copper heat sink plates 16' are accurately aligned so that they face each other with the silicon nitride ceramics assembly substrate in between. After this, the copper circuit plates 16 and the copper heat sink plates 16' may be plated with Ni, Ag, or Au.
[0035] Thereafter, the silicon nitride ceramics aggregate substrate 12a is divided along the second break lines 18, 18' to separate the circuit forming portion (corresponding to the circuit board 20) and the edge portion 17 (corresponding to the second ear portion) to obtain each circuit board 20. As shown in Fig. 7, the circuit board 20 has a copper circuit board 16, a copper heat sink (not shown), and a ceramic substrate portion 19. When viewed from a direction perpendicular to the surface of the ceramic substrate portion 19 (the surface on which the circuit board or heat sink is provided), the position of the copper circuit board 16 on the front surface and the position of the copper heat sink on the back surface within the surface of the ceramic substrate portion 19 are aligned.
[0036] (Through hole for positioning) The positioning through hole will be described with reference to FIG. 8. FIG. 8(a) is a cross-sectional view of the through hole 5 in FIG. 1 and the like, and the diameter of the through hole is emphasized. When forming the through hole, the side on the front surface of the silicon nitride ceramics aggregate substrate 12 where the laser is irradiated is the "incident side" in the figure, and the side where the laser penetrates is the "penetration side" in the figure. Depending on the laser irradiation conditions, the diameter of the through hole increases slightly from the penetration side toward the incidence side, and the diameter may widen around the edge of the incidence side, resulting in a curved inclination in the cross section. FIG. 8(b) is a cross-sectional view showing an example of another through hole 5', in which the inner wall of the through hole is actively inclined in the cross section of the silicon nitride ceramics aggregate substrate (12), and the diameter of the through hole increases from the penetration side toward the incidence side, and such a through hole 5' can also be used.
[0037] For these positioning through holes, the center (virtual center) and radius of the opening on the entrance side, and the center (virtual center) and radius of the opening on the penetration side are calculated using an image analyzer or the like when viewed from a direction perpendicular to the substrate. A vertical virtual line that passes through the center and intersects with the surface of the silicon nitride ceramics aggregate substrate is shown by a dashed line in Figures 8(a) and (b), respectively.
[0038] It is preferable that the shape of the opening of the through hole is circular when viewed from a direction perpendicular to the substrate. This is because the position of the center of the circle is the same even if the size of the circle is different between the front side and the back side. As a method for determining the center of the circular opening, for example, a method can be used in which at least three imaginary lines are drawn on the shape of the circle, and the intersection points between the edge of the circle and the imaginary lines are identified from the shading of the image of the edge of the circle, and the center of the circle (i.e., the center of the opening of the through hole) is determined from the at least three intersection points. The shape of the opening of the through hole may be other than elliptical, rectangular, or cross-shaped, but the more the shape of the opening is deformed from a circle, the more likely it is that an error will occur when calculating the center of the opening with high accuracy. In other words, there is a case in which a deviation is easily generated between the center of the shape of the opening (calculated manually by the inventor from the image) and the center of the opening calculated by the image analysis device. In contrast, even if the edge of a circular opening is affected by the curved slope of the wall surface, causing the outline to appear to have a gradation, the center of the circle is determined to be a single point, so the center of the opening can be calculated with high precision.
[0039] (Embodiment 2) FIG. 9 shows (a) another silicon nitride ceramic sintered substrate and (b) another silicon nitride ceramic aggregate substrate according to the present invention. FIG. 9(a) is the same as the first embodiment except that the corner break line 15 is not formed. Therefore, when the edge portion 11 is removed from the silicon nitride ceramic sintered substrate 1 of FIG. 9(a) by cutting, the silicon nitride ceramic aggregate substrate 12a of FIG. 9(b) having the through hole 5 for positioning is obtained. The region surrounded by the dashed line in FIG. 9(b) is the region 9 including the corner portion, and a schematic enlarged view of the region is shown in FIG. 10(a'). When the silicon nitride ceramic aggregate substrate 12a of FIG. 9(b) is turned over, the region 9 including the corner portion appears as shown in FIG. 10(a). The edge of the silicon nitride ceramic aggregate substrate, i.e., the side break line 13, is formed perpendicular to the front or back surface of the silicon nitride ceramic aggregate substrate, so that FIG. 10(a) and FIG. 10(a') are mirror images. Then, when viewed from a direction perpendicular to the front or back surface, the first center point 200 set using the positioning through hole 5 in Figure 10(a') and its position information (L1, L3) and the second center point 200' set using the positioning through hole 5 in Figure 10(a) and its position information (L1, L3) will be aligned.
[0040] (Embodiment 3) Fig. 11 is a schematic diagram for explaining the main part of another silicon nitride ceramic aggregate substrate according to the present invention, and differs from Fig. 10 in that in Fig. 11(b'), an inclined surface 13b' of the side break line 13b is visible inside the outline of the side break line 13b. Since the side break line 13b is inclined with respect to the front or back surface of the silicon nitride ceramic aggregate substrate (this inclination corresponds to the inclination of the inner wall in Fig. 8(b), for example), the outline of the side break line 13b is mirror-symmetrical in Fig. 11(a) and Fig. 11(b), but the inclined surface 13b' of the side break line 13b is visible only in Fig. 11(b). Therefore, when measuring the position information (L1, L3), the distance between the side break line 13b and the through hole 5 is measured. Then, when viewed from a direction perpendicular to the front or back surface, the first center point 200 set using the positioning through hole 5 in Figure 11(a') and its position information (L1, L3) and the second center point 200' set using the positioning through hole 5 in Figure 11(a) and its position information (L1, L3) will be aligned.
[0041] (Embodiment 4) Fig. 12 is a schematic diagram for explaining the main part of another silicon nitride ceramic aggregate substrate according to the present invention, and differs from Fig. 10 in that the side break line 13c is composed of a straight portion and a recessed portion. The recessed portion corresponds to a shape obtained by dividing the through hole in Fig. 8(a) in half, for example, so that the side break line 13c seen on the front surface in Fig. 12(c') and the side break line 13c seen on the back surface in Fig. 12(c) are mirror images. When the distance between the through hole 5 and the side break line 13c is calculated using a virtual line (a chain line in Fig. 12) connecting the multiple straight portions, the first center point 200 set using the positioning through hole 5 in Fig. 12(c') and its position information (L1, L3) and the second center point 200' set using the positioning through hole 5 in Fig. 12(c) and its position information (L1, L3) match when viewed from a direction perpendicular to the front surface or back surface.
[0042] (Embodiment 5) Fig. 13 is a schematic diagram illustrating the main parts of another silicon nitride ceramic aggregate substrate according to the present invention, and differs from Fig. 10 in that in Fig. 13(d'), a curved portion 13d' of the side break line 13d is visible inside the outline of the side break line 13d. Since the curved portion 13d' is inclined with respect to the front or back surface of the silicon nitride ceramic aggregate substrate, the outline of the side break line 13d is mirror-symmetrical in Fig. 13(d') and Fig. 13(d), but the curved portion 13d' is only visible in Fig. 13(d'). Therefore, when measuring the position information (L1, L3), the distance between the side break line 13d and the through hole 5 is measured. Then, when viewed from a direction perpendicular to the front or back surface, the first center point 200 set using the positioning through hole 5 in Figure 13(d') and its position information (L1, L3) and the second center point 200' set using the positioning through hole 5 in Figure 13(d) and its position information (L1, L3) will be aligned.
[0043] (Embodiment 6) Another method for manufacturing a silicon nitride ceramic sintered substrate and a method for manufacturing a circuit substrate according to the present invention will be described with reference to Figs. 1, 2, and 14 to 18. First, a silicon nitride ceramic sintered substrate similar to that shown in Fig. 1 is produced, and a silicon nitride ceramic aggregate substrate 12a similar to that shown in Fig. 2 is obtained from the substrate. Next, brazing material paste is applied by screen printing to the front surface of the substrate shown in Fig. 2, thereby disposing brazing material 16c as shown in Fig. 14. Furthermore, the substrate is turned over, and brazing material paste is applied by screen printing to the rear surface of the substrate, thereby disposing brazing material in the same manner as brazing material 16c.
[0044] Next, as shown in Fig. 15, an original Cu plate 16d is provided on the front surface (surface) of the substrate in Fig. 14 so as to cover the main portion of the brazing material 16c. At this time, the Cu plate 16d is made not to cover the through hole 5. Furthermore, the substrate is turned over, and another original Cu plate is provided on the back surface so as to cover the main portion of the brazing material. At this time, the Cu plate of the original is made not to cover the through hole 5. Next, the laminate in the order of Cu plate / brazing material / silicon nitride ceramics aggregate substrate (12a) / brazing material 16c / Cu plate 16d is heat-treated, and the brazing material and brazing material 16c are turned into a brazing material layer, and brazing is performed.
[0045] Next, using an image analyzer or the like, the center and radius of the positioning through hole 5 on the front surface are calculated, and the distance L1 between the positioning through hole 5 and the long side edge break line 13 and the distance L3 between the positioning through hole 5 and the short side edge break line 13 are measured in the same manner as in FIG. 1. The direction of L1 is the y-axis, and the direction of L3 is the x-axis. Based on the vertical dimension (L11) and horizontal dimension (L13) of the size of the silicon nitride ceramics aggregate substrate determined by design, L11 / 2-L1=L5 and L13 / 2-L3=L7 are calculated, and the position away from the through hole 5 toward the center of the substrate at a distance of L5 on the y-axis and a distance of L7 on the x-axis is set as the position for setting the first center point 200 (the circle of the through hole 5 and the circle drawn virtually as in FIG. 1 with the first center point 200 as the center are assumed to have the same diameter). Based on the first coordinates of the silicon nitride ceramics aggregate substrate obtained by the first center point 200 and the y-axis and x-axis, four resist patterns are formed on the Cu plate 16d using a method of forming a photoresist or a method of attaching a resist film. The center, outline and position of the resist patterns can be determined by the first coordinates.
[0046] Furthermore, the substrate is turned over, and the center and radius are calculated at the positioning through hole 5 on the back side, and the distance L1 between the positioning through hole 5 and the long side edge break line 13, and the distance L3 between the positioning through hole 5 and the short side edge break line 13 are measured. The direction of L1 is the y axis, and the direction of L3 is the x axis. Based on the vertical dimension (L11) and horizontal dimension (L13) determined by the design of the size of the silicon nitride ceramics aggregate substrate, L11 / 2-L1=L5 and L13 / 2-L3=L7 are calculated, and the position away from the through hole 5 toward the center of the substrate by a distance of L5 on the y axis and a distance of L7 on the x axis is set as the position for setting the second center point 200' (the circle of the through hole 5 and the circle drawn virtually with the second center point 200' as the center (for example, as in FIG. 5(5b)) have the same diameter). Based on the second coordinates of the silicon nitride ceramics aggregate substrate obtained by the second center point 200' and the y-axis and x-axis, four resist patterns are formed on the Cu plate on the opposite side to the Cu plate 16d using a method of forming a photoresist or a method of attaching a resist film. The center, outline and position of the resist patterns can be determined by the second coordinates. By using the same through hole 5 on the front and back surfaces (using it as a common reference for positioning), the first and second coordinates can be made common, or the first center point and the second center point can be made to coincide with each other, and the centers and positions of the resist patterns facing each other across the silicon nitride ceramics aggregate substrate can be accurately aligned so that they overlap when viewed through a see-through view.
[0047] Next, the Cu plate 16d and another Cu plate are patterned by etching, so that four copper circuit plates 16 are formed from the Cu plate 16d on the front surface, and four copper heat sinks are formed from the other Cu plate on the back surface, as shown in Fig. 16. Since they are patterned into shapes according to the areas covered with the resist pattern, the positions of the copper circuit plate 16 and the copper heat sinks are accurately aligned so that they face each other with the silicon nitride ceramics assembly substrate in between. After this, the copper circuit plate 16 and the copper heat sinks may be plated with Ni, Ag, or Au.
[0048] Next, in the configuration of Fig. 16, the brazing material layer 16c' derived from the brazing material 16c on the front surface has a portion that is not covered by the copper circuit board 16, and the brazing material layer derived from the brazing material on the back surface has a portion that is not covered by the copper heat sink, and these are exposed brazing material layers. When these exposed brazing material layers are removed by selective etching, a configuration is obtained in which the copper circuit board 16 and the copper heat sink face each other with the silicon nitride ceramics aggregate substrate sandwiched therebetween, as shown in Fig. 17. After this, the copper circuit board 16 and the copper heat sink may be plated with Ni, Ag, Au, or the like.
[0049] Next, as shown in Fig. 18, second break lines 18, 18' are formed by the second scribe holes on the surface of the silicon nitride ceramic aggregate substrate. The second break lines 18 are formed along the side break lines 13, and the distance between the side break lines 13 and the second break lines 18 is greater than the distance L1. One through hole 5 is located at a location corresponding to the second ear portion. For example, two second break lines 18' are formed so as to intersect with the midpoints of, for example, four second break lines 18.
[0050] Thereafter, the silicon nitride ceramics assembly substrate is divided along the second break lines 18, 18' to separate the circuit forming portion (corresponding to the circuit substrate 20) and the edge portion 17 (corresponding to the second ear portion) to obtain each circuit substrate 20. The circuit substrate 20 has the same configuration as that shown in Fig. 7, and has a copper circuit board 16, a copper heat sink (not shown), and a ceramic substrate portion 19. When viewed from a direction perpendicular to the surface of the ceramic substrate portion 19 (the surface on which the circuit board or heat sink is provided), the position of the copper circuit board 16 on the front surface within the surface of the ceramic substrate portion 19 matches the position of the copper heat sink on the back surface (seen through).
[0051] (Embodiment 7) FIG. 19 is a schematic diagram for explaining the main part of another silicon nitride ceramic sintered substrate according to the present invention. The difference from FIG. 1 is that a positioning through hole 5 is formed at a predetermined distance L1 on the inside (opposite side from the outer edge 10) of the edge break line 13 formed along the shorter side (i.e., the short side) of the four sides constituting the outer edge 10 of the silicon nitride ceramic sintered substrate. Except for the fact that the through hole 5 is provided near the short side, not near the long side, it is common to the silicon nitride ceramic sintered substrate of FIG. 1. For example, as shown in FIG. 15, when a brazing material 16c or a master Cu plate 16d is provided and a method of forming a photoresist or a method of attaching a resist film is used, the center, outline and position of the resist pattern are determined by the same coordinates as the first coordinates or the second coordinates. Therefore, a circuit board similar to that of FIG. 7 can be manufactured. When viewed perpendicular to the surface of the ceramic substrate portion 19 (the surface on which the circuit board or heat sink is provided), the position of the copper circuit board 16 on the front surface and the position of the copper heat sink on the back surface (seen from a perspective) are aligned within the surface of the ceramic substrate portion 19.
[0052] (Embodiment 8) FIG. 20 shows another (a) silicon nitride ceramic sintered substrate according to the present invention, and (b) silicon nitride ceramic aggregate substrate obtained therefrom. In FIG. 20(a), the side break line 13 is changed to a side break line 23 in the region 9 including the corner portion, which is the same as the embodiment 2. The side break line 23 is a dividing line that connects through holes for the side break line, and the through holes are formed while shifting them little by little to make the edge of the side break line 23 straight, so that the side break line 23 is formed in a shape that makes it easy to measure the position information (L1, L3) with high accuracy, like the side break line 13 in FIG. 11(a'). On the other hand, the side break line 13 corresponds to a dividing line that connects the scribe holes 13a as described in FIG. 1, but the accuracy for obtaining the position information (L1, L3) related to the positioning through hole 5 is not necessarily required. For example, the pitch of the scribe holes 13a can be lengthened within a range that does not impair the breakability of the substrate, thereby reducing the man-hours required for forming the side break line 13.
[0053] In Fig. 20(a), by changing the properties of the side break lines 13 and 23, the difference is reflected as a difference in the properties of the outer periphery of the silicon nitride ceramic aggregate substrate in Fig. 20(b). The difference in the properties of the side break lines 13 and 23 does not necessarily have to be limited to the combination exemplified in Fig. 20. For example, if the difference between the method of forming the side break lines 23 in a shape that makes it easy to measure the position information (L1, L3) with high accuracy and the method of reducing the man-hours for forming the side break lines 13 is a change in the pitch, opening diameter, or depth of the scribe holes (for forming the side break lines) or through holes for the side break lines, the traces of the scribe holes or through holes for the side break lines on the outer periphery of the silicon nitride ceramic aggregate substrate will also have differences in pitch, diameter due to the opening, and depth.
[0054] For example, if edge break line 23 is formed of a plurality of scribe holes in region 9 including a corner, and the pitch of those scribe holes is smaller than the pitch of the plurality of scribe holes that make up edge break line 13, then in the silicon nitride ceramics aggregate substrate, the pitch of the indentations in edge break line 23 is smaller than the pitch of the indentations in edge break line 13. Also, if edge break line 23 is formed of a plurality of scribe holes in region 9 including a corner, and the depth of those scribe holes is greater than the depth of the plurality of scribe holes that make up edge break line 13, then in the silicon nitride ceramics aggregate substrate, the depth of the indentations in edge break line 23 (corresponding to the depth in the substrate thickness direction measured from the front surface of the substrate) is greater than the depth of the indentations in edge break line 13. Furthermore, for example, when edge break line 23 is formed of a plurality of scribe holes in region 9 including a corner, and the diameter of the opening of those scribe holes is smaller than the diameter of the opening of the plurality of scribe holes that make up edge break line 13, in the silicon nitride ceramic aggregate substrate, the radius of curvature of the recess at edge break line 23 is smaller than the radius of curvature of the recess at edge break line 13.
[0055] (Embodiment 9) Fig. 21 is a schematic diagram for explaining the main part of another silicon nitride ceramic sintered substrate according to the present invention, and differs from Fig. 9 in that the number of positioning through holes is changed to three at the corners of the silicon nitride ceramic aggregate substrate. Positioning through hole 5a in Fig. 21(a') is similar to positioning through hole 5 in Fig. 9(a), but positioning through holes 5b and 5c in Fig. 21(a') are added in embodiment 9. Except for the fact that three positioning through holes 5 are formed, it is the same as the silicon nitride ceramic sintered substrate in Fig. 9. Then, using the distance L21 between the center of the through hole 5a and the center of the through hole 5c in FIG. 21(a'), and the distance L23 between the center of the through hole 5a and the center of the through hole 5b in FIG. 21(a'), the direction of L21 is the y-axis, and the direction of L23 is the x-axis, an image analyzer or the like is used to calculate the center (corresponding to the center of the opening on the entrance side) and radius of each of the positioning through holes 5a, 5b, and 5c on the front surface, and the first center point 200 can be set based on the positioning through hole 5a. Based on the first coordinates of the silicon nitride ceramics aggregate substrate obtained by the first center point 200, the y-axis, and the x-axis, four resist patterns are formed on the Cu plate 16b using a method of forming a photoresist or a method of attaching a resist film. The center, outline, and position of the resist pattern can be determined by the first coordinates.
[0056] Furthermore, by turning the substrate over, the distance L21 between the center of the through hole 5a and the center of the through hole 5c in FIG. 21(a) and the distance L23 between the center of the through hole 5a and the center of the through hole 5b in FIG. 21(a) are used on the back side, and the direction of L21 is the y-axis and the direction of L23 is the x-axis to calculate the centers (corresponding to the centers of the openings on the entrance side) and radii of the positioning through holes 5a, 5b, and 5c, respectively, and the position where the second center point 200' is set can be determined based on the center of the positioning through hole 5a. Based on the second coordinates of the silicon nitride ceramics aggregate substrate obtained by the second center point 200', the y-axis, and the x-axis, four resist patterns are formed on the Cu plate 16b' using a method of forming a photoresist or a method of attaching a resist film. The center, outline, and position of the resist patterns can be determined by the second coordinates. By using the same three through holes 5 on both the front and back surfaces (using them as a common positioning reference), the first and second coordinates can be made common, or the first center point can be made to coincide with the second center point, and the centers and positions of opposing resist patterns sandwiching the silicon nitride ceramic aggregate substrate can be accurately aligned so that they overlap when viewed through a see-through view.
[0057] In the silicon nitride ceramic sintered substrate according to the present invention, as shown in Fig. 1, corner break lines 14 are formed at corners where side break lines 13 intersect with each other in a direction inclined to the side break lines 13, so as to chamfer the corners. The corner break lines 14 may be slits penetrating the substrate, slits 14 formed by connecting through holes for chamfering, or a plurality of through holes (through holes for chamfering) arranged in series (where the pitch of the through holes is smaller than the pitch of the scribe holes of the side break lines). The presence of the corner break lines makes it possible to suppress the occurrence of cracks or chips at the four corners of the silicon nitride ceramic aggregate substrate when the silicon nitride ceramic sintered substrate 1 is bent and divided into the silicon nitride ceramic aggregate substrate 12 and the edge portions 11.
[0058] In the silicon nitride ceramic sintered substrate according to the present invention, the scribed hole 13a preferably has a diameter of, for example, 300 μm or less on the substrate surface and a depth of, for example, 1 / 3 or more of the thickness of the silicon nitride ceramic sintered substrate. The diameter of the scribed hole depends largely on the beam spot diameter of the laser used, but is more preferably 30 to 200 μm, and even more preferably 50 to 150 μm. In addition, the depth of the scribed hole is more preferably 80 to 300 μm, and even more preferably 100 to 250 μm, when the substrate thickness is, for example, 0.32 mm. In addition, the pitch of the scribed holes is preferably 2 times or less of the scribed hole diameter, more preferably equal to the scribed hole diameter, and particularly preferably determined by the cleavability when the substrate is divided. This pitch control can be adjusted by controlling the processing speed, and may be linked to the number of laser output pulses, etc.
[0059] In the silicon nitride ceramic sintered substrate according to the present invention, the slits 14 formed at the corners where the edge break lines formed by the scribed holes intersect and connecting the through holes for chamfering preferably have a slit width of 30 to 200 μm and a slit length of 2.8 to 8.4 mm. The diameter or slit width of the through holes for chamfering is more preferably 20 to 150 μm, and even more preferably 30 to 100 μm. The slit length is more preferably 3.0 to 8.0 mm, and even more preferably 3.5 to 7.5 mm. The width and length of the break lines formed by the through holes for chamfering can be the same as the slit dimensions.
[0060] In the silicon nitride ceramic sintered substrate according to the present invention, the corner break lines or slits due to the through holes are inclined at, for example, 30° to 60° with respect to the side break lines due to the scribe holes. More specifically, it is preferable to incline them at, for example, 45° with respect to the side break lines due to the scribe holes, since this allows the area of the substrate to be used effectively without waste.
[0061] In the method for manufacturing a silicon nitride ceramic sintered substrate according to the present invention, the positioning through-holes, the scribe holes, the chamfering through-holes, or the slits are preferably formed by a laser. For example, a YAG laser or a carbon dioxide laser (CO2 laser) is used. Processing by irradiation with a YAG laser or a carbon dioxide laser is suitable for forming through-holes that penetrate the substrate or for forming deep holes intermittently.
[0062] In the method for manufacturing a silicon nitride ceramic sintered substrate according to the present invention, it is preferable to repeat irradiation with a laser beam spot multiple times when forming a through hole for positioning. By repeating irradiation multiple times to dig a hole, the energy density for each irradiation can be reduced, so that cracks due to thermal shock are less likely to form on the surface (inner wall) of the through hole.
[0063] The silicon nitride ceramic sintered substrate and silicon nitride ceramic aggregate substrate according to the present invention have a thickness of, for example, 0.2 mm to 1.0 mm. More specifically, the thickness is preferably, for example, 0.25 mm to 0.65 mm. The silicon nitride ceramic sintered substrate and silicon nitride ceramic aggregate substrate according to the present invention have a fracture toughness value of, for example, 5.0 MPa m 1 / 2 More specifically, the fracture toughness value is, for example, 5.0 to 7.5 MPa m 1 / 2 In the method for manufacturing a circuit board of the present invention, the metal plate can be at least one of a Cu plate and an Al plate. The method for joining the silicon nitride ceramics assembly substrate and the metal plate is not limited to brazing, and a direct joining method or the like may also be used.
[0064] The present invention will be described in detail below with reference to examples, although the present invention is not necessarily limited to the following examples.
[0065] (Example) The raw materials for forming silicon nitride ceramics were silicon nitride powder as the main raw material, and 2 mass% MgO and 3 mass% Y2O3 were used as sintering aids. The sheet molded body was sintered in a nitrogen atmosphere at a maximum temperature of 1850°C for a holding time of 5 hours to produce a rectangular silicon nitride ceramics sintered substrate 1 with a thickness of 0.32 mm, a length of 150 mm, and a width of 200 mm. A carbon dioxide gas laser was used to form edge break lines 13 with scribe holes 13a along the outer edge 10 of the silicon nitride ceramics sintered substrate 1 from the outer edge 10 to the inner position (scribe hole forming process). The scribe holes 13a had a maximum diameter of 50 μm, a depth of 150 μm, and a pitch of 100 μm on the substrate surface, and the edge break lines 13 with scribe holes 13a were formed along each of the four sides as shown in FIG. The width of the ears 11 was 5 mm.
[0066] Next, using a carbon dioxide laser (output 100 W), the laser beam spot was scanned once to continuously form chamfering through holes from a position protruding by L2 in a direction inclined at 45° to the edge break line 13 at each of the corners (4 locations) where the edge break line 13 intersects with the scribe hole 13a, thereby forming a slit 14 consisting of connected chamfering through holes (slit formation process). Laser beam spot diameter = 0.07 mm Machining speed=15mm / s Slit protrusion length L2 = 0.7 mm Total length of slit = 4.2 mm Slit width on the substrate surface = 0.10 mm
[0067] Next, using a carbon dioxide laser with a beam spot diameter of 0.2 mm, one positioning through hole 5 was formed near one of the corners of the silicon nitride ceramics aggregate substrate at a position L1 = 0.5 mm away inside side break line 13. Here, in the direction along side break line 13, the positioning through hole 5 was formed at a position 5 mm away from the nearby slit 14.
[0068] Next, the silicon nitride ceramics sintered substrate 1 shown in Fig. 1 was bent and broken along the side break lines 13 to separate it into the silicon nitride ceramics aggregate substrate 12 and the edge portions 11 shown in Fig. 2. Next, as shown in Fig. 3, second break lines 18, 18' were formed in the silicon nitride ceramics aggregate substrate 12a to obtain the silicon nitride ceramics 12a.
[0069] Next, as shown in FIG. 4, brazing material (16a, 16a') was applied to the front and back sides of the silicon nitride ceramics assembly substrate 12a by screen printing. The brazing material was prepared by adding 0.3 parts by mass of TiH2 to an alloy powder consisting of 70% by mass of Ag, 3% by mass of In, and 27% by mass of Cu (total of 100 parts by mass), and further adding an organic solvent and an organic binder to the alloy powder and kneading the mixture to form a paste. After drying the silicon nitride ceramics assembly substrate to which the brazing material was applied, 0.3 mm copper plates, i.e., Cu plates (16b, 16b') were placed on the front and back sides of the substrate to cover the brazing material, thereby obtaining a laminate (see FIG. 5). Next, the substrate was heat-treated in a vacuum at 800°C for 20 minutes while applying pressure to produce a bonded body of the silicon nitride ceramics assembly substrate and the Cu plate. A layer of brazing material with a thickness of about 30 μm was formed between the silicon nitride ceramics assembly substrate and the Cu plate.
[0070] Next, using an image analyzer, the center (center of the circle on the entrance side) and radius of the positioning through hole 5 on the front surface were calculated, and the distance L1 = 0.5 mm between the positioning through hole 5 and the long side break line 13, and the distance L3 = 7.0 mm between the positioning through hole 5 and the short side break line 13 were measured, as shown in Figure 1. The direction of L1 is the y-axis, and the direction of L3 is the x-axis. Based on the vertical dimension (L11=140mm) and horizontal dimension (L13=190mm) of the silicon nitride ceramic aggregate substrate determined by the design, L11 / 2-L1=L5=69.5mm and L13 / 2-L3=L7=86.0mm were calculated, and the position away from the through hole 5 toward the center of the substrate by a distance of L5 on the y axis and a distance of L7 on the x axis was determined as the position for setting the first center point 200 (the circle of the through hole 5 and the circle drawn virtually with the first center point 200 as the center as shown in FIG. 1 have the same diameter). The first coordinate of the silicon nitride ceramic aggregate substrate obtained by the first center point 200, the y axis, and the x axis was determined. Next, for the bonded body, an etching resist ink that can be cured by ultraviolet light was applied to the Cu plate on the front side, and then the etching resist ink was cured by irradiating ultraviolet light to form a resist film pattern. The positioning of the mask when exposing the pattern of the resist film was performed using the above-mentioned first coordinates. The etching resist ink used was of an alkali peeling type.
[0071] Next, the substrate is turned over, and the center (center of the circle on the through side) and radius are calculated at the positioning through hole 5 on the back side, and the distance L1 between the positioning through hole 5 and the long side edge break line 13 and the distance L3 between the positioning through hole 5 and the short side edge break line 13 are measured in the same manner as for the front side. The direction of L1 is the y axis, and the direction of L3 is the x axis. Based on the vertical dimension (L11) and horizontal dimension (L13) determined by design among the sizes of the silicon nitride ceramics aggregate substrate, L11 / 2-L1=L5 and L13 / 2-L3=L7 are calculated, and the position away from the through hole 5 toward the center of the substrate by a distance of L5 on the y axis and a distance of L7 on the x axis is set as the position for setting the second center point 200' (the circle of the through hole 5 and the circle drawn virtually with the second center point 200' as the center have the same diameter). The second coordinates of the silicon nitride ceramics aggregate substrate were determined by the second center point 200' and the y- and x-axes. Next, etching resist ink was applied to the Cu plate on the back side of the bonded body, and then ultraviolet light was irradiated to harden the etching resist ink, forming a resist film pattern. The above second coordinates were used to position the mask when exposing the resist film pattern.
[0072] An etching process was performed using a copper chloride 55 etching solution (a mixed solution containing copper chloride, hydrochloric acid, and hydrogen peroxide) maintained at 30°C to remove unnecessary Cu plate outside the circuit board or heat sink pattern (i.e., the Cu plate in the part not covered with the resist film).
[0073] Next, in order to remove the portion of the brazing material protruding from the Cu plate (protruding portion of the brazing material), a first brazing material etching treatment (etching treatment with an acidic solution containing carboxylic acid and / or carboxylate, and hydrogen peroxide) and a second brazing material etching treatment (etching treatment with a solution containing ammonium hydrogen fluoride and hydrogen peroxide) were carried out in sequence to remove the protruding portion of the brazing material, thereby obtaining the joint shown in Figure 6.
[0074] The bonded body was then immersed in a 3% by mass aqueous solution of sodium hydroxide to remove the resist film. After chemical polishing and washing with ion-exchanged water, the copper plate on the front side (circuit board) and the copper plate on the back side (heat sink) were plated with Ni. This chemical polishing was performed using a commercially available sulfuric acid-based solution to achieve a glossy finish.
[0075] In this way, a circuit board assembly was obtained in which multiple sets of Ni-plated copper circuit boards 16 and copper heat sinks were joined via the silicon nitride ceramics assembly substrate and the brazing material layer. Next, by dividing the assembly at the second break lines 18, 18', multiple circuit boards 20 each having the copper circuit board 16, the copper heat sink (not shown), and the ceramic substrate portion 19 were obtained as shown in FIG.
[0076] Among the above-mentioned steps, the case where the resist film pattern was formed will be described. The resist film pattern could be formed so that the position and center of the pattern matched on the front surface side and the back surface side by using the positioning through hole and its position information, with respect to the position accuracy (corresponding to "deviation") of the center point in the long side direction (i.e., deviation was suppressed). Next, the Cu plate was patterned by etching so as to correspond to the resist film pattern, so that the circuit board and the heat sink were formed so that their positions matched. And, since deviation between the center and position of the metal plate (circuit board) on the front surface side and the center and position of the metal plate (heat sink) on the back surface side was suppressed, the level was improved from Comparative Examples 1 and 2, and the pass rate of the circuit boards could be improved.
[0077] Comparative Example 1 Without forming positioning through holes, the silicon nitride ceramics aggregate substrate was positioned by abutting the long side against a jig (other than the requirements related to the positioning through holes and their position information, the same as in the example). However, although the burrs that were generated by removing the edge portions had been removed, the position accuracy (deviation) of the resist film pattern in the long side direction was within the range of ±0.08 mm due to the influence of the unevenness of the long side itself (the side surface of the substrate along the long side).
[0078] Comparative Example 2 Without forming through holes for positioning, marks (coated or drawn marks) were formed on the front and back surfaces of the silicon nitride ceramics aggregate substrate and used for positioning. However, the positional accuracy of the resist film pattern in the long side direction was inferior to that of the example. This is thought to be because a common reference was not used between the process of marking the front surface and the process of marking the back surface, and therefore misalignment occurred during the handling process for turning over the silicon nitride ceramics aggregate substrate.
[0079] When the positional accuracy in the short side direction was compared for the above-mentioned Example, Comparative Example 1, and Comparative Example 2, it was found that the positional accuracy of the Example was within a smaller range than that of Comparative Examples 1 and 2. [Explanation of symbols]
[0080] 1: Silicon nitride ceramic sintered substrate, 5,5',5a,5b,5c: through hole, 9: Area including corners, 10: outer edge, 11: Ears, 12, 12a: silicon nitride ceramics assembly substrate, 13: edge break line, 13a: scribe hole, 13b, 13c, 13d,: Edge break lines, 13b': Inclined surface, 13d': curved section, 14: Slit, 15: Square brake line, 16: Copper circuit board, 16': Copper heat sink, 16a, 16a', 16c: brazing material, 16c': brazing layer, 16b, 16b', 16d: original Cu plate; 17: Edge, 18,18': second brake line, 19: ceramic substrate portion; 20: circuit board; 23: Edge break line, 200: first center point, 200': Second center point
Claims
1. A method for producing a silicon nitride ceramics sintered substrate, for producing a silicon nitride ceramics aggregate substrate having a circuit formation portion and an edge portion for obtaining a large number of circuit boards from a rectangular silicon nitride ceramics sintered substrate having ear portions around the periphery of the silicon nitride ceramics aggregate substrate, comprising: a scribe hole forming step of forming scribe holes for dividing the silicon nitride ceramics aggregate substrate and the ear portions; a positioning through hole forming step of forming a positioning through hole before dividing the silicon nitride ceramics aggregate substrate and the ear portions; The scribe hole forming step forms an edge break line by a scribe hole along an outer edge of the silicon nitride ceramic sintered substrate at a position inward from the outer edge of the substrate, A method for manufacturing a silicon nitride ceramic sintered substrate, characterized in that the positioning through hole forming step forms only one through hole in one of the four corners of the silicon nitride ceramic aggregate substrate, inside the side break line.
2. 2. The method for manufacturing a silicon nitride ceramic sintered substrate according to claim 1, wherein the through hole serves as a common positioning reference for the front and back surfaces of the silicon nitride ceramic sintered substrate.
3. A method for manufacturing a circuit board by adding a step of providing a metal plate on a circuit side and a step of providing a metal plate on a heat dissipation side to the method for manufacturing a silicon nitride ceramic sintered substrate according to claim 1, A method for manufacturing a circuit board, characterized in that one opening of the through hole and its position information are used when positioning the metal plate on the circuit side, and the other opening of the through hole and its position information are used when positioning the metal plate on the heat dissipation side.
4. 4. The method for manufacturing a circuit board according to claim 3, when providing a first pattern of resist on the metal plate for the circuit side, a center point of the first pattern is determined based on a center of one opening of the through hole and its position information; A method for manufacturing a circuit board, characterized in that when a second pattern of resist is formed on a metal plate for heat dissipation, the center point of the second pattern is determined by the center of the other opening of the through hole and its position information.
Citation Information
Patent Citations
Ceramic substrate, manufacturing method of ceramic circuit board, aggregate substrate and semiconductor module
JP2008198905A
Manufacturing method of multiple patterning circuit board, and intermediate product of multiple patterning circuit board
JP2009224732A
Silicon nitride based ceramic assembled board and method for manufacturing the same
JP2016195244A
Silicon nitride ceramic aggregate substrate and manufacturing method therefor, and manufacturing method for silicon nitride sintered substrate
JP2017028192A
Manufacturing method for aggregate wiring board
JP2017085069A