Paint and application method
A paint formulation with elastic and harder hollow beads addresses the challenge of maintaining uniform film thickness on vertical surfaces, achieving improved heat insulation and flexibility by forming a dense, thick coating film.
Patent Information
- Application Number
- JP2021030751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing heat-insulating coating films made of organic hollow particles face challenges in maintaining a uniform film thickness of several hundred micrometers, particularly when applied to vertical or sloped surfaces, compromising flexibility and insulation effectiveness.
A paint formulation using a combination of first and second hollow beads, where the first beads are elastic and made of the same material as the coating film-forming material, and the second beads are harder, with a particle size difference of 30 μm or more, allowing for a thicker and more durable coating film to be formed on various surfaces.
The combination of elastic and harder hollow beads enables the formation of a dense, flexible, and thick coating film, enhancing heat insulation by increasing the space for air retention and improving moldability, maintaining a film thickness of 300 μm or more, thereby reducing radiant heat transmission.
Smart Images

Figure 0007581574000002 
Figure 0007581574000003 
Figure 0007581574000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a paint for buildings, outdoor units of air conditioners, etc., and a coating method thereof. [Background technology]
[0002] In recent years, in light of environmental and energy issues, energy conservation efforts have been made in various fields. For example, in the case of air conditioners, which account for a certain amount of energy consumption in buildings, efforts have become common from both a technical perspective, such as improving compressor performance and increasing the efficiency of equipment operation through sensors and inverter control, as well as an operational perspective, such as reviewing the set temperature. In addition, energy conservation efforts are also being made for the buildings themselves, such as insulating roofs and walls.
[0003] In this context, one technology that uses paint to achieve thermal insulation is a building board having a base material, a thermal insulation coating film that covers the surface of the base material, and a transparent clear coating film that covers the thermal insulation coating film, and the thermal insulation coating film is characterized in that it contains a coating film-forming material, organic hollow particles, and a water-soluble solvent (Patent Document 1).
[0004] However, although a heat insulating coating film consisting only of organic hollow particles can be set to have high flexibility, there is a problem that it is difficult to maintain a film thickness of a specified level or more when applied. When a coating film layer is formed on the top surface of a material such as a building board in a processing plant, it is possible to achieve a desired thickness, but in situations where a coating film must be formed directly from the side or bottom surface, as in existing facilities, it is difficult to form a uniform film thickness of several hundred μm. Thus, there was a problem that the flexibility and thickness of the coating film could not be achieved at the same time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-88000 A Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved is to provide a coating material and a coating method that can be applied to buildings, outdoor units of air conditioners, etc. [Means for solving the problem]
[0007] The first invention is a paint containing elastic first hollow beads and second hollow beads, which are harder than the material of the first hollow beads, in a film-forming material, and the first hollow beads are made of the same material as the film-forming material. The second invention is the paint of the first invention, in which either or both of the first and second hollow beads are composed of a particle size of a predetermined size with a particle size difference of 30 μm or more, and the content (volume basis) of hollow beads with the maximum particle size is the largest. Here, the composition of a particle size of a predetermined size with a particle size difference of 30 μm or more can be, for example, a composition of hollow beads with a maximum particle size of 80 μm to a minimum particle size of 50 μm. However, the maximum particle size and the minimum particle size are not limited. The third invention is the paint of the second invention, in which the particle size of the hollow beads with the maximum particle size is within the range of 50 to 100 μm. The fourth invention is the paint of the third invention, in which the peak of the content (volume basis) of hollow beads with a particle size other than the maximum particle size is 50 μm or more. The fifth invention is a coating method for coating the surface of a target facility with the coating material of any one of the first to fourth inventions to a thickness of 300 μm or more. The predetermined size of the hollow beads is preferably equal to or smaller than a size at which the hollow beads are sufficiently held by the coating film formed when the beads are applied, and equal to or larger than a size at which a gas such as air that can exhibit heat insulating properties can be held therein. Effect of the Invention
[0008] In the present invention, the coating film forming material is provided with elastic hollow beads made of the same material as the coating film forming material and hollow beads that are harder than the elastic hollow beads, so that the coating film forming material and the elastic hollow beads are compatible with each other, and the flexibility is maintained, and the hard hollow beads make it possible to form a thicker coating film for insulation. That is, it is possible to form a film thickness required for insulation on vertical surfaces and inclined surfaces of existing facilities, and it is expected that a high insulation effect can be obtained. In addition, since the coating film is composed of hollow beads with different particle sizes and has the largest content of the maximum particle size, the beads can be made denser, and a dense layer of beads can be formed and maintained. That is, the space useful for insulation in the paint is increased, and the effect of further improving the insulation effect can be expected. In addition, by setting the maximum particle size of the hollow beads within the range of 50 to 100 μm and using hollow beads with a particle size that fits into the gaps between the hollow beads with the maximum particle size, it is expected that the above effect can be stably obtained. In addition, it is expected that the particle size of the hollow beads with the second and third largest particle sizes is 50 μm or more, and the moldability can be improved. In addition, by forming a coating film having a thickness of 300 μm or more, it is expected that the heat insulating effect can be maintained in various facilities. In the present invention, heat insulation means reducing or blocking radiant heat from sunlight or heat sources. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a paint according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of a layer of hollow beads in a paint. [Diagram 3] This is a conceptual diagram showing the relationship between the target equipment, the coating, and radiant heat. [Figure 4] FIG. [Diagram 5] The external appearance of the target equipment (left) and its surface temperature (right) are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the present invention will be described in detail based on the embodiments.
[0011] <Paint> As shown in Fig. 1, the paint P according to this embodiment includes a coating film-forming material 1 such as a water-based or solvent-based material, hollow beads 2 (an example of the first hollow beads) made of a soft material having elasticity, and hollow beads 3 (an example of the second hollow beads) made of a hard material. Note that Fig. 1 is an image diagram showing that there are multiple types of hollow beads, and that each type of hollow bead has a range of particle diameters.
[0012] An example of the coating film-forming material 1 is an acrylic emulsion resin. The coating film-forming material 1 may be a resin mainly composed of a urethane-based, silicone-based, or fluorine-based component in addition to an acrylic-based material.
[0013] Examples of materials for the soft hollow beads 2, which are an example of the first hollow beads having elasticity, include plastics such as acrylic, polystyrene, and polycarbonate, and elastomers such as rubber. The soft hollow beads 2 are preferably made of the same material as the coating film forming material 3, and for example, when the coating film forming material 3 is an acrylic emulsion resin, the soft hollow beads 2 are acrylic hollow beads.
[0014] The hard hollow beads 3 are, for example, ceramic hollow beads or glass hollow beads. Ceramic hollow beads include those made from volcanic ash containing 65 to 73% silicon dioxide and 12 to 18% aluminum oxide as main components.
[0015] The ratio of the soft hollow beads 2 to the hard hollow beads 3 is preferably 1:1 on a weight basis or a volume basis. The ratio of the soft hollow beads 2 to the hard hollow beads 3 should be close to 1:1 on a weight basis. If the ratio of the soft hollow beads 2 is high, the flexibility of the paint film is high when the paint dries, but the thickness of the paint film from one application is not sufficient. It is necessary to increase the number of applications. On the other hand, if the ratio of the hard hollow beads 3 is high, the thickness of the paint film from one application is thick when the paint dries, but the flexibility of the paint film is impaired. Taking into account the passage of time, the ratio of the soft hollow beads 2 is preferably 50% or more on a volume basis or a weight basis.
[0016] The reason for using multiple materials with different properties in this way is to take advantage of the bead characteristics of each material (soundproofing effect, molding effect, heat insulation effect, durability, etc. obtained from the shape and components.) In the following examples, for example, acrylic hollow beads and ceramic hollow beads were used in a 1:1 ratio by weight for the hollow beads.
[0017] Here, hollow beads refer to particles that have voids or spaces inside the beads, and may be either a closed system in which air is blocked from the inside and outside of the beads, or an open system in which the inside and outside of the beads are connected, such as a porous structure or doughnut structure.
[0018] The particle size of hollow beads such as the soft hollow beads 2 and the hard hollow beads 3 preferably has a predetermined range of particle size difference (for example, a range of particle size from 80 μm to 50 μm) based on the maximum particle size. If the particle size distribution has a predetermined range, when a solvent such as water evaporates from the paint P to form a paint film, hollow beads with smaller particle sizes will get in between the hollow beads with the largest particle size, making the hollow beads more dense. The maximum particle size of the hollow beads may be determined by the coarseness, mesh size, etc. of the filter used to filter the hollow beads.
[0019] The hollow beads for each component have a lineup of three particle sizes (particle size lineup). Here, the particle size lineup means that the particle sizes of the hollow beads are configured to have multiple intended particle sizes. In this example, the hollow beads of each material have peaks in hollowness (the ratio of the total volume of the hollow parts for each particle size in the coating film) at particle sizes of 80 μm, 60 μm, and 50 μm, and the weight ratio is 5:3:2 (including fine beads generated during the manufacturing process).
[0020] In this embodiment, the hollow beads of 80 μm are the largest in both volume and weight. The membrane thickness of the hollow beads of each diameter ranges from about 1 μm to several μm, and the volume of the hollow part inside the bead is generally 80% or more of the bead.
[0021] There are various methods for confirming the particle size distribution of hollow beads. For example, there is a method for measuring the particle size from the area of hollow beads in the enlarged image of Figure 2. There is also the Coulter method, which measures the volume of each particle to determine the corresponding particle size, as well as the so-called centrifugal sedimentation method and laser diffraction / scattering method. Note that hollow beads are very fine, so it is technically difficult to manufacture hollow beads with an accurate particle size. Therefore, the particle size distribution should be confirmed assuming manufacturing errors. For example, there is a method in which hollow beads with a particle size in the range of 80 μm ± 5 μm are counted as hollow beads with a particle size of 80 μm.
[0022] The density of the hollow beads in the coating is preferably at the level shown in Figure 2. A coating with such a density level can provide heat insulation effects, etc. Figure 3 is a conceptual diagram. A coating containing soft hollow beads 2 and hard hollow beads 3 is formed on the surface of equipment 4 by coating film forming material 1. In this way, the coating blocks and reduces radiant heat 5 transmitted from the outside.
[0023] The shape of the hollow beads such as the soft hollow beads 2 and the hard hollow beads 3 is preferably spherical as shown in Fig. 2, but may not be spherical. When the hollow beads are distorted like fragments and are not spherical, the particle size may be the average of the maximum and minimum widths of the hollow beads, the maximum width, or the minimum width of the hollow beads.
[0024] <Coating agent> The main coating agent is a mixture of methanol (90% by weight or more), water (4% by weight or more), and tin oxide (SnO2) (0.1% by weight). The coating agent may be the hydrophilic coat described in JP 2019-002671 A or a similar one. However, it is not necessarily required.
[0025] The coating agent may contain components for purposes other than heat insulation, such as photocatalysts such as titanium oxide, zinc oxide, and tin oxide. In this case, the coating film has a multifunctional structure with a lower layer for heat insulation and an upper layer for another function. For example, photocatalysts such as titanium oxide in the coating agent clean the painted surface by their hydrophilicity and photocatalytic reaction.
[0026] Example 1 The film formation and heat insulating effect of the coating material according to the present invention will be described below. In this example, the evaluation targets are the offices of multiple companies (railway, electric power, manufacturing), factory roofs and exterior walls, and air conditioning and electrical equipment (air conditioner outdoor units, substation control panels, cubicles, railway communication equipment, server rooms) (Figure 4).
[0027] The coating process consists of a process of removing dirt from the surface of the target equipment with a high-pressure water wash, and a process of applying paint to a film thickness of about 400 μm (when dry) with a roller brush. There are no limitations on the coating method. For example, spraying can be used.
[0028] Table 1 shows the results of the year-round observation of the coating. The coating surface of each facility maintained a film thickness of approximately 400 μm for one year. The presence or absence of changes in the film thickness was based on magnified photographs and visual inspection. [Table 1]
[0029] The roller brush formed a film thickness of about 200 μm (when dry) on the first coat and about 400 μm (when dry) on the second coat. This film thickness remained almost unchanged even after one year.
[0030] By using paint on the outdoor units of air conditioners, electricity consumption was reduced by an average of approximately 17% per year compared to before and after the use of the paint. The right-hand figure in Figure 5 shows an infrared thermograph of the surface temperatures of areas where paint was applied and areas where it was not. The areas surrounded by thick frames (air conditioner outdoor units, building exterior walls, and rooftop floor) are the areas where paint was used. In summer, the temperature difference between the areas where paint was applied and other areas was approximately 30 to 40 degrees Celsius.
[0031] Example 2 Verification of useful forms of the coating material according to the present invention will be described below. The paint of the present invention lowered the surface temperature of the target equipment by 30 to 40 degrees Celsius in summer compared to the surrounding area. This result suggests that the hollow bead layer in the coating film is formed homogeneously. As described above, the hollow beads in this example are ceramic beads, which are a hard material, and acrylic resin beads, which are a soft material. By using two types of materials in this way, the characteristics of each material can be utilized.
[0032] Generally, hollow beads made of ceramics or glass, which have excellent heat resistance, are used for various purposes. However, when only hollow beads made of these hard materials are used in paint, the hollow beads often break due to contact with each other. In another test, it was found that most of the beads break when only glass beads are used in the same amount as the hollow beads used in this embodiment.
[0033] On the other hand, in this example, almost no cracking of the beads was observed, suggesting that a combination of hollow beads made of a hard material and hollow beads made of a soft material can form a dense layer of hollow beads.
[0034] The advantage of using a hard material is that it makes it easier to form a coating film. The strength of the coating film is weak if the synthetic resin hollow beads are used alone. In other words, it is difficult to achieve or maintain a certain thickness using only synthetic resin hollow beads.
[0035] In this embodiment, both the film-forming material and the soft hollow beads are made of acrylic resin. The choice of material has a large influence on the strength of the coating film. When an acrylic film-forming material is combined with soft hollow beads made of a material softer than acrylic, the strength of the entire coating film is further reduced. Therefore, it is necessary that the film-forming material and the soft hollow beads are made of at least the same material.
[0036] Furthermore, these findings suggest that the combination of an acrylic film former with hollow beads that are harder than acrylic increases the strength of the coating film. Thus, the soft hollow beads must not be softer than the film former, but as long as they are hard, they do not have to be made of the same material as the film former. For example, when the film former is made of acrylic, the hollow beads may be made of urethane, silicone, or the like.
[0037] This example also suggests that a combination of hollow beads made of a hard material and hollow beads made of a soft material forms a dense hollow layer. What materials are hard and what materials are soft, and how to select the materials, are relative to each other. In this example, no cracks occurred when ceramic hollow beads and acrylic hollow beads were combined. This is thought to be due to the elasticity of the acrylic hollow beads. In this way, it is sufficient to select a material that can withstand the stress of the hollow beads of the other material.
[0038] Here, Young's modulus is an index of the elasticity of a material. Synthetic resins often have a Young's modulus of 4 or less. It is said that glass has a Young's modulus of 80, and inorganic compounds such as silicon dioxide and aluminum oxide that form ceramics have a Young's modulus of 100 or more. Taking into account this technical common knowledge and the results of this example, it is suggested that a combination of at least a soft material with a Young's modulus of 4 or less and a hard material with a Young's modulus of 80 or more can form a dense hollow bead layer in the paint.
[0039] It was also confirmed that, in addition to acrylic, urethane, silicone, and fluorine-based coating materials also provide heat insulating effects. In other words, it was suggested that synthetic resins in general can be used as coating film-forming materials according to the present invention. However, in terms of formability of the coating film, acrylic is the best coating film-forming material according to the present invention.
[0040] The amount of hollow beads used varies depending on the thickness of the coating and the particle size of the beads. The density level of the hollow beads shown in Figure 2 is a guide for forming a desired coating thickness.
[0041] In this embodiment, the hollow beads of each material have particle sizes of 80 μm, 60 μm, and 50 μm, with a weight ratio of 5:3:2. As shown in Figure 2, the proportion of hollow beads with the largest particle size is also the highest in terms of volume ratio. Thus, it has been found that the greatest insulating effect is achieved when the volume ratio of hollow beads with the largest particle size is maximized.
[0042] In this embodiment, hollow beads with a maximum particle size of 80 μm and a minimum particle size of 50 μm (particle size difference 30 μm) were mainly used. Empirically, the maximum particle size is preferably within the range of 50 to 100 μm. The minimum particle size is not limited and may be less than 1 μm. This is because it can contribute to increasing the density of the hollow beads.
[0043] The particle size lineup also allows for a dense structure of hollow beads, which increases the heat insulating effect. The same is true for combinations of hollow beads with two or more peaks in the particle size distribution. Such peaks may be 60 μm, 50 μm, or even smaller. For example, they may be of a particle size that fills the gap between adjacent hollow beads of the largest particle size. Hollow beads of such a particle size can theoretically maximize the dense state of hollow beads.
[0044] In this embodiment, hollow beads with a diameter between 80 μm and 50 μm were mainly used. This suggests that a configuration of hollow beads with a diameter difference of at least 30 μm is useful. The diameter is not limited, but an example is a configuration of hollow beads with a maximum diameter of 100 μm and a minimum diameter of 70 μm. In addition, hollow beads with a minimum diameter of less than 1 μm and a diameter of at least 30 μm larger than this may be used.
[0045] It is also suggested that it is useful for forming a film thickness to have a large proportion of ceramic hollow beads at the maximum particle size (e.g., 80 μm) and a large proportion of acrylic hollow beads at smaller particle sizes (e.g., 60 μm or 50 μm). When the beads with the maximum particle size are ceramic, the acrylic hollow beads may be of a particle size that can separate the ceramic hollow beads so that they do not come into contact with each other.
[0046] It is also suggested that the greater the ratio of acrylic hollow beads with the largest particle size, the more useful the heat insulation. That is, the hollow beads with the largest particle size may be acrylic hollow beads, and the beads with a particle size that fills the gaps between the acrylic hollow beads may be ceramic hollow beads. Furthermore, urethane hollow beads and silicone hollow beads, which are harder than acrylic hollow beads, are examples of substitutes for acrylic hollow beads. These materials may contribute to maintaining the formability of the coating film even if the amount of ceramic hollow beads used is small. In this way, it is sufficient to have a particle size and material configuration that maintains the formability of the coating film and avoids adverse effects such as cracks due to contact between hollow beads.
[0047] In addition, the thickness of the paint film changes depending on various factors. For example, the thickness of the paint film immediately after painting is smaller than that after the paint has dried. This is because the water in the paint evaporates. The thickness of the film also expands and contracts due to the influence of temperature, humidity, etc. Therefore, when the paint film shrinks between adjacent hard and soft hollow beads, it is expected that the former will deform the latter into a concave shape. It is important to select a material that can withstand the stress associated with this paint film shrinkage and maintain the hollow structure of the beads.
[0048] The choice of film-forming material is also important in forming the desired film thickness. The formability of the coating film can be improved or decreased depending on the combination of the film-forming material and the material of the soft hollow beads. At the very least, it is important for the formability of the coating film that the material of the film-forming material and the material of the soft hollow beads are the same. In this way, the choice of the three materials - the film-forming material, the soft hollow beads, and the hard hollow beads (as well as the particle size of the hollow beads) - determines the properties of the coating film. This example suggests that a paint with the desired characteristics can be obtained based on these factors.
[0049] As an example, in this embodiment, a coating film of about 400 μm formed on the surface of the target equipment maintained its thickness throughout the year and demonstrated a heat insulating effect. It is possible to realize coatings with a larger amount of hollow beads and coatings with a thickness exceeding 400 μm. Empirically, a coating thickness of 300 to 600 μm is useful as a heat insulating paint without significantly affecting moldability and durability. [Industrial Applicability]
[0050] The present invention can be used in the field of heat insulation, such as buildings and outdoor units of air conditioners. The present invention is also useful for forming a desired coating film while maintaining flexibility. Therefore, by taking advantage of this characteristic, the present invention can be used in paints in general. The present invention can also be used not only for the equipment of the present embodiment, but also for various objects such as vehicles, aircraft, and ships. [Explanation of symbols]
[0051] 1 Paint film forming material 2. First hollow bead 3. Second hollow bead P paint
Claims
1. A paint comprising first hollow beads made of a synthetic resin material having a Young's modulus of 4 or less and second hollow beads made of an inorganic compound material having a Young's modulus of 80 or more in a coating film-forming material made of an acrylic material, the first hollow beads being made of the same material as the coating film-forming material, A paint in which either or both of the first and second hollow beads are composed of particles of a predetermined size with a particle size difference of 30 μm or more, and in which the content (on a volume basis) of hollow beads with a particle size of 80 μm is the largest.
2. A coating material comprising acrylic hollow beads and ceramic hollow beads in an acrylic film-forming material, A paint in which either or both of the first and second hollow beads are composed of particles of a predetermined size with a particle size difference of 30 μm or more, and in which the content (on a volume basis) of hollow beads with a particle size of 80 μm is the largest.
3. A coating method for coating the paint according to claim 1 or 2 onto a surface of a target facility to a thickness of 300 μm or more.
Citation Information
Patent Citations
Industrial thermal insulation coating and preparation method thereof
CN102093788A
Building board and method for manufacturing the same
JP2014088000A
Aqueous paint composition
JP2017014342A
Crack resistance insulating paint
KR1020200073695A