Resin composition, paint and plastic molded product coated with said paint

A resin composition combining polyolefin-modified acrylic resin and terpene solvent addresses adhesion and storage stability issues, offering a coating solution for plastic substrates with improved appearance and environmental benefits.

JP7581780B2Active Publication Date: 2024-11-13DIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020187113
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-10
Publication Date
2024-11-13
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Conventional polyolefin-modified acrylic resins exhibit insufficient adhesion performance depending on film forming conditions, and there is a need for improved storage stability and environmental sustainability in coating applications.

Method used

A resin composition containing a polyolefin-modified acrylic resin and a terpene solvent in a specific ratio, with the terpene solvent content ranging from 50 to 500% by mass, enhances storage stability and adhesion to plastic substrates, resulting in a coating film with excellent properties.

Benefits of technology

The resin composition provides high adhesion to plastic substrates and forms a coating film with excellent appearance, suitable for various plastic molded products, including electronic device housings and automotive parts, while being environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581780000001
    Figure 0007581780000001
  • Figure 0007581780000002
    Figure 0007581780000002
  • Figure 0007581780000003
    Figure 0007581780000003
Patent Text Reader

Abstract

To provide a resin composition that has high storage stability and can give a coating layer having high adhesion to a plastic substrate and a good appearance, a coating containing the resin composition and a plastic molding coated with the coating.SOLUTION: A resin composition contains a polyolefin-modified acrylic resin and a terpene solvent, the content of the terpene solvent being 50-500 mass% of the polyolefin-modified acrylic resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a paint, and a plastic molded article coated with the paint. [Background technology]

[0002] Polyolefin-modified acrylic resins obtained by reacting unsaturated monomers in the presence of polyolefins have been proposed, and the cured coating films are known to have excellent adhesion to substrates, water resistance, etc. (See, for example, Patent Document 1.) On the other hand, in recent years, there has been a demand for reducing the burden on the environment, and a method for forming thin films at low temperatures is desired.

[0003] However, although the coating film obtained from this polyolefin-modified acrylic resin has excellent water resistance, etc., there is a problem that the adhesion performance is insufficient depending on the film-forming conditions. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-13944 A Summary of the Invention [Problem to be solved by the invention]

[0005] The problem to be solved by the present invention is to provide a resin composition, a paint, and a plastic molded article coated with the paint, which are excellent in storage stability, have high adhesion to plastic substrates, and can give a coating film having excellent appearance. [Means for solving the problem]

[0006] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that a resin composition containing a polyolefin-modified acrylic resin and a terpene solvent in a specific ratio can provide a coating film that has excellent storage stability, high adhesion to plastic substrates, and excellent appearance, thereby completing the invention.

[0007] That is, the present invention relates to a resin composition containing a polyolefin-modified acrylic resin and a terpene solvent, characterized in that the content of the terpene solvent is 50 to 500 mass% of the polyolefin-modified acrylic resin, a paint, and a plastic molded product coated with the paint. Effect of the Invention

[0008] The resin composition of the present invention has high adhesion to plastic substrates and can provide coating films with excellent appearance, and is therefore useful as a coating material, and can be applied to various plastic molded products. Therefore, the resin composition of the present invention can be suitably used as a coating material for coating various articles such as housings for electronic devices such as mobile phones, smartphones, tablet terminals, personal computers, digital cameras, and game consoles; housings for home appliances such as televisions, refrigerators, washing machines, and air conditioners; interior materials for various vehicles such as automobiles and railway cars; and toys. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The resin composition of the present invention is a resin composition containing a polyolefin-modified acrylic resin and a terpene solvent, and the content of the terpene solvent is 50 to 500% by mass of the polyolefin-modified acrylic resin.

[0010] The polyolefin-modified acrylic resin may be a mixture of polyolefin resin (A) and acrylic resin (B), or may be a combination of polyolefin resin (A) and acrylic resin (B). In view of improved storage stability, the polyolefin-modified acrylic resin preferably contains a combination of polyolefin resin (A) and acrylic resin (B).

[0011] A preferred method for obtaining the polyolefin-modified acrylic resin is to radically polymerize the unsaturated monomer mixture (b), which is the raw material for the acrylic resin (B), in the presence of the polyolefin resin (A).

[0012] As the polyolefin resin (A), chlorinated polyolefin resins and maleic acid modified polyolefin resins are preferred because they have excellent storage stability and adhesion of the resulting coating film. The polyolefin resin (A) can be used alone or in combination of two or more kinds.

[0013] The chlorinated polyolefin resin is a chlorinated polyolefin resin, and examples of the polyolefin resin include polypropylene, high density polyethylene, ultra-high molecular weight polyethylene, linear low density polyethylene, low density polyethylene, very low density polyethylene, ultra-low density polyethylene, polymethylpentene, ethylene-propylene copolymer, propylene-1-butene random copolymer, propylene-ethylene-1-butene random copolymer, copolymer of propylene and α-olefin having 5 to 12 carbon atoms, propylene-non-conjugated diene copolymer, ethylene-non-conjugated diene copolymer, ethylene-propylene-non-conjugated diene copolymer, polybutene, ethylene-vinyl acetate copolymer, ethylene-vinyltrimethoxysilane copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, styrene-butadiene block copolymer, and hydrogenated products thereof. The chlorinated polyolefin resin may be partially modified with maleic acid.

[0014] The chlorine content of the chlorinated polyolefin resin is preferably 15 to 40% by mass, since this further improves compatibility and adhesion.

[0015] The chlorinated polyolefin resins can be used alone or in combination of two or more kinds, but a polymer containing polypropylene is preferred because it has improved storage stability.

[0016] The maleic acid modified polyolefin resin is a polyolefin resin modified with maleic acid, and as the polyolefin resin, those exemplified as those usable for the chlorinated polyolefin resin can be used.

[0017] The maleic acid modified polyolefin resins can be used alone or in combination of two or more kinds, but a polymer containing polypropylene is preferred because it has improved storage stability.

[0018] The weight average molecular weight of the polyolefin resin (A) is preferably 20,000 to 250,000.

[0019] Next, the unsaturated monomer mixture (b) will be described. Since the unsaturated monomer mixture (b) can be used in two-component curing, it preferably contains an unsaturated monomer (b1) having a hydroxyl group, and more preferably contains an unsaturated monomer (b2) having a carboxyl group from the viewpoint of pot life during two-component curing.

[0020] Examples of the unsaturated monomer (b1) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerin mono(meth)acrylate, polyoxyethylene mono(meth)acrylate, polyoxypropylene mono(meth)acrylate, polyoxybutylene mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, polycaprolactone-modified hydroxyethyl mono(meth)acrylate, etc. Among these, 2-hydroxyethyl (meth)acrylate is preferred because it has better curability with polyisocyanate. These unsaturated monomers (b1) can be used alone or in combination of two or more kinds.

[0021] In the present invention, "(meth)acrylic acid" refers to either or both of methacrylic acid and acrylic acid, "(meth)acrylate" refers to either or both of methacrylate and acrylate, and "(meth)acryloyl group" refers to either or both of methacryloyl group and acryloyl group.

[0022] Examples of the unsaturated monomer (b2) having a carboxyl group include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, β-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl succinate, and 2-(meth)acryloyloxyethyl hexahydrophthalic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, or half esters of these unsaturated dicarboxylic acids. Among these, (meth)acrylic acid is preferred. These unsaturated monomers (b2) can be used alone or in combination of two or more.

[0023] Examples of the unsaturated monomer (b3) other than the unsaturated monomer (b1) and the unsaturated monomer (b2) that can be contained in the unsaturated monomer mixture (b) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, and the like. acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, benzyl (meth)acrylate; acrylamide, N,N-dimethyl (meth)acrylamide, (meth)acrylonitrile, 3-(meth)acryloyloxypropyltrimethoxysilane, N,N-dimethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl acid phosphate, glycidyl (meth)acrylate, vinyl acetate, styrene, α-methylstyrene, p-methylstyrene, p-methoxystyrene, diacrylate compounds such as ethylene glycol diacrylate, etc. Among these, (meth)acrylate compounds are preferred, and (meth)acrylates having an alkyl group with 1 to 15 carbon atoms are more preferred. These unsaturated monomers (b3) can be used alone or in combination of two or more kinds.

[0024] The mass ratio of the unsaturated monomer (b1) in the unsaturated monomer mixture (b) is preferably 1 to 20 mass %, more preferably 2 to 10 mass %, in order to further improve the balance between appearance and adhesion.

[0025] The mass ratio of the unsaturated monomer (b2) in the unsaturated monomer mixture (b) is preferably from 0.1 to 10 mass %, more preferably from 0.3 to 5 mass %, in order to further improve the balance between appearance and adhesion.

[0026] The mass ratio of methyl methacrylate in the unsaturated monomer mixture (b) is preferably from 10 to 90 mass %, more preferably from 25 to 60 mass %, in order to further improve the balance between appearance and adhesion.

[0027] The mass ratio of the pre-unsaturated monomer (b4) in the unsaturated monomer mixture (b) is preferably from 10 to 95 mass %, more preferably from 50 to 90 mass %, in order to further improve the balance between appearance and adhesion.

[0028] The radical polymerization method for obtaining the polyolefin-modified acrylic resin is a method in which each monomer, which is raw material, is polymerized in the presence of a polymerization initiator.The solvent that can be used in this case can be, for example, aromatic hydrocarbon compounds such as toluene and xylene; alicyclic hydrocarbon compounds such as cyclohexane, methylcyclohexane and ethylcyclohexane; ketone compounds such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone; ester compounds such as ethyl acetate, n-butyl acetate, isobutyl acetate and propylene glycol monomethyl ether acetate; alcohol compounds such as n-butanol, isopropyl alcohol and cyclohexanol; glycol compounds such as ethylene glycol monobutyl ether and propylene glycol monomethyl ether; aliphatic hydrocarbon compounds such as heptane, hexane, octane and mineral turpentine.

[0029] Examples of the polymerization initiator include ketone peroxide compounds such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, and 2,2-bis(4,4-ditert-butylperoxycyclohexyl). peroxyketal compounds such as 2,2-bis(4,4-ditert-amylperoxycyclohexyl)propane, 2,2-bis(4,4-ditert-hexylperoxycyclohexyl)propane, 2,2-bis(4,4-ditert-octylperoxycyclohexyl)propane, and 2,2-bis(4,4-dicumylperoxycyclohexyl)propane; hydroperoxides such as cumene hydroperoxide and 2,5-dimethylhexane-2,5-dihydroperoxide. peroxides; dialkyl peroxide compounds such as 1,3-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide, tert-butylcumyl peroxide, and di-tert-butyl peroxide; diacyl peroxide compounds such as decanoyl peroxide, lauroyl peroxide, benzoyl peroxide, and 2,4-dichlorobenzoyl peroxide; bis(tert- peroxycarbonate compounds such as tert-butylperoxy-2-ethylhexanoate, tert-butylperoxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and other peroxyester compounds; and azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methyl)butyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile).

[0030] The mass ratio of the polyolefin resin (A) to the unsaturated monomer mixture (b) [(A) / (b)] is preferably in the range of 5 / 95 to 40 / 60, more preferably 10 / 90 to 30 / 70, since this further improves the storage stability, adhesion and appearance of the resulting coating film.

[0031] The polyolefin-modified acrylic resin has a number average molecular weight (Mn) of preferably 3,000 to 50,000, more preferably 15,000 to 30,000, since this improves the storage stability, and the appearance and adhesion of the resulting coating film. The weight average molecular weight (Mw) is preferably 30,000 to 300,000, more preferably 40,000 to 100,000. Here, the average molecular weight is a value calculated in terms of polystyrene based on gel permeation chromatography (hereinafter abbreviated as "GPC") measurement.

[0032] Examples of the terpene solvent include monoterpene hydrocarbons such as α-pinene, β-pinene, dipentene, limonene, turpentine, phellandrene, α-terpinene, γ-terpinene, terpinolene, myrcene, alloocimene, camphene, bornylene, paramenthene-1, paramenthene-2, paramenthene-3, paramentadiene, paramenthane, 2-carene, 3-carene, and thujane; monoterpene alcohols such as α-terpineol, β-terpineol, γ-terpineol, 4-terpineol, paramenthenol, geraniol, linalool, nerol, citronellol, allocimenol, myrcenol, carveol, menthol, borneol, isoborneol, fenchyl alcohol, and verbenol; Examples of the terpene include terpene aldehydes such as tetrahydrofuran and citronellal, terpene ketones such as isopulegone, carvone, camphor (camphor white oil), terpene diols such as paramenthanediol, terpene ethers such as 1,4-cineole and 1,8-cineole, sesquiterpene hydrocarbons such as longifolene, caryophyllene, cadinene, thujopsene, cedrene, clobene, longipinene, and the like, and sesquiterpene alcohols such as elemol, cadinol, and eudesmol, etc. Among these, dipentene, limonene, camphor, and turpentine are preferred because they provide improved adhesion.

[0033] The content of the terpene solvent in the resin composition of the present invention is 50 to 500 mass% of the polyolefin-modified acrylic resin, but 100 to 300 mass% is preferable because this further improves the storage stability, and the appearance and adhesion of the resulting coating film.

[0034] The coating material of the present invention contains the above-mentioned resin composition, and may contain additives such as solvents other than terpene solvents, antifoaming agents, viscosity modifiers, light stabilizers, weather stabilizers, heat stabilizers, ultraviolet absorbers, antioxidants, leveling agents, pigment dispersants, etc. Also, pigments such as titanium oxide, calcium carbonate, aluminum powder, copper powder, mica powder, iron oxide, carbon black, phthalocyanine blue, toluidine red, perylene, quinacridone, and benzidine yellow may also be used.

[0035] The coating material of the present invention has high adhesion to plastic substrates and can therefore be suitably used as a coating material for painting various plastic molded products. Examples of plastic molded products to which the coating material of the present invention can be applied include housings for electronic devices such as mobile phones, smartphones, tablet terminals, personal computers, digital cameras, and game consoles; housings for home appliances such as televisions, refrigerators, washing machines, and air conditioners; and interior materials for various vehicles such as automobiles and railway cars.

[0036] Examples of methods for applying the coating material of the present invention include methods using a spray, an applicator, a bar coater, a gravure coater, a roll coater, a comma coater, a knife coater, an air knife coater, a curtain coater, a kiss coater, a shower coater, a wheeler coater, a spin coater, dipping, screen printing, etc. In addition, methods for forming a coating film after application include a method of drying at room temperature to 120°C. EXAMPLES

[0037] The present invention will be described in more detail below with reference to specific examples. The average molecular weight was measured under the following GPC measurement conditions.

[0038] [GPC measurement conditions] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 4 mg / mL in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following monodisperse polystyrene.

[0039] (monodisperse polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0040] (Synthesis Example 1: Synthesis of polyolefin modified acrylic resin (1)) In a flask equipped with a cooling tube, a thermometer, a dropping funnel, and a stirrer, 100.0 parts by mass of maleic acid-modified polyolefin ("Auroren 350S" manufactured by Nippon Paper Industries Co., Ltd.; hereinafter, abbreviated as "polyolefin resin (A-1)"), 742.5 parts by mass of butyl acetate, and 487.5 parts by mass of methyl ethyl ketone were added, and the internal temperature was raised to 80 ° C. Next, after confirming the dissolution of the maleic acid-modified polyolefin, a mixture of 360.0 parts by mass of methyl methacrylate, 485.0 parts by mass of ethyl acrylate, 50.0 parts by mass of 2-hydroxypropyl methacrylate, 5.0 parts by mass of methacrylic acid, 250.0 parts by mass of methyl ethyl ketone, and 5.0 parts by mass of tert-butylperoxy 2-ethylhexanoate was added dropwise over 4 hours. One hour after the completion of the dropwise addition, a mixture of 5.0 parts by mass of methyl ethyl ketone and 2.0 parts by mass of tert-butyl peroxy 2-ethylhexanoate was added, and then a polymerization reaction was carried out for 10 hours while maintaining the internal temperature at 80° C. Next, a mixed solvent (butyl acetate / methyl ethyl ketone=50 / 50 (mass ratio)) was added so that the nonvolatile content was 40 mass%, and a solution of polyolefin-modified acrylic resin (1) was obtained.

[0041] (Synthesis Examples 2 and 3: Synthesis of Polyolefin-Modified Acrylic Resins (2) and (3)) Solutions of polyolefin-modified acrylic resins (2) and (3) were obtained in the same manner as in Synthesis Example 1, except that the compositions of the polyolefin resin and unsaturated monomer mixture used in Synthesis Example 1 were changed as shown in Table 1.

[0042] (Synthesis Example 4: Synthesis of polyolefin modified acrylic resin (R1)) A solution of polyolefin-modified acrylic resin (R1) was obtained in the same manner as in Synthesis Example 1, except that the compositions of the polyolein resin and unsaturated monomer mixture used in Synthesis Example 1 were changed as shown in Table 1.

[0043] Table 1 shows the compositions of the polyolefin-modified acrylic resins (1) to (3) and (R1) obtained above.

[0044] [Table 1]

[0045] The abbreviations in Table 1 are as follows. Polyolefin resin (A-1): "Auroren 350S" manufactured by Nippon Paper Industries Co., Ltd. Polyolefin resin (A-2): "Hardlen 14-LLB-P" manufactured by Toyobo Co., Ltd., chlorine content 27% by mass MMA: Methyl methacrylate HPMA: 2-hydroxypropyl methacrylate AA: Acrylic acid EA: Ethyl acrylate

[0046] (Example 1: Preparation and evaluation of resin composition (1)) A resin composition (1) was obtained by blending 15 parts by mass of the solution of polyolefin-modified acrylic resin (1) obtained in Synthesis Example 1 above (non-volatile content: 40% by mass) and 12 parts by mass of dipentene.

[0047] [Evaluation of storage stability] The resin composition (1) was allowed to stand at 40° C. for one month, and the state of the solution was evaluated according to the following criteria. ○: Neither separation nor precipitation is observed △: Separation and / or precipitation was observed, but the mixture was easily dispersed by stirring. ×: Separation and / or precipitation was observed, and the mixture could not be easily dispersed by stirring.

[0048] [Paint evaluation] The resin composition (1) obtained above was diluted with a mixed solvent (butyl acetate / propylene glycol monomethyl ether acetate / ethyl acetate = 75 / 10 / 15 (mass ratio); hereinafter abbreviated as "mixed solvent (1)") so that the viscosity was about 9 seconds (23°C) in "Viscosity Cup NK-2" manufactured by Anest Iwata Corporation, to prepare a paint (1).

[0049] [Preparation of coating film for evaluation] The paint (1) obtained above was spray-coated onto a polypropylene substrate (50 mm x 50 mm) so that the film thickness after drying would be 5 to 10 μm, and the coating was dried by heating in a dryer at 70°C for 30 minutes, and then dried at 25°C for 1 day to prepare a cured coating film for evaluation.

[0050] [Evaluation of coating appearance] The coating film for evaluation obtained above was visually observed, and the appearance of the coating film was evaluated according to the following criteria. 〇: No problem △: Slightly whitened ×: Significant whitening

[0051] [Adhesion evaluation] The coating film for evaluation obtained above was cut with a cutter to make 1 mm wide squares, so that the number of squares was 100. Next, cellophane tape was applied so as to cover all the squares, and the operation of quickly peeling it off was repeated four times, and the adhesion was evaluated according to the following criteria based on the number of squares remaining. ○:100 pieces △:70~99 pieces ×: 69 or less

[0052] (Examples 2 to 8: Preparation and evaluation of resin compositions (2) to (8)) Resin compositions (2) to (8) and coating materials (2) to (8) were obtained and evaluated in the same manner as in Example 1, except that the compositions of the polyolefin-modified acrylic resin (1) and the terpene solvent used in Example 1 were changed as shown in Table 2.

[0053] (Comparative Examples 1 to 6: Synthesis of Resin Compositions (R1) to (R6)) Resin compositions (R1) to (R6) and coating materials (R1) to (R6) were obtained in the same manner as in Example 1, except that the compositions of the polyolefin-modified acrylic resin (1) and the terpene solvent used in Example 1 were changed as shown in Table 2, and each evaluation was performed.

[0054] The compositions and evaluation results of the polyolefin-modified acrylic resins (1) to (8) obtained above are shown in Tables 2 and 3.

[0055] [Table 2]

[0056] [Table 3]

[0057] Table 4 shows the compositions and evaluation results of the polyolefin-modified acrylic resins (R1) to (R6) obtained above.

[0058] [Table 4]

[0059] The abbreviations in Table 4 are as follows: Swaclean 150: Petroleum-based hydrocarbon solvent manufactured by Maruzen Petrochemical Co., Ltd. MCH: Methylcyclohexane The terpene solvents used in the examples and comparative examples were manufactured by Nippon Terpene Chemical Co., Ltd.

[0060] It was confirmed that the resin compositions of the present invention in Examples 1 to 8 had excellent storage stability, and the resulting coating films had excellent coating appearance and adhesion.

[0061] On the other hand, in Comparative Example 1, the content of Perthen solvent relative to the polyolefin-modified acrylic resin was less than 50% by mass, which is the lower limit of the present invention, but it was confirmed that the adhesion was insufficient.

[0062] Comparative Example 2 is an example in which the content of Perylene solvent relative to the polyolefin-modified acrylic resin is greater than 500% by mass, which is the upper limit of the present invention, but it was confirmed that the appearance of the coating film was insufficient.

[0063] Comparative Example 3 is an example in which an unmodified acrylic resin was used instead of the polyolefin-modified acrylic resin, but it was confirmed that the adhesion was insufficient.

[0064] Comparative Examples 4 to 6 are examples in which the terpene solvent, which is an essential component, was not used, but it was confirmed that the adhesion or coating film appearance was insufficient.

Claims

1. A resin composition containing a polyolefin-modified acrylic resin and a terpene solvent, wherein the polyolefin-modified acrylic resin is a reaction product of a polyolefin resin (A) and an unsaturated monomer mixture (b) containing an unsaturated monomer (b1) having a hydroxyl group, the mass ratio of the polyolefin resin (A) to the unsaturated monomer mixture (b) [(A) / (B)] being 5 / 95 to 60 / 40, the polyolefin resin (A) being a chlorinated polyolefin resin and / or a maleic acid-modified polyolefin resin, and the content of the terpene solvent is 100 to 500 mass% of the polyolefin-modified acrylic resin.

2. A paint comprising the resin composition according to claim 1.

3. A plastic molded product coated with the paint according to claim 2.

Citation Information

Patent Citations

  • Surface treating of polyolefinic molded article

    JP1978142471A

  • Coating composition

    JP1993009428A

  • Thermoplastic resin obtained by grafting unsaturated monomer to chlorinated polyolefin and its production

    JP1994192352A

  • Resin composition

    JP1998292085A

  • Graft polyolefin and resin composition for coating containing the same

    JP2002212241A