Mica Pigment Particles for Powder Coating Applications

The formation of spherical mica-containing pigment particles through controlled precipitation in a solvent-based process addresses the challenges of loose mica and energy inefficiency in powder coatings, achieving improved flow and consistent coating quality.

JP7580922B2Active Publication Date: 2024-11-12XEROX CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020017524
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-04
Filing Date
2020-02-05
Publication Date
2024-11-12
Estimated Expiration
2040-02-05

AI Technical Summary

Technical Problem

Existing methods for incorporating mica into powder coatings result in loose mica particles, color changes, and equipment clogging, and require energy-intensive processes, lacking control over particle size and gloss.

Method used

A process forming spherical mica-containing pigment particles by combining mica with an amorphous polyester resin and a polymeric stabilizer in a water-miscible solvent, followed by precipitation with a polar solvent, creating particles with controlled size and shape for improved application.

Benefits of technology

The method produces mica-containing powder coatings with enhanced flow properties, reduced energy consumption, and consistent color and gloss, minimizing equipment issues and improving coating quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580922000005
    Figure 0007580922000005
  • Figure 0007580922000006
    Figure 0007580922000006
  • Figure 0007580922000007
    Figure 0007580922000007
Patent Text Reader

Abstract

To provide a process for producing an improved mica-containing pigment composition having the ability to tailor particle size ranges, gloss and other desired properties, and to provide a mica-containing pigment composition.SOLUTION: There is provided a process for producing a mica-containing pigment composition comprising spherical pigment particles, comprising the steps of: providing an amorphous polyester resin, a polymeric stabilizer comprising a water-soluble polymer, and mica particles; dissolving the polyester resin and polymeric stabilizer into a water-miscible organic solvent together with the mica particles to form a first fluid mixture comprising the mica particles; adding a polar solvent to the first fluid mixture at a predetermined rate, thereby forming a second fluid mixture comprising precipitated pigment particles; and collecting the precipitated pigment particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] Powder coatings are used in a variety of applications, including the automotive, architectural, and furniture industries. Powder coatings do not contain liquid vehicles and release only small amounts of volatile organic compounds (VOCs) or hazardous air pollutants (HAPs) when applied and cured on a surface, and are therefore advantageous over traditional solvent-borne coatings when it is desirable to limit VOC emissions. To provide color to the powder coating, pigments may be included in the coating material.

[0002] One of the pigments used with powder coatings is mica, a flaky layered metal hydrate silicate / aluminosilicate mineral that can be used to add a pearlescent effect to the coating. Mica has been incorporated into powder coatings in a variety of ways, such as by dry blending the mica particles with the powder coating material and by bonding the mica particles to the particles of the powder coating. In a process called "blitz bonding," the mica particles adhere to the coarser powder particles of the powder coating to prevent separation of the mica pigment during application of the powder to a surface. However, during the manufacture and use of such coatings, grinding of the coarser blitz-bonded powder particles can result in loose mica particles in the composition. Such loose mica in blitz-bonded compositions, as well as in dry-blended powder coatings, can cause color changes in the coated surface. Unbound mica flakes also interfere with the application of powder coatings to surfaces by tribo or corona powder coating guns because the static charge of the coating gun can cause such flakes to stand on their side instead of lying down and can cause the mica flakes to stick together, thereby clogging the powder coating gun.

[0003] Another way mica has been incorporated into powder coatings is by melt extrusion. In this process, mica is mixed with a polymer, melt extruded, and then ground or pulverized to form the pigment powder coating. However, the forces of extrusion and grinding can damage the mica pigment and produce loose mica pigment in the final composition.

[0004] It would be desirable to provide improved mica-containing powder coatings with the ability to tailor particle size range, gloss, and other desired properties by using smaller, more spherical particles. It would also be desirable to provide mica-containing powder coatings prepared by more energy-efficient processes that use less energy and fewer steps. It would further be desirable to provide a process for the preparation of mica-containing powder coatings using a "bottom-up" approach. It would further be desirable to provide dramatic, decorative colored powder coatings, such as metallic (gold and silver) and pearlescent colors. Summary of the Invention

[0005] The above desired properties can be obtained using the present powder coating, which in embodiments can include a binder resin and a metal oxide mica pigment. The coating includes spherical, mica-containing pigment particles formed from a polymeric material having mica flakes incorporated both inside and outside the particle. The pigment particles can have a circularity of about 0.93 to about 0.999, and a geometric size distribution of about 1.3 to about 2.0.

[0006] To form such mica-containing pigment particles, mica particles and an amorphous polyester resin are first combined with a polymeric stabilizer, such as a water-soluble polymer. The polyester resin and polymeric stabilizer are then dissolved in a water-miscible organic solvent along with the mica particles to form a fluid mixture containing the mica particles. A polar solvent is added to the fluid mixture at a predetermined rate, and the pigment particles are precipitated from the mixture. The precipitated pigment particles are then collected.

[0007] The pigment particles can be used as a powder coating to form a pigmented coating on a substrate, for example, by applying the pigment particles to a substrate surface using an electrostatic powder coating applicator and then curing the pigment particles on the substrate to form a pigmented coating on the substrate. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 illustrates the steps of an embodiment of the present process for producing a mica-containing pigment composition for powder coating applications. [Diagram 2] 1 is a bar graph showing a digital microscope image analysis of a sample (Batch 1) of the pigment composition. [Diagram 3] 1 is a bar graph showing a digital microscope image analysis of another sample (Batch 2) of the pigment composition. [Figure 4] FIG. 3 is a scanning electron microscope (SEM) image (micrograph) of the sample (batch 1) analyzed in FIG. 2. [Diagram 5] FIG. 5 is another scanning electron microscope image of the sample analyzed in FIG. 2 at a higher resolution than the image in FIG. 4. [Figure 6] FIG. 6 is a further scanning electron microscope image of the sample analysed in FIG. 2 at a higher resolution than the image in FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] definition As used herein, the following terms and variations thereof have the meanings given below, unless a different meaning is clearly intended by the context in which such term is used.

[0010] "About" and "approximately" refer to an amount within 10% of a referenced amount, unless such usage indicates otherwise.

[0011] "Aspect ratio" refers to a dimensionless quantity used in image analysis and microscopy to numerically describe the shape of a particle independent of its diameter. The aspect ratio (A R ) is defined by the following formula:

[0012]

number

[0013] In the formula, d max is the maximum diameter of a particular particle in the sample, and d min , d max The aspect ratio is the smallest diameter of a particle perpendicular to the particle axis. In measurements using imaging, the aspect ratio can be expressed as the ratio of the width (largest observable particle dimension) of an image of a particle to its height (smallest observable particle dimension perpendicular to the width). Thus, an aspect ratio of 1 can represent a circle or a square, while a line has an aspect ratio approaching 0.

[0014] "Circularity" refers to the circumference of a circle of equivalent area divided by the actual circumference of the central cross section of the particle. If the particle is more spherical, the circularity approaches 1, but if the particle is more elongated or rough-edged, the circularity will be less.

[0015] "Concurrently" refers to the performance of a particular action or step of a process during the same time as another action or step, or within a defined time before or after the other action or step, where the performance of a particular action or step within a defined time does not adversely affect the end result of the process.

[0016] "Gloss" refers to the ability of a surface to reflect light in a specular (mirror-like) direction. Gloss can be measured in gloss units (GU), i.e., the ratio of reflected to incident light of a sample specimen measured relative to a standard ratio.

[0017] "GSD" refers to geometric standard deviation (GSD).

[0018] "Mica" refers to a layered metal hydrate silicate / aluminosilicate mineral that may be optionally coated with oxides of transition metals such as chromium, cobalt, iron, titanium, etc. Many mica minerals are generally of the chemical formula XY 2-3 Z4O 10 (OH,F)2, where: X is K, Na, Ca, HO, NH, or less commonly Ba, Rb, or Cs; Y is Al, Mg, or Fe, or less commonly Mn, Cr, Ti, Li, V, or Zn; Z is generally Si or Al, but Fe3 + Or it may also contain Ti.

[0019] For purposes of the present pigment composition, "fine particles" generally refers to particles having a particle size in the range of about 1 to about 500 micrometers, for example, about 50 to about 300 micrometers, about 70 to about 270 micrometers, or about 100 to about 220 micrometers.

[0020] "Organic solvent" refers to a liquid material that contains primarily one or more organic compounds.

[0021] "Particle size" refers to the diameter of a sphere having the same volume or surface area as a given particle.

[0022] "Powder" refers to a material composed primarily of a large number of loose solid particles that are flowable such that the particles of the powder material can move relative to one another.

[0023] "Resin" refers to a non-crystalline polymeric material, typically one that is a solid or viscous liquid at room temperature.

[0024] "Spherical" refers to a shape that is generally spherical, i.e., has a central cross section with a circularity of about 0.93 to about 0.999. It will be understood that a composition consisting primarily of spherical particles will include particles that are non-uniform, ovoid, or include other shapes. It will be understood that the spherical particles of the present compositions will also, in some cases, have mica on their surfaces, resulting in regions of the surface of such particles having a sheet-like structure rather than the curvature of a sphere.

[0025] "Substrate" refers to the article or layer to which the powder coating pigment is applied.

[0026] The term "comprise" and variations of terms such as "comprising" and "comprises" are not intended to exclude other additives, components, integers, or steps. As used herein, the terms "a," "an," and "the" and similar referents should be construed to encompass both the singular and the plural, unless the usage in context dictates otherwise. Ranges stated as "between" two values ​​include the recited values.

[0027] Overview of Micro Pigment Particles and Preparation Process The powder coating is formed from mica-containing pigment particles made of a polymeric material having mica flakes embedded on and within a polymeric matrix. The particles have a circularity of about 0.93 to about 0.999, about 0.95 to about 0.995, or about 0.96 to about 0.990, and a geometric size distribution of about 1.3 to about 2.0. The particles have an average particle size of about 50 micrometers to about 250 micrometers, about 100 micrometers to about 200 micrometers, or about 125 micrometers to about 175 micrometers.

[0028] Such spherical mica-containing pigment particles can be made by combining the mica particles with an amorphous polyester resin, a polymeric stabilizer comprising a water-soluble polymer, and a water-miscible organic solvent. The polyester resin, the polymeric stabilizer, and the mica particles can be added together before being placed in contact with the water-miscible organic solvent, or alternatively, the mica particles can be added to the water-miscible organic solvent before the polyester resin and the polymeric stabilizer are placed in contact with the water-miscible organic solvent. The polyester resin and the polymeric stabilizer are dissolved in the water-miscible organic solvent, and the combined reactants form a first fluid mixture comprising the mica particles.

[0029] The second fluid mixture is created when a polar solvent, such as an aqueous solution, is added to the first fluid mixture at a predetermined rate. The second fluid mixture can be heated to a temperature of about 75°C to about 95°C. The spherical pigment particles precipitate from the second fluid mixture, and the precipitated pigment particles are then collected for use in a powder coating application. To catalyze the precipitation of the pigment particles, colloidal silica can be added to the second fluid mixture, or alternatively, can be added to the first fluid mixture prior to adding the polar solvent solution to the first fluid mixture.

[0030] Micas having particle sizes of about 5 micrometers to about 100 micrometers can be used in this process and may be present in the precipitated particles in an amount of about 2% to about 60% by weight based on the total weight of the pigment particles. Polymeric stabilizers include polyvinyl acetate, poly(methyl methacrylate), poly(acrylonitrile), poly(dimethylsiloxane), polyvinyl chloride, polyethylene, polypropylene), poly(lauryl methacrylate), poly(oxyethylene), poly(acrylamide), poly(vinyl alcohol), poly(acrylic acid), poly(methacrylic acid), polyvinylpyrrolidone), polyethyleneimine), poly(vinyl methyl ether), poly(4-vinylpyridine), poly(12-hydroxystearic acid), poly(isobutylene), cis-1:4-poly(isopropyl ether), poly(vinyl methyl ... The polyvinyl acetate may be any of the following: polyvinyl acetate, polyvinyl acetate phthalate ...

[0031] The polyesters used in the present process may have a glass transition temperature of about 45° C. to about 75° C. and may be selected from the group consisting of poly(propoxylated bisphenol co-fumarate), poly(ethoxylated bisphenol co-fumarate), poly(butyloxylated bisphenol co-fumarate), poly(copropoxylated bisphenol co-ethoxylated bisphenol co-fumarate), poly(1,2-propylene fumarate), poly(propoxylated bisphenol co-maleate), poly(ethoxylated bisphenol co-maleate), poly(butyl ... The water-miscible organic solvent may be any of dimethylacetamide, acetic acid, diethylene glycol dimethyl ether, dimethylformamide, 1,4-dioxane, ethylene glycol, hexamethylphosphoramide, hexamethylphosphoramide, pyridine, water, and combinations thereof.

[0032] The mica-containing pigment particles can be applied as a powder coating to a substrate surface with an electrostatic powder coating applicator, for example, using tribo or corona charging. The applied powder is then cured on the surface to form a pigmented coating on the substrate.

[0033] Materials for the preparation of mica pigments The process for preparing the present mica-containing pigment composition is generally depicted in Figure 1. The process involves creating a first solution by dissolving a polyester resin and a polymeric stabilizer along with mica flakes in a water-miscible organic solvent, then adding a polar solvent as a poor solvent to precipitate the mica particles.

[0034] mica The optical properties of the mica-containing pigment composition are primarily provided by the mica flakes, which may be natural or synthetic. The mica flakes may be treated with transparent metal oxides having high reflectance values, such as oxides of transition metals including chromium, cobalt, iron, titanium, and similar metals, for example, TiO2, Fe2O3, Cr2O3, etc., to provide mica materials that impart the characteristic luster of pearlescent pigments. The color of the mica flakes with metal oxide coatings may be adjusted by applying different thicknesses of metal oxide materials to the mica flakes. For example, mica particles having a metal oxide layer having a thickness of about 40 nm to about 60 nm will reflect silver colored light, a layer of about 60 nm to about 80 nm will generally reflect a yellow / gold color, a layer of about 80 nm to about 100 nm will generally reflect a red color, a layer of about 100 nm to about 140 nm will generally reflect a blue color, and a layer of about 120 nm to about 160 nm will generally reflect a green color. In embodiments, the powder coating exhibits a decorative color such as a metallic (gold or silver) or pearlescent color.

[0035] Mica particles for use in the present mica pigments typically range in size from about 5 micrometers to about 100 micrometers. The size of the mica particles affects the appearance of a surface coated with the present composition, with smaller mica particles providing a less reflective and more opaque finish and larger particles providing a more reflective and transparent finish. Mica particles from about 1 to about 25 micrometers generally impart a "satin" (shiny, relatively low reflective) finish to a surface, particles from about 10 to about 60 micrometers generally impart a more reflective finish (having a "luster"), and particles from about 20 to about 150 micrometers can impart an even more reflective finish (having a "shine").

[0036] The mica particles also have an effect on the mechanical and electrical properties of the final mica-polymer composite of the pigment composition. For example, properties such as stiffness and Young's modulus of the mica composite increase with increasing mica loading (mica concentration). Meanwhile, elongation at break and tensile strength decrease with increasing mica loading. Dielectric strength and surface resistivity also increase with increasing mica loading, making the composition more suitable for use in electrical insulation applications.

[0037] A variety of mica-containing pigments can be used in the mica component of the present compositions. Examples of commercially available pearlescent and metallic mica-containing pigments that can be used in the present process include the following available from Merck & Company, Inc. (Kenilworth, NJ): IRIODIN 300 Gold Pearl, IRIODIN 100 Silver Pearl, TIMIRON Bronze MP60 (D50 volume average particle size of 22-37 micrometers with 50% of the pigment having a volume size less than the size indicated), TIMIRON Copper MP-65 (D50 diameter of 22-37 micrometers), COLORONA Oriental Beige (D50 diameter of 3-10 micrometers), COLORONA Aborigine Amber (D50 diameter of 18-25 micrometers), COLORONA Passion Orange (D50 diameter of 18-25 micrometers), COLORONA Bronze Fine (D50 diameter of 7-14), COLORONA Bronze (D50 diameter of 18-25 micrometers), COLORONA Bronze Sparkle (D50 diameter of 28-42 micrometers), COLORONA Copper Fine (D50 diameter of 7-14 micrometers), COLORONA Copper (D50 diameter of 18-25 micrometers), COLORONA Copper Sparkle (D50 diameter of 25-39 micrometers), COLORONA Red Brown (D50 diameter of 18-25 micrometers), COLORONA Russet (D50 diameter of 18-25 micrometers), COLORONA Tibetan Ochre (D50 diameter of 18-25 micrometers), COLORONA Sienna Fine (D50 diameter of 7-14 micrometers), COLORONA Sienna (D50 diameter of 18-25 micrometers), COLORONA Bordeaux (D50 diameter of 18-25 micrometers), COLORONA Glitter Bordeaux, and COLORONA Chameleon (D50 diameter of 18 to 25 micrometers).

[0038] Other suitable mica pigments available from Merck & Company, Inc. include TIMIRON Super Silk MP-1005 (D50 diameter 3-10 micrometers), TIMIRON Super Sheen MP-1001 (D50 diameter 7-14 micrometers), TIMIRON Super Silver Fine (D50 diameter 9-13 micrometers), TIMIRON Pearl Sheen MP-30 (D50 diameter 15-21 micrometers), TIMIRON Satin MP-11171 (D50 diameter 11-20 micrometers), TIMIRON Ultra Luster MP-111 (D50 diameter 18-25 micrometers), TIMIRON Star Luster MP-111 (D50 diameter 18-25 micrometers), TIMIRON Pearl Flake MP-10 (D50 diameter 22-37 micrometers), TIMIRON Super Silver (D50 diameter 17-26 micrometers), TIMIRON Sparkle These include MP-47 (D50 diameter of 28 to 38 micrometers), TIMIRON Arctic Silver (D50 diameter of 19 to 25 micrometers), XIRONA Silver (D50 diameter of 15 to 22 micrometers), and RONASTAR Silver (D50 diameter of 25 to 45 micrometers).In light colors, suitable mica pigments available from Merck & Company, Inc. include COLORONA Carmine Red (provides a red sheen effect, D50 diameter of 10 to 60 micrometers), COLORONA Magenta (provides a pink violet sheen effect, D50 diameter of 18 to 25 micrometers), COLORONA Light Blue (provides a light blue sheen effect, D50 diameter of 18 to 25 micrometers), COLORONA Dark Blue (provides a dark blue sheen effect, D50 diameter of 18 to 25 micrometers), COLORONA Majestic Green (provides a green sheen color, D50 diameter of 18 to 25 micrometers), COLORONA Brilliant Green (provides a golden green sheen color, D50 diameter of 19 to 26 micrometers), COLORONA Egyptian Emerald (provides a dark green sheen effect, D50 diameter of 18 to 25 micrometers), and COLORONA Patagonian and Purple (D50 diameter of 18-25 micrometers, giving a purple luster effect).Other examples of commercially available mica-containing pigments that can be used in the present process and composition include Diamond Venetian Gold (available from Black Diamond Powder Pigments, St. Augustine, FL) and SYMIC pearlescent pigments, which are based on synthetic mica and available from ECKART America Corporation, Louisville, KY.

[0039] polyester The polyester used in the present process for producing the mica-containing pigment composition is a branched or linear amorphous polyester resin. The amorphous polyester resin can be formed by reacting a diol with a diacid in the presence of any catalyst. Examples of diacids or diesters, including vinyl diacids or vinyl diesters, utilized in the preparation of the amorphous polyester include dicarboxylic acids or diesters, such as terephthalic acid, phthalic acid, isophthalic acid, fumaric acid, dimethyl fumarate, dimethyl itaconate, cis-1,4-diacetoxy-2-butene, diethyl fumarate, diethyl maleate, maleic acid, succinic acid, itaconic acid, succinic acid, succinic anhydride, dodecyl succinic acid, dodecyl succinic anhydride, Examples of suitable dibasic acids or diesters include glutaric acid, glutaric anhydride, adipic acid, pimelic acid, suberic acid, azelaic acid, dodecanedioic acid, dimethyl terephthalate, diethyl terephthalate, dimethyl isophthalate, diethyl isophthalate, dimethyl phthalate, phthalic anhydride, diethyl phthalate, dimethyl succinate, dimethyl fumarate, dimethyl maleate, dimethyl glutarate, dimethyl adipate, dimethyl dodecyl succinate, and combinations thereof. The dibasic acid or diester may be present in an amount of, for example, about 40 to about 60 mol % of the resin, about 42 to about 52 mol % of the resin, or about 45 to about 50 mol % of the resin.

[0040] Examples of diols that may be utilized in the production of the amorphous polyester include 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, pentanediol, hexanediol, 2,2-dimethylpropanediol, 2,2,3-trimethylhexanediol, heptanediol, dodecanediol, bis(hydroxyethyl)-bisphenol A, bis(2-hydroxypropyl)-bisphenol A, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, xylene dimethanol, cyclohexanediol, diethylene glycol, bis(2-hydroxyethyl) oxide, dipropylene glycol, dibutylene, and combinations thereof. The amount of diol selected may vary and may be present, for example, in an amount of about 40 to about 60 mole percent of the resin, about 42 to about 55 mole percent of the resin, or about 45 to about 53 mole percent of the resin.

[0041] Polycondensation catalysts that may be utilized in forming the amorphous polyesters used in the present process include tetraalkyl titanates, dialkyl tin oxides such as dibutyltin oxide, tetraalkyl tins such as dibutyltin dilaurate, and dialkyl tin oxide hydroxides such as butyltin oxide hydroxide, aluminum alkoxides, alkyl zincs, dialkyl zincs, zinc oxides, stannous oxides, or combinations thereof. Such catalysts may be utilized, for example, in amounts of from about 0.01 mole percent to about 5 mole percent based on the starting diacid or diester used to produce the polyester resin.

[0042] Examples of amorphous polyester resins which may be used in the present process include poly(propoxylated bisphenol co-fumarate), poly(ethoxylated bisphenol co-fumarate), poly(butyloxylated bisphenol co-fumarate), poly(copropoxylated bisphenol co-ethoxylated bisphenol co-fumarate), poly(1,2-propylene fumarate), poly(propoxylated bisphenol co-maleate), poly(ethoxylated bisphenol co-maleate), poly(butyloxylated bisphenol co-maleate), poly( Poly(1,2-propylene itaconate), poly(propoxylated bisphenol co-ethoxylated bisphenol co-maleate), poly(1,2-propylene maleate), poly(propoxylated bisphenol co-itaconate), poly(ethoxylated bisphenol co-itaconate), poly(butyloxylated bisphenol co-itaconate), poly(copropoxylated bisphenol co-ethoxylated bisphenol co-itaconate), poly(1,2-propylene itaconate), and combinations thereof.

[0043] Alkali sulfonated polyester resins may also be useful in some embodiments, examples of which include copoly(ethylene-terephthalate)-copoly(ethylene-5-sulfo-isophthalate), copoly(propylene-terephthalate)-copoly(propylene-5-sulfo-isophthalate), copoly(diethylene-terephthalate)-copoly(diethylene-5-sulfo-isophthalate), copoly(propylene-diethylene-terephthalate)-copoly(propylene-diethylene-5-sulfo-isophthalate), copoly(propylene-butylene-terephthalate)-copoly(propylene and the metal or alkali salts of copoly(ethoxylated bisphenol-A-maleate)-copoly(ethoxylated bisphenol-A-5-sulfo-isophthalate), copoly(propoxylated bisphenol-A-fumarate)-copoly(propoxylated bisphenol-A-5-sulfo-isophthalate), copoly(ethoxylated bisphenol-A-fumarate)-copoly(ethoxylated bisphenol-A-5-sulfo-isophthalate), where the alkali metals are, for example, sodium, lithium, or potassium ions.

[0044] The amorphous polyesters used in the process may advantageously have a glass transition temperature of about 40° C. to about 90° C., or about 45° C. to about 75° C. The polyesters may also have a melt viscosity of about 10 to about 1,000,000 Pa·s at about 130° C., or about 20 to about 100,000 Pa·s at about 130° C. The average molecular weight of the amorphous polyesters may also be about 2,000 to about 25,000 as measured by gel permeation chromatography (GPC) using polystyrene standards. Powdered or particulate forms of polyesters are commonly used in the process, although liquid polyester resins may also be used.

[0045] Polymer Stabilizers The present process for producing mica-containing pigments also uses a water-soluble polymer as a polymeric stabilizer. Non-limiting exemplary polymeric stabilizers include poly(vinyl acetate), poly(methyl methacrylate), poly(acrylonitrile), poly(dimethylsiloxane), poly(vinyl chloride), poly(ethylene), poly(propylene), poly(lauryl methacrylate), poly(oxyethylene), poly(acrylamide), poly(vinyl alcohol), poly(acrylic acid), poly(methacrylic acid), poly(vinylpyrrolidone), poly(ethyleneimine), poly(vinyl methyl ether), poly(4-vinylpyridine), poly(12-hydroxystearic acid), poly(isobutylene), cis-1:4-poly(isoprene), carboxymethylcellulose, gelatin, polysorbate 80 (such as TWEEN 80 available from Millipore Sigma / Merck KGaA, Darmstadt, Germany), polysorbate 2 ... Examples of suitable polyvinyl acetates include polyvinyl caprolactam-polyvinyl acetate-polyethylene glycol graft copolymers such as SOLUPLUS (available from BASF, Ludwigshafen, Germany), polyvinyl acetate phthalate, cellulose acetate phthalate, and combinations thereof.

[0046] The above-mentioned polymers contain hydrophilic groups in the backbone of the polymer. The hydrophilic groups can be nonionic, anionic, cationic, or amphoteric. Such water-soluble polymers can be either synthetic (produced by polymerization of monomers synthesized from petroleum or natural gas), semi-synthetic (produced by chemical derivatization of natural organic materials such as polysaccharides or cellulose), or natural (materials derived from microbial, plant, or animal materials, such as xanthan gum, pectin, dextran, carrageenan, guar, sodium CMC, hyaluronic acid (HA), and albumin).

[0047] Polymeric stabilizers are typically surfactants that reduce surface tension and / or dispersants such as polyelectrolytes and some inorganic salts that stabilize particles by providing a surface charge (electrostatic interaction or electrosteric hindrance). Examples of polyelectrolytes include alkali salts of poly(methyl acrylate) and poly(methyl methacrylate), magnesium and calcium carbonate, calcium phosphate, and aluminum chloride. Other stabilizers include methylcellulose and ethylcellulose, poly(vinyl alcohol), gums, water-soluble non-micelle-forming polymers such as alginates, casein, gelatin, starch, talc, silicates, clays, and nanoparticles such as bentonite.

[0048] Water-miscible organic solvents The water-miscible organic solvent used in the present process can be selected from solvents known in the art. Such organic solvents can form a homogeneous mixture with water under the conditions of the present process for a given time without separation of liquid phases (e.g., into polar and non-polar phases). For example, the solvent can be selected from the group consisting of alcohol, dimethylacetamide, acetic acid, diethylene glycol dimethyl ether, dimethylformamide, 1,4-dioxane, ethylene glycol, hexamethylphosphoramide, hexamethylphosphoramide, pyridine, water, and combinations thereof.

[0049] The water-miscible organic solvent should remain fluid and preferably have a relatively low viscosity under the conditions of the process to avoid process interference.The specific water-miscible organic solvent and the amount of this component used in the process should also be selected to avoid solvent precipitation.Flory-Huggins interaction parameters can be used to evaluate the compatibility of the polymer(s) and water-miscible organic solvent(s) used in the process.

[0050] Antisolvent A polar solvent is also used as a poor solvent in the process to induce precipitation of the mica pigment from the solution. Deionized water may be used, for example, optionally with other additives such as polyvinyl alcohol. Such additives should be selected to avoid precipitation of the additive or an undesirable increase in the viscosity of the liquid mixture. For example, polyvinyl alcohol having a molecular weight of about 10,000 to about 100,000 may be used as an additive in an amount of typically about 0.01% to about 3% by weight, or about 0.05% to about 2% by weight. Other aqueous solutions or polar solvents may also be used.

[0051] Preparation process of mica pigment As generally shown in FIG. 1, mica particles are combined with polyester and polymeric stabilizer to form a first fluid mixture in the present process for preparing mica pigment for use in powder coating applications. Preferably, the polyester is added in solid form, e.g., powdered or pelletized, and combined with the mica pigment particles to form a powder or loose particulate mixture. Alternatively, the polyester particles can be first dissolved in a solvent before being combined with the mica pigment particles. These components can be combined in various ways, e.g., before contacting them with the water-miscible organic solvent, simultaneously with the addition of the water-miscible organic solvent, or the mica component can be pre-slurried in the water-miscible organic solvent and then added to the polyester and polymeric stabilizer components. The fluid mixture is a liquid suspension due to the presence of mica particles in the mixture.

[0052] The mica particles may be included in the mica pigment in an amount of about 2% to about 60% by weight, or about 10% to about 50% by weight, or about 20% to about 40% by weight, based on the total weight of the particulates produced by the process. To produce such a pigment, the mica should be added to the first fluid mixture in an amount of about 2% to about 60% by weight, or about 10% to about 50% by weight, or about 20% to about 40% by weight, based on the total weight of the polyester in the first fluid mixture. The mica, polyester, and stabilizer components at this stage may be mixed in amounts (parts per hundred) ranging from 2 to 60 parts mica, 50 to 90 parts polyester, and 8 to 25 parts stabilizer. In one embodiment, for example, the ratio of mica / polyester / stabilizer may be 11:73:16 parts per hundred.

[0053] The mica particles, polyester, polymeric stabilizer, and water-miscible organic solvent should be heated to a temperature at which the polyester and polymeric stabilizer components dissolve in the organic solvent to form a first fluid mixture if a temperature above ambient temperature is required for this. The components of the fluid mixture may be heated after being combined, or one or more of the components may be heated before being combined with the other components of the first fluid mixture. The first fluid mixture may be heated, for example, to a temperature of about 40°C to about 90°C, or about 70°C to about 80°C.

[0054] Following the creation of the first fluid mixture, a polar solvent (anti-solvent) is added to the first fluid mixture to form a second fluid mixture. The anti-solvent is preferably added in a metered manner, i.e., in a controlled amount over a predefined time period. For example, the anti-solvent may be added to the first fluid mixture in a drop-wise manner. The anti-solvent may be added to the first fluid mixture at a rate of, for example, 0.5-20 g / min, 1-15 g / min, or 3-10 g / min, for a period of 30-120 minutes, 45-90 minutes, or 60-75 minutes. If the anti-solvent is added at a faster rate, the supersaturation level will be higher and smaller particles will be formed, while adding the anti-solvent at a slower rate will generally result in larger particles. Intimate mixing also affects the degree of supersaturation of the second fluid mixture, which affects nucleation and particle growth rates.

[0055] The second fluid mixture is preferably stirred, agitated or otherwise mixed during the addition of the antisolvent. In one embodiment, the first mixture can be heated, for example, to a temperature of about 75° C. to about 95° C., or about 80° C. to about 90° C., prior to and / or during the addition of the antisolvent. The second fluid mixture can be maintained at such temperature for a predetermined time, for example, from about 15 minutes to about 4 hours, or from about 30 minutes to about 2 hours, or from about 45 minutes to about 1 hour, following the initiation of the antisolvent addition to the first fluid mixture. Following such heating, the second fluid mixture can be cooled to promote precipitation.

[0056] Nucleating agents may also be added to the liquid mixture in the process to promote precipitation of the mica pigment product of the process. The nucleating agent may be added before the addition of the anti-solvent, after the addition of the anti-solvent, or simultaneously with the anti-solvent. An example of such a nucleating agent is colloidal silica, which may be added after or together with the addition of the anti-solvent. Other nucleating agents that may be used include minerals such as chalk, clay, kaolin, talc, and silicates, and pigments such as cadmium red, cobalt yellow, then chromium oxide, titanium dioxide, magnesium oxide, carbonates, sulfates, carbon black, salts of carboxylic acids, benzophenone, and some polymers, and other organic liquids. Other nucleating agents that may be used include molybdenum disulfide, iron sulfide, titanium dioxide, talc, and sodium phenylphosphinate, sodium benzoate boron nitride, aromatic carboxylates, sodium benzoate, talc, and some pigment colorants. New nucleating agents that may be used include phosphate ester salts and supernucleating agents with faster processing speeds.

[0057] In one embodiment, colloidal silica in water is added to the first fluid mixture to pre-nucleate or "pre-seed" the first fluid mixture. In another embodiment, the nucleating agent can be included in the anti-solvent. For example, an anti-solvent containing up to about 30% by weight colloidal silica can be added to the second fluid mixture. Nucleation affects the reaction rate and the particle size and distribution.

[0058] After addition of the anti-solvent to the first fluid mixture, a precipitate containing the mica pigment is formed in the second fluid mixture. The precipitate particles are separated from the second fluid mixture by methods known in the art, such as by centrifugation. The separated particles can be washed and further centrifuged to prepare the final mica pigment, and / or the particles can be subjected to freeze-drying to prepare the mica pigment.

[0059] Spherical particles containing mica, such as those produced by the present process, have not previously been known for use in powder coating applications. The solvent / anti-solvent system of the present method allows for better control over the properties of such particles, which can be smaller and more spherical than current mica-containing particles. The final product can be modified by varying the degree of loading of the polymer into the pigment, resulting in pigment particles of different colors and luster.

[0060] Mica Pigments for Powder Coating Applications The present mica pigments generally comprise flakes of mica incorporated within and on the surface of polymer particles. As best seen in Figure 6, flat lamellar layers of metal oxide coated mica are attached to the surface of roughly spherical polymeric material. The particles are formed by precipitation of the polymeric material in solution, and as the precipitate forms, the mica becomes incorporated within the precipitated particles as well as attached to the surface of such particles.

[0061] An advantageous feature of the particles of the present mica pigments is that they are generally spherical, even when incorporating sheet-like materials such as mica. This can be seen, for example, in Figures 4-6, which are SEM micrographs of samples of the present mica pigment compositions, showing the capture of spherical particles. The greater sphericity provides improved flow characteristics to the mica-containing pigment compositions, facilitating application of the compositions, for example, by electrostatic powder coating applicators.

[0062] The spherical nature of the mica pigment particles can be measured by their circularity. These particles can have, for example, a circularity of about 0.93 to about 0.999, about 0.95 to about 0.995, or about 0.96 to about 0.990. Circularity can be determined, for example, using a Sysmex FPIA-3000 Particle Characterization System, or a Sysmex FPIA-2100 Flow Particle Image Analyzer, available from Malvern Instruments Ltd. (Worcestershire, UK). In flow particle image analysis, a sample is taken from a dilute suspension of particles, which is then passed through a measurement cell where images of the particles are captured, such as with strobe illumination and a CCD camera. The digital image of each particle is extracted and quantified, such as by using grayscale level differences ("thresholds") to identify particle pixels from background pixels, and by tracking the perimeters of individual particles and calculating their areas by edge definition.

[0063] The particles of the mica-containing pigment composition also advantageously have a narrow particle size distribution (geometric standard deviation), such as a geometric standard deviation of about 1.3 to about 2.0. The size of such pigment particles can be determined by photographic methods, such as by use of a particle image analyzer as described above, and the GSD (geometric standard deviation) can then be calculated using methods known in the art based on such size data. One way to express the distribution width is as a span, which can be represented by the following formula:

[0064]

number

[0065] The parameter Dv0.9 [or Dv(90)] refers to the point in the size distribution up to which 90% of the total volume of material in the sample is contained.

[0066] A narrow size distribution is better for dispersing the pigment evenly from an electrostatic applicator onto a substrate and creating a thin layer of pigment on the substrate surface. An example of the narrow size distribution of the pigment particles can be seen, for example, in Figures 2 and 3, which display the particle sizes of two samples of the mica-containing pigment composition.

[0067] The average particle size of the particles of the mica-containing pigment composition can also be calculated from the size data described above. The average size of the particles comprising the pigment will vary depending in part on the size of the mica particles used to form the pigment, but can be, for example, from about 50 micrometers to about 250 micrometers, from about 100 micrometers to about 200 micrometers, or from about 125 micrometers to about 175 micrometers. The average particle size can be D50, i.e., the size at which half of the particles are larger and half are smaller, and can be determined, for example, using a Multisizer 3 Coulter Counter manufactured by Beckman Coulter (Indianapolis, IN).

[0068] The aspect ratio of the particles produced by the process is preferably in the range of about 1. Preferably, the particles have an aspect ratio of about 0.93 to about 0.999, about 0.95 to about 0.995, or about 0.96 to about 0.990. The average aspect ratio of the particles is also preferably about 0.93 to about 0.999, about 0.95 to about 0.995, or about 0.96 to about 0.990. The minimum size of the pigment particles of the present invention is limited by the size of the mica particles used in the process, and the particles can generally only be as small as the aspect ratio of the mica particles used. The diameter of the mica particles used in the process is generally 5 to 200 μm, with a thickness showing a dimension of less than 1 μm, and therefore the aspect ratio can reach values ​​of up to 200 in some cases.

[0069] The pigment particles can impart a variety of gloss finishes to a substrate surface. Gloss can be measured, for example, at angles of 20°, 45°, 60°, 75°, or 85°, as known to those skilled in the art. The pigments can have a gloss ranging, for example, from about 10GU to about 70GU, from about 20GU to about 60GU, or from about 30GU to about 50GU.

[0070] The ability to create such spherical and narrowly distributed particles can reduce material usage rates, provide better material flow during application, and provide more consistent powder coating thickness on the substrate. Power production costs are also reduced compared to current bonding techniques that use energy thermal polymers such as polyesters at their softening point. Mica-containing particles have improved mechanical properties, as well as increased dimensional stability, stiffness, and strength. Mica-reinforced plastics also have high thermal dimensional stability, reduced warpage, and are used as mold release compounds. Mica also reduces gas permeation and improves elasticity.

[0071] Mica pigment application The mica-containing pigment composition can be applied as a decorative coating to a variety of articles and surfaces, such as appliances, auto parts, consumer electronics, furniture, bicycles, and heavy machinery. As discussed above, mica particles can have a variety of colors and reflectance levels, and thus the mica pigment imparts such qualities to the substrate to which it is applied. The applied coating provides a decorative appearance due to its optical properties (interference colors), as well as a textured appearance.

[0072] The mica-containing pigment composition is preferably a powder coating applied to a substrate by electrostatic spraying using an electrostatic application device. Such devices may use tribo or corona charging. During corona charging, a high voltage potential is generated at an electrode located in or near a stream of powder containing the pigment composition. The powder particles become negatively charged and are attracted to the grounded substrate. Alternatively, a substrate may be coated with the pigment composition using a fluidized bed by passing the substrate through a charged cloud of powder containing the mica-containing pigment composition.

[0073] The mica-containing pigment composition may be applied in a variety of thicknesses depending on the particular application of the coating. In applications where the item is expected to experience significant wear and tear or harsh environmental conditions, the coating may be applied at a greater thickness, while decorative coatings may be thinner. Decorative coatings are typically applied at a thickness of 0.025 mm to 0.10 mm, such as 1.5 to 3.5 mils (0.038 mm to 0.089 mm), or 2.5 to 3 mils (0.064 mm to 0.076 mm) (1 mil = 0.0254 mm). Coatings that require more protection may be thicker, such as 0.25 mm to 0.76 mm.

[0074] After a layer of the mica-containing pigment composition is applied to a substrate, the applied coating layer is heat cured, for example, at a temperature of from about 90°C to about 180°C, or from about 100°C to about 130°C. EXAMPLES

[0075] Example 1: Preparation of Mica-Containing Pigments A golden mica material was obtained from Black Diamond pigment. The mica used in the following process was made up mainly of TiO2, while the core mica itself was mainly silica and magnesium, as well as SiO2. The elemental composition was as follows:

[0076] [table] TIFF0007580922000003.tif12168

[0077] Two sets of polyester microparticles were compounded with phlogopite pigment. One batch ("Batch 1") used both high molecular weight (50-55K) and low molecular weight (18-20K) amorphous polyester (1:1), while the second batch ("Batch 2") contained only high molecular weight polyester. The colloidal silica (Si) used in these experiments was a 30 wt. % suspension in water designated Ludox® AM (available from W. R. Grace and Company, Columbia, Maryland). The Si loading in these experiments was relatively high, about 10-20%, but the amount of Si detected after washing and drying of the final product was low. In Batch 1, the silica was added after the anti-solvent stage solution, and for Batch 2, some of the silica was added with the organic phase / polyester, while the remaining amount was mixed with the anti-solvent solution and added by a metering pump (available from Fluid Metering, Inc.).

[0078] Into a 1 L three-neck round bottom flask, 65.7 g of polyester resin was added in dimethylacetamide (DMAc, 370.2 g, water miscible high boiling point solvent) along with 10.4 g of Venetian Gold Mica pigment and 13.8 g of polyvinyl alcohol (PVA, 78K). Mixing was started at about 420 rpm to begin dissolving the polymer. While still at ambient temperature (23° C.), 42.0 g of colloidal silica (30 wt % solution, 12.6 g Si) was added to help pre-seed the organic phase before anti-solvent addition began. The polymer solution was heated to 90° C. and a solution of PVA / Si in deionized water (4.06 g 78K PVA in 224.9 g DIW as anti-solvent with 69.9 g of 30 wt % colloidal Si) was added dropwise to the flask using a metering pump while stirring at 640 RPM. Approximately 10 minutes after the addition of the PVA aqueous solution, the solvent solution went from a clear light yellow to a white opaque color. The PVP / Si aqueous solution was added over approximately 75 minutes and heating was stopped within 30 minutes. The opaque solution was left to cool and stirred at 370 RPM overnight. The next day, the solution was transferred to a 1 L centrifuge bottle and centrifuged at 3000 RPM for 15 minutes to remove the DMAc / DIW mixture. The particles were resuspended in DIW and mixed by shaking for approximately 30 seconds before centrifuging them again for 15 minutes at 3000 RPM. This washing / centrifugation procedure was repeated one more time to concentrate the particles and transfer them to a freeze-drying bottle. The particle slurry was quickly frozen and then placed in a freeze-dryer where the bottled particles were subjected to a high vacuum that removed the ice by sublimation.

[0079] The particles were submitted for thermogravimetric analysis, gel permeation chromatography (GPC), and inductively coupled plasma (ICP) analysis. Digital microscopy and SEM were also used to characterize the particle shape, surface structure, particle size, and particle size distribution. Figure 2 shows the size data collected from image analysis of batch 1, and Figure 3 shows the size data collected from image analysis of batch 2. Figures 4 to 6 are SEM images of the particles of batch 1. The SEM images clearly show the presence of phlogopite pigment on the surface of the spherical particles.

[0080] Example 2: Properties of mica pigments The properties of the mica-containing pigment composition produced in Example 1 are listed in Table 1 below.

[0081] [Table 1]

[0082] The size distribution of the particles produced in Example 1 is shown in Figures 2 and 3. Figure 2 is a bar graph showing the digital microscope image analysis of batch 1, whereas Figure 3 is a bar graph showing the digital microscope image analysis of batch 2.

[0083] Although the present invention has been described in some detail with reference to certain preferred embodiments, other embodiments are possible. The steps disclosed in the method are, for example, not intended to be limiting and are not intended to indicate that each step is necessarily essential to the method, but are instead merely exemplary steps. Therefore, the scope of the appended claims should not be limited to the description of the preferred embodiments contained in this disclosure.

[0084] The recitation of ranges of values ​​herein is intended merely to serve as a shorthand method for individually referring to each separate value falling within the range. Unless otherwise stated herein, each separate value is incorporated herein as if it were individually recited herein. All references cited herein are incorporated by reference in their entirety.

Claims

1. 1. A method for producing a mica-containing pigment composition comprising spherical pigment particles, comprising: providing an amorphous polyester resin, a polymeric stabilizer comprising a water soluble polymer, and mica particles; dissolving said polyester resin and a polymeric stabilizer together with said mica particles in a water-miscible organic solvent to form a first fluid mixture including said mica particles; adding a polar solvent to the first fluid mixture at a predetermined rate, thereby forming a second fluid mixture containing precipitated pigment particles; and collecting the precipitated pigment particles. The polymeric stabilizer may be selected from the group consisting of polyvinyl acetate, poly(methyl methacrylate), poly(acrylonitrile), poly(dimethylsiloxane), polyvinyl chloride, polyethylene, polypropylene, poly(lauryl methacrylate), poly(oxyethylene), poly(acrylamide), poly(vinyl alcohol), poly(acrylic acid), poly(methacrylic acid), polyvinylpyrrolidone, polyethyleneimine, poly(vinyl methyl ether), poly(4-vinylpyridine), poly(12-hydroxystearic acid), poly(isobutylene), cis-1:4-poly(isoprene), carboxymethylcellulose, gelatin, polysorbate 80, polysorbate 20, hydroxypropyl methylcellulose, copovidone, and polyvinylpyrrolidone, polyethylene glycol (PEG), polymethacrylate, hypromellose acetate succinate, hypromellose phthalate, polyvinyl caprolactam-polyvinyl acetate- The polymer is selected from the group consisting of polyethylene glycol graft copolymer, polyvinyl acetate phthalate, cellulose acetate phthalate, and combinations thereof.

2. The method of claim 1 further comprising the step of adding silica to the second fluid mixture.

3. 10. The method of claim 1 further comprising the step of adding silica to the first fluid mixture prior to the addition of the polar solvent solution to the first fluid mixture.

4. The method of claim 1 , wherein the polyester resin, the polymeric stabilizer, and the mica particles are added together before being placed in contact with the water-miscible organic solvent.

5. 10. The method of claim 1, wherein the mica particles are added to the water-miscible organic solvent before the polyester resin and polymeric stabilizer are placed in contact with the water-miscible organic solvent.

6. 2. The method of claim 1, wherein the water-miscible organic solvent is selected from the group consisting of dimethylacetamide, acetic acid, diethylene glycol dimethyl ether, dimethylformamide, 1,4-dioxane, ethylene glycol, hexamethylphosphoramide, hexamethylphosphoramide, pyridine, and combinations thereof.

7. The polyester resin is selected from the group consisting of poly(propoxylated bisphenol co-fumarate), poly(ethoxylated bisphenol co-fumarate), poly(butyloxylated bisphenol co-fumarate), poly(copropoxylated bisphenol co-ethoxylated bisphenol co-fumarate), poly(1,2-propylene fumarate), poly(propoxylated bisphenol co-maleate), poly(ethoxylated bisphenol co-maleate), poly(butyloxylated bisphenol co-maleate), poly(copro 2. The method of claim 1, wherein the poly(1,2-propylene itaconate) is selected from the group consisting of poly(1,2-propylene maleate), poly(1,2-propylene itacon ...

8. The method of claim 1, wherein the polyester resin has a glass transition temperature of from about 45° C. to about 75° C., where "about" refers to an amount within 10% of the referenced amount.

9. The method of claim 1 , wherein the mica has a particle size of about 5 micrometers to about 200 micrometers, where "about" refers to an amount within 10% of a referenced amount.

10. 10. The method of claim 1, wherein the second mixture is heated to a temperature of about 75° C. to about 95° C., where "about" refers to an amount within 10% of a referenced amount.

11. The method of claim 1, wherein the pigment particles comprise a polymeric material having mica flakes embedded therein and thereon, and the pigment particles of the composition have a circularity of from about 0.93 to about 0.999 and a geometric size distribution of from about 1.3 to about 2.

0.

12. The method of claim 11, wherein the pigment particles have a circularity of from about 0.95 to about 0.995, "about" referring to an amount within 10% of a referenced amount.

13. 12. The method of claim 11, wherein the pigment particles have an average particle size of from about 50 micrometers to about 250 micrometers, "about" referring to an amount within 10% of a referenced amount.

14. The method of claim 11, wherein the mica is present in the pigment particles in an amount of from about 2% to about 60% by weight of the particles, "about" referring to an amount within 10% of a referenced amount.

15. The method of claim 11, wherein the mica has an average particle size of from about 5 micrometers to about 150 micrometers, "about" referring to an amount within 10% of a referenced amount.

16. The method of claim 11 , wherein the composition has a metallic color.

17. The method of claim 11, wherein the composition has a gloss in the range of about 10 GU to about 70 GU, "about" referring to an amount within 10% of a referenced amount.

18. 1. A method for forming a pigmented coating on a substrate, comprising: applying the mica-containing pigment composition produced by the method of claim 11 to the substrate using an electrostatic powder coating applicator; and curing the pigment composition on the substrate.

19. The coating is electrostatically transferred to the substrate via tribo- or corona charging.

20. The method of claim 18.

Citation Information

Patent Citations

  • Flaky base material having modified surface and improved in Anti-settling characteristic and re-dispersibility

    JP1993186707A

  • Pigment treatment method

    JP1993500984A

  • Surface-modified micaceous particle having improved dispersibility in aqueous medium

    JP1994025267A

  • Mica-based pigment coated with alkylene glycol alkyl ether

    JP1996508061A

  • Inorganic fine particles for electrostatic charge image developing toner, electrostatic charge image developing toner, developer, image forming apparatus, and image forming method

    JP2004252147A