Manufacturing method for frost-resistant concrete

By integrating superabsorbent resin particles to form voids via hydration, the method addresses instability in air-entrained concrete, enhancing freeze-thaw resistance and durability in concrete structures.

JP7580230B2Active Publication Date: 2024-11-11PS CONSTRUCTION CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020154658
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-15
Publication Date
2024-11-11
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Existing methods for enhancing freeze-thaw resistance in concrete, such as using air-entrained concrete (AE concrete) and hollow microspheres, face challenges like air bubble instability and increased material costs, while the use of superabsorbent resin to form voids for resistance is unclear regarding dehydration conditions and required amounts.

Method used

Incorporating superabsorbent resin particles with an average diameter of 100 μm or less, mixed in a swollen state, which form voids through hydration with cement, achieving a volume ratio of 1-3% in concrete, thereby improving freeze-thaw resistance without an AE agent.

Benefits of technology

The method results in a concrete structure with enhanced freeze-thaw resistance and durability, demonstrated by improved durability indices and reduced compressive strength loss, particularly at water-cement ratios of 30-35% and SAP volume ratios of 1-3%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580230000001
    Figure 0007580230000001
  • Figure 0007580230000002
    Figure 0007580230000002
  • Figure 0007580230000003
    Figure 0007580230000003
Patent Text Reader

Abstract

To provide frost resistant concrete improved in freeze-thaw durability and a structure using the same.SOLUTION: The frost resistant concrete contains particles of a superabsorbent resin having an average particle diameter of 100 μm or less after swelling, and has a water-cement ratio of 40% or less. The concrete includes minute voids formed by consuming at least a part of the water contained in the particles of the superabsorbent resin by the hydration reaction of the cement.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a frost-resistant concrete for use in snowy and cold regions. Manufacturing method Regarding. [Background technology]

[0002] In cold regions with heavy snowfall, frost damage to concrete structures is an issue. Frost damage to concrete structures is evident on the surface of the concrete as scaling, microcracks, and pop-outs. Deterioration progresses as the water in the concrete expands in volume when it freezes and the water is supplied when it thaws, resulting in repeated freezing and thawing. To prevent deterioration due to frost damage, voids are required to relieve the expansion pressure caused by the freezing of water. For this reason, AE concrete, which contains entrained air (independent microscopic air bubbles), is used.

[0003] Due to the deterioration mechanism of concrete caused by freezing and thawing, freeze-thaw resistance is closely related to the spacing between air bubbles. The smaller the spacing between air bubbles, the better the freeze-thaw resistance, and an effective spacing is considered to be 200 μm or less. However, since the spacing coefficient must be measured on hardened concrete, the reality is that freeze-thaw resistance is controlled by measuring the amount of air when fresh.

[0004] It is also known that air entrainment using AE agents can cause various instabilities, such as adhesion of air bubbles and reduction in air volume during transportation and compaction. For this reason, in areas with a high incidence of frost damage, there is a movement to increase the air volume when fresh to ensure resistance to freeze-thaw. On the other hand, an increase in air volume leads to a decrease in compressive strength, so it becomes necessary to set the mix strength higher for quality assurance purposes, which leads to increased material costs.

[0005] In order to impart freeze-thaw resistance, a method of mixing hollow microspheres instead of entrained air is known (see Patent Document 1). When mixing hollow microspheres, the number and particle size do not change as in the case of coalescence of air bubbles. Furthermore, there is an advantage that the amount of air does not decrease due to loss of air, and the air bubble interval can be controlled by the amount of hollow microspheres mixed. However, since the density is extremely low, it is necessary to devise a method of measuring and adding hollow microspheres during concrete production, and a method of adding a water-soluble paper bag containing hollow microspheres at a predetermined timing during concrete mixing (see Patent Document 2) has been devised. Naturally, the low density of hollow microspheres also affects their transportation costs. For this reason, Patent Document 3 shows a method of using expandable polymer microspheres that expand to become hollow microspheres during concrete production. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 08-188458 [Patent Document 2] JP 2017-159532 A [Patent Document 3] Patent No. 6328101 Summary of the Invention [Problem to be solved by the invention]

[0007] Air entrained concrete is often used as a method to ensure the freeze-thaw resistance of concrete. However, it is known that there are various unstable factors in air entrainment, such as adhesion between air bubbles and loss of air volume during transportation and compaction. Therefore, a method of mixing hollow microspheres or expansive polymer microspheres that have a void structure in advance has been proposed to introduce voids into concrete instead of air bubbles.

[0008] Superabsorbent polymers are materials that swell by absorbing tens to hundreds of times their own amount of water, and are used for various purposes. When they are dried after absorbing water and swelling, they are dehydrated and their volume decreases. Therefore, when swollen superabsorbent polymer particles are mixed during concrete production, they are dehydrated by the hydration reaction of cement and voids are formed. Therefore, it is possible to form voids in concrete in the same way as when the above-mentioned hollow microspheres and expandable polymer microspheres are used. Since the swelling ability of superabsorbent polymers due to water absorption is high, the amount added to form the same amount of voids is less than that of hollow microspheres. However, the conditions under which swollen superabsorbent polymer particles are dehydrated and become voids have not been clarified. Furthermore, the amount of addition that can obtain the required freeze-thaw resistance has also been unknown.

[0009] The object of the present invention is to solve the above problems, and to provide a frost-resistant concrete having improved freeze-thaw resistance. To The purpose is to provide. [Means for solving the problem]

[0010] In order to solve the above problems, one embodiment of the frost-resistant concrete according to the present invention comprises: The present invention includes particles of a highly absorbent resin having an average particle size of 100 μm or less after swelling, The water-cement ratio is 40% or less. The present invention is made of a frost-resistant concrete containing minute voids formed when at least a portion of the water contained in the highly water-absorbent resin particles is consumed by the cement hydration reaction.

[0011] The volume ratio of the swollen particles of the superabsorbent resin to the concrete in the frost-resistant concrete is in the range of 1-3%. In this range, the resin particles can significantly improve the freeze-thaw resistance. In particular, when the water-cement ratio is 30% and the volume ratio is 1%, and when the water-cement ratio is 35% and the volume ratio is 3%, a high durability index is obtained, and the freeze-thaw resistance can be greatly improved. The average particle size of the highly water-absorbent resin particles after swelling may be 50 μm or less. The frost-resistant concrete may not contain an air-entraining agent.

[0012] The superabsorbent polymer particles are mixed with the concrete material in a water-absorbent, swollen state, and during curing, the water in the superabsorbent polymer particles is consumed by the cement hydration reaction and replaced by voids in the concrete. These voids act to protect the concrete from damage caused by freeze-thaw cycles by mitigating the changes in hydraulic pressure caused by the freeze-thaw cycles of concrete. However, whether or not the required voids are actually obtained in the concrete as described above depends on whether the water in the swollen particles of the superabsorbent polymer is actually consumed by the hydration reaction of cement, etc. As a result of intensive research, the inventors have found that if the water-cement ratio in the concrete mix plan is 40% or less, voids can be obtained in the concrete to an extent that the freeze-thaw resistance can be improved, and further, they have obtained the volume ratio of superabsorbent polymer particles in the concrete mix that can significantly improve the freeze-thaw resistance. Effect of the Invention

[0013] According to the present invention, a frost-thaw resistant concrete structure having improved freeze-thaw resistance can be obtained. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing a concrete mix of a frost-resistant concrete according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing actual measured values ​​of temperature during heat curing when producing a test specimen for a strength test. [Diagram 3] 1 is a graph showing the results of a compressive strength test. [Figure 4] 1 is a graph summarizing the change in relative dynamic modulus of elasticity as a result of a freeze-thaw test. [Diagram 5] 5 is a graph showing a durability index calculated based on FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Next, an embodiment of the present invention will be described.

[0016] (Outline of the frost-resistant concrete of this embodiment) In the frost-resistant concrete of this embodiment, superabsorbent polymer particles (hereinafter referred to as "SAP") are added along with other materials when mixing the concrete, and absorb water and swell. These particles are dehydrated through cement hydration reactions, etc., to form voids. These microvoids mitigate changes in liquid pressure caused by the freeze-thaw cycle of the concrete, thereby improving the freeze-thaw resistance. The SAP used is a material that has stable water absorption ability even in a highly alkaline and highly electrolyte-concentrated environment such as fresh concrete, and the average particle size of the SAP that can be used in this embodiment in a water-absorbed and swollen state is 100 μm or less, more specifically, in the range of 50 μm to 100 μm.

[0017] The higher the SAP content in concrete (the volume ratio of SAP in a swollen state to the concrete), the higher the void ratio in the hardened concrete, which improves the freeze-thaw resistance, but on the other hand, the compressive strength decreases. ,water If the cement ratio is too high, the SAP will remain swollen without forming voids, and sufficient freeze-thaw resistance may not be exhibited. Therefore, several concrete specimens with different SAP dosage rates and water-cement ratios were produced, and compressive strength tests and freeze-thaw tests were conducted on each specimen to examine the appropriate conditions.

[0018] (Materials used) First, the following materials were used for the test specimens: Cement: High-early-strength Portland cement (manufactured by Ube Mitsubishi Cement Co., Ltd.), density: 3.14 g / cm 3 Water: Tap water Fine aggregate: crushed sand (Kanuma City), surface dry density: 2.61g / cm 3 , Water absorption rate: 1.07%, Coarse particle rate: 3.01 Coarse aggregate: crushed stone (Kanuma City), surface dry density: 2.64g / cm3 , Water absorption rate: 0.72%, Coarse particle rate: 6.62, Maximum dimension: 20mm High performance water reducer: Mastergranium 8000S M type (manufactured by Pozzolith Solutions) Air content regulator (defoamer): Master Air 404 (Pozzolith Solutions) SAP: AQUALIC CS-6S (manufactured by Nippon Shokubai Co., Ltd.), water absorption capacity: approx. 40 times, average particle size before water absorption and swelling: approx. 15 μm, maximum particle size before water absorption and swelling: approx. 38 μm, average particle size after swelling: approx. 50 μm, maximum particle size after swelling: approx. 130 μm

[0019] (Concrete mix) The concrete mix for each test specimen is shown in Figure 1. Eight types of specimens with different SAP dosage rates and water-cement ratios, A0, A1, B0, B1, B2, B3, C0, and C1, were prepared. Specimens A0 and A1 are in the 30% water-cement ratio group, specimens B0, B1, B2, and B3 are in the 35% water-cement ratio group, and specimens C0 and C1 are in the 40% water-cement ratio group. Note that "water absorption" in the figure refers to the amount of water required for SAP to absorb water and swell, and the amount of water in the water-cement ratio does not include the amount of water absorbed by SAP. The SAP dosage rates were 0% (no SAP dosage), 1%, 2%, and 3%, and the SAP dosage rates of specimens A0, B0, and C0 were 0% (no SAP dosage), specimens A1, B1, and C1 were 1%, specimens B2 was 2%, and specimen B3 was 3%. Note that the SAP dosage rate is the volume ratio of swollen SAP to concrete. In order to standardize the unit mortar volume in concrete, the unit coarse aggregate amount was fixed for all mixes. The unit fine aggregate amount was fixed for each water-cement ratio mix, and the unit paste volume was standardized. The amount of swollen SAP and the amount of air were both included in the paste volume.

[0020] (How to mix concrete) The cement with powdered SAP and fine aggregate were put into a mixer and dry mixed for 30 seconds. Next, the total amount of water, which was the amount of water in the mix design and the amount of water required to absorb and swell the SAP, was added and mixed for 90 seconds, and then the coarse aggregate was added and mixed for 60 seconds. The slump and air content during the fresh test were adjusted to be within the target range by adding a high-performance water-reducing agent and an air content regulator (antifoaming agent). These admixtures were added to the mixing water.

[0021] (Method of manufacturing compressive strength test specimens) To obtain specimens for the compressive strength tests, concrete was poured into a cylindrical formwork measuring φ10 x 20 cm, and then heat curing was carried out using a variable temperature and humidity chamber to reproduce the steam curing that occurs in precast factories. Figure 2 shows the temperature history of heat curing. After heat curing was completed, the specimens were subjected to sealed curing indoors at 20°C and 60% RH until they reached the test age, at which point they were removed from the formwork and the compressive strength tests were carried out.

[0022] (Compression strength test results) Figure 3 shows the results of compressive strength tests at ages of 7 days and 28 days. In all types of specimens, the higher the SAP content, the lower the compressive strength. This behavior is similar to that when the air content in the concrete is increased, and the strength decreased by about 4-6% for every 1% of SAP, just as in the case of air.

[0023] (Manufacturing method of freeze-thaw test specimen) The freeze-thaw test was conducted in accordance with JIS A1148 Method A. After pouring concrete into a 10x10x40cm square column formwork, the heat supply curing shown in Figure 2 was carried out, and then the square column-shaped test specimen was removed from the formwork and subjected to sealed curing indoors at 20℃ and 60% RH until the material was 6 days old. This was followed by underwater curing for 24 hours, after which the freeze-thaw test was carried out from the 7th day old material.

[0024] (Freeze-thaw test results) FIG. 4 is a graph showing the change in the relative dynamic modulus of elasticity of the three test specimens, which is the average value, and FIG. 5 is a graph showing the durability index calculated based on FIG. From the graph in Figure 5, it was confirmed that the addition of SAP significantly improved freeze-thaw resistance, and the higher the SAP dosage rate, the better the freeze-thaw resistance. Also, the smaller the water-cement ratio, the more pronounced the effect of adding SAP on improving freeze-thaw resistance, and the effect was confirmed at water-cement ratios of 40% or less. In particular, the durability index was 80% or more for test specimen A1, which had a water-cement ratio of 30% and a SAP dosage rate of 1.0%, and test specimen B3, which had a water-cement ratio of 35% and a SAP dosage rate of 3.0%, confirming high freeze-thaw resistance.

[0025] In this embodiment, the test was performed using SAP with an average particle size after swelling of about 50 μm. However, since the maximum particle size after swelling of the SAP used as the material of the test specimen was about 130 μm, it is estimated that a similar effect can be expected if the average particle size after swelling is about 100 μm or less. Although an example of the present embodiment has been described above, the present invention is not limited to this, and may take various forms within the scope of the claims.

Claims

[Claim 1] The water-cement ratio is 40% or less, and powdered superabsorbent resin particles with an average particle size of 100 μm or less after swelling are added so that the volume of the powdered superabsorbent resin in the water-absorbed and swollen state is 1-3% of the volume of fresh concrete. The amount of water required for water absorption and swelling is added to the amount of water in the mix design, and curing including mixing and heat supply curing is performed to produce the product. A method for producing frost-resistant concrete.

Citation Information

Patent Citations

  • Application of modified water-absorbing resin as concrete antifreezing reinforcing material

    CN104558370A

  • Waveguide switch

    JP1988028101A

  • Hydraulic composition

    JP1988089446A

  • Lightweight cement building material

    JP1991146478A

  • Concrete composition inseparable in water

    JP1996188458A