Acrylic adhesive composition

A novel PSA composition with C6-C10 alkyl acrylate, methyl (meth)acrylate, and polyhydrazide crosslinking addresses the imbalance in adhesion and cohesion, improving performance for recyclable polymer packaging.

JP7581316B2Active Publication Date: 2024-11-12ROHM & HAAS CO
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022502164
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-07-18
Publication Date
2024-11-12
Estimated Expiration
2039-07-18

AI Technical Summary

Technical Problem

Existing pressure sensitive adhesive (PSA) products either have good adhesion but unsatisfactory cohesive strength, or vice versa, lacking a balance between adhesion and cohesion, which is crucial for recyclable polymer packaging materials.

Method used

A novel PSA composition comprising 40-90% C6-C10 alkyl acrylate, 3-15% methyl (meth)acrylate, 0.1-5% ethylenically unsaturated compounds with keto or aldehyde groups, 0-2% ethylenically unsaturated acid, and 0-30% other monomers, crosslinked with a polyhydrazide compound having at least two hydrazide functional groups.

Benefits of technology

The composition achieves improved adhesion and cohesion, or a balanced adhesion-cohesion performance, enhancing the suitability of PSA products for recyclable polymer packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581316000001
    Figure 0007581316000001
  • Figure 0007581316000002
    Figure 0007581316000002
Patent Text Reader

Abstract

A) (a) 40-90 wt% C6-C 10 Disclosed is an acrylic adhesive composition comprising: a polymer polymerized from a monomer mixture comprising: (a) an alkyl acrylate; (b) 3-15 wt% methyl (meth)acrylate; (c) 0.1-5 wt% ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0-2 wt% ethylenically unsaturated acid; and (e) 0-30 wt% other ethylenically unsaturated monomers (where the percentages are based on the total weight of the monomer mixture); and B) a polyhydrazide compound having at least two hydrazide functional groups that react with the keto or aldehyde groups by a crosslinking reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to acrylic adhesive compositions, and in particular to acrylic pressure sensitive adhesive compositions.

[0002] Introduction In recent years, the use of polymer packaging (e.g., polyethylene terephthalate (PET), high density polyethylene (HDPE), polyvinyl chloride (PVC), polypropylene (PP), or other plastic types) has increased due to their light weight and good puncture resistance. Pressure-sensitive film labels have also increased in use in polymer packaging systems due to improved moisture resistance and appearance, and it is desirable that such packaging materials be recyclable. Adhesion (peel properties) and cohesion (shear properties) are the most important performances of pressure-sensitive adhesive (PSA) products. In the prior art, there are some pressure-sensitive adhesive products with good adhesion, but their cohesion is not satisfactory. Or, there are also some pressure-sensitive adhesive products with good cohesion, but their adhesion is not satisfactory. A pressure-sensitive adhesive product with balanced adhesion and cohesion is desirable.

[0003] Thus, there is a strong need in the art for alternative pressure sensitive adhesive compositions that have desirable performance properties, such as improved adhesion and / or cohesion, or balanced adhesion and cohesion. Summary of the Invention

[0004] The present disclosure provides novel pressure sensitive adhesive compositions having desirable performance properties such as improved adhesion and / or cohesion, or balanced adhesion and cohesion.

[0005] In a first aspect, the present disclosure provides a method for producing a pharmaceutical composition comprising: A) (a) 40-90% by weight of C6-C 10 Alkyl acrylate, (b) 3 to 15% by weight of methyl (meth)acrylate; (c) 0.1 to 5 weight percent of an ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0 to 2% by weight of an ethylenically unsaturated acid; (e) 0 to 30% by weight of other ethylenically unsaturated monomers a polymer polymerized from the monomer mixture, comprising: B) a polyhydrazide compound having at least two hydrazide functional groups that react with keto or aldehyde groups by a crosslinking reaction.

[0006] In a second aspect, the present disclosure provides a method for producing a PET film comprising: A) (a) 40-90% by weight of C6-C 10 Alkyl acrylate, (b) 3 to 15% by weight of methyl (meth)acrylate; (c) 0.1 to 5 weight percent of an ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0 to 2% by weight of an ethylenically unsaturated acid; (e) 0 to 30% by weight of other ethylenically unsaturated monomers a polymer polymerized from the monomer mixture, comprising: B) a polyhydrazide compound having at least two hydrazide functional groups that react with keto or aldehyde groups by a crosslinking reaction.

[0007] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.

[0009] As disclosed herein, the terms "composition," "formulation," or "mixture" refer to a physical blend of different components obtained by simply mixing the different components by physical means.

[0010] As disclosed herein, the term "glass transition temperature" (T g The term ) can be measured by a variety of techniques including, for example, differential scanning calorimetry (DSC) or calculation using the Fox equation.

[0011] Throughout this document, the word fragment "(meth)acrylic" refers to both "methacrylic" and "acrylic." For example, (meth)acrylic acid refers to both methacrylic acid and acrylic acid, methyl (meth)acrylate refers to both methyl methacrylate and methyl acrylate, and (meth)acrylamide refers to both methacrylamide and acrylamide.

[0012] An "aqueous" composition or dispersion herein means that the particles are dispersed in an aqueous medium. By "aqueous medium" herein is meant water and 0-30% by weight based on the weight of the medium of a water-miscible compound(s), such as, for example, alcohols, glycols, glycol ethers, glycol esters, and the like.

[0013] The present disclosure relates to A) (a) 40-90% by weight of C6-C 10 Alkyl acrylate, (b) 3 to 15% by weight of methyl (meth)acrylate; (c) 0.1 to 5 weight percent of an ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0 to 2% by weight of an ethylenically unsaturated acid; (e) 0 to 30% by weight of other ethylenically unsaturated monomers a polymer polymerized from the monomer mixture, comprising: B) a polyhydrazide compound having at least two hydrazide functional groups that react with keto or aldehyde groups by a crosslinking reaction.

[0014] Preferably, C6 to C 10 The alkyl acrylate is selected from 2-ethylhexyl acrylate and 2-propylheptyl acrylate. More preferably, the alkyl acrylate is selected from C6 to C 10 The alkyl acrylate is 2-ethylhexyl acrylate.

[0015] Preferably, the C6 to C6 10 The amount of alkyl acrylate (a) may be 50% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, but 90% by weight or less, preferably 85% by weight or less, more preferably 80% by weight or less. More preferably, C6 to C 10 The amount of alkyl acrylate is 65-90% by weight of the monomer mixture.

[0016] The monomeric methyl (meth)acrylate (b) can be methyl acrylate and / or methyl methacrylate.

[0017] Preferably, the amount of methyl (meth)acrylate (b) in the monomer mixture is 3% by weight or more, preferably 4% by weight or more, more preferably 5% by weight or more, even more preferably 6% by weight or more, even more preferably 8% by weight or more, but may be 15% by weight or less, preferably 13% by weight or less, more preferably 12% by weight or less, even more preferably 11% by weight or less, even more preferably 10% by weight or less.

[0018] Ethylenically unsaturated compounds (c) having at least one keto or aldehyde group are, for example, acrolein, methacrolein, vinyl alkyl ketones having 1 to 20, preferably 1 to 10, carbon atoms in the alkyl radical, formylstyrene, (meth)acrylic acid alkyl esters having one or two keto or aldehyde or one aldehyde and one keto group in the alkyl radical, the alkyl radical preferably containing a total of 3 to 10 carbon atoms, examples being (meth)acryloyloxyalkylpropanals as described in DE-A 2722097. Furthermore, N-oxoalkyl(meth)acrylamides, as known, for example, from US Pat. No. 4,228,007, DE-A 2061213 or DE-A 2207209, are also suitable.

[0019] Particularly preferred are acetoacetyl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, and especially diacetone acrylamide (DAAM).

[0020] The amount of monomer (c) in the monomer mixture is from 0.1 to 5% by weight, preferably from 0.1 to 2% by weight, and more preferably from 0.2 to 1% by weight.

[0021] The ethylenically unsaturated acid (d) may be a sulfonic acid, a phosphoric acid, or preferably a carboxylic acid. Suitable examples include maleic acid, fumaric acid and itaconic acid, or preferably acrylic acid and / or methacrylic acid. Preferably, the ethylenically unsaturated acid (d) is acrylic acid.

[0022] Preferably, the amount of ethylenically unsaturated acid (d) in the monomer mixture is 0.1 wt% or more, preferably 0.15 wt% or more, more preferably 0.20 wt% or more, even more preferably 0.25 wt% or more, but may be 5 wt% or less, preferably 4 wt% or less, more preferably 3 wt% or less, even more preferably 2 wt% or less, and even more preferably 1 wt% or less.

[0023] The other ethylenically unsaturated monomer (e) may be of any type. Preferred examples include C1-C ethylenically unsaturated monomers other than the monomer (a) or the monomer (b). 18 Examples of the monomers include alkyl (meth)acrylates, (meth)acrylamides, vinyl aromatic compounds, and phosphorus-functional monomers. 18 Preferred examples of alkyl (meth)acrylates include ethyl acrylate, n-butyl acrylate, and n-butyl methacrylate. Preferred examples of vinyl aromatic compounds include styrene and alpha-methylstyrene. Phosphorus-functional monomers include phosphorus-containing (meth)acrylates, such as phosphoethyl (meth)acrylate, phosphopropyl (meth)acrylate, phosphobutyl (meth)acrylate, salts thereof, and mixtures thereof; CH2=C(R)-C(O)-O-(R1O) such as SIPOMER PAM-100, SIPOMER PAM-200, and SIPOMER PAM-300, all available from Solvay. n -P(O)(OH)2 (wherein R=H or CH3, R1=alkyl, and n=2 to 6); phosphoalkoxy(meth)acrylates such as phosphoethylene glycol (meth)acrylate, phosphodiethylene glycol (meth)acrylate, phosphotriethylene glycol (meth)acrylate, phosphopropylene glycol (meth)acrylate, phosphodipropylene glycol (meth)acrylate, phosphotripropylene glycol (meth)acrylate, salts thereof, and mixtures thereof.

[0024] The amount of ethyl acrylate may be 10-30% by weight. Preferably, the amount of ethyl acrylate in the monomer mixture is 10% by weight or more, 12% by weight or more, 15% by weight or more, 16% by weight or more, but 30% by weight or less, preferably 25% by weight or less, more preferably 20% by weight or less. More preferably, the amount of ethyl acrylate is 15-20% by weight.

[0025] The amount of phosphorus functional monomer may be 0.01-2 wt%. Preferably, the amount of phosphorus functional monomer in the monomer mixture is 0.02 wt% or more, 0.04 wt% or more, 0.06 wt% or more, 0.08 wt% or more, but 2 wt% or less, preferably 1 wt% or less, more preferably 0.5 wt% or less, more preferably 0.3 wt% or less. More preferably, the amount of phosphorus functional monomer is 0.06-0.3 wt%.

[0026] The amount of (meth)acrylamide can be 0.01 wt.% or more, preferably 0.05 wt.% or more, more preferably 0.10 wt.% or more, even more preferably 0.15 wt.% or more, but can be 4 wt.% or less, preferably 3 wt.% or less, more preferably 2 wt.% or less, even more preferably 1 wt.% or less, and even more preferably 0.5 wt.% or less.

[0027] In a preferred embodiment, the polymer A) is prepared by emulsion polymerization and is therefore an emulsion polymer.

[0028] In the case of emulsion polymerization, suitable surfactant systems and / or protective colloids, or stabilizers are used.

[0029] Examples of suitable surfactant systems are known in the art and include anionic, nonionic, cationic, or amphoteric emulsifiers, and mixtures thereof. Examples of anionic surfactants include, but are not limited to, alkyl sulfates, sulfates of ethoxylated alcohols, aryl sulfonates, phosphates of ethoxylated alcohols, sulfosuccinates, sulfates and sulfonates of ethoxylated alkylphenols, and mixtures thereof. Examples of nonionic surfactants include, but are not limited to, ethoxylated alcohols, ethoxylated alkylphenols, and mixtures thereof. Examples of cationic surfactants include, but are not limited to, ethoxylated fatty amines. The typical weight of surfactant is 0.1-5.0% by weight, more preferably 0.3-5.0% by weight, and most preferably 0.5-3.0% by weight, based on the total weight of monomers. The surfactant is utilized by conventional methods well known in the art. In one embodiment, the process for preparing the PSA involves emulsification of the monomer mix with a surfactant system prior to the polymerization reaction.

[0030] Examples of surfactant trade names are AEROSOL® A-102, Disponil® FES77, Dowfax™ 2A1, Abex® 2535, and RHODACAL® DS-4.

[0031] Water-soluble initiators for the emulsion polymerization are, for example, the ammonium and alkali metal salts of peroxodisulfuric acid, such as sodium peroxodisulfate, ammonium persulfate, hydrogen peroxide, or organic peroxides, such as tert-butyl hydroperoxide.

[0032] Also suitable are what are known as reduction-oxidation (redox) initiator systems.

[0033] A redox initiator system consists of at least one reducing agent, usually inorganic, and one oxidizing agent, which can be organic or inorganic.

[0034] The oxidizing component includes, for example, an emulsion polymerization initiator as already mentioned above.

[0035] The reducing components include reducing agents such as, for example, alkali metal salts of sulfite, such as sodium sulfite, sodium hydrogen sulfite, alkali metal salts of disulfite, such as sodium disulfite, bisulfite adducts with aliphatic aldehydes and ketones, such as acetone bisulfite, or hydroxymethanesulfinic acid and its salts, or ascorbic acid. Redox initiator systems can be used with soluble metal compounds whose metal components can exist in multiple valence states.

[0036] Examples of typical redox initiator systems include ascorbic acid / ferrous sulfate / sodium peroxodisulfate, tert-butyl hydroperoxide / sodium disulfate, and tert-butyl hydroperoxide / Na hydroxymethanesulfinic acid. Individual components, such as the reducing component, may be mixtures, such as a mixture of the sodium salt of hydroxymethanesulfinic acid and sodium disulfite.

[0037] These compounds are mostly used in the form of an aqueous solution, with low concentrations being determined by the amount of water tolerated in the dispersion, and high concentrations being determined by the solubility of each compound in water. The concentration is generally 0.1 to 30% by weight, preferably 0.5 to 20% by weight, particularly preferably 1.0 to 10% by weight, based on the solution.

[0038] The amount of initiator is generally 0.1-10% by weight, preferably 0.3-5% by weight, based on the monomers to be polymerized. It is also possible to use two or more different initiators for the emulsion polymerization.

[0039] Emulsion polymerization is generally carried out at temperatures between 30 and 130°C., preferably between 60 and 95°C. The polymerization medium may consist either of water alone or of a mixture of water and a water-miscible liquid such as methanol. Preferably, only water is used. Emulsion polymerization may be carried out as a batch operation or in the form of a feed process, including stepwise or gradient. Preference is given to a feed process in which a part of the polymerization mixture is introduced as an initial charge and heated to the polymerization temperature to initiate the polymerization of this initial charge, and then the remainder of the polymerization mixture is fed to the polymerization zone, usually by two or more spatially separated feed streams, one or more of which contain the monomers neat or in emulsified form, the addition being carried out continuously, stepwise or under a concentration gradient, and polymerization being maintained during the addition. It is also possible to include polymer seeds in the initial charge to the polymerization, for example to more effectively adjust the particle size.

[0040] The methods of adding initiator to the polymerization vessel during free radical aqueous emulsion polymerization are known to the skilled researcher. The initiator is either included in its entirety in the initial charge to the polymerization vessel or it is introduced continuously or in stages during the free radical aqueous emulsion polymerization depending on the rate at which it is consumed. In each particular case, this will depend both on the chemical nature of the initiator system and on the polymerization temperature. It is preferred to include a part of the initiator in the initial charge and to feed the remainder to the polymerization zone depending on the rate at which the initiator is consumed.

[0041] In order to remove residual monomer, it is common to also add initiator after the end of the actual emulsion polymerization, ie after at least 95% monomer conversion.

[0042] In the feed process, the individual components can be added to the reactor from the top, the side, or the bottom through the reactor bed.

[0043] In the case of emulsion polymerization, aqueous polymer dispersions are obtained which generally have a solids content of 15 to 75% by weight, preferably 40 to 75% by weight.

[0044] For a high space / time yield in the reactor, a dispersion with as high a solids content as possible is preferred. To be able to achieve a solids content of more than 60% by weight, a bimodal or multimodal particle size should be adjusted, since otherwise the viscosity becomes too high and the dispersion can no longer be handled. The generation of new particles can be carried out, for example, by adding seeds (EP81083), by adding an excess of emulsifier, or by adding a miniemulsion. Another advantage associated with a low viscosity at high solids is the improved coating behavior at high solids. The generation of one or more new particles can be carried out at any time. It is guided by a particle size distribution aimed at a low viscosity.

[0045] The polymer thus prepared is preferably used in the form of its aqueous dispersion.

[0046] The pH of the polymer dispersion is preferably adjusted to a pH above 4.5, in particular to a pH between 5 and 9.

[0047] The glass transition temperature of the polymer or polymers is preferably from -60 to -30°C, particularly preferably from -55 to -30°C, and extremely particularly preferably from -50 to -35°C.

[0048] The glass transition temperature can be determined by conventional techniques such as differential thermal analysis or differential scanning calorimetry (see, for example, ASTM 3418 / 82, Midpoint Temperature).

[0049] Compound B) is a polyhydrazide compound having at least two hydrazide functional groups.Specific examples of polyhydrazide compounds include oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide; adipic acid dihydrazide, sebacic acid dihydrazide; monoolefin unsaturated dicarboxylic acid dihydrazide such as maleic acid dihydrazide, fumaric acid dihydrazide, itaconic acid dihydrazide; carbonic acid dihydrazide, such as carbonic acid dihydrazide; phthalic acid dihydrazide, terephthalic acid dihydrazide, isophthalic acid dihydrazide. The polyhydrazides include, but are not limited to, aromatic dihydrazides such as hydrazides; trihydrazides such as 1,2,4-butane tricarbhydrazide, 1,1,4-butane tricarbhydrazide, 1,2,5-pentane tricarbhydrazide, 1,3,6-hexane tricarbhydrazide, 1,3,7-heptane tricarbhydrazide, and I-hydroxy-1,2,4-butane tricarbhydrazide, and mixtures or any subsets thereof. In one embodiment, the polyhydrazide comprises adipic dihydrazide, isophthalic dihydrazide, sebacic dihydrazide, bis-semicarbizide, and mixtures thereof. In another embodiment, the polyhydrazide is adipic dihydrazide.

[0050] An effective amount of polyhydrazide crosslinker is such that the ratio of hydrazine functional groups is from about 0.02 to about 5 equivalents per equivalent of ketone or aldehyde functional groups of the ethylenically unsaturated compound having at least one keto or aldehyde group, or from about 0.1 to about 3 equivalents per equivalent of ketone or aldehyde functional groups of the ethylenically unsaturated compound having at least one keto or aldehyde group, or from about 0.2 to about 1 equivalent per equivalent of ketone or aldehyde functional groups of the ethylenically unsaturated compound having at least one keto or aldehyde group.

[0051] The polyhydrazide compound B) can be added at any point in the process. In one embodiment, it is added after the emulsion reaction.

[0052] The weight fraction of B) is preferably 0.05 to 2 parts by weight, in particular 0.05 to 1 part by weight, very preferably 0.1 to 0.7 parts by weight, per 100 parts by weight of polymer A), more preferably 0.1 to 0.3 parts by weight, per 100 parts by weight of polymer A).

[0053] The polymer A) or an aqueous dispersion of the polymer can be mixed with the compound B) in a simple manner. The resulting mixture is stable on storage.

[0054] The pressure sensitive adhesives (PSA) may consist of only the polymer or of an aqueous dispersion of the polymer A) and the compound B).

[0055] The PSAs may contain further additives: thickeners, defoamers, wetting agents, mechanical stabilizers, pigments, fillers, freeze-thaw agents, neutralizers, plasticizers, tackifiers (tackifying resins), adhesion promoters, and combinations thereof. Examples of tackifiers are natural resins such as rosin and its derivatives formed by disproportionation or isomerization, polymerization, dimerization and / or hydrogenation. They may be present in the form of their salts (e.g., in the form of salts with monovalent or polyvalent counterions (cations)) or, preferably, in their esterified form. The alcohols used for esterification may be monovalent or polyvalent. Examples are methanol, ethanediol, diethylene glycol, triethylene glycol, 1,2,3-propanethiol, and pentaerythritol.

[0056] Additionally, hydrocarbon resins may be used, such as non-hydrogenated aliphatic C5 resins, hydrogenated aliphatic C5 resins, aromatic modified C5 resins, terpene resins, hydrogenated C9 resins, and combinations thereof.

[0057] Other compounds increasingly used as tackifiers include polyacrylates with low molecular weight, which preferably have a weight-average molecular weight MW of less than 30,000. In a preferred case, the polyacrylate is composed of at least 60% by weight, in particular at least 80% by weight, of C1-C8 alkyl (meth)acrylates.

[0058] The preferred tackifier is natural or chemically modified rosin, which is composed primarily of abietic acid or its derivatives.

[0059] The amount by weight of the tackifier is preferably 5 to 100 parts by weight, particularly preferably 10 to 50 parts by weight, per 100 parts by weight of the polymer (solid / solid).

[0060] The PSA may include 0 to 5 weight percent thickener, based on the total weight of the adhesive composition. All individual values ​​and subranges from 0 to 5 weight percent are included herein and disclosed herein. For example, the weight percent of neutralizing agent may range from lower limits of 0, 0.5, or 1 weight percent to upper limits of 1, 3, or 5 weight percent. Examples of thickeners include, but are not limited to, ACRYSOL™, UCAR™, and CELOSIZE™, available from The Dow Chemical Company, Midland, Michigan.

[0061] The PSA may include 0 to 2 weight percent of a neutralizing agent, based on the total weight of the adhesive composition. All individual values ​​and subranges from 0 to 2 weight percent are included herein and disclosed herein. For example, the weight percent of the neutralizing agent may be from a lower limit of 0, 0.3, or 0.5 weight percent to an upper limit of 0.5, 1, or 2 weight percent. Neutralizing agents are typically used to control the pH to provide stability to the formulated pressure-sensitive adhesive composition. Examples of neutralizing agents include, but are not limited to, aqueous ammonia, aqueous amine solutions, and other aqueous inorganic salts.

[0062] PSAs are used to produce self-adhesive articles such as labels, adhesive tapes or sheets, e.g., protective films.

[0063] Self-adhesive articles generally consist of a backing with a layer of adhesive applied to one or both sides, preferably one side.

[0064] Backing materials may include, for example, paper, metal foil, polymeric films preferably made of polyolefins including polyethylene and polypropylene, polyethylene terephthalate (PET), polyvinyl chloride (PVC), polystyrene or polyamide, which may be biaxially or uniaxially oriented.

[0065] The present disclosure provides a self-adhesive article comprising a backing material and the pressure-sensitive adhesive composition disclosed herein.

[0066] To produce an adhesive layer on the backing material, the backing material can be conventionally coated. Typical application rates are, for example, 5 to 50 g / m 2 (solid, no water).

[0067] The constructed coated substrate is used as a self-adhesive article, such as, for example, a label, an adhesive tape or sheet, e.g., a protective film, etc. For subsequent use, the PSA-coated side of the substrate, e.g., a label, can be covered with a release paper, such as a silicone-treated paper.

[0068] The self-adhesive articles of the present invention have good performance properties, particularly improved adhesion and cohesion and / or improved adhesion / cohesion balance. EXAMPLES

[0069] Some embodiments of the present invention are now described in the following examples, in which all parts and percentages are by weight unless otherwise specified. Raw materials: [Table 1]

[0070] Emulsion Polymerization In general, an emulsion mixture according to the present disclosure is prepared as follows: A 4 liter, 5-neck reactor equipped with a condenser, mechanical stirrer, temperature controlled thermocouple, and inlets for initiator and monomer is charged with 675 g of deionized ("DI") water and heated to 88°C under a gentle N2 flow. In a separate container, a monomer emulsion is prepared by mixing 275 g of DI water, 10 g of RHODACAL DS-4, 12 g of AEROSOL A-102, 2.5 g of Na2CO3, and 1,672 g of a monomer mixture including at least one of 2-ethylhexyl acrylate ("2-EHA"), butyl acrylate ("BA"), ethyl acrylate ("EA"), methyl methacrylate ("MMA"), acrylic acid ("AA"), AM, PEM, and DAAM.

[0071] Next, a solution of a mixture of Na2CO3 and ammonium persulfate ("APS") in 40 g DI water is added to the reactor. Immediately after the addition of the Na2CO3 and APS solutions, the monomer emulsion is fed into the reactor. The feeds are continued for 80 minutes.

[0072] Once the addition of the monomer emulsion is complete, the reaction mixture is allowed to cool to 60° C., after which a solution of tert-butyl hydroperoxide (70%) (“t-BHP”) (9.2 g in 32 g DI water), and a reducing agent such as BRUGGOLITE FF6 M (“FF6”) from Bruggemann Chemical US Company, Chadds Ford, Pennsylvania, 6.8 g in 34.5 g DI water, is slowly added through two separate pipes over a period of 30 minutes. Once the feeds are complete, the reaction is allowed to cool to room temperature. The resulting composition is then filtered through a 325 mesh filter cloth to prepare the composition for subsequent evaluation runs.

[0073] Pressure Sensitive Adhesive Formulation All samples are slightly formulated with a wetting agent, such as 0.3% (wet / wet) Surfynol 420 Wetting Agent ("420") from Evonik Industries, based on total emulsion, to improve wetting for laboratory drawdowns, unless otherwise noted. ADH was also added. The viscosity is then adjusted to approximately 600 cps (Brookfield, RVDV, 30 rpm, 63#) using a thickener, such as ACRYSOL RM-2020 ("RM-2020") from The Dow Chemical Company, Midland, Michigan, and the final pH is adjusted to 7.0-7.5 using ammonia.

[0074] Laboratory Drawdown Polypropylene ("PP") film (60 micrometers thick) is pretreated by corona treatment prior to lamination. The formulated adhesive is applied at a concentration of 17 g / m2 on a dry weight basis. 2 onto a release liner and dried for 2 minutes at 105° C. The PE film is laminated with the pressure sensitive adhesive coated release liner at 40° C. under a pressure of 40 psi.

[0075] Application Test Performance testing can be performed after conditioning the adhesive laminates for 5 days in a testing laboratory with a controlled environment (22-24°C, 50-60% relative humidity).

[0076] Peel strength testing: Peel strength testing at 90° to both glass and high density polyethylene (HDPE) test plates was according to FINAT Test Method No. 1. Prior to testing, sample strips (formulated without wax) were affixed to the test plates for 20 minutes and 1 day dwell times.

[0077] Cohesion / shear test: The shear resistance test against a glass test plate uses FINAT test method No. 8.

[0078] The failure mode is recorded after the test value: "AF" indicates adhesive failure, "AFB" indicates adhesive failure from the backing, "MF" indicates mixed failure, and "CF" indicates cohesive failure. Illustrative Examples ("IE") and Comparative Examples ("CE") are detailed below in Table 1, which details the formulations and PSA properties of the compositions of Examples IE and CE. [Table 2]

[0079] Compared to the CE1 formulation, IE1-IE5 formulations had better HDPE peel. IE1, IE2 and IE5 formulations had better 1 day glass peel. IE1-IE5 shear performance was adhesive failure, meaning that the cohesive strength was better than the adhesive strength. IE3 and IE4 formulations had shear strength over 200 hours, which was much better than CE1 and CE2.

[0080] Compared to the CE2 formulation, the IE5 formulation had higher shear and slightly lower HDPE peel. The 1-day glass peel was comparable.

[0081] Much better shear properties were obtained for formulations IE1-IE5 compared to formulation CE3, which contained 30% EHA in the monomer mix.

[0082] If the EA content of the monomer mix is ​​too high, the Tg will be too high. If the MMA content of the monomer mix is ​​too high, the Tg will be too high. An increase in Tg can make the polymer more rigid, less wettable, and less adhesive. A polymer with a Tg that is too high will not be compatible enough to exhibit adequate pressure sensitive adhesion, especially on surfaces with low surface energy.

[0083] Compared to formulations CE3 and CE4, formulation IE4 had much better shear and equal or better adhesion to both glass and HDPE. CE6 had good adhesion but too low shear performance (cohesion), while CE7 had adequate shear but lower adhesion than all inventive examples IE1-IE5. Both CE6 and CE7 have a poorer adhesion / cohesion balance than the inventive examples. The invention as originally claimed in the present application is set forth below. [1] A) (a) 40 to 90% by weight of C 6 ~C 10 Alkyl acrylate, (b) 3 to 15% by weight of methyl (meth)acrylate; (c) 0.1 to 5 weight percent of an ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0 to 2% by weight of an ethylenically unsaturated acid; (e) 0 to 30% by weight of other ethylenically unsaturated monomers a polymer polymerized from a monomer mixture comprising: B) a polyhydrazide compound having at least two hydrazide functional groups that react with said keto or aldehyde groups by a crosslinking reaction; 1. A pressure sensitive adhesive composition comprising: [2] C in the monomer mixture 6 ~C 10 The pressure-sensitive adhesive composition according to [1], wherein the amount of the alkyl acrylate is 65 to 90% by weight. [3] Above C 6 ~C 10 The pressure-sensitive adhesive composition according to [1], wherein the alkyl acrylate is selected from the group consisting of 2-ethylhexyl acrylate and 2-propylheptyl acrylate. [4] The pressure-sensitive adhesive composition according to [1], wherein the ethylenically unsaturated compound having at least one keto or aldehyde group is selected from the group consisting of acetoacetyl (meth)acrylate, acetoacetoxyethyl (meth)acrylate and diacetone acrylamide. [5] The pressure-sensitive adhesive composition according to [1], wherein the amount of the ethylenically unsaturated compound having at least one keto or aldehyde group in the monomer mixture is 0.1 to 2% by weight. [6] The pressure-sensitive adhesive composition of [1], wherein the other ethylenically unsaturated monomer (e) is selected from the group consisting of ethyl acrylate, n-butyl acrylate, n-butyl methacrylate, (meth)acrylamide, vinyl aromatic compounds, and phosphorus-functional monomers. [7] The pressure-sensitive adhesive composition of [1], wherein the ethylenically unsaturated acid is selected from the group consisting of sulfonic acid, phosphoric acid, and carboxylic acid. [8] The pressure sensitive adhesive composition of [1], wherein the polyhydrazide compound having at least two hydrazide functional groups that react with the keto or aldehyde groups by a crosslinking reaction is selected from the group consisting of oxalic dihydrazide, malonic dihydrazide, succinic dihydrazide, glutaric dihydrazide; adipic dihydrazide, sebacic dihydrazide; monoolefinic unsaturated dicarboxylic acid dihydrazides; carbonic acid 10 polyhydrazides; aromatic dihydrazides; trihydrazides, and mixtures or any subsets thereof. [9] The pressure-sensitive adhesive composition of [1], wherein the amount of polyhydrazide crosslinker is such that the ratio of hydrazine functional groups is from about 0.02 to about 5 equivalents per equivalent of ketone or aldehyde functional groups of the ethylenically unsaturated compound having at least one keto or aldehyde group.

[10] A self-adhesive article comprising a backing material according to any one of [1] to [9] and a pressure-sensitive adhesive composition.

[11] The self-adhesive article of

[10] , wherein the backing material is paper, metal foil or polymer film.

Claims

1. A) (a) 40 to 90% by weight of C 6 ~C 10 Alkyl acrylate, (b) 3 to 15 weight percent methyl (meth)acrylate; (c) 0.1 to 5 weight percent of an ethylenically unsaturated compound having at least one keto or aldehyde group; (d) 0.20 to 2 weight percent of an ethylenically unsaturated acid which is acrylic acid, and (e) 10 to 30 weight percent of ethyl acrylate, 0.01 to 4 weight percent of (meth)acrylamide, 0.01 to 2 weight percent of phosphorus-functional monomers, and combinations thereof, provided that the other ethylenically unsaturated monomers include at least ethyl acrylate and (meth)acrylamide. a polymer polymerized from a monomer mixture comprising: B) a polyhydrazide compound having at least two hydrazide functional groups that react with said keto or aldehyde groups by a crosslinking reaction; 1. A pressure sensitive adhesive composition comprising:

2. C in the monomer mixture 6 ~C 10 2. The pressure sensitive adhesive composition of claim 1, wherein the amount of alkyl acrylate is from 65 to 90 weight percent.

3. Said C 6 ~C 10 2. The pressure sensitive adhesive composition of claim 1, wherein the alkyl acrylate is selected from the group consisting of 2-ethylhexyl acrylate and 2-propylheptyl acrylate.

4. 2. The pressure sensitive adhesive composition of claim 1, wherein the ethylenically unsaturated compound having at least one keto or aldehyde group is selected from the group consisting of acetoacetyl (meth)acrylate, acetoacetoxyethyl (meth)acrylate and diacetone acrylamide.

5. 2. The pressure sensitive adhesive composition of claim 1, wherein the amount of the ethylenically unsaturated compound having at least one keto or aldehyde group in the monomer mixture is 0.1 to 2 weight percent.

6. 2. The pressure sensitive adhesive composition of claim 1, wherein the other ethylenically unsaturated monomer (e) is a combination of ethyl acrylate and (meth)acrylamide.

7. 2. The pressure sensitive adhesive composition of claim 1, wherein the polyhydrazide compound having at least two hydrazide functional groups that react with the keto or aldehyde groups by a crosslinking reaction is selected from the group consisting of oxalic dihydrazide, malonic dihydrazide, succinic dihydrazide, glutaric dihydrazide; adipic dihydrazide, sebacic dihydrazide; monoolefinic unsaturated dicarboxylic acid dihydrazides; carbonic acid 10 polyhydrazide; aromatic dihydrazides; trihydrazides, and mixtures or any subsets thereof.

8. 2. The pressure sensitive adhesive composition of claim 1, wherein the amount of polyhydrazide crosslinker is such that the ratio of hydrazine functional groups is from about 0.02 to about 5 equivalents per equivalent of ketone or aldehyde functional groups of said ethylenically unsaturated compound having at least one keto or aldehyde group.

9. A self-adhesive article comprising a backing material according to any one of claims 1 to 8 and a pressure sensitive adhesive composition.

10. The self-adhesive article of claim 9, wherein the backing material is paper, metal foil, or polymeric film.

Citation Information

Patent Citations

  • Water-base hardenable pressure-sensitive adhesive composition

    JP1994158010A

  • Repeelable aqueous pressure-sensitive adhesive composition and pressure-sensitive adhesive product

    JP2004277711A

  • Peelable aqueous adhesive composition, peelable adhesive, and curing adhesive sheet / tape using it

    JP2009138152A

  • Pressure sensitive adhesive and the removable articles

    WO2017216108A1