Positive electrode active material for all-solid-state lithium ion battery, positive electrode for all-solid-state lithium ion battery, all-solid-state lithium ion battery, and method for producing positive electrode active material for all-solid-state lithium ion battery

A high nickel composition for all-solid-state lithium-ion batteries is achieved by coating LiNiCoMnO2 core particles with LiNbO3, addressing high resistance issues and improving battery output through reduced interfacial reactions and diffusion resistance.

JP7581102B2Active Publication Date: 2024-11-12JX NIPPON MINING & METALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021047832
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-11-12
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing all-solid-state lithium-ion batteries face high resistance issues due to the formation of a high-resistance layer between the positive electrode active material and the solid electrolyte, particularly in high nickel compositions where the nickel ratio exceeds 80 mol%, which affects the battery's output and performance.

Method used

A positive electrode active material with a high nickel composition is developed, featuring core particles of LiNiCoMnO2 coated with a thin layer of LiNbO3, produced using an alkoxide solution in a tumbling fluidized bed apparatus to minimize interfacial reactions and resistance.

Benefits of technology

The solution results in a low-resistance NiCoMn-based positive electrode active material with improved output characteristics by reducing interfacial resistance and diffusion transfer resistance, enhancing the performance of all-solid-state lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581102000002
    Figure 0007581102000002
  • Figure 0007581102000001
    Figure 0007581102000001
Patent Text Reader

Abstract

To provide a low-resistance NiCoMn-based cathode active material, which is a cathode active material for an all-solid lithium ion battery and which has a high nickel composition of 80 mol% or more in Ni proportion.SOLUTION: A cathode active material for an all-solid lithium ion battery comprises: a core cathode active material particle; and a coating layer. The core cathode active material particle is represented by a composition given by the following formula (1): LiaNibCocMndOe (1). (In the formula (1), 1.0≤a≤1.05, 0.8≤b≤0.9, 1.8≤e≤2.2 and b+c+d=1.) The coating layer is composed of oxide of Li and Nb; a specific surface area X(m2 / g) of the cathode active material and a Nb content Y (mass%) in the cathode active material (mass%) satisfy the relation given by the following expression (2): 0.65≤Y / X≤1.20 (2).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for an all-solid-state lithium ion battery, a positive electrode for an all-solid-state lithium ion battery, an all-solid-state lithium ion battery, and a method for producing the positive electrode active material for an all-solid-state lithium ion battery. [Background technology]

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium ion batteries have attracted attention from the viewpoint of their high energy density. In addition, there is a demand for improvements in the energy density and battery characteristics of lithium secondary batteries for large-scale applications such as vehicle-mounted power sources and load leveling.

[0003] However, in the case of lithium-ion batteries, the electrolyte is mostly organic compounds, and even if a flame-retardant compound is used, it cannot be said that there is no risk of fire. As an alternative to these liquid-based lithium-ion batteries, all-solid-state lithium-ion batteries, which use a solid electrolyte, have been attracting attention in recent years. Among them, all-solid-state lithium-ion batteries that use sulfides such as Li2S-P2S5 as the solid electrolyte or that add lithium halides to them are becoming mainstream.

[0004] In all-solid-state lithium-ion batteries that use sulfide-based solid electrolytes, a high-resistance layer is formed due to a reaction between the positive electrode active material and the solid electrolyte, resulting in a decrease in output. A method for suppressing the formation of this high-resistance layer is known in which the surface of the positive electrode active material is coated with a Li composite oxide. A typical Li composite oxide for coating the surface of the positive electrode active material is LiNbO3, which exhibits high ionic conductivity.

[0005] Patent Document 1 discloses an all-solid-state battery having a cathode active material having an oxide cathode active material, a coating portion made of a lithium niobate-based compound formed on the surface of the oxide cathode active material, and a solid electrolyte layer containing a sulfide solid electrolyte material. The oxide cathode active material is LiNiO2, and the oxide cathode active material is coated with LiNbO3 using an alkoxide solution.

[0006] Patent Document 2 describes a battery having an active material and lithium niobate attached to the surface of the active material, and having a BET specific surface area S [m 2 / g] is greater than 0.93 and less than 1.44.

[0007] Patent Document 3 discloses an all-solid-state lithium battery using a lithium ion conductive solid electrolyte as an electrolyte, characterized in that the lithium ion conductive solid electrolyte is mainly composed of sulfide and the surface of the positive electrode active material is coated with a lithium ion conductive oxide. LiCoO is used as the core particle of the positive electrode active material, and the core particle is coated with LiNbO3 using an alkoxide solution. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2010-225309 A [Patent Document 2] JP 2015-56307 A [Patent Document 3] Patent No. 4982866 Summary of the Invention [Problem to be solved by the invention]

[0009] In Patent Documents 1 to 3, materials such as LiCoO, NiCoMn with a molar ratio of 1:1:1, or LiNiO2 are used as core particles of the positive electrode active material. These documents do not describe a technique for producing a so-called high-nickel product in which the ratio of Ni exceeds 80 mol% in a ternary (Li(Ni,Co,Mn)O2) positive electrode active material.

[0010] However, in a NiCoMn-based positive electrode active material having a so-called high nickel composition in which the Ni ratio is 80 mol % or more, there is a problem that the resistance becomes high when the material is coated with an oxide of Li and Nb such as LiNbO3. [Means for solving the problem]

[0011] The present invention has been made to solve the above-mentioned problems, and aims to provide a low-resistance NiCoMn-based positive electrode active material for all-solid-state lithium-ion batteries, which has a so-called high-nickel composition in which the ratio of Ni is 80 mol % or more. Another aim of the present invention is to provide a positive electrode for all-solid-state lithium-ion batteries, an all-solid-state lithium-ion battery, and a method for producing the positive electrode active material for all-solid-state lithium-ion batteries, which use the positive electrode active material for all-solid-state lithium-ion batteries.

[0012] The present invention, which has been completed based on the above findings, is defined in the following items 1 to 7. 1. A positive electrode active material for an all-solid-state lithium-ion battery, comprising core positive electrode active material particles and a coating layer, The core positive electrode active material particles are represented by the composition shown in the following formula (1): Li a Ni b Co c Mn d O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.) The coating layer is an oxide of Li and Nb, The specific surface area X (m 2 / g) and a Nb content Y (mass %) in the positive electrode active material satisfy the relationship of the following formula (2): 0.65≦Y / X≦1.20 (2) 2. The positive electrode active material for an all-solid-state lithium ion battery according to 1 above, wherein the positive electrode active material for an all-solid-state lithium ion battery has a 50% cumulative volume particle size D50 of 3 to 7 μm. 3. The positive electrode active material for an all-solid-state lithium ion battery according to 1 or 2 above, wherein the coating layer contains LiNbO3. 4. A positive electrode for an all-solid-state lithium ion battery, comprising the positive electrode active material for an all-solid-state lithium ion battery according to any one of 1 to 3 above. 5. An all-solid-state lithium ion battery comprising: a positive electrode layer composed of the positive electrode for an all-solid-state lithium ion battery according to 4 above; a negative electrode layer; and a solid electrolyte layer. 6. A step of preparing core positive electrode active material particles represented by the composition shown in the following formula (1); Li a Ni b Co c Mn d O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.) A step of forming a coating layer made of an oxide of Li and Nb on the surface of the core positive electrode active material particles by using an alkoxide solution containing Li and Nb with a tumbling fluidized bed apparatus; The method for producing a positive electrode active material for an all-solid-state lithium ion battery includes the steps of: 7. The method for producing a positive electrode active material for an all-solid-state lithium ion battery according to 6 above, wherein the alkoxide solution is a solution containing: (1) one of methoxylithium, ethoxylithium, and isopropoxylithium as a lithium source for a solute; (2) one of pentamethoxyniobium, pentaethoxyniobium, and pentaisopropoxyniobium as a niobium source; and (3) one of ethanol, methanol, and isopropanol as a solvent. Effect of the Invention

[0013] According to the present invention, it is possible to provide a low-resistance NiCoMn-based positive electrode active material for an all-solid-state lithium-ion battery having a so-called high nickel composition with a Ni ratio of 80 mol % or more. Also, according to the present invention, it is possible to provide a positive electrode for an all-solid-state lithium-ion battery using the positive electrode active material for an all-solid-state lithium-ion battery, an all-solid-state lithium-ion battery, and a method for producing the positive electrode active material for an all-solid-state lithium-ion battery. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram of an all-solid-state lithium-ion battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0016] (Positive electrode active material for all-solid-state lithium-ion batteries) The positive electrode active material for an all-solid-state lithium ion battery according to an embodiment of the present invention includes core positive electrode active material particles and a coating layer. The core positive electrode active material particles have a composition represented by the following formula (1). Li a Ni b Co c Mn d O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.)

[0017] In the above formula (1), the core positive electrode active material particles have a controlled lithium composition a of 1.0≦a≦1.05. Since the lithium composition a is 1.0 or more, it is possible to suppress the reduction of nickel due to lithium deficiency. Furthermore, since the lithium composition a is 1.05 or less, it is possible to suppress residual alkaline components such as lithium carbonate and lithium hydroxide present on the surface of the core positive electrode active material particles, which may become resistance components when used in a battery.

[0018] In the core positive electrode active material particles, the nickel composition b in the above formula (1) is controlled to be 0.8≦b≦0.9, which is a so-called high nickel composition. Since the nickel composition b is 0.8 or more, a good battery capacity of the all-solid-state lithium ion battery can be obtained.

[0019] In the core positive electrode active material particles, the sum of c, which indicates the cobalt composition, and d, which indicates the manganese composition, satisfies b+c+d=1 in the above formula (1), that is, 0.1≦c+d≦0.2, so that the cycle characteristics are improved and the expansion and contraction behavior of the crystal lattice due to the insertion and desorption of lithium during charging and discharging can be reduced. If the c+d is less than 0.1, it becomes difficult to obtain the effects of the cycle characteristics and expansion and contraction behavior described above, and if the c+d exceeds 0.2, the amount of cobalt and manganese added is too large, which may result in a large decrease in the initial discharge capacity or may be disadvantageous in terms of cost.

[0020] The core positive electrode active material particles may have a form in which a majority of a plurality of primary particles are aggregated into secondary particles, and may partially contain primary particles that are not aggregated as secondary particles. The shapes of the primary particles constituting the secondary particles and the primary particles existing alone are not particularly limited, and may be various shapes such as, for example, substantially spherical, substantially elliptical, substantially plate-like, and substantially needle-like. The form in which a plurality of primary particles are aggregated is also not particularly limited, and may be various forms such as, for example, a form in which the particles are aggregated in a random direction, or a form in which the particles are aggregated almost uniformly radially from the center to form substantially spherical or substantially elliptical secondary particles.

[0021] When the core positive electrode active material particles contain lithium hydroxide, which is excess lithium generated in the manufacturing process, etc., the content of the lithium hydroxide is preferably 1.5 mass% or less, and more preferably 1.0 mass% or less. If the lithium hydroxide content in the core positive electrode active material particles exceeds 1.5 mass%, the lithium hydroxide is oxidized and decomposed, and gas is likely to be generated when the positive electrode active material is charged in a high-temperature environment.

[0022] When the core positive electrode active material particles contain lithium carbonate, which is excess lithium generated in the manufacturing process, etc., the content of the lithium carbonate is preferably 1.5 mass% or less, and more preferably 1.0 mass% or less. If the lithium carbonate content in the core positive electrode active material particles exceeds 1.5 mass%, the lithium carbonate is oxidized and decomposed, and gas is easily generated when the positive electrode active material is charged in a high-temperature environment.

[0023] The contents of lithium hydroxide and lithium carbonate contained in the core positive electrode active material particles can be determined by neutralization titration. Lithium hydroxide and lithium carbonate as excess lithium present on the surface of the lithium metal composite oxide particles are dissolved in water, and hydroxide ions and carbonate ions are ionized from the lithium ions, respectively. These ionized anions can be titrated with an inorganic acid, etc., which makes it possible to separately quantify lithium hydroxide and lithium carbonate.

[0024] The moisture content of the core positive electrode active material particles is preferably 0.10% by mass or less, more preferably 0.05% by mass or less. If the moisture content of the core positive electrode active material particles exceeds 0.10% by mass, the metal elements constituting the positive electrode may be damaged, and various battery characteristics may be deteriorated. The moisture content of the core positive electrode active material particles may be measured by dry weight method, Karl Fischer titration method, distillation method, etc.

[0025] The coating layer is an oxide of Li and Nb. By coating the surface of the core positive electrode active material particle with a coating layer of this configuration, the reaction occurring at the interface between the core positive electrode active material particle and the solid electrolyte is suppressed. Therefore, it is possible to suppress deterioration of the core positive electrode active material particle. Examples of the oxide of Li and Nb that constitutes the coating layer include LiNbO3.

[0026] The positive electrode active material for an all-solid-state lithium ion battery according to the embodiment of the present invention has a specific surface area X (m 2 / g) and the Nb content Y (mass %) in the positive electrode active material satisfy the relationship of the following formula (2). 0.65≦Y / X≦1.20 (2)

[0027] If the surface of the core positive electrode active material particle can be covered as entirely and as thinly as possible with a coating layer made of an oxide of Li and Nb, the resistance component of the battery can be reduced and the output characteristics can be improved. More specifically, if the surface of the core positive electrode active material particle can be covered as entirely as possible with a coating layer made of an oxide of Li and Nb, the resistance increase due to the interface reaction between the solid electrolyte and the positive electrode active material when exposed to a high potential during charging can be suppressed. In addition, by forming a coating layer made of an oxide of Li and Nb as thin as possible on the surface of the core positive electrode active material particle, the movement of Li ions in the coating layer during charging and discharging can be shortened, and the diffusion movement resistance can also be reduced. As described above, the resistance is particularly problematic in a positive electrode active material having a so-called high nickel composition in which the ratio of Ni is 80 mol % or more. From this viewpoint, in the positive electrode active material according to the embodiment of the present invention having a high nickel composition, the specific surface area X (m 2A low-resistance NiCoMn-based positive electrode active material can be obtained by controlling Y / X, which is the ratio of the Nb content Y (mass%) in the positive electrode active material to the specific surface area (m2 / g), to 0.65≦Y / X≦1.20. If the Y / X ratio is less than 0.65, there will be many uncoated portions, which may cause the solid electrolyte and the positive electrode active material to come into direct contact with each other, resulting in the problem of a high-resistance layer being formed. If the Y / X ratio exceeds 1.20, the coating layer will become too thick, which may cause the problem of increased resistance to the diffusion and migration of Li ions. The specific surface area X (m2) of the positive electrode active material can be calculated by controlling the specific surface area X (m2 / g) of the positive electrode active material to 0.65≦Y / X≦1.20. 2 The ratio Y / X of the Nb content Y (mass %) in the positive electrode active material to the Nb content (mass %) of the positive electrode active material (Nb / g) is preferably 0.65≦Y / X≦1.0, and more preferably 0.65≦Y / X≦0.75.

[0028] The 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is preferably 3 to 7 μm. Here, the 50% cumulative volume particle size D50 is the volume particle size at 50% accumulation in a volume-based cumulative particle size distribution curve. When the 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is 3 μm or more, the specific surface area is suppressed and the amount of Li and Nb oxide coating can be suppressed. When the 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is 7 μm or less, the specific surface area can be suppressed from becoming excessively small. The 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is more preferably 3 to 6 μm, and even more preferably 4 to 5 μm. The 50% cumulative volume particle size D50 can be measured by a Microtrac laser diffraction type particle size distribution measuring device "MT3300EXII".

[0029] (Method of manufacturing positive electrode active material for all-solid-state lithium-ion batteries) Next, a method for producing a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention will be described in detail. In the method for producing a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention, first, core positive electrode active material particles having a composition represented by the following formula (1) are prepared. Li a Ni b Co c Mnd O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.)

[0030] The method for producing the core positive electrode active material particles is not particularly limited, and can be appropriately adjusted based on a known production method. For example, first, a NiCoMn-based composite hydroxide with a Ni composition of 0.8 to 0.9 in molar ratio is prepared. Next, the composite hydroxide is mixed with a Li source (Li carbonate, Li hydroxide, etc.) in a dry state using a Henschel mixer or the like by adjusting the mixing ratio of each raw material, and then fired at a temperature of 700 to 800°C for 12 to 24 hours to obtain a fired body. Thereafter, if necessary, the fired body can be crushed using, for example, a pulverizer to obtain core positive electrode active material particles.

[0031] Next, a coating liquid used for surface coating of the core positive electrode active material particles by the rolling fluidized bed apparatus is prepared. An alkoxide solution containing Li and Nb is used as the coating liquid. Using such an alkoxide solution containing Li and Nb as the coating liquid, a coating layer made of an oxide of Li and Nb is formed on the surface of the core positive electrode active material particles by a wet method using the rolling fluidized bed apparatus. By surface coating of the core positive electrode active material particles using the rolling fluidized bed apparatus, the particles constituting the coating layer are coated as thinly as possible over the entire surface of the core positive electrode active material particles as much as possible, which makes it possible to suppress the reaction between the positive electrode active material and the solid electrolyte and to reduce the diffusion movement resistance in the coating layer. In addition, since the coating state of the coating layer changes from partial coating to complete coating at a certain film thickness, the output of the all-solid-state battery is further improved by performing complete coating as close as possible to the critical point. In addition, the present inventors have found that when an alkoxide solution is used as the coating liquid, a gel is generated due to partial hydrolysis immediately after coating, making it easier to cover the surface, and thus the above-mentioned coating layer can be obtained.

[0032] The alkoxide solution used as the coating liquid is preferably a solution containing (1) any one of methoxylithium, ethoxylithium, and isopropoxylithium as a solute lithium source, (2) any one of pentamethoxyniobium, pentaethoxyniobium, and pentaisopropoxyniobium as a niobium source, and (3) any one of ethanol, methanol, and isopropanol as a solvent. With this configuration, the coating layer formed on the surface of the core positive electrode active material particles by the tumbling fluidized bed device can be formed more favorably and as thin as possible over the entire surface. The LiNbO3 concentration of the alkoxide solution is preferably 5 mass% or less. With this configuration, the coating layer is formed slowly, and it can be formed more favorably and as thin as possible over the entire surface.

[0033] The tumbling fluidized bed apparatus has a rotor at the bottom, and can fluidize the particles in the apparatus by sucking in the supply gas. Specifically, the core positive electrode active material particles are fluidized in the tumbling fluidized bed apparatus, and the alkoxide solution of the coating raw material is sprayed onto the core positive electrode active material particles and dried to form granules. The resulting granules are then fired in air or in an inert atmosphere to form a coating layer on the surface of the core positive electrode active material particles.

[0034] In the coating treatment using a tumbling fluidized bed device, the ratio of the alkoxide solution of the coating raw material to the core positive electrode active material particles is preferably in the range of 2:1000 to 1:100 in mass ratio, i.e., coating raw material (solute component):core positive electrode active material particles. In addition, in the above method, the intake air volume for fluidizing the core positive electrode active material particles is 0.15 to 0.3 m 3 It is preferable that the rate is about / min.

[0035] In the coating process using a tumbling fluidized bed apparatus, the intake air temperature in the tumbling fluidized bed apparatus is set to, for example, at least room temperature or higher and 80°C or lower, so that the alkoxide solution containing the coating raw material is coated on the surface of the core positive electrode active material particles. Then, the core positive electrode active material is baked at 200 to 350°C for about 1 to 5 hours in an oxygen atmosphere or in the air. In this way, the positive electrode active material for an all-solid-state lithium-ion battery according to the embodiment of the present invention is obtained, which has the core positive electrode active material particles and the coating layer formed on the surface of the core positive electrode active material particles.

[0036] (Positive electrodes for all-solid-state lithium-ion batteries and all-solid-state lithium-ion batteries) A positive electrode is formed by the positive electrode active material for an all-solid-state lithium ion battery according to the embodiment of the present invention, and the positive electrode is used as a positive electrode layer, and an all-solid-state lithium ion battery including the positive electrode layer, a solid electrolyte layer, and a negative electrode layer can be produced. The solid electrolyte layer and the negative electrode layer constituting the all-solid-state lithium ion battery according to the embodiment of the present invention are not particularly limited and can be formed of known materials and can have a known configuration as shown in FIG.

[0037] The positive electrode layer of the lithium ion battery can be a layer of a positive electrode mixture obtained by mixing the positive electrode active material for all-solid-state lithium ion batteries according to the embodiment of the present invention with a solid electrolyte. The content of the positive electrode active material in the positive electrode layer is, for example, preferably 50% by mass or more and 99% by mass or less, and more preferably 60% by mass or more and 90% by mass or less.

[0038] The positive electrode mixture may further include a conductive assistant. As the conductive assistant, a carbon material, a metal material, or a mixture thereof may be used. The conductive assistant may include at least one element selected from the group consisting of, for example, carbon, nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc. The conductive assistant is preferably a highly conductive carbon element, a metal element, a mixture, or a compound containing carbon, nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium. As the carbon material, for example, carbon black such as Ketjen Black, acetylene black, denka black, thermal black, and channel black, graphite, carbon fiber, activated carbon, and the like may be used.

[0039] The average thickness of the positive electrode layer of the lithium ion battery is not particularly limited and can be appropriately designed depending on the purpose. The average thickness of the positive electrode layer of the lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0040] The method for forming the positive electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the positive electrode layer of the lithium ion battery includes a method of compression molding positive electrode active material particles.

[0041] The negative electrode layer of the lithium ion battery may be a layer of a known negative electrode active material for all-solid-state lithium ion batteries. The negative electrode layer may be a layer of a negative electrode mixture obtained by mixing a known negative electrode active material for lithium ion batteries with a solid electrolyte. The content of the negative electrode active material in the negative electrode layer is, for example, preferably 10% by mass or more and 99% by mass or less, and more preferably 20% by mass or more and 90% by mass or less.

[0042] The negative electrode layer may contain a conductive assistant, as in the positive electrode layer. The conductive assistant may be the same material as that described in the positive electrode layer. As the negative electrode active material, for example, a carbon material, specifically, artificial graphite, graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, non-graphitizable carbon, or a mixture thereof may be used. As the negative electrode material, for example, a metal itself, such as metallic lithium, metallic indium, metallic aluminum, or metallic silicon, or an alloy in combination with other elements or compounds may be used.

[0043] The average thickness of the negative electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. The average thickness of the negative electrode layer of the lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0044] The method for forming the negative electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method for forming the negative electrode layer of the lithium ion battery include a method of compressing and molding negative electrode active material particles and a method of depositing a negative electrode active material.

[0045] The solid electrolyte can be a known solid electrolyte for all-solid-state lithium-ion batteries. Even if an oxide-based solid electrolyte is used as the solid electrolyte, the resistance in the all-solid-state lithium-ion battery using the positive electrode active material according to the embodiment of the present invention can be reduced. In particular, when a sulfide-based solid electrolyte is used as the solid electrolyte, a high-resistance layer is formed due to a reaction between the positive electrode active material and the solid electrolyte, which has been a problem in the past, and the output is reduced. However, according to the positive electrode active material according to the embodiment of the present invention, the entire positive electrode active material is covered as much as possible, so that the formation of a high-resistance layer can be well suppressed even in an all-solid-state lithium-ion battery having a sulfide-based solid electrolyte. In addition, by forming the coating layer as thin as possible, the movement of Li ions in the coating layer during charging and discharging is shortened, and the diffusion movement resistance can also be reduced. The resistance can be reduced by these two effects. Furthermore, as the solid electrolyte, a lithium-containing compound containing lithium and at least one element selected from niobium, tantalum, silicon, phosphorus, and boron may be used.

[0046] Examples of oxide-based solid electrolytes include LiTi2(PO4)3, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3, and Li2O-B2O3-ZnO.

[0047] Examples of sulfide-based solid electrolytes include LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li3PS4, and Li2S-P2S5.

[0048] Examples of solid electrolytes using a lithium-containing compound containing lithium and at least one element selected from niobium, tantalum, silicon, phosphorus, and boron include LiNbO3, Li 1.3 Al 0.3 Ti 0.7 (PO4)3, Li 1+x+y A x Ti 2-x S y P3-y O 12 (A=Al or Ga, 0≦x≦0.4, 0 <y≦0.6)、[(B 1 / 2 Li 1 / 2 ) 1-z C z ]TiO3(B=La, Pr, Nd, Sm, C=Sr or Ba, 0≦x≦0.5), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , LiPO (4-3 / 2w) N w (w<1), and Li 3.6 S 0.6 P 0.4 O4, etc., and LiI, LiI-Al2O3, LiN3, Li3N-LiI-LiOH, etc.

[0049] The average thickness of the solid electrolyte layer of the lithium ion battery is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the solid electrolyte layer of the lithium ion battery may be, for example, 50 μm to 500 μm, or 50 μm to 100 μm.

[0050] The method for forming the solid electrolyte layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the solid electrolyte layer of the lithium ion battery includes sputtering using a target material of the solid electrolyte, or compression molding of the solid electrolyte.

[0051] Other members constituting the lithium ion battery are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a positive electrode collector, a negative electrode collector, and a battery case.

[0052] The size and structure of the positive electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the positive electrode current collector include die steel, stainless steel, aluminum, aluminum alloys, titanium alloys, copper, gold, and nickel. The positive electrode current collector may have, for example, a foil shape, a plate shape, a mesh shape, etc. The average thickness of the positive electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0053] The size and structure of the negative electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the negative electrode current collector include die steel, gold, indium, nickel, copper, and stainless steel. The negative electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the negative electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0054] The battery case is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include known laminate films that can be used in conventional all-solid-state batteries, etc. Examples of the laminate film include a resin laminate film and a film in which a metal is vapor-deposited on a resin laminate film. The shape of the battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape of the battery include cylindrical, square, button, coin, and flat types. EXAMPLES

[0055] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0056] (Examples 1 to 6, Comparative Examples 1 to 6) First, a NiCoMn-based composite hydroxide with a Ni composition of 0.82 to 0.9 in molar ratio was prepared. Next, the composite hydroxide was mixed with Li hydroxide in a Henschel mixer while adjusting the mixing ratio of each raw material, and then fired at a temperature of 700 to 780°C for 12 to 24 hours to obtain a fired body. The fired body was then crushed with a pulverizer to obtain core positive electrode active material particles.

[0057] Next, a coating liquid used for surface coating of the core positive electrode active material particles by a tumbling fluidized bed apparatus was prepared. An alkoxide solution that becomes an ethanol solution of ethoxylithium and pentaethoxyniobium was used as the coating liquid. Specifically, the core positive electrode active material particles were fluidized in the tumbling fluidized bed apparatus, and the alkoxide solution of the coating raw material was sprayed onto the core positive electrode active material particles and dried to form a granule. Next, the obtained granule was fired in air or an inert atmosphere to form a coating layer on the surface of the core positive electrode active material particles.

[0058] In the wet coating process using the tumbling fluidized bed device, the concentration of the alkoxide solution, the ratio of the alkoxide solution to the core positive electrode active material particles, and the intake air volume and intake air temperature in the tumbling fluidized bed device were appropriately adjusted based on the target value of the coating amount of LiNbO3 (Nb content Y in the positive electrode active material). For example, in Example 1, the concentration of the alkoxide solution was 4.1 wt% in terms of LiNbO3, and 125 g of the alkoxide solution was sprayed at a rate of 2.0 g / min for 800 g of the core positive electrode active material particles. The intake air volume in the tumbling fluidized bed device was 0.2 m 3 / min and the intake temperature is 90°C.

[0059] Subsequently, calcination was performed by heating for 3 hours in an oxygen atmosphere at a temperature shown in Table 1. In this manner, for each of Examples 1 to 6 and Comparative Examples 1 to 6, a sample of a positive electrode active material for an all-solid-state lithium ion battery having a core positive electrode active material particle and a coating layer formed on the surface of the core positive electrode active material particle was obtained.

[0060] (Composition of positive electrode active material, Nb content Y in positive electrode active material) 0.2 g of each of the obtained positive electrode active material samples (powder) was weighed out and decomposed by an alkali fusion method, and then the composition was analyzed using an inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800" manufactured by Hitachi High-Tech Corp. The Nb content Y in the positive electrode active material was also measured by the composition analysis.

[0061] (50% cumulative volumetric particle size D50) 100 mg of each positive electrode active material sample (powder) was dispersed by irradiating 40 W ultrasonic waves for 60 seconds at 50% flow rate using a Microtrac laser diffraction particle size distribution analyzer "MT3300EXII", and then the particle size distribution was measured to obtain a volume-based cumulative particle size distribution curve. In the obtained cumulative particle size distribution curve, the volume particle size at 50% accumulation was taken as the 50% cumulative volume particle size D50 of the positive electrode active material powder.

[0062] (Specific surface area of ​​positive electrode active material X) 1.5 g of each obtained sample (powder) of the positive electrode active material was weighed into a glass cell, set in a degassing device, and filled with nitrogen gas in the glass cell, and then heat-treated in a nitrogen gas atmosphere at 150°C for 1 hour to degas the sample. The glass cell containing the degassed sample (powder) was then set in a Quantachrome specific surface area measuring device "Monosorb", and the specific surface area X was measured by the BET method (one-point method) while flowing a He: 70 at %-N2: 30 at % mixed gas as the adsorption gas.

[0063] (Initial resistance of all-solid-state batteries) 75 mg of the positive electrode active material and 25 mg of the sulfide solid electrolyte material Li3PS4 were mixed to obtain a positive electrode mixture. In addition, 80 mg of sulfide solid electrolyte material Li3PS4 was placed inside a φ10 mm battery test cell and pressed at a pressure of 37 MPa using a pellet molding machine to form a solid electrolyte layer. 10 mg of the positive electrode composite was placed on the solid electrolyte layer and pressed at a pressure of 330 MPa to form a composite layer. Next, the obtained composite layer of the solid electrolyte layer and the positive electrode active material layer was turned over, and a SUS plate with Li foil (10 mm diameter × 0.1 mm thickness) and In foil (9 mm diameter × 0.1 mm thickness) attached thereto was placed on the solid electrolyte layer side, and pressed at a pressure of 20 MPa to form a Li-In negative electrode layer. This produced a laminate in which the positive electrode active material layer, the solid electrolyte layer, and the Li-In negative electrode layer were laminated in this order. Next, the laminate was placed in a battery test cell made of SUS304 and a confining pressure of 2.5 N·m was applied to create an all-solid-state secondary battery. Next, the all-solid-state secondary battery was charged to 3.7 V (vs. Li-In), and the AC impedance of the charged cell was measured. The initial resistance was calculated from the arc obtained from the Nyquist plot. The above manufacturing conditions and test results are shown in Table 1.

[0064] [Table 1]

[0065] (Evaluation Results) The positive electrode active materials of Examples 1 to 6 all have a specific surface area X (m 2 / g) and the Nb content Y (mass%) in the positive electrode active material satisfied the relationship of the following formula (2). Therefore, the initial resistance evaluated as an all-solid-state battery was kept low. 0.65≦Y / X≦1.20 (2)

[0066] On the other hand, the positive electrode active materials of Comparative Examples 1 to 6 all have a specific surface area X (m 2 / g) and the Nb content Y (mass %) in the positive electrode active material did not satisfy the relationship of the above formula (2). Therefore, the initial resistance evaluated as an all-solid-state battery was large.

Claims

1. A positive electrode active material for an all-solid-state lithium ion battery, comprising core positive electrode active material particles and a coating layer, The core positive electrode active material particles are represented by the composition shown in the following formula (1): Li a Ni b Co c Mn d O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.) The coating layer is an oxide of Li and Nb, The specific surface area X (m 2 / g) and a Nb content Y (mass%) in the positive electrode active material satisfy the relationship of the following formula (2): 0.65≦Y / X≦1.20 (2)

2. The positive electrode active material for an all-solid-state lithium ion battery according to claim 1, wherein the 50% cumulative volume particle size D50 of the positive electrode active material for an all-solid-state lithium ion battery is 3 to 7 μm.

3. The coating layer is LiNbO 3 The positive electrode active material for an all-solid-state lithium ion battery according to claim 1 or 2, comprising:

4. A positive electrode for an all-solid-state lithium ion battery comprising the positive electrode active material for an all-solid-state lithium ion battery according to any one of claims 1 to 3.

5. An all-solid-state lithium ion battery comprising: a positive electrode layer formed of the positive electrode for an all-solid-state lithium ion battery according to claim 4; a negative electrode layer; and a solid electrolyte layer.

6. A step of preparing core positive electrode active material particles represented by a composition shown in the following formula (1); Li a Ni b Co c Mn d O e (1) (In the formula (1), 1.0≦a≦1.05, 0.8≦b≦0.9, 1.8≦e≦2.2, and b+c+d=1.) A step of forming a coating layer made of an oxide of Li and Nb on the surface of the core positive electrode active material particles by using an alkoxide solution containing Li and Nb with a tumbling fluidized bed apparatus; The method for producing a positive electrode active material for an all-solid-state lithium ion battery according to any one of claims 1 to 3, comprising:

7. 7. The method for producing a positive electrode active material for an all-solid-state lithium ion battery according to claim 6, wherein the alkoxide solution is a solution containing: (1) any one of methoxylithium, ethoxylithium, and isopropoxylithium as a lithium source for a solute; (2) any one of pentamethoxyniobium, pentaethoxyniobium, and pentaisopropoxyniobium as a niobium source; and (3) any one of ethanol, methanol, and isopropanol as a solvent.

Citation Information

Patent Citations

  • JP1974082866A

  • Method for manufacturing cathode active material

    JP2010225309A

  • Active material composite powder and lithium battery, and method for producing the same

    JP2015056307A

  • Method of manufacturing active material powder

    JP2015201252A

  • Positive electrode active material for lithium ion battery, positive electrode for lithium ion battery, and lithium ion battery

    JP2017084674A