Boron nitride particles, resin composition, and method for producing resin composition

Boron nitride particles with a gradually increasing diameter shape improve thermal conductivity in heat dissipation materials by reducing overlap and heat transfer loss, offering lightweight options.

JP7580512B2Active Publication Date: 2024-11-11DENKA CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023033538
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-20
Filing Date
2023-03-06
Publication Date
2024-11-11
Estimated Expiration
2041-08-19

AI Technical Summary

Technical Problem

Conventional boron nitride particles are scaly, spherical, or irregularly shaped, which limits their effectiveness as heat dissipation materials due to inefficient stacking and increased heat transfer loss.

Method used

Boron nitride particles with a shape that gradually increases in diameter from one end to the other end, facilitating easier standing in the thickness direction of heat dissipation materials, reducing overlap and heat transfer loss.

Benefits of technology

Enhances thermal conductivity in heat dissipation materials by minimizing particle overlap and reducing heat transfer loss, while also allowing for lightweight options with hollow particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580512000001
    Figure 0007580512000001
  • Figure 0007580512000002
    Figure 0007580512000002
  • Figure 0007580512000003
    Figure 0007580512000003
Patent Text Reader

Abstract

To provide novel boron nitride particles. [Solution] One aspect of the present invention is a boron nitride particle having a shape in which the diameter gradually increases from one end to the other. Another aspect of the present invention is a boron nitride particle having a plurality of portions each having a shape in which the diameter gradually increases from one end to the other, the plurality of portions being bonded to each other at the other end.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to boron nitride particles, a resin composition, and a method for producing the resin composition. [Background technology]

[0002] Boron nitride has lubricity, high thermal conductivity, and insulating properties, and is used in a variety of applications, such as solid lubricants, mold release agents, cosmetic ingredients, heat dissipation materials, and heat-resistant, insulating sintered bodies.

[0003] For example, Patent Document 1 describes a hexagonal boron nitride powder that can be filled into a resin to impart high thermal conductivity and high dielectric strength to the resulting resin composition, which contains agglomerated particles made of primary particles of hexagonal boron nitride and has a BET specific surface area of ​​0.7 to 1.3 m. 2 / g and an oil absorption of 80 g / 100 g or less as measured in accordance with JIS K 5101-13-1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2016-160134 Summary of the Invention [Problem to be solved by the invention]

[0005] A primary object of the present invention is to provide novel boron nitride particles. [Means for solving the problem]

[0006] One aspect of the present invention is a boron nitride particle having a shape in which the diameter gradually increases from one end to the other end.

[0007] The length from the one end to the other end may be 80 μm or more.

[0008] Another aspect of the present invention is a boron nitride particle having a plurality of portions each having a shape whose diameter gradually increases from one end to the other end, and the plurality of portions being bonded to each other on the other end side.

[0009] The length of each of the plurality of portions in the direction from the one end to the other end may be 80 μm or more.

[0010] Another aspect of the present invention is a resin composition containing the above boron nitride particles and a resin.

[0011] Another aspect of the present invention is a method for producing a resin composition, comprising the steps of preparing the boron nitride particles and mixing the boron nitride particles with a resin, and may further comprise the step of pulverizing the boron nitride particles. [Effects of the Invention]

[0012] According to one aspect of the present invention, novel boron nitride particles can be provided. [Brief explanation of the drawings]

[0013] [Figure 1] 1 is a graph showing the results of X-ray diffraction measurement of the boron nitride particles of Example 1. [Figure 2] 1 is an SEM image of boron nitride particles of Example 1. [Figure 3] 1 is an SEM image of boron nitride particles of Example 2. [Figure 4] 1 is an SEM image of boron nitride particles of Example 3. DETAILED DESCRIPTION OF THE INVENTION

[0014] Hereinafter, an embodiment of the present invention will be described in detail. One embodiment of the present invention is a boron nitride particle (the boron nitride particle is referred to as boron nitride particle A) having a shape in which the diameter gradually increases from one end to the other end.

[0015] In this specification, the direction from one end to the other end of the boron nitride particle A is referred to as the axial direction, and the direction perpendicular to the axial direction is referred to as the radial direction. Furthermore, in this specification, the diameter of the boron nitride particle A refers to the size of the boron nitride particle in the radial direction.

[0016] While conventional boron nitride particles have a scaly, spherical, or irregular shape, the diameter of the boron nitride particles A according to one embodiment gradually increases from one end to the other. Therefore, the center of gravity of the boron nitride particles A in the axial direction is located at the other end. Therefore, when used in a heat dissipating material (heat dissipating sheet), the boron nitride particles A are likely to stand in the thickness direction of the heat dissipating material, with one end (the side with a relatively small diameter) facing up and the other end (the side with a relatively large diameter) facing down. Therefore, the boron nitride particles A are suitable for use in heat dissipating materials. While heat dissipating materials have been exemplified as an application of the boron nitride particles A, the boron nitride particles A can be used for a variety of applications, not limited to heat dissipating materials.

[0017] The fact that boron nitride particle A has the above-mentioned shape can be seen by observing boron nitride particle A with an SEM, where the diameters of boron nitride particle A at 10 equally spaced points in the axial direction of boron nitride particle A are denoted as A1, A2, . . . , A1 in the order from one end of boron nitride particle A to the other end. 10 (The diameter of one end of boron nitride particle A is A1, and the diameter of the other end is A 10 ), then A1, A2,..., A 10 This can be confirmed by the gradual increase in the diameter A of boron nitride particle A. n (n is an integer between 2 and 10) is A2~A 10 At all nine points, diameter A n-1 It is preferable that it is larger than A n A n-1 The diameter of the boron nitride particles A may be measured by importing the SEM image into image analysis software (for example, "Mac-view" manufactured by Mountec Co., Ltd.).

[0018] Diameter A of boron nitride particle A10 is larger relative to the diameter A1 of the boron nitride particles A, the more the center of gravity is located toward the other end in the axial direction of the boron nitride particles A. Therefore, for example, when the boron nitride particles A are mixed with a resin to make a heat dissipating material, the boron nitride particles A tend to stand upright in the thickness direction of the heat dissipating material, and the heat dissipating material is thought to have excellent thermal conductivity. 10 may be 1.2 times or more, 1.4 times or more, 1.6 times or more, 1.8 times or more, or 2 times or more the diameter A1 of the boron nitride particles A, and may be 10 times or less, 8 times or less, or 6 times or less.

[0019] The maximum axial length of the boron nitride particles A may be 80 μm or more, 100 μm or more, 125 μm or more, 150 μm or more, 175 μm or more, 200 μm or more, 225 μm or more, 250 μm or more, 300 μm or more, or 350 μm or more, or may be 500 μm or less. The maximum length of the boron nitride particles A may be measured by importing an SEM image into image analysis software (for example, "Mac-view" manufactured by Mountech Co., Ltd.).

[0020] The large axial length of the boron nitride particles A means that, for example, when the boron nitride particles A stand in the thickness direction of the heat dissipation material as described above, the number of boron nitride particles aligned in the thickness direction of the heat dissipation material is reduced, thereby reducing the heat transfer loss between the boron nitride particles, and therefore the heat dissipation material is thought to have excellent thermal conductivity.

[0021] The maximum diameter of the boron nitride particles A may be 50 μm or more, 80 μm or more, 100 μm or more, 125 μm or more, 150 μm or more, 175 μm or more, 200 μm or more, 225 μm or more, 250 μm or more, 300 μm or more, or 350 μm or more, and may be 500 μm or less.

[0022] The minimum diameter of the boron nitride particles A may be 1 μm or more, 2 μm or more, 5 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more, and may be 100 μm or less, 80 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, or 40 μm or less.

[0023] The average diameter of the boron nitride particles A (the above diameters A1 to A 10 The average value of the thickness may be 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more, and may be 200 μm or less, 150 μm or less, 100 μm or less, 80 μm or less, 70 μm or less, or 60 μm or less.

[0024] The aspect ratio of the boron nitride particles A may be 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 2.0 or more, 3.0 or more, 5.0 or more, or 7.0 or more, and may be 12.0 or less, 10.0 or less, 9.5 or less, 9.0 or less, or 8.0 or less. The aspect ratio of the boron nitride particles A is determined by the ratio of the maximum axial length (L1) of the boron nitride particles A to the diameters A1 to A2 of the boron nitride particles A. 10 It is defined as the ratio (L1 / L2) of the mean value (L2) of the

[0025] The larger the aspect ratio of boron nitride particles A, the more elongated and slender the boron nitride particles A will be. Therefore, for example, when boron nitride particles A are mixed with resin to form a heat dissipating material, boron nitride particles A will be more likely to overlap with other boron nitride particles. Furthermore, when boron nitride particles A overlap with other boron nitride particles, it is thought that the overlapping of the elongated and slender boron nitride particles A will occur at an angle. Therefore, the number of boron nitride particles aligned in the thickness direction of the heat dissipating material will be reduced, and heat transfer loss between boron nitride particles will be reduced, which is thought to result in the heat dissipating material having excellent thermal conductivity.

[0026] The boron nitride particles A may be solid or hollow. When the boron nitride particles A are hollow, they may have an outer shell formed of boron nitride and a hollow portion surrounded by the outer shell. The hollow portion may extend in the axial direction of the boron nitride particles A and may have a shape substantially similar to the external shape of the boron nitride particles A. In this case, the boron nitride particles A can also be said to be tubular boron nitride particles whose diameter gradually increases from one end to the other.

[0027] One or both of the ends of the boron nitride particles A may be open. The open ends may be connected to the hollow portions described above. Since the boron nitride particles A are hollow and at least one of the ends of the boron nitride particles A is open, when the boron nitride particles A are mixed with a resin and used as a heat dissipating material, for example, a resin lighter than the boron nitride particles A is filled into the hollow portions, which is expected to result in a heat dissipating material that has good thermal conductivity and is lightweight.

[0028] In another embodiment, the boron nitride particles may be boron nitride particles having a plurality of portions each having a shape whose diameter gradually increases from one end to the other end, and the plurality of portions being bonded to each other at the other end (these boron nitride particles will be referred to as boron nitride particles B).

[0029] In boron nitride particles B, the direction from one end to the other of each portion is the axial direction, and the direction perpendicular to the axial direction is the radial direction. The fact that each portion of boron nitride particles B has the above-mentioned shape may be confirmed by the same method as the above-mentioned method for confirming the shape of boron nitride particles A. The maximum axial length, etc. of each portion of boron nitride particles B may be the same as the range explained above as the maximum axial length, etc. of boron nitride particles A.

[0030] While conventional boron nitride particles have a scaly, spherical, or irregular shape, boron nitride particles B according to one embodiment have a plurality of portions whose diameters gradually increase from one end to the other, and the plurality of portions are bonded together at the other end. Therefore, the center of gravity of the boron nitride particles B is located at the other end (the side where the plurality of portions are bonded together). Therefore, when used in a heat dissipating material (heat dissipating sheet), the boron nitride particles B are likely to stand with the other end facing downward in the thickness direction of the heat dissipating material. Therefore, these boron nitride particles B can also be suitably used in heat dissipating materials. These boron nitride particles B can also be used for various purposes, not just heat dissipating materials.

[0031] The boron nitride particles B may be solid or hollow. When the boron nitride particles B are hollow, the boron nitride particles B may have an outer shell formed of boron nitride and a hollow portion surrounded by the outer shell. The hollow portion may extend in the axial direction in one of the multiple portions of the boron nitride particles B, or may extend in the axial direction in two or more of the multiple portions. The hollow portion may have a shape that is approximately similar to the external shape of each portion of the boron nitride particles B. When the hollow portion extends in the axial direction in multiple portions of the boron nitride particles B, the boron nitride particles B can also be said to be boron nitride particles having multiple tube-shaped portions whose diameters gradually increase from one end to the other, and the multiple portions are bonded to each other at the other end.

[0032] Each of the plurality of portions of the boron nitride particles B may have one or both of its ends open. The open ends may be connected to the hollow portions described above. Since the boron nitride particles B are hollow and at least one of their ends is open, when the boron nitride particles B are mixed with a resin and used as a heat dissipating material, for example, a resin lighter than the boron nitride particles B is filled into the hollow portions, which is expected to result in a heat dissipating material that has good thermal conductivity and is lightweight.

[0033] The above-mentioned boron nitride particles (boron nitride particles A and boron nitride particles B) may consist essentially of boron nitride. That the above-mentioned boron nitride particles consist essentially of boron nitride can be confirmed by detecting only peaks derived from boron nitride in X-ray diffraction measurement.

[0034] Next, a method for producing the above-mentioned boron nitride particles (boron nitride particles A and boron nitride particles B) will be described below. The above-mentioned boron nitride particles can be produced, for example, by a method for producing boron nitride particles comprising the steps of: placing a mixture containing boron carbide, boron nitride, and boric acid and a substrate made of a carbon material in a container made of a carbon material (placement step); and heating and pressurizing the container in a nitrogen atmosphere to produce boron nitride particles on the substrate (production step). Another embodiment of the present invention relates to such a method for producing boron nitride particles.

[0035] The container made of a carbon material is a container that can accommodate the mixture and the substrate. The container may be, for example, a carbon crucible. The container is preferably a container that can enhance airtightness by covering the opening. In the placement step, for example, the mixture may be placed at the bottom of the container, and the substrate may be placed so as to be fixed to the side wall surface of the container or the inside of the lid. The substrate made of a carbon material may be, for example, in the form of a sheet, plate, or rod. The substrate made of a carbon material may be, for example, a carbon sheet (graphite sheet), a carbon plate, or a carbon rod.

[0036] The diameter of one end of the boron nitride particles can be adjusted by adjusting the distance between the mixture and the substrate surface. When the distance between the mixture and the substrate surface is long (for example, 2.0 cm or more), the diameter of one end of the boron nitride particles tends to be half or less of the diameter of the other end.

[0037] The boron carbide in the mixture may be, for example, in powder form (boron carbide powder). The boron nitride in the mixture may be, for example, in powder form (boron nitride powder). The boric acid in the mixture may be, for example, in powder form (boric acid powder). The mixture can be obtained, for example, by mixing boron carbide powder, boron nitride powder, and boric acid powder by a known method.

[0038] Boron carbide powder can be produced by known production methods. For example, boron carbide powder can be produced by mixing boric acid and acetylene black, followed by heating in an inert gas (e.g., nitrogen gas) atmosphere at 1800 to 2400°C for 1 to 10 hours to obtain aggregated boron carbide particles. The aggregated boron carbide particles obtained by this method can be crushed, sieved, washed, impurity-removed, dried, etc., as appropriate to obtain boron carbide powder.

[0039] The average particle size of the boron carbide powder can be adjusted by adjusting the grinding time of the aggregated boron carbon particles. The average particle size of the boron carbide powder may be 5 μm or more, 7 μm or more, or 10 μm or more, and may be 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less. The average particle size of the boron carbide powder can be measured by a laser diffraction scattering method.

[0040] The boron nitride powder can be produced by a known production method, for example, by mixing boric acid or boron oxide with melamine and water, removing the water from the mixture by filtration, centrifugation, drying, or other methods, and then firing the mixture in a non-oxidizing gas atmosphere.

[0041] The average particle size of the boron nitride powder may be 5 μm or more, 7 μm or more, or 10 μm or more, and may be 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less. The average particle size of the boron nitride powder can be measured by a laser diffraction scattering method.

[0042] The mixing ratio of boron carbide, boron nitride, and boric acid can be selected appropriately. The content of boron nitride in the mixture is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, and may be 150 parts by mass or less, 120 parts by mass or less, or 100 parts by mass or less, relative to 100 parts by mass of boron carbide, from the viewpoint of suppressing changes in the distance between the mixture and the substrate surface due to expansion of boron carbide. The content of boric acid in the mixture is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 8 parts by mass or more, and may be 100 parts by mass or less, 90 parts by mass or less, or 80 parts by mass or less, relative to 100 parts by mass of boron carbide, from the viewpoint of easily increasing the size of boron nitride particles. When the content of boric acid in the mixture is 10% by mass or more, based on the total mass of the mixture, boron nitride particles B are easily produced.

[0043] The mixture containing boron carbide, boron nitride, and boric acid may further contain other components, such as silicon carbide, carbon, iron oxide, etc. When the mixture containing boron carbide, boron nitride, and boric acid further contains silicon carbide, it becomes easier to obtain boron nitride particles that do not have open ends.

[0044] The interior of the container is a nitrogen atmosphere containing, for example, 95% by volume or more of nitrogen gas. The nitrogen gas content in the nitrogen atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more, and may be substantially 100% by volume. In addition to nitrogen gas, the nitrogen atmosphere may also contain ammonia gas, etc.

[0045] The heating temperature is preferably 1450°C or higher, more preferably 1600°C or higher, and even more preferably 1800°C or higher, from the viewpoint that boron nitride particles tend to grow larger. The heating temperature may be 2400°C or lower, 2300°C or lower, or 2200°C or lower.

[0046] The pressure applied when pressing is preferably 0.3 MPa or more, more preferably 0.6 MPa or more, from the viewpoint that boron nitride particles tend to become large, and may be 1.0 MPa or less, or 0.9 MPa or less.

[0047] The time for which heating and pressure are applied is preferably 3 hours or more, more preferably 5 hours or more, from the viewpoint that boron nitride particles tend to become large. The time for which heating and pressure are applied may be 40 hours or less, or 30 hours or less.

[0048] According to this manufacturing method, the above-mentioned boron nitride particles are produced on a substrate made of a carbon material. Therefore, boron nitride particles can be obtained by recovering the boron nitride particles on the substrate. The particles produced on the substrate are boron nitride particles, which can be confirmed by recovering a portion of the particles from the substrate, performing X-ray diffraction measurement on the recovered particles, and detecting a peak derived from boron nitride.

[0049] The boron nitride particles obtained as described above may be subjected to a classification step (classification step) so as to obtain only boron nitride particles having a maximum length within a specific range.

[0050] The boron nitride particles obtained as described above can be mixed with a resin to form a resin composition. That is, another embodiment of the present invention is a resin composition containing the boron nitride particles and a resin.

[0051] Examples of resins include epoxy resin, silicone resin, silicone rubber, acrylic resin, phenolic resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin.

[0052] When the resin composition is used as a heat dissipation material, the content of the boron nitride particles may be 15% by volume or more, 20% by volume or more, 30% by volume or more, 40% by volume or more, 50% by volume or more, or 60% by volume or more, based on the total volume of the resin composition, from the viewpoint of improving the thermal conductivity of the heat dissipation material and easily obtaining excellent heat dissipation performance. The content of the boron nitride particles may be 85% by volume or less, 80% by volume or less, 70% by volume or less, 60% by volume or less, 50% by volume or less, or 40% by volume or less, based on the total volume of the resin composition, from the viewpoint of suppressing the generation of voids when the resin composition is molded into a sheet-shaped heat dissipation material and suppressing a decrease in the insulation properties and mechanical strength of the sheet-shaped heat dissipation material.

[0053] The resin content may be adjusted appropriately depending on the application, required properties, etc. of the resin composition. The resin content may be, for example, 15% by volume or more, 20% by volume or more, 30% by volume or more, 40% by volume or more, 50% by volume or more, or 60% by volume or more, and may be 85% by volume or less, 70% by volume or less, 60% by volume or less, 50% by volume or less, or 40% by volume or less, based on the total volume of the resin composition.

[0054] The resin composition may further contain a curing agent for curing the resin. The curing agent is appropriately selected depending on the type of resin. For example, curing agents used with epoxy resins include phenol novolac compounds, acid anhydrides, amino compounds, and imidazole compounds. The content of the curing agent may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or more, and 15 parts by mass or less or 10 parts by mass or less, relative to 100 parts by mass of the resin.

[0055] The resin composition may further contain other components, such as a curing accelerator (curing catalyst), a coupling agent, a wetting / dispersing agent, and a surface conditioner.

[0056] Examples of the curing accelerator (curing catalyst) include phosphorus-based curing accelerators such as tetraphenylphosphonium tetraphenylborate and triphenylphosphate, imidazole-based curing accelerators such as 2-phenyl-4,5-dihydroxymethylimidazole, and amine-based curing accelerators such as boron trifluoride monoethylamine.

[0057] Examples of the coupling agent include a silane-based coupling agent, a titanate-based coupling agent, an aluminate-based coupling agent, etc. Examples of the chemical bonding group contained in these coupling agents include a vinyl group, an epoxy group, an amino group, a methacryl group, a mercapto group, etc.

[0058] Examples of wetting and dispersing agents include phosphate ester salts, carboxylic acid esters, polyesters, acrylic copolymers, and block copolymers.

[0059] Examples of the surface conditioner include acrylic surface conditioners, silicone surface conditioners, vinyl surface conditioners, and fluorine surface conditioners.

[0060] The resin composition can be produced, for example, by a method for producing a resin composition, including a step of preparing boron nitride particles according to one embodiment (preparation step) and a step of mixing the boron nitride particles with a resin (mixing step). Another embodiment of the present invention is a method for producing such a resin composition. In the mixing step, in addition to the boron nitride particles and the resin, the above-mentioned curing agent and other components may also be mixed.

[0061] The method for producing a resin composition according to one embodiment may further include a step of pulverizing the boron nitride particles (pulverizing step). The pulverizing step may be performed between the preparing step and the mixing step, or may be performed simultaneously with the mixing step (the boron nitride particles may be pulverized simultaneously with mixing the boron nitride particles with the resin).

[0062] The above-mentioned resin composition can be used, for example, as a heat dissipation material. The heat dissipation material can be produced, for example, by curing the resin composition. The method for curing the resin composition is appropriately selected depending on the type of resin (and the curing agent used as needed) contained in the resin composition. For example, when the resin is an epoxy resin and the above-mentioned curing agent is used together, the resin can be cured by heating. [Example]

[0063] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples.

[0064] Example 1 The boron carbide particles were crushed in a grinder to obtain boron carbide powder with an average particle size of 10 μm. 50 parts by mass of the resulting boron carbide powder, 45 parts by mass of boron nitride powder (GP grade, manufactured by Denka Co., Ltd.), and 9 parts by mass of boric acid were mixed together. The resulting mixture was filled into a carbon crucible, and the opening of the carbon crucible was covered with a carbon sheet (manufactured by NeoGraf). The carbon sheet was fixed by sandwiching it between the carbon crucible lid and the carbon crucible. The distance between the mixture and the carbon sheet was 2.0 cm. The covered carbon crucible was heated in a resistance heating furnace under a nitrogen gas atmosphere at 2000°C and 0.85 MPa for 10 hours, producing particles on the carbon sheet.

[0065] A portion of the particles formed on the carbon sheet was collected and subjected to X-ray diffraction analysis using an X-ray diffractometer (Rigaku Corporation, "ULTIMA-IV"). Figure 1 shows the results of this X-ray diffraction analysis, as well as the results of X-ray diffraction analysis of boron nitride powder (GP grade) manufactured by Denka Company Limited for comparison. As can be seen from Figure 1, only peaks attributable to boron nitride were detected, confirming the formation of boron nitride particles. Figure 2 shows an SEM image of the obtained boron nitride particles. One of the obtained boron nitride particles (the boron nitride particle indicated by the arrow in Figure 2) had a shape in which the diameter gradually increased from one end to the other. The maximum axial length of the boron nitride particle was 184 μm, and the maximum diameter was 108 μm. The diameters of the boron nitride particles at 10 equally spaced points along the axial direction of the boron nitride particle were designated A1, A2, . . . , A3, A4, A5, A6, A7, A8, A9, A10, A11, A12, A13, A14, A15, A16, A17, A18, A19, A19, A20, A21, A22, A23, A24, A25, A26, A27, A28, A29, A30, A31, A32, A33, A34, A35, A36, A37, A38, A39, A40, A41, A42, A43, A44, A45, A46, A47, A48, A49, A50, A51, A52, A53, A54, A55, A56, A57, A58, A59, A60, A61, A62, A63, A64, A65, A66, A67, A68, A 10 (The diameter of one end of the boron nitride particle is A1, and the diameter of the other end is A 10 ), A1 is 33 μm, and A 10 is 108 μm, and A1 to A 10 The average value was 63 μm.

[0066] Example 2 A mixture was obtained by changing the boron nitride powder to SGP-grade boron nitride powder manufactured by Denka Co., Ltd., and particles were formed on a carbon sheet in the same manner as in Example 1, except that the distance between the resulting mixture and the carbon sheet was changed to 1.5 cm. A portion of the particles formed on the carbon sheet was collected and subjected to X-ray diffraction measurement. Only peaks derived from boron nitride were detected, confirming the formation of boron nitride particles. An SEM image of the resulting boron nitride particles is shown in Figure 3. One of the resulting boron nitride particles (the boron nitride particle indicated by the arrow in Figure 3) had a shape in which the diameter gradually increased from one end to the other. The maximum axial length of the boron nitride particle was 153 μm, and the maximum diameter was 106 μm. The diameters of the boron nitride particles at 10 equally spaced points in the axial direction of the boron nitride particle were designated A1, A2, ..., A3, in order from one end to the other of the boron nitride particle. 10 (The diameter of one end of the boron nitride particle is A1, and the diameter of the other end is A 10 ), A1 is 51 μm, and A 10 is 106 μm, and A1 to A 10 The average value was 80 μm.

[0067] Example 3 Particles were formed on a carbon sheet in the same manner as in Example 1, except that the amount of boric acid was changed to 12 parts by mass to obtain a mixture. A portion of the particles formed on the carbon sheet was collected and subjected to X-ray diffraction measurement. Only peaks attributable to boron nitride were detected, confirming that boron nitride particles had been formed. An SEM image of the obtained boron nitride particles is shown in Figure 4. One of the obtained boron nitride particles (the boron nitride particle indicated by the arrow in Figure 4) had multiple portions whose diameters gradually increased from one end to the other, and these multiple portions were bonded to each other at the other end.

Claims

1. The diameter gradually increases from one end to the other end. The minimum diameter is 1 μm or more, The diameter of the other end is 1.2 times or more and 10 times or less than the diameter of the one end, Boron nitride particles that are hollow.

2. 2. The boron nitride particle according to claim 1, wherein the length in the direction from said one end to said other end is 80 μm or more.

3. The device has a plurality of portions each having a shape whose diameter gradually increases from one end to the other end, The plurality of portions are joined to each other at the other end, The minimum diameter is 1 μm or more, The diameter of the other end is 1.2 times or more and 10 times or less than the diameter of the one end, Boron nitride particles that are hollow.

4. The boron nitride particle according to claim 3 , wherein the length of each of the plurality of portions in the direction from the one end to the other end is 80 μm or more.

5. A resin composition comprising the boron nitride particles according to any one of claims 1 to 4 and a resin.

6. A step of preparing boron nitride particles according to any one of claims 1 to 4; and mixing the boron nitride particles with a resin.

7. The method for producing a resin composition according to claim 6, further comprising a step of pulverizing the boron nitride particles.

Citation Information

Patent Citations

  • Flexible boron nitride nano-belt aerogel and preparation method therefor

    CN109704296A

  • Dispersion of boron nitride nanotubes and nonwoven fabric obtained by using the same

    JP2008214130A

  • Boron nitride aggregates, methods for producing the same, and their use

    JP2013543834A

  • Hexagonal boron nitride powder and method for producing the same

    JP2016160134A

  • Hexagonal crystal boron nitride powder and cosmetic

    JP2019043792A