Method for producing hollow inorganic particles and chain-like hollow inorganic particles

By adding polyhydric alcohols to an aqueous solution of polyacrylic acid and ammonia, followed by a sol-gel process, the method controls the shape of hollow inorganic particles, enabling chain-like or independently dispersed structures.

JP7580704B2Active Publication Date: 2024-11-12NAGOYA INSTITUTE OF TECHNOLOGY +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021000825
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-06
Publication Date
2024-11-12
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

Conventional emulsion template methods struggle to control the shape of hollow inorganic particles, particularly in forming chain-like or independently dispersed hollow inorganic particles.

Method used

A method involving the addition of alcohol, specifically polyhydric alcohols like ethylene glycol, to an aqueous solution of polyacrylic acid and ammonia, followed by a sol-gel process to form an inorganic film on dispersed particles, and subsequent elution of the solution, allowing control over the shape and linkage of hollow inorganic particles.

Benefits of technology

Enables the production of chain-like hollow inorganic particles bonded together or independently dispersed particles, facilitating the formation of chain-shaped or tubular structures with controlled properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580704000001
    Figure 0007580704000001
  • Figure 0007580704000002
    Figure 0007580704000002
  • Figure 0007580704000003
    Figure 0007580704000003
Patent Text Reader

Abstract

To provide a method for producing hollow inorganic particles capable of controlling the formation of chain hollow inorganic particles in a chained state by bonding hollow inorganic particles to each other or hollow inorganic particles each independently dispersed.SOLUTION: A method for producing hollow inorganic particles according to the present invention comprises a first step of adding an alcohol to an aqueous solution containing a polyacrylic acid and ammonia having an equivalent amount or more of a carboxyl group present in the polyacrylic acid to form a mixed aqueous solution, a second step of mixing the mixed aqueous solution with ethanol and / or methanol to form an emulsion, a third step of forming an inorganic film on a surface of dispersed particles present in the emulsion by a sol-gel method, and a fourth step of eluting the solution contained in the dispersed particles on which the inorganic film is formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing hollow inorganic particles and chain-like hollow inorganic particles. [Background technology]

[0002] Hollow inorganic particles have properties such as a high specific surface area, low density, and low thermal conductivity compared to solid inorganic particles, and are therefore used as functional materials in insulation materials and the like that take advantage of these properties. The emulsion template method is known as one type of method for producing hollow inorganic particles (see, for example, Patent Document 1). In this method, 1) an emulsion in which particles containing a polymer electrolyte are dispersed is prepared, 2) an inorganic film is formed on the surface of the dispersed particles of the emulsion using a sol-gel method, and then 3) the polymer electrolyte present inside the inorganic film is extracted and removed by putting the particles into water, and the particles are dried to obtain hollow inorganic particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-40858 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the conventional emulsion template method, it is difficult to control the shape of the hollow inorganic particles, and therefore it is not possible to control whether the hollow inorganic particles are linked together to form chain-like hollow inorganic particles or whether the hollow inorganic particles are independently dispersed. The present invention has been made in view of the above circumstances, and aims to provide a method for producing hollow inorganic particles that can control whether the hollow inorganic particles are bonded together to form a chain-like hollow inorganic particle or whether the hollow inorganic particles are dispersed independently without being linked to each other. Another aim of the present invention is to provide a method for producing hollow inorganic particles that can control whether the hollow inorganic particles are bonded together to form a chain-like hollow inorganic particle or whether the hollow inorganic particles are dispersed independently without being linked to each other. Another aim of the present invention is to provide a method for producing hollow inorganic particles that are bonded together to form a chain-like hollow inorganic particle. [Means for solving the problem]

[0005] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that in the conventional emulsion template method, the above-mentioned problems can be solved by adding an alcohol to an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent amount of carboxy groups present in the polyacrylic acid, and have thus completed the present invention.

[0006] That is, the method for producing hollow inorganic particles of the first invention is characterized by comprising a first step of adding an alcohol to an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent amount of carboxy groups present in the polyacrylic acid to obtain a mixed aqueous solution, a second step of mixing the mixed aqueous solution with ethanol and / or methanol to obtain an emulsion, a third step of forming an inorganic coating on the surfaces of dispersed particles present in the emulsion by a sol-gel method, and a fourth step of dissolving the solution contained in the dispersed particles on which the inorganic coating has been formed.

[0007] In the method for producing hollow inorganic particles of the present invention, first, in the first step, alcohol is added to an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent amount of carboxyl groups present in the polyacrylic acid to obtain a mixed aqueous solution. This mixed aqueous solution is a homogeneous solution and does not form an emulsion. Next, in the second step, this mixed aqueous solution is mixed with ethanol and / or methanol to form an emulsion. Furthermore, in the third step, an inorganic coating is formed on the surface of the dispersed particles present in the emulsion by a sol-gel method. Finally, in the fourth step, the solution contained in the dispersed particles on which the inorganic coating has been formed is dissolved. The hollow inorganic particles thus obtained can be produced as shown in the following 1) to 3) by controlling the type of alcohol used in the first step and its addition ratio, and by controlling the molecular weight and addition amount of polyacrylic acid. 1) Chained hollow inorganic particles in which hollow inorganic particles are linked together to form a chain. 2) Chained hollow inorganic particles in which the hollow spaces of adjacent hollow inorganic particles are connected to form a tube shape. 3) Hollow inorganic particles in which individual hollow inorganic particles are not linked together and are dispersed independently.

[0008] The alcohol added in the first step in the first invention can be a polyhydric alcohol. According to the results of the inventors' tests, the use of a polyhydric alcohol makes it easier to control the shape of the resulting hollow inorganic particles, and makes it easier to prepare chain-like hollow inorganic particles in which hollow inorganic particles are bonded to each other to form a chain state. In order to further facilitate control of the shape of the hollow inorganic particles, the polyhydric alcohol is preferably at least one selected from the group consisting of ethylene glycol, glycerin, and polyvinyl alcohol, and is most preferably ethylene glycol.

[0009] The number average molecular weight of polyacrylic acid is preferably 1000 or more and 50000 or less. According to the test results of the inventors, if the number average molecular weight of polyacrylic acid is in the range of 1000 or more and 50000 or less, the shape of hollow inorganic particles can be easily controlled. The range of 5000 or more and 25000 or less is particularly preferable.

[0010] The inorganic coating can be any of SiO2, TiO2, and ZrO2. These inorganic coatings can be easily formed by the sol-gel method.

[0011] The method for producing hollow inorganic particles of the second invention is characterized by comprising: a first step of preparing an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the number of moles of the polyacrylic acid; a second step of mixing the aqueous solution with an alcohol mixture in which a polyhydric alcohol is added to ethanol to prepare an emulsion; a third step of forming an inorganic coating on the surfaces of dispersed particles present in the emulsion by a sol-gel method; and a fourth step of dissolving a solution contained in the dispersed particles on which the inorganic coating has been formed.

[0012] In the method for producing hollow inorganic particles of the second invention, first, in the first step, an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent of the carboxyl groups present in the polyacrylic acid is prepared. This aqueous solution is a homogeneous solution and does not form an emulsion. Next, in the second step, this aqueous solution is mixed with an alcohol mixture in which a polyhydric alcohol is added to ethanol to form an emulsion. Furthermore, in the third step, an inorganic coating is formed on the surface of the dispersed particles present in the emulsion by a sol-gel method. Finally, in the fourth step, the solution contained in the dispersed particles on which the inorganic coating has been formed is dissolved. The hollow inorganic particles thus obtained can be made to be independently dispersed hollow inorganic particles without being bonded to each other by controlling the ratio of the polyhydric alcohol used in the second step.

[0013] Also in the second invention, the inorganic coating can be any one of SiO2, TiO2, and ZrO2. These inorganic coatings can be easily formed by the sol-gel method. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a process diagram showing a method for producing hollow inorganic particles according to a first aspect of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a process for forming hollow inorganic particles in the first invention. [Diagram 3]FIG. 1 is a schematic cross-sectional view showing chain-like hollow inorganic particles (a) in which the hollow portions are not interconnected, chain-like hollow inorganic particles (b) in which the hollow portions are interconnected, and hollow inorganic particles (c) in which the hollow inorganic particles are not bonded to each other and are dispersed independently. [Figure 4] FIG. 2 is a process diagram showing a method for producing hollow inorganic particles according to a second aspect of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing a process for forming hollow inorganic particles in the second invention. [Figure 6] 3 is a scanning electron microscope photograph of hollow silica particles when the amount of ethylene glycol added is changed in the method for producing hollow silica particles of the first invention. [Figure 7] 1 shows scanning electron microscope photographs (right side) and schematic diagrams (left side) of hollow silica particles when the amount of ethylene glycol added is changed in the method for producing hollow silica particles of the first invention. [Figure 8] 3A to 3C are scanning electron microscope photographs of hollow inorganic particles when the amount of ethanol added is changed in the method for producing hollow silica particles of the first invention. [Figure 9] 1 is a scanning electron microscope photograph of the chain-like hollow silica particles of Example 11 in which the hollow silica particles are in a chain state with each other. [Figure 10] 3A to 3C are scanning electron microscope photographs of hollow silica particles when the amount of glycerin added is changed in the method for producing hollow silica particles of the first invention. [Figure 11] 1 is a scanning electron microscope photograph of the chain-like hollow silica particles of Example 15 in which the hollow silica particles are in a chain state. [Figure 12] 3A to 3C are scanning electron microscope photographs of hollow silica particles when the amount of methanol added is changed in the method for producing hollow silica particles of the first invention. [Figure 13] 1 is a scanning electron microscope photograph of the chain-like hollow silica particles of Example 18 in which the hollow silica particles are in a chain state with each other. [Figure 14] 1 is a scanning electron microscope photograph of hollow silica particles when the amount of polyacrylic acid added is changed in the method for producing hollow silica particles of the first invention. [Figure 15] 3 is a scanning electron microscope photograph of hollow silica particles when the amount of ethylene glycol added is changed in the method for producing hollow silica particles of the first invention. [Figure 16] 1 is a scanning electron microscope photograph of hollow silica particles when the amount of polyvinyl alcohol added is changed in the method for producing hollow silica particles of the first invention. [Figure 17] 3 is a scanning electron microscope photograph of hollow silica particles when methanol is used instead of ethanol as a dispersion medium in the second step in the method for producing hollow silica particles of the first invention. [Figure 18] 4 is a scanning electron microscope photograph of hollow silica particles prepared by the method for producing hollow silica particles of the second invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. <Method for producing hollow inorganic particles according to the first aspect of the present invention> ·1st process S1 1 is a process diagram of the method for producing hollow inorganic particles according to the first aspect of the present invention. First, in the first step S1, ammonia water is added to an aqueous polyacrylic acid solution. The amount of ammonia water added is equal to or greater than the equivalent of the carboxyl groups present in the polyacrylic acid. In other words, the aqueous solution contains an excess of ammonia compared to the carboxyl groups, making it an alkaline aqueous solution.

[0016] ·2nd process S2 Next, in the second step S2, the mixed aqueous solution obtained in the first step S1 is mixed with ethanol. As shown in Figure 2(a), this mixed solution becomes an emulsion state in which an aqueous solution containing polyacrylic acid 2 is dispersed as fine droplets 3 in ethanol 1, which is a poor solvent for polyacrylic acid. It is presumed that the surface of the droplets 3 becomes a positively charged colloid due to the ammonium ions, stabilizing the colloidal dispersion.

[0017] ·3rd process S3 Furthermore, in the third step S3, an inorganic film 4 is formed on the surface of the dispersed particles present in the emulsion by the sol-gel method (see FIG. 2(b)). The sol-gel method is a technique for forming an inorganic oxide film of SiO2, TiO2, or ZrO2 on the surface of the dispersed particles by hydrolyzing and polymerizing alkoxides of silicon, titanium, or zirconium. In FIG. 1, the SiO2 film is formed on the surface of the dispersed particles using tetraethoxysilane (TEOS), but another alkoxysilane may be used instead of TEOS. Also, it is possible to form a TiO2 film using an alkoxide of titanium such as titanic acid tetraisopropoxide, or to form a ZrO2 film using an alkoxide of zirconium such as zirconium tetrapropoxide.

[0018] ·4th process S4 Finally, in a fourth step S4, the solution contained in the dispersed particles on which the inorganic coating 4 is formed is eluted to obtain inorganic particles 6 having hollow portions 5 (see FIG. 2(c)). The solution contained in the inorganic particles 6 can be eluted by centrifuging the particles or leaving them to settle, and then placing them in a large amount of water 7. Furthermore, by repeating the separation and recovery of the inorganic particles 6 and the immersion in the water 7, the solution contained in the inorganic particles 6 can be eluted reliably.

[0019] In the above-mentioned method for producing hollow inorganic particles, by controlling the type and mixing ratio of the alcohol used in the first step and the molecular weight of the polyacrylic acid, it is possible to form chain-like hollow inorganic particles in which the hollow inorganic particles are bonded together to form a chain (see FIG. 3(a)), and further, to form hollow inorganic particles in which the hollow portions of the chain-like hollow inorganic particles are connected to each other to form tube-like particles (see FIG. 3(b)), or to form hollow inorganic particles in which the hollow inorganic particles are not bonded together but are dispersed independently (see FIG. 3(c)). The mechanism by which the chain-like hollow inorganic particles are formed in the first invention is not clear, but is presumed to be as follows. When the mixed aqueous solution and ethanol are mixed in the second step S2, as shown in Fig. 2(a), an emulsion state is formed in which the aqueous solution containing polyacrylic acid 2 is dispersed as fine droplets 3 in ethanol 1, which is a poor solvent for polyacrylic acid. Since the droplets 3 also contain the alcohol added in the first step, the surface tension of the droplets 3 is reduced by the added alcohol. This makes it easier for the droplets 3 to join together, forming a chain.

[0020] The alcohol added in the first step of the first invention can be a polyhydric alcohol. According to the results of the inventors' tests, the use of a polyhydric alcohol makes it easier to control the shape of the resulting hollow inorganic particles, and makes it easier to prepare chain-like hollow inorganic particles in which hollow inorganic particles are bonded to each other to form a chain state. As the polyhydric alcohol, at least one selected from the group consisting of ethylene glycol, glycerin, and polyvinyl alcohol can be used, and ethylene glycol is the most preferred.

[0021] <Method for producing hollow inorganic particles according to the second aspect of the present invention> ·1st process S5 A process diagram of the method for producing hollow inorganic particles according to the second invention is shown in FIG. 4. First, in the first step S5, ammonia water is added to polyacrylic acid. The amount of ammonia water added is equal to or greater than the equivalent of the carboxyl groups present in polyacrylic acid. In other words, the aqueous solution contains an excess of ammonia compared to the carboxyl groups, making it an alkaline aqueous solution. However, unlike the first invention described above, no alcohol is added in the first step S5.

[0022] ·2nd process S6 Next, in the second step S6, a mixed solution is prepared by adding a polyhydric alcohol (e.g., ethylene glycol or glycerin) to ethanol (or methanol), and this mixed solution is mixed with the mixed aqueous solution of polyacrylic acid and ammonia prepared in the first step. As a result, as shown in Figure 5(a), the mixed solution becomes an emulsion state in which an aqueous solution containing polyacrylic acid 12 is dispersed as fine droplets 13 in a mixed solution 11 of ethanol and a polyhydric alcohol, which is a poor solvent for polyacrylic acid. It is believed that the surfaces of the droplets 13 become positively charged colloids due to the ammonium ions, stabilizing the colloidal dispersion.

[0023] ·3rd process S7 Furthermore, in a third step S7, an inorganic coating 14 is formed on the surface of the dispersed particles present in the emulsion by a sol-gel method (see FIG. 5(b)).

[0024] ·4th process S8 Finally, in the fourth step S8, the solution contained in the dispersed particles on which the inorganic coating 14 is formed is eluted to obtain inorganic particles 16 having hollow portions 15 (see FIG. 5(c)). The solution contained in the dispersed particles can be eluted by centrifuging the inorganic particles 16 or leaving them to settle, recovering them, and then placing them in a large amount of water 17. The hollow inorganic particles 16 thus obtained can be made into independently dispersed hollow inorganic particles by controlling the type and mixing ratio of the polyhydric alcohol used in the second step S6 (see FIG. 3(c)). The mechanism behind this is not clear, but is presumed to be as follows. When the aqueous solution of polyacrylic acid and ammonia prepared in the first step S5 is dispersed in a mixed solution of ethanol and a polyhydric alcohol in the second step S6 to form an emulsion, an emulsion state is obtained in which an aqueous solution containing polyacrylic acid 2 is dispersed as fine droplets 3 in ethanol 1, which is a poor solvent for polyacrylic acid, as shown in FIG. 5(a). However, unlike the first invention, the polyhydric alcohol is not present in the droplets 3, but in the mixed solution 11 which surrounds the droplets 3 and is a poor solvent for polyacrylic acid. At this time, the polyhydric alcohol in the mixed solution 11 is adsorbed to the droplets 3 and plays the role of a protective colloid, resulting in independently dispersed hollow inorganic particles. EXAMPLES

[0025] Hereinafter, specific examples of the present invention will be described in detail. <Examples related to the first aspect of the invention> (Examples 1 to 8) ·1st process 0.12g of polyacrylic acid (PAA) 25% by weight aqueous solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., number average molecular weight M = 25,000) was mixed with 2.0ml of 25% aqueous ammonia solution and stirred for 24 hours to prepare a polyacrylic acid / ammonia water mixed solution, and then ethylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added in a predetermined amount (0.2ml in Example 1, 0.5ml in Example 2, 1.0ml in Example 3, 1.5ml in Example 4, 2.0ml in Example 5, 3.0ml in Example 6, 1.0ml in Example 7, and 5.0ml in Example 8) and stirred for 2 minutes to prepare a polyacrylic acid / ammonia water / ethylene glycol mixed solution. Note that ethylene glycol was not added in Comparative Example 1. The rest is the same as in Examples 1 to 8, and the explanation will be omitted.

[0026] ·Second process The polyacrylic acid / ammonia water / ethylene glycol mixed solution obtained in the first step was added to 35 ml of ethanol and stirred to obtain an emulsion. ·3rd process The emulsion obtained in the second step was stirred for 2 minutes, after which 2 ml of tetraethoxysilane (TEOS) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added at a rate of 40 μL / min and stirred for one day. ·4th process The emulsion obtained in the third step was subjected to solid-liquid separation using a cooling / high-speed centrifuge (H-9R, Kokusan Co., Ltd.) at 15,000 rpm for 10 minutes to obtain a powder. After washing with water, the powder was dried at 180°C for 24 hours and observed by a scanning electron microscope.

[0027] The results are shown in Figures 6 and 7. From these figures, it was found that when the amount of ethylene glycol added was 0 ml, hollow silica particles were dispersed alone (Comparative Example 1), but as the amount of ethylene glycol added was increased, hollow silica particles gradually became chain-like hollow silica particles in which the hollow portions of adjacent hollow silica particles were linked together (Examples 2 to 4), and as the amount of ethylene glycol added was further increased, the hollow silica particles became tubular chain-like hollow silica particles in which the hollow portions of adjacent hollow silica particles were connected (Examples 5 to 8) (see the schematic diagram shown on the left side of Figure 7).

[0028] (Examples 9 to 13) In Examples 9 to 13, ethanol was added instead of the ethylene glycol added in the first step in Examples 1 to 8. The amount of ethanol added was 0.5 ml in Example 9, 0.9 ml in Example 10, 1.0 ml in Example 11, 1.2 ml in Example 12, and 2.0 ml in Example 13. Note that no ethanol was added in Comparative Example 2. The rest is the same as in Examples 1 to 8, and a description thereof will be omitted.

[0029] The results are shown in Figures 8 and 9. From these figures, it was found that in Comparative Example 2 in which ethanol was not added, hollow silica particles were dispersed alone, but as the amount of ethanol added was increased, the hollow silica particles gradually became linked together to form chain-like hollow silica particles (Examples 9 to 12), and as the amount of ethanol added was further increased, the hollow silica particles returned to a state in which they were dispersed alone (however, the wall thickness of the hollow silica particles became thicker and the diameter of the hollow portion became smaller) (Example 13).

[0030] (Examples 14 to 16) In Examples 14 to 16, glycerin was added instead of the ethylene glycol added in the first step in Examples 1 to 8. The amount of glycerin added was 0.5 ml in Example 14, 1.0 ml in Example 15, and 3.0 ml in Example 16. Note that no glycerin was added in Comparative Example 3. The rest of the procedures were the same as in Examples 1 to 8, and a description thereof will be omitted.

[0031] The results are shown in Figures 10 and 11. From these figures, it can be seen that in Comparative Example 3 where no glycerin was added, hollow silica particles were dispersed alone, but as the amount of glycerin added was increased, the hollow silica particles gradually became chain-like hollow silica particles in which the hollow silica particles were linked together (Examples 14 to 16). However, in Example 16 where the amount of glycerin added was the highest at 3.0 ml, the wall thickness of the chain-like hollow silica particles became thicker and the diameter of the hollow portion became smaller (see Example 16).

[0032] (Examples 17 to 20) In Examples 17 to 20, methanol was added instead of the ethylene glycol added in the first step in Examples 1 to 8. The amount of methanol added was 0.5 ml in Example 17, 1.0 ml in Example 18, 2.0 ml in Example 19, and 3.0 ml in Example 20. Note that no methanol was added in Comparative Example 4. The rest of the procedures were the same as in Examples 1 to 8, and a description thereof will be omitted.

[0033] The results are shown in Figures 12 and 13. It was found from these figures that in Comparative Example 4, in which no methanol was added, hollow silica particles were dispersed singly, but as the amount of methanol added was increased, the hollow silica particles gradually became linked together to form chain-like hollow silica particles (Examples 17 and 18), and as the amount of methanol added was further increased, the chain-like hollow silica particles changed to individually dispersed hollow silica particles with large particle sizes (see Examples 19 and 20).

[0034] (Examples 21 to 23) In Examples 21 to 23, the amount of 25 wt % polyacrylic acid (PAA) aqueous solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., number average molecular weight M = 25,000) added was changed (0.04 g in Example 21, 0.06 g in Example 22, and 0.08 g in Example 23), and the other conditions were the same as in Example 11 (i.e., 1.0 ml of ethanol was added in the first step).

[0035] The results are shown in Figure 14. It was found from this figure that when the amount of polyacrylic acid (PAA) added in the first step was in the range of 0.04 g to 0.08 g, the hollow silica particles were linked together to form chain-like hollow silica particles.

[0036] (Examples 24 to 27) In Examples 24 to 27, polyacrylic acid (PAA) with a number average molecular weight of 5,000 was used, and ethylene glycol was used as the alcohol added in the first step. The amount of ethylene glycol added was 2.0 ml in Example 24, 4.0 ml in Example 25, 7.0 ml in Example 26, and 10.0 ml in Example 27. The other conditions were the same as in Examples 1 to 8, and therefore the explanation will be omitted.

[0037] The results are shown in FIG. 15. In the column of shape in FIG. 15, "chain-like" indicates that the hollow silica particles are chain-like hollow silica particles in which the hollow silica particles are bonded to each other to form a chain. Also, "tube-like" indicates that the hollow silica particles are chain-like hollow inorganic particles in which the hollow portions of adjacent hollow silica particles are connected to each other. From this figure, it was found that even if the number average molecular weight of polyacrylic acid (PAA) is 5,000, which is smaller than the 25,000 used in Examples 1 to 8, hollow silica particles are chain-like hollow silica particles in which the hollow silica particles are chain-like. It was also found that when the amount of ethylene glycol added is increased, the hollow silica particles are chain-like hollow silica particles in which the hollow portions of adjacent hollow silica particles are connected to each other.

[0038] (Examples 28 to 30) In Examples 28 to 30, the alcohol added in the first step was polyvinyl alcohol (PVA) having a number average molecular weight of 5,000 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and the amount added was 2 ml in Example 28, 3 ml in Example 29, and 4 ml in Example 30. The rest is the same as in Examples 1 to 8, and the explanation will be omitted.

[0039] The results are shown in Figure 16. From these figures, it was found that when PVA was used as the alcohol in the first step, hollow silica particles were chained together in Example 28, where the amount of PVA added was small, to form chain-like hollow silica particles. However, when the amount of PVA added was increased, single hollow silica particles with large particle diameters were formed, and the film thickness was also thick (see Examples 29 and 30 in Figure 16).

[0040] (Examples 31 to 34) In Examples 31 to 34, methanol was used as the dispersion medium of the emulsion used in the second step. The alcohol added in the first step was 2 ml of ethylene glycol, and the stirring time was 1 minute in Example 31, 2 minutes in Example 32, 5 minutes in Example 33, and 10 minutes in Example 34. The rest is the same as in Examples 1 to 8, and the explanation will be omitted.

[0041] The results are shown in Figure 17. It was found from these figures that even when methanol was used instead of ethanol as the dispersion medium in the second step, hollow silica particles formed into chains were formed into tubular chain-like hollow silica particles. <Examples related to the second invention> (Examples 35 to 37) ·1st process 0.12 g of a 25 wt % aqueous solution of polyacrylic acid (PAA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., number average molecular weight M=5,000) was mixed with 2.0 ml of a 25% aqueous ammonia solution and stirred for 24 hours to prepare a polyacrylic acid / ammonia water mixed solution. ·Second process A given amount of ethylene glycol (1 ml in Example 35, 2 ml in Example 36, and 10 ml in Example 37) was added to 35 ml of ethanol and stirred for one day to obtain an ethanol / ethylene glycol mixed solution. The polyacrylic acid / aqueous ammonia mixed solution prepared in the first step was added to this ethanol / ethylene glycol mixed solution and stirred to obtain an emulsion. ·3rd process The emulsion obtained in the second step was stirred for 2 minutes, after which 2 ml of tetraethoxysilane (TEOS) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added at a rate of 40 μL / min and stirred for one day. ·4th process The reaction solution obtained in the third step was subjected to solid-liquid separation using a cooling / high-speed centrifuge (H-9R, Kokusan Co., Ltd.) at 15,000 rpm for 10 minutes to obtain a powder. After washing this powder with water, it was dried at 180°C for 24 hours and observed by a scanning electron microscope.

[0042] The results are shown in Figure 18. It can be seen from these figures that as the amount of ethylene glycol added increases, the hollow silica particles become separated from each other and dispersed independently without agglomerating.

[0043] The present invention is not limited to the above-mentioned embodiment. Various modifications within the scope of the claims and within the scope of those skilled in the art are also included in the present invention. [Industrial Applicability]

[0044] By using the method for producing hollow inorganic particles of the present invention, it is possible to produce chain-like hollow inorganic particles in which hollow inorganic particles are bonded to each other to form a chain. Hollow inorganic particles have different heat insulating properties, dielectric constant, and optical properties from solid particles, but if these are chain-like hollow inorganic particles, they can be given anisotropy in addition to these properties. Therefore, it is possible to provide functional anisotropic materials such as light guide plates for LEDs, heat dissipation anisotropic materials, and electrically anisotropic materials. [Explanation of symbols]

[0045] 1...Ethanol, 2...Polyacrylic acid, 3...Droplets, 4...Inorganic film 5...Hollow part, 6...Inorganic particles, 7...Water 11 ... mixed solution, 12 ... polyacrylic acid, 13 ... droplet, 14 ... inorganic coating, 15...Hollow part, 16...Inorganic particles, 17...Water S1, S5…1st process S2, S6…2nd process S3,S7…3rd process S4,S8…4th process

Claims

1. A first step of adding an alcohol to an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent amount of a carboxyl group present in the polyacrylic acid to obtain a mixed aqueous solution; A second step of mixing the mixed aqueous solution with ethanol and / or methanol to form an emulsion; a third step of forming an inorganic coating on the surface of dispersed particles present in the emulsion by a sol-gel method; A fourth step of dissolving a solution contained in the dispersed particles on which the inorganic coating is formed, In the first step, the type of the alcohol, the mixing ratio of the alcohol, and the molecular weight of the polyacrylic acid are controlled to form chain-like hollow inorganic particles in which the hollow inorganic particles are bonded to each other.

2. 2. The method for producing hollow inorganic particles according to claim 1, wherein the alcohol used in the first step is a polyhydric alcohol.

3. 3. The method for producing hollow inorganic particles according to claim 2, wherein the polyhydric alcohol is at least one selected from the group consisting of ethylene glycol, glycerin, and polyvinyl alcohol.

4. The method for producing hollow inorganic particles according to any one of claims 1 to 3, wherein the number average molecular weight of the polyacrylic acid is 1,000 or more and 50,000 or less.

5. The inorganic coating is SiO 2 ,TiO 2 , and ZrO 2 4. The method for producing hollow inorganic particles according to claim 1, wherein the hollow inorganic particles are formed by the above-mentioned method.

6. A first step of preparing an aqueous solution containing polyacrylic acid and ammonia in an amount equal to or greater than the equivalent amount of carboxyl groups present in the polyacrylic acid, and not containing alcohol; a second step of mixing the aqueous solution with an alcohol mixture in which a polyhydric alcohol is added to ethanol to form an emulsion; a third step of forming an inorganic coating on the surface of dispersed particles present in the emulsion by a sol-gel method; and a fourth step of dissolving the solution contained in the dispersed particles on which the inorganic coating is formed.

7. The inorganic coating is SiO 2 ,TiO 2 , and ZrO 2 7. The method for producing hollow inorganic particles according to claim 6, wherein the method is any one of the above.

Citation Information

Patent Citations

  • Prepn process of hollow silica ball

    CN1931718A

  • Method for manufacturing porous structure, optical material, and insulation material

    JP2012188323A

  • Mixed viscous heat-storage material and production method therefor

    JP2017206571A

  • Production method of nanosilica hollow particle

    JP2018035031A

  • Method for producing hollow silica particles

    JP2020040858A