Organotin copolymers as polymer crosslinking catalysts
The (meth)acrylic copolymer with tin-containing side chains and ester groups addresses the challenges of catalyst systems by providing a stable, low-temperature bake coating with uniform catalyst distribution and extended pot life through chemical encapsulation.
Patent Information
- Application Number
- JP2021527810
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-22
- Filing Date
- 2019-11-22
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2039-11-22
AI Technical Summary
Existing catalyst systems for crosslinking reactions in coating compositions, particularly hydroxyl/isocyanate reactions, face challenges in achieving a balance between reactivity and stability, leading to inconsistent pot life and curing rates, and often result in non-uniform catalyst distribution and insufficient temperature reduction.
Development of a (meth)acrylic copolymer with a polymer main chain and two types of side chains, one containing a tin-containing moiety and the other an ester group, allowing for controlled catalyst release through chemical encapsulation, ensuring uniform distribution and predictable activity.
The copolymer system provides a stable, low-temperature bake coating with extended pot life and uniform catalyst delivery, overcoming the limitations of physical absorption-desorption methods by ensuring catalysts are encapsulated until the desired release temperature is reached, thereby maintaining performance and reducing toxicity.
Smart Images

Figure 0007580374000001 
Figure 0007580374000002 
Figure 0007580374000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymeric polymer having a polymer backbone and at least two different side chains (S1) and (S2) attached to the polymer backbone, i.e., one or more side chains (S1) containing at least one tin-containing moiety and one or more side chains of the formula -OC(=O)-R 1 (In the formula, R 1 and one or more side chains (S2) carrying at least one ester group of a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), a method for making said copolymer, a method for using said copolymer as a catalyst for a crosslinking reaction in a coating composition and / or for increasing the pot life of a coating composition and / or for reducing the curing temperature of a coating composition, a coating composition comprising said copolymer, and a method for coating a substrate comprising the step of applying said coating composition to a substrate. [Background technology]
[0002] In today's efforts to lighten vehicles to reduce emissions and fuel consumption, automotive original equipment manufacturers (OEMs) are increasingly using lighter materials, including aluminum, magnesium, and polymer substrates. For polymer substrates, lower curing temperatures are required because the substrates typically deform at standard bake temperatures applied to metal substrates. The use of catalysts has emerged as a viable approach to provide lower temperature curing, as the desired crosslinking reaction of the coating composition proceeds at such low temperatures.
[0003] However, there are drawbacks associated with the use of catalysts. Standard tin catalysts, such as dibutyltin dilaurate, which is widely used especially in 2K automotive coatings as a catalyst for isocyanate / hydroxyl crosslinking reactions, only provide acceptable fast cure speeds and sufficient end-product properties at levels that result in short application time windows. Due to the genetic shortcomings of the catalysts, it seems very difficult to achieve a working balance between reactivity and stability in the crosslinking reaction by simply manipulating the amount of catalyst.
[0004] To avoid the shortcomings of prior art catalysts, such as conventional tin catalysts, such as organotin compounds and / or tin salts, catalyst encapsulation has become a very promising solution, because successful catalyst encapsulation allows the catalyst to be delivered in a controlled manner to avoid premature degradation of the coating composition containing the catalyst. Many such systems use polymeric carriers to physically absorb-desorb the catalyst used. Depending on the properties of the carrier, some systems can even control the release of the catalyst when shear forces are applied to the carrier. Prior art encapsulation systems are disclosed, for example, in US2015 / 132592A1A1, US2015 / 133595A1A1 and US2016 / 090455A1. US2015 / 132592A1A1 relates to coating compositions containing a film-forming resin and a catalyst, such as a tin catalyst, such as dibutyltin dilaurate, contained within or encapsulated by a carrier, with the aim of providing control of the cure rate and improved pot life of the coating system at ambient temperature. The catalyst may be released when applying shear forces to cure. US2015 / 133595A1A1 discloses catalysts such as organotin compounds, e.g. dibutyltin dilaurate, which are encapsulated in polymers prepared from ethylenically unsaturated monomers and can be used in water-based coating systems. The document aims to accelerate the cure rate and extend the pot life for coating systems. Finally, US2016 / 090455A1 relates to a composition comprising a thermosetting resin and polymer nanoparticles, which releases a catalyst during the curing process, among other things. The document aims to allow low cure temperatures, short cure times and at the same time long out times.
[0005] However, a drawback of these encapsulated systems, such as those disclosed in US2015 / 132592A1A1, US2015 / 133595A1A1 and US2016 / 090455A1, is that they rely on a physical absorption-desorption process, which often results in the fact that the desired uniform distribution of the catalyst throughout the system is not always observed. Furthermore, the pot life and / or the cure speed are not always satisfactory and / or the reduction of the cure temperature is not always achievable to a sufficient extent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] US2015 / 132592A1A1 [Patent Document 2] US2015 / 133595A1A1 [Patent Document 3] US2016 / 090455A1 Summary of the Invention [Problem to be solved by the invention]
[0007] The object underlying the present invention was therefore to provide a catalyst useful for crosslinking reactions, particularly hydroxyl / isocyanate crosslinking reactions, in coating compositions, which does not exhibit the aforementioned drawbacks of the prior art catalyst systems. In particular, the object underlying the present invention was to provide such a catalyst, when used in coating compositions, which not only allows control of the catalytic activity, but also provides these compositions with an improved pot life and uniform distribution of the catalyst therein. [Means for solving the problem]
[0008] This object has been solved by the subject matter of the present application and by the preferred embodiments thereof disclosed herein, namely the subject matter described herein.
[0009] A first subject of the present invention is therefore a (meth)acrylic copolymer, which comprises a polymer backbone and at least two different side chains (S1) and (S2) attached to said polymer backbone, i.e. one or more side chains (S1) containing at least one tin-containing moiety, i.e., an organotin moiety; and, Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) with at least one ester group (S2) Includes:
[0010] A further subject of the present invention is a process for the preparation of the inventive (meth)acrylic copolymers, comprising at least one step, in which (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), and optionally, (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form a copolymer, or (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form a copolymer, followed by a polymer-analogous reaction in which at least one functional group of the structural unit resulting from at least one monomer (s2) is converted into a functional group of the formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) to at least one ester group of
[0011] A further subject of the present invention is the use of the inventive (meth)acrylic copolymers as catalysts, in particular as encapsulated catalysts, in crosslinking reactions in coating compositions and / or for increasing the pot life of coating compositions and / or for reducing the curing temperature of coating compositions.
[0012] A further subject of the present invention is a coating composition comprising at least one polymer as binder component (a) and at least one inventive (meth)acrylic as component (b), where the polymer of binder component (a) is different from the (meth)acrylic copolymer of component (b).
[0013] A further subject is a method for coating a substrate, comprising at least one step (1), namely, (1) applying to the substrate a coating composition according to the invention containing a copolymer according to the invention.
[0014] Surprisingly, it has been found that by providing the copolymers of the present invention, a new catalyst encapsulation system can be established, which utilizes chemical reactions to incorporate tin catalytic sites into the copolymer, and which is very special compared to the purely physical absorption-desorption based catalyst encapsulation systems of the prior art.
[0015] Moreover, it has been surprisingly found that the side chains (S2) on the copolymers of the present invention help to maintain the copolymers immiscible in hydrocarbon solvents within a certain temperature range, for example from room temperature (18° C.) to the upper critical solution temperature (UCST). In other words, due to the presence of these side chains (S2), the organotin moieties present in the side chains (S1) of the copolymers of the present invention are surprisingly present in an encapsulated state. A controlled release of the catalyst from this encapsulated state can be achieved as soon as said UCST is reached, since the copolymers of the present invention become fully miscible and their tin-containing moieties for use as catalytic moieties are free to interact with the functional moieties of interest in the coating composition to be crosslinked. The advantages of this system are, among others, that a coating composition with a long pot life is provided, but also that the performance of the catalyst, i.e. the tin-containing moieties of the copolymers of the present invention, can be controlled at the selected application temperature, without adversely affecting the catalytic performance at the application temperature. As a result, a stable low-bake coating system can be reached. In particular, it has been surprisingly found that this unexpected effect occurs when the copolymer of the present invention is incorporated into a coating composition, such as an organic solvent(s) based coating composition. A good dispersion of the copolymer in a solvent such as a solvent naphtha and / or toluene mixture at room temperature (18°C) results in a uniform distribution of the copolymer throughout the solution, ensuring good encapsulation by maintaining phase separation. Upon heating, particularly to 55-60°C, the copolymer dispersion becomes a fully miscible solution, releasing the catalyst and allowing each catalytic site of the copolymer of the present invention to freely interact with the functional groups of interest in the coating composition. In particular, the release temperature range of 55-60°C is ideal, as it is high enough to overcome the storage temperatures of typical coating compositions, yet low enough to release the catalyst before the bake temperature is reached.
[0016] Thus, it has been further surprisingly found that, in contrast to the physical absorption-desorption processes of prior art encapsulated catalyst systems, the copolymers of the present invention distribute the tin-containing catalytic sites much more uniformly throughout the system, making the catalytic activity of the tin within these sites expected to be more predictable and allowing for a more uniform delivery of catalyst.
[0017] The preparation of the copolymers of the invention for use as catalysts can also benefit from their chemical modification, which is the result of the presence of one or more side chains, since the preparation process is much easier to reproduce.
[0018] Finally, it has been surprisingly found that in copolymers having tin-containing structural units derived from monomers derived from dibutyltin oxide, a trend towards reduced toxicity is observed relative to structural units derived from monomers derived from dioctyltin oxide. Thus, the use of longer alkyl chains in the tin-containing structural units of the copolymers of the invention can limit and in particular reduce toxicity. This can provide a "greener" catalytic system and thus enable more sustainable chemistry. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Copolymer The (meth)acrylic copolymer of the present invention comprises a polymer backbone and at least two different side chains (S1) and (S2) attached to the polymer backbone, i.e., one or more side chains (S1) containing at least one tin-containing moiety and one or more side chains of the formula -OC(=O)-R 1 (In the formula, R 1 and one or more side chains (S2) carrying at least one ester group of a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms.
[0020] The (meth)acrylic copolymer according to the invention is herein also called "copolymer according to the (present) invention" or "copolymer of the present invention" or "(meth)acrylic copolymer of the present invention".
[0021] The term "(meth)acrylic" means "acrylic" and / or "methacrylic". Similarly, "(meth)acrylate" means acrylate and / or methacrylate. Thus, a "(meth)acrylic copolymer" may generally be formed only from "acrylic monomers", only from "methacrylic monomers", or both from "acrylic and methacrylic monomers". However, an ethylenically unsaturated monomer other than an acrylic monomer and / or a methacrylic monomer, such as styrene, may also be additionally contained in the "(meth)acrylic copolymer". In other words, a (meth)acrylic copolymer may be, but is not necessarily, composed of only acrylic and / or methacrylic monomer units. Preferably, the backbone of the (meth)acrylic copolymer is formed from more than 50 mol%, even more preferably more than 75 mol%, particularly 100 mol% of (meth)acrylic monomers.
[0022] The (meth)acrylic copolymer of the present invention contains at least two different structural units (SU1) and (SU2). The structural unit (SU1) contains at least one side chain (S1) and is prepared using at least one monomer (s1), which is suitable for introducing at least one side chain (S1) into the copolymer and for forming the structural unit (SU1) therein. The structural unit (SU2) contains at least one side chain (S2) and is prepared using at least one monomer (s2), which is suitable for introducing at least one side chain (S2) into the copolymer and for forming the structural unit (SU2) therein during the polymerization or in a subsequent polymer-analogous reaction. The copolymer of the present invention may further contain at least one additional structural unit (SU3) containing at least one side chain (S3) and prepared using at least one monomer (s3). This monomer is suitable for introducing at least one side chain (S3) into the copolymer and for forming the structural unit (SU3) within the copolymer.
[0023] Preferably, the amount (mol %) of structural unit (SU1) in the copolymer of the present invention is greater than the amount (mol %) of structural unit (SU2) in the copolymer of the present invention.
[0024] Preferably, the relative molar ratio of the at least one structural unit (SU1) to the at least one structural unit (SU2) in the (meth)acrylic copolymer is in the range of from 20:1 to 1:5, more preferably in the range of from 15:1 to 1:2.5, even more preferably in the range of from 12:1 to 1:1, even more preferably in the range of from 10:1 to 1:1, in particular in the range of from 2:1 to 1:1.
[0025] Preferably, the amount of structural units (SU1) in the (meth)acrylic copolymer is at least 15 mol%, more preferably at least 20 mol%, even more preferably at least 25 mol%, or at least 30 mol%, even more preferably at least 35 mol%, in particular at least 40 mol%, in each case based on the total amount of all structural units of the copolymer.
[0026] Preferably, the amount of structural units (SU2) in the (meth)acrylic copolymer is at least 5 mol %, more preferably at least 10 mol %, even more preferably at least 15 mol % and in particular at least 20 mol %, in each case based on the total amount of all structural units of the copolymer.
[0027] Preferably, the amount of the optional structural unit (SU3) in the (meth)acrylic copolymer is at least 5 mol %, more preferably at least 10 mol %, even more preferably at least 20 mol %, in particular at least 40 mol %, in each case based on the total amount of all structural units of the copolymer.
[0028] Preferably, the copolymer according to the invention has the following molar percentages, based on the total amount of the at least two structural units (SU1) and (SU2) and, optionally, at least one further structure (SU3): 10 to 70 mol %, preferably 20 to 60 mol %, more preferably 30 to 50 mol % of the structural unit (SU1); 10 to 40 mol %, preferably 10 to 35 mol %, more preferably 10 to 30 mol % of structural units (SU2), and 0 to 60 mol %, preferably 5 or 10 or 15 to 60 mol %, more preferably 30 to 50 mol % of the structural unit (SU3) Contains:
[0029] Here, it is clear to the skilled person that the total content of the at least two structural units (SU1) and (SU2) and optionally at least one further structure (SU3) in the copolymers according to the invention in each case amounts to 100 mol %.
[0030] Preferably, the (meth)acrylic copolymer of the present invention has a mass average molecular weight (M) in the range of 1,000 to 200,000 g / mol, more preferably in the range of 1,000 to 100,000 g / mol, even more preferably in the range of 1,500 to 50,000 g / mol, even more preferably in the range of 2,000 to 20,000 g / mol, and even more preferably in the range of 2,000 to 15,000 g / mol. w ).
[0031] The weight average molecular weight of the copolymers used in the present invention is determined by the method described below ("Test Method"), namely, by GPC using polystyrene standards and THF as eluent.
[0032] Preferably, the copolymers of the present invention are non-ionic copolymers and do not contain any ionic groups, such as, for example, ammonium salt groups. Preferably, the (meth)acrylic copolymers of the present invention do not contain any acidic groups, in particular any carboxylic acid groups, either in free form or in salt form.
[0033] The polymerization reaction for preparing the copolymers of the present invention can be carried out by any method known in the literature, such as free radical polymerization, controlled / living radical polymerization, ionic polymerization, or group transfer polymerization. It is well known that the average molecular weight and its distribution of the copolymers of the present invention can be controlled by using chain transfer agents or by utilizing controlled / living polymerization techniques. Branched or star-shaped structures can be obtained, for example, by using bifunctional or higher functional comonomers during the copolymerization and / or by utilizing multifunctional initiators and / or multifunctional chain transfer agents. Free radical polymerization is preferred. Preferably, at least two ethylenically unsaturated monomers different from each other are used. Each of these monomers contains at least one, preferably exactly one, terminal ethylenically unsaturated group, i.e. at least one monomer (s1) and at least one monomer (s2).
[0034] Preferably, the copolymer of the present invention is a random copolymer or a structured copolymer. Structured copolymers are, for example, block copolymers, such as linear block copolymers, branched block copolymers, star block copolymers, gradient copolymers and comb copolymers. Thus, the copolymers used in the present invention may have a random arrangement, or a gradient arrangement or a block arrangement of copolymerized structural units derived from suitable ethylenically unsaturated monomers.
[0035] In particular, the copolymers of the present invention have a random arrangement of copolymerized structural units. The structure of the copolymers of the present invention is preferably linear or branched, in particular linear.
[0036] Side Chain(s) (S1) One or more of the side chains (S1) comprises at least one tin-containing moiety, said tin-containing moiety being an organotin-containing moiety.
[0037] Tin-containing polymers are generally known from the prior art. For example, a diblock copolymer made from methyl methacrylate and acetyl dibutyltin methacrylate and a study of the morphology of this copolymer are disclosed in Lei et al., J. Organomet. Chem. 2011, 696, 14116-1424. Tin-containing copolymers obtained by polymerization of tributyltin methacrylate with different lower alkyl methacrylates are known from Ghanem et al., European Polymer 1979, 15, 823-826. Furthermore, copolymers made from styrene, butyl acrylate and one of dibutyl citraconate and dibutyl maleate are disclosed in Al-Deyab et al., Molecules 2010, 15, 1784-1797.
[0038] Preferably, one or more side chains (S1) are of the substructure (PS1) [ka] It is expressed as During the ceremony, symbol [ka] indicates the covalent bond of the substructure (PS1) to the main chain of the copolymer, The parameter a is 0 or 1, and R 2 , R 3 and R 4 represent, independently of each other, a linear saturated alkyl group having 1 to 30 carbon atoms, a branched saturated alkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an alkylaryl group or arylalkyl group in each case having 7 to 30 carbon atoms.
[0039] Preferably, the parameter a is 1 and R 2 , R 3 and R 4 each independently represents a linear saturated alkyl group having 1 to 20 carbon atoms, or a branched saturated alkyl group having 3 to 20 carbon atoms.
[0040] More preferably, the parameter a is 1 and R 2 represents a linear saturated alkyl group having 1 to 8, in particular 1 to 6 or 2 to 4, carbon atoms, and R 3 and R 4 are each independently a linear saturated alkyl group having 1 to 8, in particular 1 to 6 or 2 to 4 carbon atoms. 2 The number of carbon atoms in R 3 and R 4 fewer than the number of carbon atoms in
[0041] Examples of monomers (monomers (s1)) suitable for constructing the polymer backbone of the copolymer of the present invention and incorporating one or more side chains (S1) are lauryl dibutyltin (meth)acrylate, acetyl dibutyltin (meth)acrylate and acetyl dioctyltin (meth)acrylate. Particularly preferred are acetyl dibutyltin (meth)acrylate and acetyl dioctyltin (meth)acrylate. Particularly preferred are acetyl dioctyltin (meth)acrylate in terms of toxicity.
[0042] Side Chain(s) (S2) One or more side chains (S2) are of the formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) containing at least one ester group. Preferably, one or more of the side chains (S2) further contains at least one hydroxyl group.
[0043] Preferably, the radical R 1 is a linear or branched, saturated or unsaturated acyclic aliphatic residue having 18 to 65 carbon atoms, more preferably 18 to 60, even more preferably 19 to 58, even more preferably 20 to 56, and particularly preferably 25 to 55 carbon atoms.
[0044] residue R 1 is preferably an aliphatic residue of a fatty acid, such as a primary carboxylic fatty acid. The term "fatty acid" refers to an aliphatic C 19 ~C 65 Monocarboxylic acids, preferably aliphatic C having a total of 19 to 60 carbon atoms 19 ~C 60 Monocarboxylic acids, more preferably aliphatic C having a total of 20 to 58 carbon atoms 20 -C 58 Monocarboxylic acids, especially aliphatic C having a total of 22 to 56 carbon atoms 22 -C 56It particularly refers to monocarboxylic acids, each having exactly one -C(=O)-OH group in each case. Here, the expression "aliphatic" encompasses acyclic saturated or unsaturated, preferably unsaturated, branched or unbranched (straight-chain) aliphatic radicals. Here, unsaturated aliphatic radicals have at least one, preferably 1, 2, 3, 4 or 5, more preferably 1, 2, 3 or 4, very preferably 1, 2 or 3 carbon double bond(s). The fatty acids may be natural or synthetically produced fatty acids. Exemplary fatty acids include nonadecanoic acid, arachidic acid, heneicosanoic acid, docosanoic acid, gadoleic acid, icosenoic acid, cetylene acid, erucacic acid, arachidonic acid, timnodonic acid, clupanodonic acid, cervonic acid, hexadecatrienoic acid, rumellic acid, α-parinaric acid, β-parinaric acid, eicosatrienoic acid, eicosatetraenoic acid, eicosapentaenoic acid, heneicosapentaenoic acid, docosapentaenoic acid, and docosapentaenoic acid. Selected from the group consisting of hexaenoic acid, tetracosapentaenoic acid, tetracosahexaenoic acid (nisinic acid), eicosadienoic acid, podocarpic acid, bosseopentaenoic acid, docosadienoic acid, docosatetraenoic acid, docosapentaenoic acid, tetracosatetraenoic acid, tetracosapentaenoic acid, rumenic acid, paulic acid, 15-docosenoic acid, 17-tetracosenoic acid, gondonic acid, meadic acid, erucic acid and nervonic acid.
[0045] Preferably, one or more side chains (S2) are of the substructure (PS2) [ka] It is expressed as During the ceremony, symbol [ka] indicates the covalent bond of the substructure (PS2) to the main chain of the copolymer, Parameter b is 0 or 1; The parameter c is in the range of 2 to 20. R 1 has the meaning defined hereinabove, Each R5 independently represent hydrogen, hydroxyl, a linear saturated alkyl group having 1 to 30 carbon atoms, or a branched saturated alkyl group having 3 to 30 carbon atoms, and Each R 6 each independently represents a hydrogen atom, a linear saturated alkyl group having 1 to 30 carbon atoms, or a branched saturated alkyl group having 3 to 30 carbon atoms.
[0046] Preferably, parameter b is 1, parameter c is in the range of 2 to 10, in particular 2 to 8 or 2 to 6, most preferably 3, and each R 5 represents hydrogen or hydroxyl, more preferably the radical R 5 One of the radicals represents hydroxyl, the remaining radicals represent hydrogen, and each R 6 represents hydrogen.
[0047] Examples of monomers (monomers (s2)) suitable for constructing the polymer backbone of the copolymers of the invention and for incorporating one or more side chains (S2) are reaction products of epoxide-functional (meth)acrylates, such as glycidyl (meth)acrylate, with monobasic carboxylic acids having a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 and especially 18 to 60 carbon atoms. Alternatively, glycidyl (meth)acrylate can be used itself as monomer (s2) and, after forming the copolymer in a polymer-analogous reaction, esterification can be carried out with a monobasic carboxylic acid having a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 or 18 to 60 carbon atoms, using a suitable base, such as dimethylethanolamine, as catalyst.
[0048] Alternatively, instead of epoxide-functional (meth)acrylates such as glycidyl (meth)acrylate, simply OH-functional monomers can be used. In that case, the OH group of such monomers can be subsequently subjected to esterification with monovalent carboxylic acids having a linear or branched, saturated or unsaturated acyclic aliphatic residue having at least 8 or 8 to 40 carbon atoms. Examples of such monomers (s2) are 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 3-phenoxy-2-hydroxypropyl (meth)acrylate, glycerol mono(meth)acrylate, N-(2-hydroxypropyl)(meth)acrylamide, allyl alcohol, hydroxystyrene, hydroxyalkyl vinyl ethers such as hydroxybutyl vinyl ether and vinylbenzyl alcohol.
[0049] The monovalent carboxylic acid used in the present invention is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 8 or 8 to 40 carbon atoms, for example the commercially available product Unicid (registered trademark) 350.
[0050] Optional further side chain(s) (S3) Preferably, the copolymer of the present invention has at least one further side chain (S3) attached to its polymer backbone, which is different from both side chains (S1) and (S2), i.e. Partial structure (PS3) [ka] and having one or more side chains (S3) represented by In the formula, R 7 represents a linear saturated alkyl group having 1 to 30 carbon atoms, a branched saturated alkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an alkylaryl or arylalkyl group in each case having 7 to 30 carbon atoms.
[0051] Examples of monomers (monomers (s3)) suitable for constructing the polymer backbone of the copolymer of the invention and for incorporating one or more side chains (S3) are aliphatic C1-C 30 (Meth)acrylic acid esters of monoalcohols, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl acrylate, n-butyl methacrylate, i-butyl acrylate, i-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, lauryl acrylate, lauryl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, stearyl acrylate, stearyl methacrylate, behenyl acrylate, behenyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, isobornyl acrylate and isobornyl methacrylate. Aromatic C6-C 30 An example of the monomer (s3) which is a (meth)acrylic acid ester of a monoalcohol is phenyl (meth)acrylate. 30 Examples of monomers (s3) which are (meth)acrylic acid esters of monoalcohols are benzyl acrylate and benzyl methacrylate. Particularly preferred are aliphatic C8-C 25 - (meth)acrylic acid esters of monoalcohols, most preferably aliphatic C8-C 18 - (meth)acrylic acid esters of monoalcohols. Preferred monomers are n-butyl acrylate, n-butyl methacrylate, lauryl acrylate, lauryl methacrylate, 2-ethylhexyl acrylate and 2-ethylhexyl methacrylate. Most preferred are lauryl acrylate, lauryl methacrylate, 2-ethylhexyl acrylate and 2-ethylhexyl methacrylate.
[0052] It is also possible to use other ethylenically unsaturated monomers as monomers (s3) for constructing the polymer backbone of the copolymer of the invention and incorporating one or more side chains (S3), namely monomers having at least one amino group, such as N,N-dimethylaminoethyl acrylate, N,N-dimethylaminoethyl methacrylate, N,N-dimethylaminopropyl acrylate, N,N-dimethylaminopropyl methacrylate, 2-(N,N-diethylamino)ethyl (meth)acrylate, 2-(N,N-dimethylamino)ethyl (meth)acrylate, N-[3-(N,N-dimethylamino)propyl](meth)acrylamide, 3-dimethylaminoneopentyl (meth)acrylate, 2-N-morpholinoethyl (meth)acrylate, N-[3 -(N,N-dimethylamino)propyl](meth)acrylamide, 2-(N,N-diethylamino)ethyl(meth)acrylamide, 2-(tert-butylamino)ethyl(meth)acrylate, 2-diisopropylaminoethyl(meth)acrylate, N-dodecylacrylamide and N-[2-(N,N-dimethylamino)ethyl](meth)acrylamide, 2-vinylpyridine, 4-vinylpyridine, allylamine, and vinylimidazole, as well as N,N-diethylaminostyrene (all isomers) and N,N-diethylamino-alpha-methylstyrene (all isomers). Among these examples, (meth)acrylate-based monomers and (meth)acrylamide-based monomers are preferred. (Meth)acrylate monomers are highly preferred. Particularly preferred amino group-containing monomers are N,N-dimethylaminoethyl acrylate, N,N-dimethylaminoethyl methacrylate, N,N-dimethylaminopropyl acrylate, and N,N-dimethylaminopropyl methacrylate or mixtures thereof.
[0053] As monomer (s3), it is also possible to use other ethylenically unsaturated monomers, such as styrene, alpha-alkylstyrenes, in particular alpha-methylstyrene, and / or vinyltoluene, vinylbenzoic acid (all isomers), alpha-methylvinylbenzoic acid (all isomers), and / or p-vinylbenzenesulfonic acid, maleic acid and / or fumaric acid and / or itaconic acid and their esters, amides, imides, and (meth)acrylic acid, nitriles such as acrylonitrile and / or methacrylonitrile, methoxypolyethylene glycol monoacrylates, methoxypolyethylene glycol monomethacrylates, and methoxypolypropylene glycol monoacrylates and methoxypolypropylene glycol monomethacrylates, divinylbenzene, di(meth)acrylate monomers, tri(meth)acrylate monomers and tetra(meth)acrylate monomers.
[0054] Preparation of copolymers Preferably, the copolymer of the invention comprises at least one of the monomers (s1) and (s2) and, optionally, at least the monomer (s3), i.e. (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), and optionally, (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); or can be obtained by copolymerization of (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); followed by a polymer-analogous reaction in which at least one functional group of the structural unit resulting from at least one monomer (s2) is converted to a functional group of the formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) It can be obtained by
[0055] Each monomer (s1) used contains at least one tin-containing moiety, which becomes part of each side chain (S1) after formation of the copolymer of the invention. The structural unit (SU1) is obtained by using a monomer (s1). Each monomer (s2) has the formula -OC(=O)-R, which becomes part of each side chain (S2) after formation of the copolymer of the invention. 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) or, after formation of a copolymer in a polymer-analogous reaction, contains at least one ester group of the formula -OC(=O)-R 1 The structural unit (SU2) is obtained by using a monomer (s2).
[0056] In particular, the copolymers of the invention comprise at least one of the monomers (s1) and (s2) and also at least one monomer (s3), i.e. (s1) 10 to 70 mol %, preferably 20 to 60 mol %, more preferably 30 to 50 mol % of at least one (meth)acrylic monomer containing at least one tin-containing moiety; (s2) 10 to 40 mol %, preferably 10 to 35 mol %, more preferably 10 to 30 mol % of a compound represented by the formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), (s3) 0 to 60 mol %, preferably 5 or 10 or 15 to 60 mol %, more preferably 30 to 50 mol % of at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2). or (s1) 10 to 70 mol %, preferably 20 to 60 mol %, more preferably 30 to 50 mol % of at least one (meth)acrylic monomer containing at least one tin-containing moiety; (s2) 10 to 40 mol %, preferably 10 to 35 mol %, more preferably 10 to 30 mol % of a compound represented by the formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), (s3) 0 to 60 mol %, preferably 5 or 10 or 15 to 60 mol %, more preferably 30 to 50 mol % of at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2). followed by a polymer-analogous reaction in which at least one functional group of the structural unit resulting from at least one monomer (s2) is converted to a functional group of the formula -OC(=O)-R 1 (In the formula, R 1is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) It can be obtained by Here, the sum of all monomers used to prepare the copolymers of the present invention add up to 100 mole %.
[0057] Method for preparing copolymers A further subject of the present invention is a process for the preparation of the inventive (meth)acrylic copolymers, comprising at least one step, in which (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), and optionally, (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form a copolymer, or (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form a copolymer, followed by a polymer-analogous reaction in which at least one functional group of the structural unit resulting from at least one monomer (s2) is converted into a functional group of the formula -OC(=O)-R 1 (In the formula, R1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) to at least one ester group of
[0058] All preferred embodiments described herein above in relation to the inventive copolymer and its preferred embodiments are also preferred embodiments of the inventive process for preparing said copolymer.
[0059] Use of copolymers A further subject of the present invention is the use of the inventive (meth)acrylic copolymers as catalysts, in particular as encapsulated catalysts, in crosslinking reactions in coating compositions and / or for increasing the pot life of coating compositions and / or for reducing the curing temperature of coating compositions.
[0060] All preferred embodiments described herein above in relation to the inventive copolymer, the inventive process for preparing said copolymer and preferred embodiments thereof are also preferred embodiments of the inventive use.
[0061] Coating Composition A further subject of the present invention is a coating composition comprising at least one polymer as binder component (a) and at least one inventive (meth)acrylic as component (b), where the polymer of binder component (a) is different from the (meth)acrylic copolymer of component (b).
[0062] All preferred embodiments described herein above in relation to the inventive copolymer, the inventive method for preparing said copolymer, the inventive method of use and preferred embodiments thereof are also preferred embodiments of the inventive coating composition.
[0063] Preferably, the coating composition of the present invention contains at least one (meth)acrylic copolymer as component (b) in an amount of 0.05 to 10% by weight, more preferably 0.1 to 7.5 or 5% by weight, even more preferably 0.2 to 4.5% by weight, even more preferably 0.3 to 4 or 3 or 2% by weight and in particular 0.4 to 1.5% by weight, based on the total weight of the coating composition.
[0064] The coating composition may be aqueous or essentially non-aqueous (i.e., based on an organic solvent). Preferably, the coating composition is based on at least one organic solvent, and more preferably is essentially non-aqueous. This means that the amount of solvent present in the composition is mainly due to the presence of at least one organic solvent. Preferably, water is not intentionally added to the composition. However, it is not determined that the composition is water-free, since one or more components used in the preparation of the composition may contain (residues of) water.
[0065] The amount of the at least one organic solvent present in the coating composition is preferably in the range of 5 to 50% by weight, more preferably in the range of 10 to 40% by weight, based on the total weight of the composition.
[0066] At least one polymer of the binder component (a) preferably has at least one crosslinkable functional group. Any conventional crosslinkable functional group known to those skilled in the art is possible here. In particular, the crosslinkable functional group is selected from the group consisting of hydroxyl groups, amino groups, carboxylic acid groups and epoxides. Particularly preferred is a hydroxyl group. Preferably, the at least one polymer is selected from the group consisting of polyurethanes, polyesters, polyamides, polyureas, poly(meth)acrylates and mixtures thereof, and hybrid polymers thereof, such as polyurethane(meth)acrylates. Polymers such as poly(meth)acrylates may be homopolymers or copolymers. Particularly preferred are OH-functional poly(meth)acrylates, such as OH-functional (meth)acrylic copolymers and / or OH-functional polyesters.
[0067] The binder component (a) may comprise a second polymer, such as a melamine resin, a melamine-formaldehyde resin, a free and / or blocked polyisocyanate. Preferably, the binder component (a) comprises at least one polyisocyanate, preferably blocked, as the second polymer. In particular, such preferably blocked polyisocyanates are used in combination with at least one OH-functional polymer, such as an OH-functional (meth)acrylic copolymer.
[0068] The amount of the at least one polymer of binder component (a) present in the coating composition is preferably in the range of 10 to 70% by weight, more preferably in the range of 15 to 60% by weight, even more preferably in the range of 20 to 55% by weight, based on the total weight of the composition.
[0069] Coating Method A further subject is a method for coating a substrate, comprising at least one step (1), namely, (1) applying to the substrate a coating composition according to the invention containing a copolymer according to the invention.
[0070] All preferred embodiments described herein above in relation to the inventive copolymer, the inventive method for preparing said copolymer, the inventive method of use, the inventive coating composition and preferred embodiments thereof are also preferred embodiments of the inventive coating method.
[0071] Preferably, the coating composition is a primer or clear coat composition, in particular a clear coat composition. The substrate used thus preferably has at least one coating layer, and the coating composition of the present invention is applied onto said layer. The substrate may be made of metal or at least partially made of plastic. EXAMPLES
[0072] method 1. Solids The amount of solids was determined according to DIN EN ISO 3251:2008-06 at 110° C. for 60 min.
[0073] 2. Number average and mass average molecular weight The number average (M n ) and mass average (M w ) The molecular weight and molecular weight distribution were determined by GPC-analysis (gel permeation chromatography analysis) according to DIN 55672-1:2007-08 using a high pressure liquid chromatography pump at 40 °C. The eluent used for the copolymers was tetrahydrofuran, the elution rate was 1 ml / min. Conventional calibration was performed using polystyrene standards.
[0074] 3. Viscosity measurement The viscosities of the application examples (see items 4. and 5. in the experimental part) were determined at 24°C or 40°C with a Brookfield 1 / 23 CAP2000+L viscometer. Kegel CAP-06 was used. The viscosities of the examples 2A-2C (see item 2. in the experimental part) were determined at 60°C with a Brookfield CAP2000+H viscometer. Kegel CAP-03 was used.
[0075] 4. Curing start temperature The cure onset temperatures were determined for the configurations listed in Table 1 using a Rheometrics DMTA Mark V Dynamic Mechanical Thermal Analysis (DMTA).
[0076] [Table 1]
[0077] Each sample was deposited (a few drops) onto a single layer of fiberglass string that had been previously attached to the DMTA (tensile configuration).
[0078] The samples were run using the following time / temperature sweep program: 1. The sample is first cooled to 25°C (77°F). 2. Heat at a rate of 2°K (5.4°F) per minute to 200°C (392°F).
[0079] Example (Experimental Part) The present invention is further illustrated by the following examples, which are not to be construed as limiting the scope of the invention. In the following, all amounts listed in the tables are in parts by weight unless otherwise indicated.
[0080] 1. Synthesis of organotin (meth)acrylate monomer (monomer (s1)) Example 1A: Acetyl dibutyltin methacrylate 111.65 g of dibutyltin oxide and 200 mL of toluene were added to a 500 mL round bottom flask equipped with a thermocouple, condenser, N2 inlet and paddle blade stirrer. The resulting suspension was heated to 50° C. under a N2 blanket and 39.01 g of methacrylic acid in 20 mL of toluene was added over 30 minutes. Stirring of the reaction mixture was continued at 50° C. for 2 hours until a homogeneous solution was obtained. The reaction mixture was then cooled to room temperature followed by the addition of 29.63 g of acetic acid in 20 mL of toluene over 20 minutes. The reactor contents were stirred at room temperature for 2 hours and then filtered. The solution was recovered and the volatile components were removed under reduced pressure. The remaining liquid was dried under reduced pressure at 50° C. for 1 hour leaving the product as a colorless liquid.
[0081] The reaction scheme for the preparation of Example 1A is shown below: [ka]
[0082] Example 1B: Lauryl dibutyltin methacrylate 90.11 g of dibutyltin oxide and 150 mL of toluene were added to a 500 mL round bottom flask equipped with a thermocouple, condenser, N2 inlet, and paddle blade stirrer. The resulting suspension was heated to 50°C under a N2 blanket and 31.50 g of methacrylic acid in 20 mL of toluene was added over 30 minutes. Stirring of the reaction mixture was continued at 50°C for 2 hours until a homogeneous solution was obtained. The reaction mixture was then cooled to room temperature followed by the addition of 40.05 g of lauric acid in 100 mL of MEK over 1 hour. The reactor contents were stirred at room temperature for an additional 2 hours before filtration. The solution was recovered and the volatile components were removed under reduced pressure. The remaining liquid was dried under reduced pressure at 50°C for 1 hour leaving the product as a colorless liquid.
[0083] Example 1C: Acetyldioctyltin methacrylate 40.75 g of dioctyltin oxide and 150 mL of toluene were added to a 500 mL round bottom flask equipped with a thermocouple, condenser, N2 inlet, and paddle blade stirrer. The resulting suspension was heated to 50°C under a N2 blanket and 9.71 g of methacrylic acid in 10 mL of toluene was added. Stirring of the reaction mixture was continued at 50°C for 2 hours until a homogeneous solution was obtained. The reaction mixture was then cooled to room temperature followed by the addition of 7.11 g of acetic acid in 10 mL of toluene. The reactor contents were stirred at room temperature for an additional 2 hours before filtration. The solution was recovered and the volatile components were removed under reduced pressure. The remaining liquid was dried under reduced pressure at 50°C for 1 hour leaving the product as a colorless liquid.
[0084] 2. Synthesis of organotin polymers Example 2A: The tin-containing polymer was prepared from the following ingredients:
[0085] [Table 2]
[0086] VAZO® 67 is a commercially available radical initiator (2,2'-azobis(2-methylbutyronitrile)). Unicid® 350 Acid is a commercially available product containing linear monocarboxylic fatty acids. Solvesso® 100 is a commercially available organic solvent mixture.
[0087] Charge 1 was added to a reactor equipped with a stirrer, thermocouple, condenser, and N2 inlet. A N2 blanket was applied and the reaction mixture was heated to 105°C. Two drops of dimethylethanolamine were added to Charge 1 and the reactor contents were stirred at 105°C for 4 hours. The reaction mixture was then cooled to 100°C and Charge 2 was added over 60 minutes. Upon completion, Charge 3 was added as a rinse for Charge 2. The reaction mixture was held at 100°C for 120 minutes. The resulting material was a clear resin above 60°C but a waxy solid at room temperature. The solids (110°C, 1 hour) was 60.07% and its viscosity was 233.2 cps at 60°C.
[0088] Example 2B: The tin-containing polymer was prepared from the following ingredients:
[0089] [Table 3]
[0090] Charge 1 was added to a reactor equipped with stirrer, thermocouple, condenser, and N2 inlet. A N2 blanket was applied and the reaction mixture was heated to 105°C. Two drops of dimethylethanolamine were added and the reactor contents were stirred at 105°C for 4 hours. The reaction mixture was then cooled to 100°C and Charge 2 was added over 50 minutes. Upon completion, Charge 3 was added as a rinse for Charge 2. The reaction mixture was held at 100°C for 120 minutes. The resulting material was a clear resin above 60°C but a waxy solid at room temperature. The solids (110°C, 1 hour) was 60.59% and its viscosity was 67.5 cps at 60°C.
[0091] Example 2C: The tin-containing polymer was prepared from the following ingredients:
[0092] [Table 4]
[0093] Charge 1 was added to a reactor equipped with stirrer, thermocouple, condenser, and N2 inlet. A N2 blanket was applied and the reaction mixture was heated to 105°C. Two drops of dimethylethanolamine were added and the reactor contents were stirred at 105°C for 4 hours. The reaction mixture was then cooled to 100°C and Charge 2 was added over 60 minutes. Upon completion, Charge 3 was added as a rinse for Charge 2. The reaction mixture was held at 100°C for 120 minutes. The resulting material was a clear resin above 60°C but a waxy solid at room temperature. The solids (110°C, 1 hour) was 58.33% and its viscosity was 71.3 cps at 60°C.
[0094] 3. Synthesis of poly(meth)acrylate polyols Example 3: Preparation of poly(meth)acrylate polyol Into a reactor flushed with nitrogen and fitted with a condenser, 157.90 parts by weight of amyl acetate were placed and this initial charge was heated to 142° C. with stirring. In parallel, two separate feeds were prepared. Feed 1 consisted of 307.78 parts by weight of 2-hydroxyethyl methacrylate, 98.86 parts by weight of 2-ethylhexyl methacrylate, 63.41 parts by weight of 2-ethylhexyl acrylate, 151.72 parts by weight of cyclohexyl methacrylate, and 7.77 parts by weight of Solvesso® 100. Feed 2 consisted of 68.40 parts by weight of tert-butyl peroxyacetate (50 wt.% in odorless mineral spirits) and 7.77 parts by weight of Solvesso® 100. When the temperature reached 142° C., feeds 1 and 2 were metered in simultaneously at a uniform rate over a period of 240 minutes. After the end of the metered addition, the reaction mixture was stirred for a further 45 min at 142° C. for post-polymerization. Feed 3 consisted of 6.39 parts by weight of tert-butyl peroxyacetate (50% by weight in odorless mineral spirits) and 3.94 parts by weight of Solvesso® 100, which were metered in at a uniform rate over a period of 30 min. After the end of the metered addition, the reaction mixture was stirred for a further 60 min at 142° C. for post-polymerization. The solids content of the resulting product was adjusted with 116.06 parts by weight of amyl acetate and determined to be 67.0%, OH number 213.4 mg KOH / g (based on solids), viscosity (23° C.) 38 dPa·S.
[0095] 4. Preparation of Coating Composition Examples A, B and C: Preparation of coating compositions containing a tin-containing polymer according to any one of Examples 2A, 2B or 2C as the polymer catalyst. The catalyst amount was adjusted to have the same tin equivalent.
[0096] The ingredients listed in Table 1 were added to a mixing cup and mixed to obtain Examples A to C. Desmodur® PL350MPA / SN is a commercially available aliphatic blocked polyisocyanate. BYK® 325 is a commercially available modified polysiloxane used as a surface additive.
[0097] Comparative Examples Comparative Example 1 and Comparative Example 2: Preparation of a comparative coating composition that does not contain any tin-containing catalyst (Comparative Example 1) or contains a commercial non-polymeric tin catalyst, i.e., the product Durastab® LT-2DBTDL, which contains dibutyltin dilaurate as the monomeric tin catalyst (Comparative Example 2).
[0098] The raw materials shown in Table 1 were added to a mixing cup and mixed to obtain Comparative Example 1 and Comparative Example 2, which are comparative examples.
[0099] [Table 5]
[0100] 5. Application and Performance The viscosities of Examples A, B, and C, and Comparative Examples 1 and 2 were measured immediately after preparation (initial) and after storage at 24°C or 40°C for one month. In addition, the cure onset temperature E' and tan delta were also measured. All measurements were performed according to the methods disclosed herein. The results are shown in Table 2.
[0101] [Table 6]
Claims
1. A polymer main chain and at least two different side chains (S1) and (S2) bonded to the polymer main chain, i.e. one or more side chains (S1) comprising at least one tin-containing moiety; and, Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms) and The one or more side chains (S1) are each a moiety represented by the following formula (PS1): [Formula 1] It is expressed as During the ceremony, symbol [Case 2] represents a covalent bond of the partial structure (PS1) to the main chain of the copolymer, The parameter a is 0 or 1, and R 2 , R 3 and R 4 denote, independently of one another, a linear saturated alkyl group having 1 to 30 carbon atoms, a branched saturated alkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an alkylaryl or arylalkyl group in each case having 7 to 30 carbon atoms.
2. 2. The copolymer according to claim 1, characterized in that the relative molar ratio of the at least one structural unit (SU1) containing one or more side chains (S1) to the at least one structural unit (SU2) containing one or more side chains (S2) in the (meth)acrylic copolymer is in the range of 15:1 to 1:2.
5.
3. 3. The copolymer according to claim 1 or 2, characterized in that the amount of structural units (SU1) containing one or more side chains (S1) is at least 20 mol %, based on the total amount of all structural units of the copolymer, and the amount of structural units (SU2) containing one or more side chains (S2) is at least 10 mol %, based on the total amount of all structural units of the copolymer.
4. The parameter a is 1, and R 2 , R 3 and R 4 4. The copolymer according to claim 3, characterized in that: each independently represents a linear saturated alkyl group having 1 to 20 carbon atoms or a branched saturated alkyl group having 3 to 20 carbon atoms.
5. R 1 5. The copolymer according to claim 1, wherein is a linear or branched, saturated or unsaturated acyclic aliphatic residue having from 18 to 60 carbon atoms.
6. The one or more side chains (S2) are each a partial structure (PS2) [C3] It is expressed as During the ceremony, symbol [C4] indicates the covalent bond of the substructure (PS2) to the main chain of the copolymer, Parameter b is 0 or 1; The parameter c ranges from 2 to 20; R 1 has the meaning defined in claim 1 or 5, Each R 5 represent independently hydrogen, hydroxyl, a linear saturated alkyl group having 1 to 30 carbon atoms, or a branched saturated alkyl group having 3 to 30 carbon atoms; and Each R 66. The copolymer according to claim 1 , wherein: independently represent hydrogen, a saturated linear alkyl group having 1 to 30 carbon atoms, or a saturated branched alkyl group having 3 to 30 carbon atoms.
7. Parameter b is 1, parameter c is in the range of 2 to 10, and each R 5 independently represents hydrogen or hydroxyl, and each R 6 7. The copolymer according to claim 6, characterized in that represents hydrogen.
8. 8. A copolymer according to claim 1 , comprising at least one further side chain (S3) attached to the polymer backbone, which is different from both the side chains (S1) and (S2), namely Partial structure (PS3) [C5] and having one or more side chains (S3) represented by In the formula, the symbol [C6] indicates the covalent bond of the substructure (PS3) to the main chain of the copolymer, R 7 denotes a linear saturated alkyl group having 1 to 30 carbon atoms, a branched saturated alkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an alkylaryl or arylalkyl group in each case having 7 to 30 carbon atoms.
9. 10. A copolymer according to claim 8, comprising at least one of the structural units (SU1), (SU2) and (SU3) which are different from one another, in which (SU1) contains at least one side chain (S1), (SU2) contains at least one side chain (S2) and (SU3) contains at least one side chain (S3), in the following mole % proportions, based on the total amount of the structural units (SU1), (SU2) and (SU3): 10 to 70 mol % of structural units (SU1), 10 to 40 mol % of structural units (SU2), and 5 to 60 mol% of structural units (SU3) The present invention is characterized in that it contains A copolymer, wherein the total content of structural units (SU1), (SU2) and (SU3) in said copolymer adds up to 100 mol %.
10. A method for producing the (meth)acrylic copolymer according to any one of claims 1 to 9, comprising at least one step, in which (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; (s2) Formula -OC(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), and optionally (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form said copolymer, or or (s1) at least one (meth)acrylic monomer comprising at least one tin-containing moiety; and (s2) at least one (meth)acrylic monomer having at least one functional group, the at least one functional group being represented by the formula -O-C(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms), and optionally (s3) at least one ethylenically unsaturated monomer different from both monomers (s1) and (s2); to form said copolymer, and subsequently, in a polymer-analogous reaction, modifying at least one functional group of the structural unit resulting from at least one monomer (s2) with a functional group of the formula -O-C(=O)-R 1 (In the formula, R 1 is a linear or branched, saturated or unsaturated, acyclic aliphatic residue having at least 18 carbon atoms, to at least one ester group represented by the formula:
11. 10. Use of a (meth)acrylic copolymer according to any one of claims 1 to 9 as a catalyst in a crosslinking reaction in a coating composition and / or for increasing the pot life of a coating composition and / or for reducing the curing temperature of a coating composition.
12. 10. A coating composition comprising at least one polymer as binder component (a) and at least one (meth)acrylic copolymer according to any one of claims 1 to 9 as component (b), wherein said polymer of said binder component (a) is different from said (meth)acrylic copolymer of component (b).
13. 13. The coating composition of claim 12, comprising the at least one (meth)acrylic copolymer as component (b) in an amount of 0.1 to 5% by weight, based on the total weight of the coating composition.
14. 14. A method for coating a substrate, comprising at least one step (1), namely (1) applying a coating composition according to claim 12 or 13 to the substrate.
Citation Information
Patent Citations
Antifoulant paint
JP1985231771A
Antifouling agent
JP1988107906A
Antifouling paint composition for application in water
JP1988304069A
Aqueous dispersion
JP2004161782A
Curable film-forming compositions comprising catalyst associated with a carrier and methods for coating a substrate
US20150132592A1