Boron nitride powder, thermally conductive resin composition, heat dissipation sheet and electronic component structure
A boron nitride powder with a vinyl group-containing silane coupling agent and tailored particle size distribution enhances thermal conductivity and insulation in heat dissipation sheets, addressing the thermal management needs of miniaturized electronic components.
Patent Information
- Application Number
- JP2021000871
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-01-06
AI Technical Summary
Existing heat dissipation sheets for electronic components, particularly those using boron nitride powder, do not provide sufficient thermal conductivity to meet the demands of miniaturized devices generating increased heat.
A boron nitride powder is developed with specific particle size distribution and containing a vinyl group-containing silane coupling agent, which enhances thermal conductivity and insulation properties when molded into a heat dissipation sheet.
The resulting heat dissipation sheet exhibits improved thermal conductivity and insulation, effectively managing heat in miniaturized electronic components.
Smart Images

Figure 0007580273000004 
Figure 0007580273000001 
Figure 0007580273000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a boron nitride powder consisting of agglomerated boron nitride particles formed by agglomerating hexagonal boron nitride primary particles, a thermally conductive resin composition containing the boron nitride powder and a resin, a heat dissipation sheet formed by molding the thermally conductive resin composition, and an electronic component structure using the heat dissipation sheet. [Background technology]
[0002] For heat-generating electronic components such as power devices, transistors, thyristors, and CPUs, how to efficiently dissipate the heat generated during use is an important issue. Conventionally, the most common heat dissipation measures have been (1) to make the insulating layer of the printed wiring board on which the heat-generating electronic components are mounted highly thermally conductive, and (2) to attach the heat-generating electronic components or the printed wiring board on which the heat-generating electronic components are mounted to a heat sink via electrically insulating thermal interface materials. Silicone resin or epoxy resin filled with ceramic powder is used as the insulating layer and thermal interface material for the printed wiring board.
[0003] As a ceramic powder, boron nitride powder has attracted attention because of its properties such as high thermal conductivity, high insulation, low dielectric constant, etc. For example, Patent Document 1 discloses a boron nitride powder formed by agglomeration of primary particles of boron nitride, which has peak A present in the region of 5 μm or more and less than 30 μm and peak B present in the region of 50 μm or more and less than 100 μm in a volume-based particle size distribution. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-164365 A Summary of the Invention [Problem to be solved by the invention]
[0005] A heat dissipation sheet with excellent thermal conductivity can be obtained by using the boron nitride powder described in Patent Document 1. However, with the recent trend toward miniaturization of electronic devices and an increase in the amount of heat generated by heat-generating electronic components, there is a demand for heat dissipation sheets with even better thermal conductivity. Therefore, an object of the present invention is to provide agglomerated boron nitride particles for obtaining a heat dissipation sheet with excellent thermal conductivity, a boron nitride powder consisting of the agglomerated boron nitride particles, a thermally conductive resin composition containing the boron nitride powder, and a heat dissipation sheet obtained by molding the thermally conductive resin composition. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by using a boron nitride powder containing a silane coupling agent containing a vinyl group. The present invention is based on the above findings and has the following gist. [1] A boron nitride powder containing at least aggregated boron nitride particles formed by agglomeration of hexagonal boron nitride primary particles, which contains a vinyl group-containing silane coupling agent and has an infrared absorption peak (3076 cm) derived from the vinyl group. -1 ±2cm -1 ) and the infrared absorption peak (1377 cm) due to boron nitride -1 ±2cm -1 ) to strength Ib ratio ((Ia / Ib) × 100) is in the range of 0.1 to 10. [2] The boron nitride powder according to [1] above, wherein the particle size distribution of the boron nitride powder has at least a first maximum point, a second maximum point larger in particle size than the first maximum point, and a third maximum point larger in particle size than the second maximum point, the particle size of the first maximum point being 0.4 μm or more and less than 10 μm, the particle size of the second maximum point being 10 μm or more and less than 40 μm, and the particle size of the third maximum point being 40 μm or more and 110 μm or less. [3] The boron nitride powder according to the above [2], wherein the absolute value of the difference between the particle size at which the integrated amount of frequency in the particle size distribution of the boron nitride powder is 10% and the particle size of the minimum point between the smallest particle size maximum point and the second smallest particle size maximum point in the particle size distribution of the boron nitride powder is 3 to 30 μm. [4] The boron nitride powder according to the above [2] or [3], wherein the maximum point adjacent to the first maximum point is the second maximum point, the maximum point adjacent to the second maximum point is the third maximum point, and an absolute value of a difference between a particle size of a first minimum point between the first maximum point and the second maximum point and a particle size of a second minimum point between the second maximum point and the third maximum point is 15 to 60 μm. [5] The boron nitride powder according to any one of the above [2] to [4], wherein the half width of the peak having the third maximum point is 20 to 60 μm. [6] The boron nitride powder according to any one of the above [1] to [5], wherein the agglomerated boron nitride particles have a crushing strength of 5 to 18 MPa. [7] A thermally conductive resin composition comprising the boron nitride powder according to any one of [1] to [6] above. [8] A heat dissipation sheet obtained by molding the thermally conductive resin composition according to [7] above. [9] An electronic component structure in which the heat dissipation sheet according to [8] above is attached to an electronic component via grease. Effect of the Invention
[0007] According to the present invention, it is possible to provide a boron nitride powder for obtaining a heat dissipation sheet having excellent thermal conductivity, a heat conductive resin composition, and a heat dissipation sheet having excellent thermal conductivity. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a conceptual diagram of the particle size distribution of the boron nitride powder of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Boron nitride powder] The boron nitride powder of the present invention is a boron nitride powder containing at least aggregated boron nitride particles formed by aggregation of hexagonal boron nitride primary particles, and is characterized by containing a vinyl group-containing silane coupling agent. The boron nitride powder containing a vinyl group-containing silane coupling agent can be identified by infrared spectroscopy (hereinafter referred to as "IR"), and an infrared absorption peak (3076 cm) derived from the vinyl group can be identified. -1 ±2cm -1 ) and the infrared absorption peak due to boron nitride (1377 cm -1 ±2cm -1 ) can be detected. For the IR measurement, Fourier transform infrared spectroscopy (hereinafter referred to as "FT-IR") was used. The detailed measurement method will be described in the Examples.
[0010] In the present invention, the infrared absorption peak (3076 cm) derived from the vinyl group -1 ±2cm -1 ) and the infrared absorption peak (1377 cm) due to boron nitride -1 ±2cm -1 The ratio of the strength Ia to the strength Ib ((Ia / Ib)×100) is in the range of 0.1 to 10. When the strength ratio is in this range, the insulation and thermal conductivity of the heat dissipation sheet are excellent. From the above viewpoints, (Ia / Ib)×100 is preferably in the range of 0.5 to 8, and more preferably in the range of 1 to 7.
[0011] <Vinyl group-containing silane coupling agents> Examples of vinyl group-containing silane coupling agents include silane coupling agents having a vinyl group as a reactive organic group and a silicon atom bonded to at least one alkoxy group, and specifically, are represented by the following general formula (1).
[0012] [ka]
[0013] (In formula (1), at least one of R is an alkoxy group, and n is an integer of 0 to 12.) By using a silane coupling agent having such a composition, the generation of voids in the heat dissipation sheet can be effectively suppressed.
[0014] In the above formula (1), in the silane coupling agent where n is 0, that is, in the silane coupling agent where the silicon atom and the vinyl group are directly bonded, it is preferable that the silicon atom bonded to at least one alkoxy group is a silicon atom bonded to at least two alkoxy groups. In addition, the alkoxy group is preferably a methoxy group or an ethoxy group, and more preferably a methoxy group. Specific examples include vinyltrimethoxysilane, vinyltriethoxysilane, vinyldimethoxymethylsilane, vinyldimethoxyethylsilane, vinyldiethoxymethylsilane, and vinyldiethoxyethylsilane. In addition, R may have an ether bond, and examples thereof include vinyltris(2-methoxyethoxysilane), vinyltris(2-ethoxyethoxysilane), vinyltris(2-methoxymethoxysilane), and vinyltris(2-ethoxymethoxysilane). Among these, from the viewpoint of improving the dielectric breakdown characteristics, it is preferable to have two alkoxy groups and one alkyl group, and vinyldimethoxymethylsilane is particularly preferable. Furthermore, when R has an ether bond, it is preferable that all the groups are alkoxy groups, and vinyltris(2-methoxyethoxysilane) is particularly preferable.
[0015] Furthermore, when n is not 0, from the viewpoint of improving the dielectric breakdown characteristics, the number of carbon atoms (n) of the alkylene group arranged between the vinyl group and the silicon atom is preferably 2 to 12, more preferably 3 to 11, even more preferably 4 to 10, still more preferably 5 to 9, and particularly preferably 6 to 8. Furthermore, it is preferable that the alkylene group arranged between the reactive organic group and the silicon atom is linear. In the formula (1), specific examples of the vinyl group-containing silane coupling agent in which n is greater than 0 and an alkylene group is present between the vinyl group and the silicon atom include, for example, propenyltrimethoxysilane, propenyltriethoxysilane, propenylmethyldimethoxysilane, propenylmethyldiethoxysilane, butenyltrimethoxysilane, butenyltriethoxysilane, butenylmethyldimethoxysilane, butenylmethyldiethoxysilane, pentenyltrimethoxysilane, pentenyltriethoxysilane, pentenylmethyldimethoxysilane, pentenylmethyldiethoxysilane, hexenyltrimethoxysilane, hexenyltriethoxysilane, hexenylmethyldimethoxysilane, hexenylmethyldiethoxysilane, heptenyltrimethoxysilane, heptenyltriethoxysilane, Examples of the silane include heptenylmethyldimethoxysilane, heptenylmethyldiethoxysilane, octenyltrimethoxysilane, octenyltriethoxysilane, octenylmethyldimethoxysilane, octenylmethyldiethoxysilane, nonenyltrimethoxysilane, nonenyltriethoxysilane, nonenylmethyldimethoxysilane, nonenylmethyldiethoxysilane, dekenyltrimethoxysilane, dekenyltriethoxysilane, dekenylmethyldimethoxysilane, dekenylmethyldiethoxysilane, undekenyltrimethoxysilane, undekenyltriethoxysilane, undekenylmethyldimethoxysilane, undekenylmethyldiethoxysilane, dodekenyltrimethoxysilane, dodekenyltriethoxysilane, dodekenylmethyldimethoxysilane, and dodekenylmethyldiethoxysilane. Among these, from the viewpoint of improving the dielectric breakdown characteristics of the heat dissipation sheet, vinyl group-containing silane coupling agents having long organic chains are more preferred, specifically, octenyltrimethoxysilane (7-oct-1-enyltrimethoxysilane), octenyltriethoxysilane, octenylmethyldimethoxysilane, octenylmethyldiethoxysilane, nonenyltrimethoxysilane, nonenyltriethoxysilane, nonenylmethyldimethoxysilane, nonenylmethyldiethoxysilane, dekenyltrimethoxysilane, dekenyltriethoxysilane, dekenylmethyldimethoxysilane, and dekenylmethyldiethoxysilane are more preferred, octenyltrimethoxysilane, octenyltriethoxysilane, octenylmethyldimethoxysilane, and octenylmethyldiethoxysilane are even more preferred, and octenyltrimethoxysilane is particularly preferred. These may be used alone or in combination of two or more.
[0016] The content of the vinyl group-containing silane coupling agent in the boron nitride powder of the present invention is adjusted so that the above (Ia / Ib)×100 is in the range of 0.1 to 10, preferably in the range of 0.5 to 8, and more preferably in the range of 1 to 7.
[0017] <Specific surface area> The specific surface area of the aggregated boron nitride particles constituting the boron nitride powder of the present invention, as measured by the BET method, is preferably 2 to 7 m 2 / g. The specific surface area of the agglomerated boron nitride particles measured by the BET method is 2 m 2 When the boron nitride powder has a molecular weight of 1000 or more, the contact area between the boron nitride powder and the resin can be increased, suppressing the generation of voids in the heat dissipation sheet, and the aggregate morphology that exhibits high thermal conductivity can be easily maintained, improving the dielectric breakdown characteristics and the thermal conductivity of the heat dissipation sheet. On the other hand, the specific surface area of agglomerated boron nitride particles measured by the BET method is 7 m 2When the specific surface area of the agglomerated boron nitride particles is less than 2 to 6 m / g, the boron nitride powder can be highly loaded into the resin, and the generation of voids in the heat dissipation sheet can be suppressed and the dielectric breakdown characteristics can be improved. From the above viewpoint, the specific surface area of the agglomerated boron nitride particles measured by the BET method is more preferably 2 to 6 m 2 / g, and more preferably 3 to 6m 2 The specific surface area of the agglomerated boron nitride particles measured by the BET method can be measured by the BET single point method using a specific surface area measuring device (Cantersorb, manufactured by Yuasa Ionics, Inc.).
[0018] <Crushing strength> The crushing strength of the agglomerated boron nitride particles constituting the boron nitride powder of the present invention is preferably 5 to 18 MPa. When the crushing strength of the agglomerated boron nitride particles is 5 MPa or more, the agglomerated boron nitride particles can be prevented from being destroyed during the production of the heat dissipation sheet. When the crushing strength of the agglomerated boron nitride particles is 18 MPa or less, the resin can be sufficiently infiltrated into the agglomerated boron nitride particles in the heat dissipation sheet, and air can be prevented from remaining in the agglomerated boron nitride particles in the heat dissipation sheet. From this viewpoint, the crushing strength of the agglomerated boron nitride particles of the present invention is more preferably 6 to 15 MPa, and further preferably 7 to 13 MPa. The crushing strength of the agglomerated boron nitride particles can be measured by the method described in the Examples below.
[0019] <Ratio of major axis to thickness of primary particles of hexagonal boron nitride> The ratio of the major axis to the thickness (major axis / thickness) of the hexagonal boron nitride primary particles in the agglomerated boron nitride particles of the present invention is preferably 7 to 16. When the ratio of the major axis to the thickness (major axis / thickness) of the hexagonal boron nitride primary particles is 7 to 16, the insulation breakdown characteristics of the heat dissipation sheet are further improved. From the above viewpoint, the ratio of the major axis to the thickness (major axis / thickness) of the hexagonal boron nitride primary particles is more preferably 8 to 15, and further preferably 8 to 13. The ratio of the major axis to the thickness (major axis / thickness) of the hexagonal boron nitride primary particles is a value obtained by dividing the average major axis value of the hexagonal boron nitride primary particles by the average thickness value. The average major axis length and the average thickness of the hexagonal boron nitride primary particles are obtained by the following method. The produced agglomerated boron nitride particles are observed so that the major and minor diameters can be confirmed on the surface, and observed using a scanning electron microscope at a magnification of 1000 to 5000. The obtained particle images are imported into image analysis software to measure the major diameter and thickness of the particles, and the major diameters and thicknesses of 100 random particles are calculated and their average values are taken as the average major diameter and average thickness.
[0020] <Long axis of hexagonal boron nitride primary particles> The average value of the major axis of the hexagonal boron nitride primary particles in the aggregated boron nitride particles of the present invention is preferably 2 to 12 μm. When the average value of the major axis of the hexagonal boron nitride primary particles is 2 μm or more, the thermal conductivity of the aggregated boron nitride particles is good. When the average value of the major axis of the hexagonal boron nitride primary particles is 2 μm or more, the resin is easily permeated into the aggregated boron nitride particles, and the generation of voids in the heat dissipation sheet can be suppressed. On the other hand, when the average value of the major axis of the hexagonal boron nitride primary particles is 12 μm or less, the inside of the aggregated boron nitride particles becomes a dense structure, and the crushing strength of the aggregated boron nitride particles can be increased and the thermal conductivity of the aggregated boron nitride particles can be improved. From the above viewpoint, the average value of the major axis of the hexagonal boron nitride primary particles is more preferably 3 to 11 μm, and further preferably 3 to 10 μm.
[0021] <Particle size distribution of boron nitride powder> Fig. 1 is a conceptual diagram showing the particle size distribution of the boron nitride powder of the present invention. The vertical axis of the particle size distribution shown in Fig. 1 is linear, and the horizontal axis is logarithmic. Note that the particle size distribution of the boron nitride powder shown in Fig. 1 is merely a conceptual diagram and does not limit the boron nitride powder of the present invention.
[0022] As shown in FIG. 1, the particle size distribution of the boron nitride powder of the present invention preferably has at least a first maximum point (MAX1), a second maximum point (MAX2) having a particle size larger than the first maximum point (MAX1), and a third maximum point (MAX3) having a particle size larger than the second maximum point (MAX2). The particle size of the first maximum point (MAX1) is preferably 0.4 μm or more and less than 10 μm, the particle size of the second maximum point (MAX2) is preferably 10 μm or more and less than 40 μm, and the particle size of the third maximum point (MAX3) is preferably 40 μm or more and 110 μm or less. This can increase the filling property of the boron nitride powder in the heat dissipation sheet, and can provide excellent thermal conductivity of the heat dissipation sheet. The particle size distribution of the boron nitride powder of the present invention can be measured by the method of the examples described later.
[0023] As described above, the particle size distribution of the boron nitride powder of the present invention has at least a first maximum point (MAX1), a second maximum point (MAX2) that is larger than the first maximum point (MAX1), and a third maximum point (MAX3) that is larger than the second maximum point (MAX2). If the particle size distribution of the boron nitride powder does not have at least one maximum point among the first maximum point (MAX1), the second maximum point (MAX2), and the third maximum point (MAX3), the filling property of the boron nitride powder in the heat dissipation sheet decreases, and the thermal conductivity of the heat dissipation sheet deteriorates.
[0024] The particle size at the first maximum point (MAX1) is preferably 0.4 μm or more and less than 10 μm. When the particle size at the first maximum point (MAX1) is 0.4 μm or more and less than 10 μm, the filling of the boron nitride powder in the heat dissipation sheet is improved, and the thermal conductivity of the heat dissipation sheet is further improved. From this viewpoint, the particle size at the first maximum point (MAX1) is more preferably 1.0 to 8.0 μm, and more preferably 3.0 to 6.0 μm.
[0025] The particle size at the second maximum point (MAX2) is preferably 10 μm or more and less than 40 μm. When the particle size at the second maximum point (MAX2) is 10 μm or more and less than 40 μm, the filling of the boron nitride powder in the heat dissipation sheet is improved, and the thermal conductivity of the heat dissipation sheet is further improved. From this viewpoint, the particle size at the second maximum point (MAX2) is preferably 15 to 35 μm, and more preferably 18 to 30 μm.
[0026] The particle size at the third maximum point (MAX3) is preferably 40 to 110 μm. When the particle size at the third maximum point (MAX3) is 40 μm or more and 110 μm or less, the filling of the boron nitride powder in the heat dissipation sheet is improved, and the thermal conductivity of the heat dissipation sheet is further improved. From this viewpoint, the particle size at the third maximum point (MAX3) is more preferably 55 to 95 μm, and more preferably 65 to 90 μm.
[0027] The maximum point adjacent to the first maximum point (MAX1) is the second maximum point (MAX2), the maximum point adjacent to the second maximum point (MAX2) is the third maximum point (MAX3), and the absolute value of the difference between the particle size of the first minimum point (MIN1) between the first maximum point (MAX1) and the second maximum point (MAX2) and the particle size of the second minimum point (MIN2) between the second maximum point (MAX2) and the third maximum point (MAX3) is preferably 15 to 60 μm. When the absolute value of the difference between the particle size of the first minimum point (MIN1) and the particle size of the second minimum point (MIN2) is 15 to 60 μm, the filling property of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the absolute value of the difference between the particle size at the first minimum point (MIN1) and the particle size at the second minimum point (MIN2) is preferably 21 to 43 μm, and more preferably 25 to 35 μm.
[0028] The half-width of the peak having the third maximum point (MAX3) is preferably 20 to 60 μm. When the half-width of the peak having the third maximum point (MAX3) is 20 to 60 μm, the filling of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the half-width of the peak having the third maximum point (MAX3) is preferably 28 to 53 μm, and more preferably 40 to 50 μm. The half-width of the peak having the third maximum point (MAX3) is the width of the peak at a frequency half that of the third maximum point (MAX3).
[0029] The absolute value of the difference between the particle size at which the cumulative frequency in the particle size distribution of the boron nitride powder is 10% and the particle size of the minimum point between the smallest particle size maximum point and the second smallest particle size maximum point in the particle size distribution of the boron nitride powder is preferably 3 to 30 μm. For example, in the case of the particle size distribution of the boron nitride powder shown in FIG. 1, the symbol D10 indicates the particle size at which the cumulative frequency is 10%, the smallest particle size maximum point in the particle size distribution of the boron nitride powder is the first maximum point (MAX1), the second smallest particle size maximum point in the particle size distribution of the boron nitride powder is the second maximum point (MAX2), and the minimum point between the smallest particle size maximum point and the second smallest particle size maximum point is the first minimum point (MIN1). When the absolute value of the difference in particle size is 3 to 30 μm, the filling property of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the absolute value of the difference in particle size is preferably 4 to 17 μm, and more preferably 6 to 15 μm.
[0030] The integrated amount (V1) of the frequency between the peak start and the peak end in the peak having the first maximum point (MAX1) is preferably 2 to 25% by volume. When the integrated amount (V1) is 2 to 25% by volume, the filling of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the integrated amount (V1) is more preferably 5 to 20% by volume. The peak start in the peak having the first maximum point (MAX1) is a minimum point on the side of the smaller particle size relative to the first maximum point (MAX1). When there is no minimum point on the side of the smaller particle size relative to the first maximum point (MAX1), the peak start is the end (DS) of the particle size distribution on the smaller particle size side. In addition, the peak end in the peak having the first maximum point (MAX1) is a minimum point (MIN1) on the side of the larger particle size relative to the first maximum point (MAX1). The cumulative frequency (V1) is a value obtained by subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from the cumulative frequency from the particle size of the minimum point on the smaller particle size side than the first maximum point (MAX1) or the particle size of the end (DS) of the particle size distribution on the smaller particle size side than the first maximum point (MAX1). The reason for subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) is to prevent the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from being added to both the cumulative frequency from the peak start to the peak end in the peak having the first maximum point (MAX1) and the cumulative frequency from the peak start to the peak end in the peak having the second maximum point (MAX2).
[0031] The integrated amount (V2) of the frequency between the peak start and the peak end in the peak having the second maximum point (MAX2) is preferably 15 to 50 volume %. When the integrated amount (V2) is 15 to 50 volume %, the filling of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the integrated amount (V2) is more preferably 20 to 45 volume %. The peak start in the peak having the second maximum point (MAX2) is the minimum point (MIN1) on the side of the smaller particle size relative to the second maximum point (MAX2). The peak end in the peak having the second maximum point (MAX2) is the minimum point (MIN2) on the side of the larger particle size relative to the second maximum point (MAX2). The integrated amount of frequency (V2) is a value obtained by subtracting the frequency of the particle size of the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from the integrated amount of frequency from the particle size of the minimum point (MIN1) on the smaller particle size side of the second maximum point (MAX2) to the particle size of the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2). The reason for subtracting the frequency of the particle size of the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) is to prevent the frequency of the particle size of the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from being added to both the integrated amount of frequency from the peak start to the peak end of the peak having the second maximum point (MAX2) and the integrated amount of frequency from the peak start to the peak end of the peak having the third maximum point (MAX3).
[0032] The integrated amount (V3) of the frequency between the peak start and the peak end in the peak having the third maximum point (MAX3) is preferably 30 to 80% by volume. When the integrated amount (V3) is 30 to 80% by volume, the filling of the boron nitride powder in the heat dissipation sheet can be further improved, and the thermal conductivity of the heat dissipation sheet can be further improved. From this viewpoint, the integrated amount (V3) is more preferably 45 to 75% by volume. The peak start in the peak having the third maximum point (MAX3) is the minimum point (MIN2) on the side of the smaller particle size relative to the third maximum point (MAX3). The peak end in the peak having the third maximum point (MAX3) is the minimum point on the side of the larger particle size relative to the third maximum point (MAX3). When there is no minimum point on the side of the larger particle size relative to the third maximum point (MAX3), the peak end is the end (DE) on the larger particle size side of the particle size distribution. The cumulative frequency (V3) is the cumulative frequency from the particle size of the minimum point (MIN2) on the smaller particle size side of the third maximum point (MAX3) to the particle size of the minimum point on the larger particle size side of the third maximum point (MAX3) minus the frequency of the particle size of the minimum point on the larger particle size side of the third maximum point (MAX3), or the cumulative frequency from the particle size of the minimum point (MIN2) on the smaller particle size side of the third maximum point (MAX3) to the particle size at the larger particle size end (PE) of the particle size distribution. The frequency of particle sizes of minimum points on the larger particle size side of the third maximum point (MAX3) is subtracted to prevent the frequency of particle sizes of minimum points on the larger particle size side of the third maximum point (MAX3) from being added to both the integrated amount of frequency from the peak start to the peak end of a peak having the third maximum point (MAX3) and the integrated amount of frequency from the peak start to the peak end of a peak having a maximum point adjacent to the third maximum point (MAX3) and on the larger particle size side of the third maximum point.
[0033] As long as the packing ability of the boron nitride powder in the heat dissipation sheet can be increased, the particle size distribution of the boron nitride powder of the present invention may have other maximum points in addition to the above-mentioned first to third maximum points.
[0034] <Manufacturing method of boron nitride powder> An example of a method for producing the boron nitride powder of the present invention will now be described. The boron nitride powder of the present invention can be produced, for example, by preparing a first boron nitride powder having a particle size distribution with the above-mentioned first maximum point, a second boron nitride powder having a particle size distribution with the above-mentioned second maximum point, and a third boron nitride powder having a particle size distribution with the above-mentioned third maximum point, and mixing the first to third boron nitride powders thus prepared.
[0035] Of the first to third boron nitride powders, the second and third boron nitride powders are preferably boron nitride powders containing at least aggregated boron nitride particles formed by aggregation of hexagonal boron nitride primary particles. The first boron nitride powder may be aggregated boron nitride particles, but is preferably hexagonal boron nitride primary particles. The maximum point of each of the first to third boron nitride powders means the apex of the peak in the particle size distribution of each of the first to third boron nitride powders. The particle size distribution of the first to third boron nitride powders is measured in the same manner as the particle size distribution of the boron nitride powder described above.
[0036] In the mixing step, the first to third boron nitride powders may be mixed so that the volumetric ratio of the third boron nitride powder is greater than the volumetric ratio of the second boron nitride powder, and the volumetric ratio of the second boron nitride powder is greater than the volumetric ratio of the first boron nitride powder. This can further increase the packing property of the boron nitride powder. From the viewpoint of improving the thermal conductivity of the heat dissipation sheet, the volumetric ratio of the third boron nitride powder is preferably 30 to 80 parts by volume, more preferably 45 to 75 parts by volume, and even more preferably 50 to 70 parts by volume, relative to a total of 100 parts by volume of the first to third boron nitride powders. From the viewpoint of improving the thermal conductivity of the heat dissipation sheet, the volumetric ratio of the second boron nitride powder is preferably 15 to 50 parts by volume, more preferably 20 to 45 parts by volume, and even more preferably 25 to 35 parts by volume, relative to a total of 100 parts by volume of the first to third boron nitride powders. From the viewpoint of improving the thermal conductivity of the heat dissipation sheet, the volume proportion of the first boron nitride powder is preferably 2 to 25 volume parts per 100 volume parts combined of the first to third boron nitride powders, more preferably 5 to 20 volume parts, and even more preferably 8 to 15 volume parts.
[0037] Each of the first to third boron nitride powders can be produced, for example, by a production method including a crushing step of crushing lump boron carbide, a nitriding step of nitriding the crushed boron carbide to obtain boron carbonitride, and a decarburizing step of decarbonizing the boron carbonitride.
[0038] In the pulverization step, the boron carbide lumps (boron carbide lumps) are pulverized using a general pulverizer or crusher. At this time, for example, by adjusting the pulverization time and the amount of boron carbide lumps charged, boron carbide powder having a desired maximum point can be obtained. The maximum point of the boron carbide powder can be measured in the same manner as the maximum point of the boron nitride powder described above. In this way, by adjusting the maximum point of the boron carbide powder so that it approaches the maximum point of the desired boron nitride powder, the first to third boron nitride powders having the above-mentioned maximum points can be obtained.
[0039] Next, in the nitriding step, the boron carbide powder is fired under pressurized conditions in an atmosphere that allows the nitriding reaction to proceed, thereby obtaining boron carbonitride.
[0040] The atmosphere in the nitriding step is an atmosphere that allows the nitriding reaction to proceed, and may be, for example, nitrogen gas, ammonia gas, or the like, and may be one kind or a combination of two or more kinds thereof. From the viewpoint of ease of nitriding and cost, the atmosphere is preferably nitrogen gas. The content of nitrogen gas in the atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more.
[0041] The pressure in the nitriding step is preferably 0.6 MPa or more, more preferably 0.7 MPa or more, and preferably 1.0 MPa or less, more preferably 0.9 MPa or less. The pressure is further preferably 0.7 to 1.0 MPa. The firing temperature in the nitriding step is preferably 1800° C. or more, more preferably 1900° C. or more, and preferably 2400° C. or less, more preferably 2200° C. or less. The firing temperature is further preferably 1900 to 2200° C. The pressure conditions and firing temperature are preferably 1800° C. or more and 0.7 to 1.0 MPa, since they further suitably advance the nitridation of boron carbide and are industrially appropriate conditions.
[0042] The firing time in the nitriding step is appropriately selected within a range in which nitriding proceeds sufficiently, and is preferably 6 hours or more, more preferably 8 hours or more, and is preferably 30 hours or less, more preferably 20 hours or less.
[0043] In the decarburization step, the boron carbonitride obtained in the nitridation step is subjected to a heat treatment in an atmosphere of atmospheric pressure or higher at a predetermined holding temperature for a certain period of time, thereby obtaining aggregated boron nitride particles formed by aggregation of decarburized and crystallized hexagonal boron nitride primary particles.
[0044] The atmosphere in the decarburization step is an atmosphere of normal pressure (atmospheric pressure) or a pressurized atmosphere. In the case of a pressurized atmosphere, the pressure may be, for example, 0.5 MPa or less, preferably 0.3 MPa or less.
[0045] In the decarburization step, for example, the temperature is first raised to a predetermined temperature (temperature at which decarburization can start), and then further raised to a holding temperature at a predetermined heating rate. The predetermined temperature (temperature at which decarburization can start) can be set according to the system, and may be, for example, 1000°C or higher, 1500°C or lower, and preferably 1200°C or lower. The rate at which the temperature is raised from the predetermined temperature (temperature at which decarburization can start) to the holding temperature may be, for example, 5°C / min or lower, and preferably 4°C / min or lower, 3°C / min or lower, or 2°C / min or lower.
[0046] The holding temperature is preferably 1800° C. or higher, more preferably 2000° C. or higher, from the viewpoint of favorable grain growth and further improving the thermal conductivity of the obtained boron nitride powder. The holding temperature may be preferably 2200° C. or lower, more preferably 2100° C. or lower.
[0047] The holding time at the holding temperature is appropriately selected within a range in which crystallization sufficiently proceeds, and may be, for example, more than 0.5 hours, and from the viewpoint of favorable grain growth, is preferably 1 hour or more, more preferably 3 hours or more, even more preferably 5 hours or more, and particularly preferably 10 hours or more. The holding time at the holding temperature may be, for example, less than 40 hours, and from the viewpoint of preventing excessive grain growth and thus reducing particle strength, is preferably 30 hours or less, more preferably 20 hours or less, in order to reduce costs.
[0048] In the decarburization step, a boron source may be mixed with the boron carbonitride obtained in the nitridation step as a raw material to carry out decarburization and crystallization. The boron source may be boric acid, boron oxide, or a mixture thereof. In this case, other additives used in the art may be further used as necessary.
[0049] The mixing ratio of boron carbonitride and the boron source is appropriately selected. When boric acid or boron oxide is used as the boron source, the ratio of boric acid or boron oxide may be, for example, 100 parts by mass or more, preferably 150 parts by mass or more, and may be, for example, 300 parts by mass or less, preferably 250 parts by mass or less, relative to 100 parts by mass of boron carbonitride.
[0050] The boron nitride powder obtained as described above may be subjected to a classification step (classification step) using a sieve to obtain boron nitride powder having a desired particle size distribution, which more suitably obtains the first to third boron nitride powders having the desired maximum points.
[0051] The obtained first to third boron nitride powders can be mixed to obtain the boron nitride powder of the present invention. The mixing method is not particularly limited as long as the first to third boron nitride powders can be mixed uniformly. For example, the first to third boron nitride powders may be mixed using a container rotation type mixer, the first to third boron nitride powders may be mixed using a container fixed type mixer, or the first to third boron nitride powders may be mixed using a fluid motion type mixer.
[0052] [Thermal conductive resin composition] The thermally conductive resin composition can be produced by mixing the boron nitride powder of the present invention with a resin. Alternatively, the thermally conductive resin composition may be produced by mixing the first to third boron nitride powders described above with a resin.
[0053] (resin) Examples of the resin of the thermally conductive resin composition include epoxy resin, silicone resin (including silicone rubber), acrylic resin, phenolic resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyamide (e.g., polyimide, polyamideimide, polyetherimide, etc.), polyester (e.g., polybutylene terephthalate, polyethylene terephthalate, etc.), polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, etc. Among these, silicone resin is preferred from the viewpoint of heat resistance, flexibility, and adhesion to heat sinks, etc. Silicone resin is preferably vulcanized and cured by organic peroxide. In addition, the viscosity of the thermally conductive resin composition at 25°C is, for example, 100,000 cp or less from the viewpoint of improving the flexibility of the sheet-shaped molded body.
[0054] The content of boron nitride powder in the thermally conductive resin composition relative to the total 100% by volume of the boron nitride powder and the resin is preferably 30 to 85% by volume, more preferably 40 to 80% by volume. When the content of boron nitride powder is 30% by volume or more, the thermal conductivity is improved and sufficient heat dissipation performance is easily obtained. When the content of boron nitride powder is 85% by volume or less, the tendency of voids to be generated during molding can be reduced, and the deterioration of insulation and mechanical strength can be suppressed. Furthermore, the content of resin relative to the total 100% by volume of the boron nitride powder and the resin is preferably 15 to 70% by volume, more preferably 20 to 60% by volume.
[0055] (solvent) In order to adjust the viscosity of the thermally conductive resin composition, the thermally conductive resin composition may further contain a solvent. The solvent is not particularly limited as long as it can dissolve the resin and can be easily removed from the thermally conductive resin composition after the thermally conductive resin composition is applied. When the resin is a silicone resin, examples of the solvent include toluene, xylene, and chlorine-based hydrocarbons. Among these solvents, toluene is preferred from the viewpoint of ease of removal. The content of the solvent can be appropriately selected according to the target viscosity of the thermally conductive resin composition. The content of the solvent is, for example, 40 to 200 parts by mass with respect to 100 parts by mass of the components other than the solvent of the thermally conductive resin composition.
[0056] The thermally conductive resin composition may contain components other than the boron nitride powder, the resin component, and the solvent. The other components are inorganic fillers other than the boron nitride powder, additives, impurities, etc., and the content of the other components is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 1 part by mass or less, relative to 100 parts by mass of the total of the boron nitride powder and the resin.
[0057] [Heat dissipation sheet] The heat dissipation sheet of the present invention is obtained by molding the above-mentioned thermally conductive resin composition. (Thickness of heat dissipation sheet) The thickness of the heat dissipation sheet of the present invention is preferably 100 to 1200 μm. When the thickness of the heat dissipation sheet is 100 μm or more, the heat dissipation sheet can be more reliably attached to the heat-generating electronic component. When the thickness of the heat dissipation sheet is 1200 μm or less, the heat dissipation properties of the heat dissipation sheet can be further improved. From such a viewpoint, the thickness of the heat dissipation sheet of the present invention is more preferably 150 to 800 μm, and further preferably 200 to 600 μm.
[0058] [Method of manufacturing heat dissipation sheet] The method for producing the heat dissipation sheet of the present invention includes the steps of: (A) blending the boron nitride powder of the present invention with a resin to prepare a thermally conductive resin composition; (B) forming the thermally conductive resin composition into a sheet to prepare a thermally conductive resin composition sheet; and (C) heating and pressurizing the thermally conductive resin composition sheet under vacuum.
[0059] (Process (A)) In step (A), the boron nitride powder of the present invention is mixed with a resin to prepare a thermally conductive resin composition. The boron nitride powder and the resin used in step (A) have already been described, so a description thereof will be omitted.
[0060] (Process (B)) In step (B), the thermally conductive resin composition is formed into a sheet to produce a thermally conductive resin composition sheet. For example, the thermally conductive resin composition can be formed into a sheet by a doctor blade method or a calendar process. However, when the thermally conductive resin composition passes through a calendar roll, the aggregated boron nitride particles in the thermally conductive resin composition may be broken. Therefore, it is preferable to form the thermally conductive resin composition into a sheet by a doctor blade method.
[0061] (Process (C)) In step (C), the thermally conductive resin composition sheet is heated and pressurized under vacuum. This can further increase the packing of the boron nitride powder in the heat dissipation sheet, and further improve the thermal conductivity of the heat dissipation sheet. This can also reduce microvoids in the heat dissipation sheet, and therefore the thermal conductivity of the heat dissipation sheet can be further improved, and the insulation of the heat dissipation sheet can be improved. From the viewpoint of improving the packing of the boron nitride powder and reducing the microvoids in the heat dissipation sheet, the pressure of the vacuum environment when the thermally conductive resin composition sheet is heated and pressurized is preferably 0.1 to 5 kPa, and more preferably 0.1 to 3 kPa. The heating temperature of the thermally conductive resin composition sheet is preferably 120 to 200°C, and more preferably 130 to 180°C. Furthermore, the pressure when pressing the thermally conductive resin composition sheet is preferably 80 to 250 kg / cm.2 and more preferably 100 to 200 kg / cm 2 It is. As described above, in the present invention, the boron nitride powder contains a vinyl group-containing silane coupling agent, and since the vinyl group of the coupling agent is a reactive functional group with a double bond having π electrons, it forms a covalent bond with the resin and has a strong bond. Therefore, in this step (C), the coupling agent can firmly bond the filler (BN) and the resin, and it is believed that voids can be reduced more effectively.
[0062] [Electronic component structure] The electronic component structure of the present invention is formed by attaching the heat dissipation sheet of the present invention to an electronic component via grease. By attaching the heat dissipation sheet of the present invention to the electronic component via grease, the adhesion between the heat dissipation sheet and the electronic component is improved, and the heat dissipation efficiency is improved. The grease is not particularly limited as long as it can improve the adhesion between the heat dissipation sheet and the electronic components, but it is preferable that the grease itself has thermal conductivity. Specifically, grease to which inorganic materials, ceramic fillers, metal fillers, etc., which have excellent thermal conductivity, are added are preferably used, and examples of the grease include silicone-based grease and acrylic-based grease, with silicone-based grease being particularly preferable. The electronic component is not particularly limited, but it is more effective to use the composition in heat-generating electronic components, such as power devices, transistors, thyristors, and CPUs. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0064] [Evaluation method] ((Ia / Ib) x 100) The boron nitride powder obtained in each of the examples and comparative examples was subjected to FT-IR measurement using Bruker's "INVENIO S" (resolution 4 cm-1 Measurement range: 4000~650cm -1 ). After performing background measurement using a single reflection ATR, a sample made of boron nitride powder was set and the sample surface was measured with 32 scans. The measurement results were output with absorbance on the vertical axis (Y axis) and wave number on the horizontal axis, with the infrared absorption peak (3076 cm) derived from vinyl groups. -1 ±2cm -1 ) and the infrared absorption peak (1377 cm) due to boron nitride -1 ±2cm -1 ) and Ib were calculated using OPUS analysis software, and the intensity ratio (Ia / Ib) was calculated.
[0065] (particle size distribution) The particle size distribution of the boron nitride powder was measured using a laser diffraction scattering particle size distribution analyzer (LS-13 320) manufactured by Beckman Coulter, Inc. From the obtained particle size distribution, the particle size of the first to third maximum points (first to third maximum values), the integrated value of the frequency from the peak start to the peak end in the peak having the first to third maximum points (integrated value of the first to third frequencies), the absolute value of the difference between the particle size at which the integrated value of the frequency is 10% and the particle size of the minimum point between the maximum point with the smallest particle size and the maximum point with the second smallest particle size (D10 and the distance between the first minimum value), the absolute value of the difference between the particle size of the first minimum point and the particle size of the second minimum point (distance between the minimum values), and the half-width of the peak having the third maximum point (half-width of maximum value 3) were obtained.
[0066] (Crushing strength) The crushing strength of the agglomerated boron nitride particles was measured in accordance with JIS R1639-5:2007. Specifically, the agglomerated boron nitride particles were spread on the sample stage of a microcompression tester ("MCT-W500", manufactured by Shimadzu Corporation), and then five agglomerated boron nitride particles were selected and subjected to a crushing test one by one. The crushing strength (σ: MPa) was calculated as σ = α × P / (π × d 2The crushing strength of the five inorganic filler components was plotted in accordance with JIS R1625:2010, and the crushing strength at which the cumulative fracture rate was 63.2% was determined as the crushing strength of the agglomerated boron nitride particles.
[0067] The heat dissipation sheets of the examples and comparative examples were evaluated as follows. (Insulating) The dielectric breakdown voltage of the heat dissipation sheet was evaluated based on the value measured in a short-time breakdown test (room temperature 23°C) in accordance with the method described in JIS C2110-1:2016. The evaluation criteria for insulation are as follows. ◎: Dielectric breakdown voltage is 10kV or more ○: Breakdown voltage is 5 kV or more and less than 10 kV ×: Breakdown voltage is less than 5 kV
[0068] (Thermal Conductivity) The thermal resistance of the heat dissipation sheet was evaluated based on the measured value in accordance with the method described in ASTM D5470:2017. The evaluation criteria for thermal conductivity are as follows: ◎: Thermal conductivity is 5W / (m K) or more ○: Thermal conductivity is 3W / (m K) or more and less than 5W / (m K) ×: Thermal conductivity is less than 3W / (m K)
[0069] (Production of boron nitride powder with one maximum point) Boron nitride powders A to L each having one maximum point, which serve as raw materials for boron nitride powder having multiple maximum points, were prepared as follows.
[0070] (Boron nitride powder A) Boron nitride powder A was produced through the following steps: boron carbide synthesis, pressure nitridation process, and decarburization crystallization process.
[0071] (Boron carbide synthesis) 100 parts by mass of orthoboric acid (hereinafter referred to as boric acid) manufactured by Nippon Denko Co., Ltd. and 35 parts by mass of acetylene black (HS100) manufactured by Denka Co., Ltd. were mixed using a Henschel mixer, then charged into a graphite crucible and heated in an arc furnace in an argon atmosphere at 2200°C for 5 hours to synthesize boron carbide (B4C). The synthesized boron carbide block was pulverized in a ball mill for 1 hour, sieved using a sieve to particles of 75 μm or less, and further washed with an aqueous nitric acid solution to remove impurities such as iron, and then filtered and dried to produce boron carbide powder with an average particle size of 4 μm.
[0072] (Pressure nitriding process) The synthesized boron carbide was loaded into a boron nitride crucible and then heated in a resistance heating furnace at 2000°C and 9 atm (0.8 MPa) for 10 hours in a nitrogen gas atmosphere to obtain boron carbonitride (B4CN4).
[0073] (Decarburization crystallization process) 100 parts by mass of the synthesized boron carbonitride and 90 parts by mass of boric acid were mixed using a Henschel mixer, then filled into a boron nitride crucible, and heated in a nitrogen gas atmosphere at a pressure of 0.2 MPa using a resistance heating furnace at a heating rate of 10 ° C / min from room temperature to 1000 ° C, and a heating rate of 2 ° C / min from 1000 ° C, and heated at a firing temperature of 2020 ° C, and held for 10 hours to synthesize aggregated boron nitride particles in which primary particles were aggregated into lumps. The synthesized aggregated boron nitride particles were decomposed and crushed in a Henschel mixer, and then classified using a nylon sieve with a mesh size of 150 μm. Boron nitride powder A was obtained by crushing and classifying the fired product.
[0074] The average particle size (D50) of the obtained boron nitride powder A measured by a laser scattering method was 4.5 μm. As a result of SEM observation, the obtained boron nitride powder A was found to be scaly particles.
[0075] (Boron nitride powder B) Boron nitride powder B was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 6 μm was used. The average particle size (D50) of the obtained boron nitride powder B measured by laser scattering method was 8 μm. SEM observation showed that the obtained boron nitride powder B was a scaly particle.
[0076] (Boron nitride powder C) Boron nitride powder C was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 1 μm was used. The average particle size (D50) of the obtained boron nitride powder C measured by a laser scattering method was 1 μm. SEM observation revealed that the obtained boron nitride powder C was a scaly particle.
[0077] (Boron nitride powder D) Boron nitride powder D was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 15 μm was used. The average particle size (D50) of the obtained boron nitride powder D measured by a laser scattering method was 23 μm. SEM observation revealed that the obtained boron nitride powder D was an aggregated particle formed by agglomeration of primary particles.
[0078] (Boron nitride powder E) Boron nitride powder E was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 10 μm was used. The average particle size (D50) of the obtained boron nitride powder E measured by a laser scattering method was 15 μm. SEM observation revealed that the obtained boron nitride powder E was an aggregated particle formed by agglomeration of primary particles.
[0079] (Boron nitride powder F) Boron nitride powder F was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 25 μm was used. The average particle size (D50) of the obtained boron nitride powder F measured by a laser scattering method was 35 μm. SEM observation revealed that the obtained boron nitride powder F was an aggregated particle formed by agglomeration of primary particles.
[0080] (Boron nitride powder G) Boron nitride powder G was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 12 μm was used. The average particle size (D50) of the obtained boron nitride powder G measured by a laser scattering method was 18 μm. SEM observation revealed that the obtained boron nitride powder G was an aggregated particle formed by agglomeration of primary particles.
[0081] (Boron nitride powder H) Boron nitride powder H was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 55 μm was used. The average particle size (D50) of the obtained boron nitride powder H measured by a laser scattering method was 78 μm. SEM observation showed that the obtained boron nitride powder H was an agglomerated particle formed by agglomeration of primary particles. The half-width of the peak of the particle size distribution of boron nitride powder H was 46 μm.
[0082] (Boron nitride powder I) Boron nitride powder I was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 70 μm was used. The average particle size (D50) of the obtained boron nitride powder I measured by a laser scattering method was 95 μm. SEM observation showed that the obtained boron nitride powder I was an agglomerated particle formed by agglomeration of primary particles. The half-width of the peak of the particle size distribution of boron nitride powder I was 53 μm.
[0083] (Boron nitride powder J) Boron nitride powder J was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 40 μm was used. The average particle size (D50) of the obtained boron nitride powder J measured by laser scattering method was 55 μm. SEM observation showed that the obtained boron nitride powder J was an agglomerated particle formed by agglomeration of primary particles. The half-width of the peak of the particle size distribution of boron nitride powder J was 28 μm.
[0084] (Boron nitride powder K) Boron nitride powder J was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 65 μm was used. The average particle size (D50) of the obtained boron nitride powder J measured by a laser scattering method was 82 μm. SEM observation showed that the obtained boron nitride powder K was an agglomerated particle formed by agglomeration of primary particles. The half-width of the peak of the particle size distribution of boron nitride powder K was 45 μm.
[0085] (Boron nitride powder L) Boron nitride powder L was produced in the same manner as boron nitride powder A, except that boron carbide powder with an average particle size of 50 μm was used. The average particle size (D50) of the obtained boron nitride powder L measured by a laser scattering method was 73 μm. As a result of SEM observation, the obtained boron nitride powder L was an aggregated particle formed by agglomeration of primary particles. The half-width of the peak of the particle size distribution of boron nitride powder L was 48 μm.
[0086] Examples 1 to 8 Boron nitride powders were blended as shown in Table 1 to prepare a boron nitride mixture, which was then subjected to the following surface treatment. Heat dissipation sheets were then produced as shown below and the above evaluations were carried out. The evaluation results are shown in Table 2.
[0087] (Surface treatment) A silane coupling agent shown in Table 1 was added to 100 parts by mass of boron nitride powder (mixture) in the amount shown in Table 1, dry mixed for 0.5 hours, and then passed through a 75 μm sieve to obtain a surface-treated boron nitride powder.
[0088] (Making heat dissipation sheets) The boron nitride powder and liquid silicone resin (methylvinylpolysiloxane, Dow Toray Co., Ltd., product name "CF-3110") obtained were mixed with 60% by volume of boron nitride powder and 40% by volume of silicone resin 1, 1 part by mass of curing agent (2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, Kayaku Nouryon Co., Ltd., product name "Trigonox 101") per 100 parts by mass of silicone resin, and 0.5 parts by mass of silane coupling agent (dimethyldimethoxysilane, Dow Toray Co., Ltd., product name "DOWSIL Z-6329") per 100 parts by mass of boron nitride powder. Silane, viscosity at 25°C: 1 cp), 15 parts by mass of water per 100 parts by mass of the silane coupling agent, and 110 parts by mass of toluene per 100 parts by mass of the above-mentioned raw materials were charged into a mixer (manufactured by HEIDON, product name "Three-One Motor") and mixed for 15 hours using a turbine-type mixing blade to prepare a slurry of a thermally conductive resin composition. The slurry was then coated on a 0.05 mm thick PET film (carrier film) to a thickness of 1.2 mm by a doctor blade method and dried at 75°C for 5 minutes to produce a sheet-like molded product with a PET film. A 0.05 mm thick PET film was laminated on the thermally conductive resin composition surface of the sheet-like molded product with the PET film to produce a laminate. The layer structure of this laminate was PET film / thermally conductive resin composition / PET film. Next, the obtained laminate was subjected to a vacuum (pressure 3.5 kPa), temperature 150°C, and pressure 160 kg / cm. 2 The PET film on both sides was peeled off to obtain a sheet with a thickness of 1.0 mm. This was then subjected to secondary heating at normal pressure and 150°C for 4 hours to obtain a heat dissipation sheet.
[0089] Comparative Example 1 A boron nitride powder and a heat dissipation sheet were obtained in the same manner as in Example 1, except that the surface treatment with a silane coupling agent having a vinyl group was not carried out in Example 1. The evaluation results are shown in Table 2.
[0090] [Table 1]
[0091] Vinyl group-containing silane coupling agent A: Tokyo Chemical Industry Co., Ltd., product name "T3359", 7-oct-1-enyltrimethoxysilane Vinyl group-containing silane coupling agent B: Evonik, trade name "Dynasylan VTMOEO", vinyltris(2-methoxyethoxy)silane Vinyl-containing silane coupling agent C: Wacker, product name "GENIOSIL XL 12", vinyldimethoxymethylsilane
[0092] [Table 2]
[0093] From the evaluation results of the heat dissipation sheets of the examples and the comparative examples, it was found that by performing surface treatment with a silane coupling agent having a vinyl group, both the insulation properties and thermal conductivity of the heat dissipation sheet were improved. It was also found that the insulating properties and thermal conductivity of the heat dissipation sheet can be further improved by setting the ratio of the intensity of the infrared absorption peak derived from vinyl groups to the intensity of the infrared absorption peak derived from boron nitride within a specific range, and by controlling the particle size distribution of the boron nitride powder that constitutes the heat dissipation sheet within a specific range.
Claims
1. A boron nitride powder containing at least aggregated boron nitride particles formed by agglomeration of hexagonal boron nitride primary particles, which contains a vinyl group-containing silane coupling agent and has an infrared absorption peak (3076 cm) derived from the vinyl group. -1 ±2cm -1 ) and the infrared absorption peak (1377 cm ) due to boron nitride -1 ±2cm -1 a ratio ((Ia / Ib)×100) of an intensity Ib of the boron nitride powder to an intensity Ib of the boron nitride powder is in the range of 0.1 to 10, and the particle size distribution of the boron nitride powder has at least a first maximum point, a second maximum point having a particle size larger than that of the first maximum point, and a third maximum point having a particle size larger than that of the second maximum point; The particle size at the first maximum point is 0.4 μm or more and less than 10 μm, The particle size at the second maximum point is 10 μm or more and less than 40 μm, The particle size at the third maximum point is 40 μm or more and 110 μm or less, The boron nitride powder has an absolute value of 3 to 30 μm between a particle size at which the integrated amount of frequency in the particle size distribution of the boron nitride powder is 10% and a particle size of a minimum point between the smallest maximum point and the second smallest maximum point in the particle size distribution of the boron nitride powder.
2. A boron nitride powder comprising at least aggregated boron nitride particles formed by the aggregation of hexagonal boron nitride primary particles, comprising a vinyl group-containing silane coupling agent, wherein the ratio ((Ia / Ib)×100) of the intensity Ia of the infrared absorption peak (3076 cm −1 ±2 cm −1 ) derived from the vinyl groups to the intensity Ib of the infrared absorption peak (1377 cm −1 ±2 cm −1 ) derived from boron nitride is in the range of 0.1 to 10, and the particle size distribution of the boron nitride powder has at least a first maximum point, a second maximum point having a particle size larger than the first maximum point, and a third maximum point having a particle size larger than the second maximum point, The particle size at the first maximum point is 0.4 μm or more and less than 10 μm, The particle size at the second maximum point is 10 μm or more and less than 40 μm, The particle size at the third maximum point is 40 μm or more and 110 μm or less, a maximum point adjacent to the first maximum point is the second maximum point, a maximum point adjacent to the second maximum point is the third maximum point, and an absolute value of a difference between a particle size of a first minimum point between the first maximum point and the second maximum point and a particle size of a second minimum point between the second maximum point and the third maximum point is 15 to 60 μm.
3. A boron nitride powder comprising at least aggregated boron nitride particles formed by the aggregation of hexagonal boron nitride primary particles, comprising a vinyl group-containing silane coupling agent, wherein the ratio ((Ia / Ib) x 100) of the intensity Ia of the infrared absorption peak (3076 cm -1 ±2 cm -1 ) derived from the vinyl groups to the intensity Ib of the infrared absorption peak (1377 cm -1 ±2 cm -1 ) derived from boron nitride is in the range of 0.1 to 10, and the particle size distribution of the boron nitride powder has at least a first maximum point, a second maximum point having a particle size larger than the first maximum point, and a third maximum point having a particle size larger than the second maximum point, The particle size at the first maximum point is 0.4 μm or more and less than 10 μm, The particle size at the second maximum point is 10 μm or more and less than 40 μm, The particle size at the third maximum point is 40 μm or more and 110 μm or less, The boron nitride powder has a half-width of the peak having the third maximum point of 20 to 60 μm.
4. The boron nitride powder according to any one of claims 1 to 3, wherein the agglomerated boron nitride particles have a crushing strength of 5 to 18 MPa.
5. A thermally conductive resin composition comprising the boron nitride powder according to any one of claims 1 to 4.
6. A heat dissipation sheet obtained by molding the thermally conductive resin composition according to claim 5.
7. 7. An electronic component structure comprising the heat dissipation sheet according to claim 6 attached to an electronic component via grease.
Citation Information
Patent Citations
Hexagonal boron nitride powder and high heat conductivity and high moisture resistance heat radiation sheet using the same
JP2012056818A
Resin composition and method for producing the same
JP2016108457A
Hexagonal boron nitride primary particle agglomerate
JP2018052782A
Boron nitride powder and resin composition
JP2020164365A
Boron nitride aggregated particles, thermal conductive resin composition, and heat dissipation member
WO2020196643A1