Binder for secondary battery electrodes and its use

A crosslinked polymer binder with specific monomer components addresses the issues of high viscosity and peeling in secondary battery electrodes, enhancing binding properties and durability, especially with silicon-based materials.

JP7581878B2Active Publication Date: 2024-11-13TOAGOSEI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020553866
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-31
Filing Date
2019-10-25
Publication Date
2024-11-13
Estimated Expiration
2039-10-25

AI Technical Summary

Technical Problem

Existing binders for secondary battery electrodes, while providing good binding properties, increase slurry viscosity, leading to decreased coatability, and the use of silicon-based active materials results in electrode mixture layer peeling due to volumetric changes during charging and discharging, affecting battery capacity and durability.

Method used

A crosslinked polymer binder containing non-crosslinked and crosslinked structural units, derived from ethylenically unsaturated carboxylic acid monomers and crosslinkable monomers with (meth)acryloyl groups and hydroxyl groups, which reduces slurry viscosity and enhances binding properties.

Benefits of technology

The binder achieves low slurry viscosity and excellent binding properties, ensuring electrode integrity and durability, particularly with silicon-based active materials, by uniformly distributing crosslinks and suppressing surface swelling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581878000001
    Figure 0007581878000001
  • Figure 0007581878000002
    Figure 0007581878000002
Patent Text Reader

Abstract

In order to achieve both good binding properties in secondary battery electrodes and suppressed viscosity of electrode slurry, a secondary battery electrode binder is provided, which comprises a crosslinked polymer or a salt thereof, which comprises a non-crosslinked structural unit and a crosslinked structural unit, wherein the non-crosslinked structural unit includes a non-crosslinked structural unit derived from an ethylenically unsaturated carboxylic acid monomer, and the crosslinked structural unit includes a crosslinked structural unit derived from a crosslinkable monomer having two or more (meth)acryloyl groups in one molecule and having a hydroxyl group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present specification relates to a binder for secondary battery electrodes and its use. (CROSS REFERENCE TO RELATED APPLICATIONS) This application is a related application of Japanese patent application No. 2018-205228, filed on October 31, 2018, and claims priority to said Japanese application, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] Various types of power storage devices, such as nickel-hydrogen secondary batteries, lithium-ion secondary batteries, and electric double-layer capacitors, have been put to practical use as secondary batteries. Electrodes used in these secondary batteries are produced by coating a composition for forming an electrode mixture layer containing an active material and a binder on a current collector, followed by drying, etc. For example, in lithium-ion secondary batteries, a water-based binder containing styrene butadiene rubber (SBR) latex and carboxymethyl cellulose (CMC) is used as the binder for the negative electrode mixture layer composition.

[0003] On the other hand, as the applications of various secondary batteries expand, there is a tendency for the demand for improved energy density, reliability, and durability to increase. For example, in order to increase the electric capacity of lithium-ion secondary batteries, specifications using silicon-based active materials as negative electrode active materials are increasing. However, it is known that silicon-based active materials have a large volume change during charging and discharging, and as they are used repeatedly, peeling or falling off of the electrode mixture layer occurs, resulting in a decrease in the capacity of the battery and a deterioration in cycle characteristics (durability). In order to suppress such defects, it is generally effective to increase the binding property of the binder, and studies on improving the binding property of the binder have been conducted in order to improve durability.

[0004] As a binder having good binding properties and effective in improving durability, a binder using the above-mentioned acrylic acid polymer has been proposed. Patent Document 1 describes that by using a polymer obtained by crosslinking polyacrylic acid with a specific crosslinking agent as a binder, it is possible to provide an electrode whose electrode structure is not destroyed even when an active material containing silicon is used. Patent Document 2 describes that an electrode obtained by using a binder containing a crosslinked polymer or a salt thereof having a carboxy group, which has a sufficiently small particle size when dispersed in salt water after neutralization, exhibits excellent binding properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2014 / 065407 [Patent Document 2] International Publication No. 2017 / 073589 Summary of the Invention [Problem to be solved by the invention]

[0006] Although the binders disclosed in each patent document can provide good binding properties, with the improvement of the performance of secondary batteries, an electrode mixture layer with even higher binding properties is required. In addition, when the amount of binder is increased to improve the binding properties, the slurry viscosity of the electrode mixture layer composition increases, and the coating properties are reduced. For this reason, a binder capable of reducing the slurry viscosity is required.

[0007] The present specification provides a binder capable of achieving both improved binding property and reduced viscosity of a slurry for an electrode mixture layer, and use thereof. [Means for solving the problem]

[0008] The present inventors have conducted various studies, focusing on crosslinkable monomers, on improving the binding property without increasing the slurry viscosity, and have found that the above-mentioned problems can be solved by a crosslinked polymer using a crosslinkable monomer having two or more (meth)acryloyl groups having high radical reactivity and a hydroxyl group. According to the present specification, the following means are provided based on such findings.

[0009] [1] A secondary battery electrode binder having a crosslinked polymer or a salt thereof, The crosslinked polymer or salt thereof has a non-crosslinked structural unit and a crosslinked structural unit, The non-crosslinked structural unit includes a non-crosslinked structural unit derived from an ethylenically unsaturated carboxylic acid monomer, The crosslinked structural unit includes a crosslinked structural unit derived from a crosslinkable monomer having two or more (meth)acryloyl groups and a hydroxyl group in one molecule. binder. [2] The binder according to [1], which contains non-crosslinked structural units derived from the ethylenically unsaturated monomer in an amount of 30 mass % or more and 100 mass % or less based on the total amount of the non-crosslinked structural units. [3] A composition for a secondary battery electrode, [1] or [2], An active material; Water, A composition comprising: [4] A secondary battery electrode, [1] or [2], An active material; An electrode comprising: [5] The electrode according to [4], further comprising: the active material being a silicon-containing material. [6] A method for producing a binder for a secondary battery electrode, comprising the steps of: A step of polymerizing a monomer composition containing an ethylenically unsaturated carboxylic acid monomer and a crosslinkable monomer having two or more (meth)acryloyl groups and a hydroxyl group in one molecule; The manufacturing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The binder for secondary battery electrodes disclosed in this specification (hereinafter, also simply referred to as the present binder) can contain a crosslinked polymer or a salt thereof (hereinafter, also simply referred to as the present polymer). The present polymer has a non-crosslinked structural unit and a crosslinked structural unit, the non-crosslinked structural unit containing a non-crosslinked structural unit derived from an ethylenically unsaturated monomer, and the crosslinked structural unit containing a crosslinked structural unit containing two or more (meth)acryloyl groups in one molecule and a crosslinked monomer containing a hydroxyl group.

[0011] The present polymer has a carboxylic acid in the non-crosslinked structural unit, and therefore serves as a binder with good binding properties. The present polymer also contains a crosslinked structural unit derived from a crosslinkable monomer having two or more (meth)acryloyl groups in the crosslinked structural unit. Such a crosslinkable monomer has a relatively high radical polymerizability, and therefore crosslinked structural units are formed relatively uniformly from the inside of the polymer particle to the surface portion. In other words, it is considered that the crosslink density of the surface of the present polymer particle obtained by crosslinking polymerization can be suppressed from increasing excessively, and as a result, the swelling degree of the surface of the present polymer particle in water is relatively high, and the adhesive area with the active material and the current collector can be secured, and it is considered that the binder containing the present polymer particle exhibits good binding properties.

[0012] In addition, since the present polymer has hydroxyl groups in the crosslinked structural units, the swelling degree of the present polymer particles can be suppressed by interactions (hydrogen bonds, etc.) due to the hydroxyl groups within the polymer particles, thereby suppressing an increase in the slurry viscosity.

[0013] The composition for secondary battery electrodes contains the binder, and therefore has ease of application. In addition, secondary battery electrodes containing the binder exhibit excellent binding properties. In addition, the method for producing the binder, the composition for secondary battery electrodes, and the method for producing a secondary battery electrode can provide an electrode with excellent binding properties by suppressing the increase in viscosity during preparation of a slurry for an electrode.

[0014] The binder contains the polymer, and can be mixed with an active material and water to form a composition for a secondary battery electrode (electrode mixture layer composition, hereinafter also simply referred to as the composition). The composition may be in a slurry state that can be applied to a current collector, or may be prepared in a wet powder state so that it can be pressed onto the surface of the current collector. The secondary battery electrode disclosed in the present specification (hereinafter also simply referred to as the electrode) can be obtained by forming a mixture layer formed from the composition on the surface of a current collector such as copper foil or aluminum foil.

[0015] Representative and non-limiting specific examples of the present binder, the present composition, the method for producing the present binder, the method for producing the present composition, and the method for producing the present electrode will be described in detail below with reference to the drawings as appropriate. This detailed description is intended simply to provide those skilled in the art with details for carrying out preferred examples of the present disclosure, and is not intended to limit the scope of the present disclosure. In addition, the additional features disclosed below can be used separately or together with other features and disclosures to provide a further improved "binder for secondary battery electrode and use thereof".

[0016] In addition, the combinations of features and steps disclosed in the following detailed description are not essential to the implementation of the present disclosure in the broadest sense, but are described only to specifically illustrate representative embodiments of the present disclosure. Furthermore, the various features of the representative embodiments described above and below, and the various features of those described in the independent and dependent claims, do not have to be combined in the specific examples described herein or in the order listed to provide additional and useful embodiments of the present disclosure.

[0017] All features described in the specification and / or claims are intended to be disclosed individually and independently of one another as limitations to the original disclosure and claimed particulars, apart from any configuration of features described in the examples and / or claims. Furthermore, all numerical ranges and group or aggregate descriptions are intended to disclose their intermediate configurations as limitations to the original disclosure and claimed particulars.

[0018] In this specification, "(meth)acrylic" means acrylic and / or methacrylic, "(meth)acrylate" means acrylate and / or methacrylate, and "(meth)acryloyl group" means acryloyl group and / or methacryloyl group.

[0019] <Binder> The binder can contain the polymer, i.e., a crosslinked polymer or a salt thereof. The binder can contain only the polymer, or can contain other binder components as described below. Preferably, the binder contains the polymer in an amount of 50% by mass or more, such as 60% by mass or more, such as 70% by mass or more, such as 80% by mass or more, such as 90% by mass or more, such as 95% by mass or more, or such as 100% by mass.

[0020] <Structural unit of crosslinked polymer> <Non-crosslinked structural unit> The polymer has a non-crosslinked structural unit and a crosslinked structural unit. The non-crosslinked structural unit is not particularly limited, and may include a structural unit derived from various non-crosslinkable monomers that can be used in a crosslinked polymer that can be used as a binder for a secondary battery electrode.

[0021] The non-crosslinked structural unit may have, for example, a structural unit derived from an ethylenically unsaturated carboxylic acid monomer (hereinafter, also referred to as "component (a)"). By having a carboxyl group in the structural unit, the adhesion to the current collector is improved, and the lithium ion desolvation effect and ion conductivity are excellent, so that an electrode with low resistance and excellent high-rate characteristics can be obtained. In addition, since water swelling is imparted, the dispersion stability of the active material in the composition can be improved. The above structural unit can be introduced into the polymer by, for example, polymerizing a monomer containing an ethylenically unsaturated carboxylic acid monomer. In addition, it can also be obtained by (co)polymerizing a (meth)acrylic acid ester monomer and then hydrolyzing it. In addition, after polymerizing (meth)acrylamide and (meth)acrylonitrile, etc., a strong alkali treatment may be performed, or a method of reacting an acid anhydride with the polymer having a hydroxyl group may be used.

[0022] Examples of the ethylenically unsaturated carboxylic acid monomer include (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, and fumaric acid; (meth)acrylamidoalkyl carboxylic acids such as (meth)acrylamidohexanoic acid and (meth)acrylamidododecanoic acid; ethylenically unsaturated monomers having a carboxy group such as monohydroxyethyl succinate (meth)acrylate, ω-carboxy-caprolactone mono(meth)acrylate, and β-carboxyethyl (meth)acrylate, or their (partial) alkali neutralization products. One of these may be used alone, or two or more may be used in combination. Among the above, a compound having an acryloyl group as a polymerizable functional group is preferred, in that a polymer with a long primary chain length is obtained due to a high polymerization rate, and the binding strength of the binder is good, and acrylic acid is particularly preferred. When acrylic acid is used as the ethylenically unsaturated carboxylic acid monomer, a polymer with a high carboxy group content can be obtained.

[0023] The carboxyl group of the ethylenically unsaturated carboxylic acid monomer may be free or at least a part of the carboxyl group may be a salt. The type of salt is not particularly limited, and examples thereof include alkali metal salts such as lithium, sodium, and potassium; alkaline earth metal salts such as calcium salts and barium salts; other metal salts such as magnesium salts and aluminum salts; ammonium salts, and organic amine salts. Among these, alkali metal salts and magnesium salts are preferred from the viewpoint of less adverse effect on battery characteristics, and alkali metal salts are more preferred. A particularly preferred alkali metal salt is lithium salt.

[0024] The content of the (a) component in the present polymer is not particularly limited, but may be, for example, 10% by mass or more and 100% by mass or less based on the total amount of the non-crosslinked structural units of the present polymer. By containing the (a) component in such a range, excellent adhesion to the current collector can be easily ensured. The lower limit is, for example, 20% by mass or more, for example, 30% by mass or more, and for example, 40% by mass or more. The lower limit may be 50% by mass or more, for example, 60% by mass or more, for example, 70% by mass or more, and for example, 80% by mass or more. When the content is 30% by mass or more, adhesion to the current collector can be ensured, and an electrode with excellent high-rate characteristics can be obtained because of the excellent lithium ion desolvation effect and ion conductivity. In addition, the dispersion stability of the active material in the present composition can be improved due to the water swelling property. Such effects tend to be improved by increasing the content of the (a) component.

[0025] Also, the upper limit is 100% by mass, and although 100% by mass may be suitable, it is, for example, 99% by mass or less, such as 98% by mass or less, such as 95% by mass or less, and for example 90% by mass or less.

[0026] The range of the (a) component can be a range that appropriately combines these lower and upper limits, and can be, for example, 10% by mass or more and 100% by mass or less, for example, 20% by mass or more and 100% by mass or less, for example, 30% by mass or more and 100% by mass or less, for example, 50% by mass or more and 100% by mass or less, for example, 60% by mass or more and 100% by mass or less, or for example, 70% by mass or more and 100% by mass or less, etc. If the ratio of the (a) component to all structural units is less than 10% by mass, the dispersion stability, binding property, and durability as a battery may be insufficient.

[0027] The content of the component (a) relative to the total amount of non-crosslinked structural units can also be obtained, for example, as the content of the ethylenically unsaturated carboxylic acid monomer relative to the total amount of non-crosslinkable monomers used in the present polymer.

[0028] <Other structural units> In addition to the component (a), the polymer may contain a structural unit derived from another ethylenically unsaturated monomer copolymerizable therewith (hereinafter also referred to as "component (b)"). Examples of the component (b) include structural units derived from an ethylenically unsaturated monomer compound having an anionic group other than a carboxy group, such as a sulfonic acid group and a phosphoric acid group, or a nonionic ethylenically unsaturated monomer. These structural units can be introduced by copolymerizing an ethylenically unsaturated monomer compound having an anionic group other than a carboxy group, such as a sulfonic acid group and a phosphoric acid group, or a monomer containing a nonionic ethylenically unsaturated monomer. Among these, as the component (b), a structural unit derived from a nonionic ethylenically unsaturated monomer is preferred from the viewpoint of obtaining an electrode with good bending resistance, and (meth)acrylamide and its derivatives are preferred from the viewpoint of excellent binder binding property and slurry viscosity. In addition, when a structural unit derived from a hydrophobic ethylenically unsaturated monomer having a solubility in water of 1 g / 100 ml or less is introduced as component (b), it can exert a strong interaction with the electrode material and exhibit good binding properties to the active material. This is preferable because it is possible to obtain a firm and well-integrated electrode mixture layer. In particular, a structural unit derived from an alicyclic structure-containing ethylenically unsaturated monomer is preferable.

[0029] As the nonionic ethylenically unsaturated monomer, (meth)acrylamide and its derivatives are preferred because of their excellent binder binding property and slurry viscosity. Examples of (meth)acrylamide derivatives include N-alkyl (meth)acrylamide compounds such as isopropyl (meth)acrylamide, t-butyl (meth)acrylamide, Nn-butoxymethyl (meth)acrylamide, and N-isobutoxymethyl (meth)acrylamide; and N,N-dialkyl (meth)acrylamide compounds such as dimethyl (meth)acrylamide and diethyl (meth)acrylamide. One of these may be used alone, or two or more may be used in combination.

[0030] The ratio of the (b) component, which is (meth)acrylamide and its derivatives, can be, for example, 0% by mass or more and 90% by mass or less, based on the total amount of non-crosslinked structural units. The ratio of the (b) component can also be, for example, 1% by mass or more and 70% by mass or less, for example, 2% by mass or more and 60% by mass or less, for example, 5% by mass or more and 50% by mass or less, or for example, 10% by mass or more and 30% by mass or less. When the (b) component is contained in an amount of 1% by mass or more based on the total amount of non-crosslinked structural units, the affinity to the electrolyte is improved, and therefore the effect of improving lithium ion conductivity can also be expected. When the (b) component is contained in an amount of 70% by mass or less based on the total amount of non-crosslinked structural units, it may be useful for suppressing the slurry viscosity.

[0031] Other nonionic ethylenically unsaturated monomers may include, for example, (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include (meth)acrylic acid alkyl ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; (meth)acrylic acid cycloalkyl ester compounds such as cyclohexyl (meth)acrylate and methylcyclohexyl (meth)acrylate; (meth)acrylic acid alkoxyalkyl ester compounds such as 2-methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; (meth)acrylic acid hydroxyalkyl ester compounds such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate, and the like. One of these may be used alone, or two or more may be used in combination. When a (meth)acrylic acid ester is used as the nonionic ethylenically unsaturated monomer, the ratio of structural units derived from the (meth)acrylic acid ester is preferably 1 to 30 mass%, more preferably 5 to 30 mass%, and even more preferably 10 to 30 mass%, based on the total amount of non-crosslinked structural units of the present polymer. In this case, the ratio of the above component (a) is preferably 70 to 99 mass%, more preferably 70 to 95 mass%, and even more preferably 70 to 90 mass%, based on the total amount of structural units of the present polymer.

[0032] Among the above, compounds having an ether bond, such as alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, are preferred, from the viewpoint of high lithium ion conductivity and further improved high-rate characteristics, and 2-methoxyethyl (meth)acrylate is more preferred.

[0033] Among nonionic ethylenically unsaturated monomers, compounds having an acryloyl group are preferred because they have a fast polymerization rate, resulting in a polymer with a long primary chain length, and because they provide good binding strength for the binder. As nonionic ethylenically unsaturated monomers, compounds having a homopolymer glass transition temperature (Tg) of 0° C. or less are preferred because they provide good bending resistance for the resulting electrodes.

[0034] <Cross-linking structural unit> The present polymer may have, as a crosslinked structural unit, a crosslinked structural unit (hereinafter also referred to as "component (c)") derived from a crosslinkable monomer having two or more (meth)acryloyl groups in one molecule and having a hydroxyl group.

[0035] The two or more (meth)acryloyl groups that the component (c) can have can be two or more methacryloyl groups, one or more acryloyl groups and one or more methacryloyl groups, two or more acryloyl groups, etc. Although not particularly limited, for example, it can have 2 to 6 (meth)acryloyl groups, for example, 2 to 5 (meth)acryloyl groups, for example, 2 to 4 (meth)acryloyl groups, for example, 2 to 3 (meth)acryloyl groups, or for example, 2 (meth)acryloyl groups.

[0036] The (meth)acryloyl group can reduce the crosslink density of the particle surface of the polymer and reduce the degree of swelling in water. From the viewpoint of improving the binding property, the (meth)acryloyl group of the (c) component is more preferably a methacryloyl group. Therefore, when the (c) component is a bifunctional compound having two (meth)acryloyl groups, the (c) component has, for example, a dimethacryloyl group, a methacryloyl group and an acryloyl group, and a diacryloyl group, in order of preference, from the viewpoint of improving the binding property. Moreover, the (meth)acryloyl group of the (c) component is more preferably an acryloyl group, in order of preference, from the viewpoint of the viscosity of the mixture layer composition (slurry). Therefore, the bifunctional compound has, for example, a diacryloyl group, a methacryloyl group and an acryloyl group, and a dimethacryloyl group, in order of preference, from the viewpoint of suppressing the viscosity of the slurry. The number and combination of (meth)acryloyl groups in component (c) can be appropriately selected taking into consideration the amount of crosslinked structural units as well as the binding ability and slurry viscosity intended for the secondary battery electrode binder.

[0037] The number of hydroxyl groups that component (c) can have is not particularly limited as long as it is one or more, and is, for example, 1 to 3, or for example, 1 to 2, or for example, 1. It is considered that the more hydroxyl groups there are, the greater the interaction within the polymer particles tends to be. The number of hydroxyl groups in component (c) can be appropriately selected in consideration of the amount of crosslinked structural units as well as the slurry viscosity, etc., intended as a binder for secondary battery electrodes.

[0038] The component (c) is not particularly limited, but examples thereof include trimethylolpropane di(meth)acrylate, di- or tri(meth)acrylate of pentaerythritol, di-, tri-, tetra- or penta(meth)acrylate of dipentaerythritol, glycerin di(meth)acrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, etc. The component (c) may be used alone or in combination of two or more.

[0039] The (c) component is not particularly limited, but for example, when the total amount of the non-crosslinked structural units is 100 parts by mass, it is 0.01 parts by mass or more and 20 parts by mass or less. If it is less than 0.01 parts by mass, the binding property is not obtained and the slurry viscosity becomes too high, and if it exceeds 20 parts by mass, the binding property is not obtained. The (c) component is, for example, 0.02 parts by mass or more, for example, 0.04 parts by mass or more, for example, 0.05 parts by mass or more, for example, 0.1 parts by mass or more, and for example, 0.2 parts by mass or more. The (c) component is, for example, 15 parts by mass or less, for example, 12 parts by mass or less, for example, 10 parts by mass or less, for example, 9 parts by mass or less, for example, 7 parts by mass or less, for example, 5 parts by mass or less, for example, 3 parts by mass or less, for example, 2 parts by mass or less, or 1 part by mass or less. The preferred range of the content of component (c) can be any combination of these upper and lower limits, and is, for example, from 0.1 to 15 parts by mass, for example, from 0.1 to 10 parts by mass, for example, from 0.2 to 9 parts by mass, for example, from 0.2 to 7 parts by mass, for example, from 0.2 to 5 parts by mass, for example, from 0.2 to 2 parts by mass, and for example, from 0.2 to 1 part by mass.

[0040] The polymer may also have a crosslinking structural unit other than the component (c). Examples of such crosslinking structural units include structural units derived from a polyfunctional polymerizable monomer having two or more polymerizable unsaturated groups and a monomer having a self-crosslinkable crosslinking functional group such as a hydrolyzable silyl group. The polyfunctional polymerizable monomer is a compound having two or more polymerizable functional groups such as a (meth)acryloyl group and an alkenyl group in the molecule, and examples of such compounds include a polyfunctional (meth)acrylate compound, a polyfunctional alkenyl compound, and a compound having both a (meth)acryloyl group and an alkenyl group. These compounds may be used alone or in combination of two or more.

[0041] Examples of the polyfunctional (meth)acrylate compound include di(meth)acrylates of dihydric alcohols such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate; tri(meth)acrylates of trihydric or higher polyhydric alcohols such as trimethylolpropane tri(meth)acrylate, tri(meth)acrylate of an ethylene oxide modified trimethylolpropane, glycerin tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and poly(meth)acrylates such as tetra(meth)acrylate; and bisamides such as methylene bisacrylamide and hydroxyethylene bisacrylamide.

[0042] Examples of polyfunctional alkenyl compounds include polyfunctional allyl ether compounds such as trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, tetraallyloxyethane, and polyallylsucrose; polyfunctional allyl compounds such as diallyl phthalate; and polyfunctional vinyl compounds such as divinylbenzene.

[0043] Examples of compounds having both a (meth)acryloyl group and an alkenyl group include allyl (meth)acrylate, isopropenyl (meth)acrylate, butenyl (meth)acrylate, pentenyl (meth)acrylate, and 2-(2-vinyloxyethoxy)ethyl (meth)acrylate.

[0044] Specific examples of the monomer having a self-crosslinkable crosslinkable functional group include a hydrolyzable silyl group-containing vinyl monomer, N-methylol (meth)acrylamide, N-methoxyalkyl (meth)acrylate, etc. These compounds can be used alone or in combination of two or more.

[0045] The vinyl monomer containing hydrolyzable silyl group is not particularly limited as long as it is a vinyl monomer having at least one hydrolyzable silyl group.For example, vinyl silanes such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, vinyl dimethyl methoxysilane, etc.; silyl group-containing acrylic acid esters such as trimethoxysilylpropyl acrylate, triethoxysilylpropyl acrylate, methyl dimethoxysilylpropyl acrylate, etc.; silyl group-containing methacrylic acid esters such as trimethoxysilylpropyl methacrylate, triethoxysilylpropyl methacrylate, methyl dimethoxysilylpropyl methacrylate, dimethyl methoxysilylpropyl methacrylate, etc.; silyl group-containing vinyl ethers such as trimethoxysilylpropyl vinyl ether, etc.; silyl group-containing vinyl esters such as vinyl trimethoxysilyl undecanoate, etc.

[0046] The crosslinked structural unit other than component (c) is not particularly limited, but may be, for example, 0.1 part by mass or more and 5.0 parts by mass or less relative to 100 parts by mass of the total amount of non-crosslinkable monomers. The amount of the crosslinked structural unit may be 0.2 parts by mass or less and 3.0 parts by mass or less, 0.3 parts by mass or less and 2.0 parts by mass or less, or 0.5 parts by mass or less and 1.0 part by mass or less.

[0047] <Neutralization level> In the present composition, the present polymer is preferably used in the form of a salt in which acid groups such as carboxyl groups derived from ethylenically unsaturated carboxylic acid monomers are neutralized so that the degree of neutralization is 20 to 100 mol%. The degree of neutralization is more preferably 50 to 100 mol%, for example 60 mol% or more, for example 65 mol% or more, for example 70 mol% or more, for example 75 mol% or more, for example 80 mol% or more, for example 85 mol% or more, for example 90 mol% or more, for example 95 mol% or more. When the degree of neutralization is 50 mol% or more, it is preferable in that the water swelling property is good and the dispersion stabilization effect is easily obtained.

[0048] In this specification, the neutralization degree can be calculated from the amount of a monomer having an acid group such as a carboxyl group and a neutralizing agent used for neutralization. The neutralization degree can be confirmed by IR measurement of the powder of the polymer after drying treatment at 80°C for 3 hours under reduced pressure conditions, and by the intensity ratio of the peak derived from the C=O group of the carboxylic acid to the peak derived from the C=O group of the carboxylate.

[0049] <Method for producing crosslinked polymer or its salt / Method for producing binder for secondary battery electrode> The present polymer, which is the binder component of the present binder, can be produced by the following preparation step (polymerization step): The method for producing the present polymer described below can also be carried out as a method for producing the present binder.

[0050] <Preparation process> The preparation step is a step of preparing the present polymer. The polymerization step is a step of obtaining the present polymer or obtaining the present polymer by polymerization (polymerization step). The polymerization step is a step of polymerizing a monomer composition containing at least the non-crosslinkable monomer from which the above-mentioned component (a) is derived and the crosslinkable monomer from which the component (c) is derived.

[0051] <Polymerization process> <Polymerization method> The polymer can be prepared by known polymerization methods such as solution polymerization, precipitation polymerization, suspension polymerization, and emulsion polymerization, but precipitation polymerization and suspension polymerization (reverse phase suspension polymerization) are preferred in terms of productivity. Heterogeneous polymerization methods such as precipitation polymerization, suspension polymerization, and emulsion polymerization are preferred in terms of obtaining better performance in terms of binding properties, and among them, precipitation polymerization is more preferred in terms of easily obtaining small-particle polymer particles with excellent uniformity. Precipitation polymerization is a method for producing a polymer by carrying out a polymerization reaction in a solvent that dissolves the raw material unsaturated monomer but does not substantially dissolve the polymer produced. As the polymerization proceeds, the polymer particles become larger due to aggregation and growth, and a dispersion of polymer particles in which primary particles of tens to hundreds of nm are secondary aggregated to several μm to tens of μm is obtained. A dispersion stabilizer can also be used to control the particle size of the polymer. The secondary aggregation can also be suppressed by selecting a dispersion stabilizer, polymerization solvent, etc. In general, precipitation polymerization in which secondary aggregation is suppressed is also called dispersion polymerization.

[0052] <Polymerization solvent> In the case of precipitation polymerization, the polymerization solvent may be selected from water and various organic solvents, etc., taking into consideration the type of monomer to be used, etc. In order to obtain a polymer having a longer primary chain length, it is preferable to use a solvent having a small chain transfer constant.

[0053] Specific polymerization solvents include water-soluble solvents such as methanol, t-butyl alcohol, acetone, methyl ethyl ketone, acetonitrile, and tetrahydrofuran, as well as benzene, ethyl acetate, dichloroethane, n-hexane, cyclohexane, and n-heptane. One of these can be used alone or two or more can be used in combination. Alternatively, these can be used as a mixed solvent with water. In this specification, the water-soluble solvent refers to a solvent having a solubility in water of more than 10 g / 100 ml at 20° C. Among the above, methyl ethyl ketone and acetonitrile are preferred in terms of the following: the generation of coarse particles and adhesion to the reactor are small, the polymerization stability is good, the precipitated polymer fine particles are unlikely to undergo secondary aggregation (or even if secondary aggregation occurs, they are easily dissolved in an aqueous medium), a polymer with a small chain transfer constant and a large degree of polymerization (primary chain length) can be obtained, and the operation is easy during the neutralization process described below.

[0054] Similarly, in order to stably and rapidly proceed with the neutralization reaction in the neutralization step, it is preferable to add a small amount of a highly polar solvent to the polymerization solvent. As the highly polar solvent, water and methanol are preferable. The amount of the highly polar solvent used is preferably 0.05 to 10.0% by mass, more preferably 0.1 to 5.0% by mass, and even more preferably 0.1 to 1.0% by mass, based on the total mass of the medium. If the proportion of the highly polar solvent is 0.05% by mass or more, the effect on the neutralization reaction is observed, and if it is 10.0% by mass or less, no adverse effect on the polymerization reaction is observed. In addition, in the polymerization of highly hydrophilic ethylenically unsaturated carboxylic acid monomers such as acrylic acid, the polymerization rate is increased when a highly polar solvent is added, making it easier to obtain a polymer with a long primary chain length. Among the highly polar solvents, water is particularly preferable because it has a large effect of improving the polymerization rate.

[0055] <Monomer and its usage amount> In the present production method, for example, it is preferable to have a polymerization step of polymerizing a monomer composition containing 10% by mass or more and 100% by mass or less of the ethylenically unsaturated carboxylic acid monomer from which the component (a) is derived and 0% by mass or more and 90% by mass or less of other ethylenically unsaturated monomers from which the component (b) is derived, relative to the total amount of the non-crosslinkable monomer, and 0.01 parts by mass or more and 20 parts by mass or less of the crosslinkable monomer from which the component (c) is derived, relative to 100 parts by mass of the non-crosslinkable monomer. By the above polymerization step, the component (a) is introduced into the present polymer in an amount of 10% by mass or more and 100% by mass or less, and the component (b) is introduced in an amount of 0% by mass or more and 90% by mass or less, relative to the non-crosslinkable structural unit. The amount of the ethylenically unsaturated carboxylic acid monomer from which the component (a) is derived and the amount of the other ethylenically unsaturated monomer from which the component (b) is derived are appropriately set so as to correspond to the content relative to the non-crosslinkable structural unit as already explained. The amount of the crosslinkable monomer from which the component (c) is derived is also appropriately set so as to correspond to the content of the component (c) already explained.

[0056] The ethylenically unsaturated carboxylic acid monomer may be in an unneutralized state, or may be in a state of a salt in which at least a part of the monomer is neutralized. From the viewpoint of polymerization rate and binding property, the degree of neutralization of the ethylenically unsaturated carboxylic acid monomer is, for example, 10 mol% or less, and, for example, 5 mol% or less, and it is preferably in an unneutralized state.

[0057] According to the present specification, such a monomer composition is a suitable composition for producing a binder for a secondary battery electrode.

[0058] The total concentration of the monomers in the polymerization step may be, for example, 2.0% by mass or more, for example, 4.0% by mass or more, or for example, 10.0% by mass or more, but from the viewpoint of binding, it is preferably, for example, 10.0% by mass or more, or for example, 13.0% by mass or more. As described later, when the polymerization step is carried out in the presence of a basic compound, the polymerization reaction can be stably carried out even at a high monomer concentration. The monomer concentration is more preferably 15.0% by mass or more, even more preferably 17.0% by mass or more, and even more preferably 19.0% by mass or more. The monomer concentration is still more preferably 20.0% by mass or more, even more preferably 22.0% by mass or more, and even more preferably 25.0% by mass or more. In general, the higher the monomer concentration during polymerization, the higher the molecular weight is possible, and a polymer with a long primary chain length can be produced. Since this polymer is a slightly crosslinked polymer obtained by subjecting a polymer having a sufficiently long primary chain length to moderate crosslinking, it is analytically difficult to directly measure its primary chain length. Generally, it is known that the primary chain length of a polymer correlates with the solution viscosity, but in the case of the present polymer, the solution viscosity also varies depending on the degree of crosslinking. Therefore, it is very difficult to define the present polymer obtained by the above method by the structure or properties of the present polymer. In this specification, the "monomer concentration" refers to the monomer concentration in the reaction solution at the time when polymerization is started.

[0059] The upper limit of the monomer concentration varies depending on the types of monomer and solvent used, as well as the polymerization method and various polymerization conditions, and the like. However, if it is possible to remove the heat of the polymerization reaction, the upper limit is approximately 40% by mass in precipitation polymerization, approximately 50% by mass in suspension polymerization, and approximately 70% by mass in emulsion polymerization.

[0060] <Use of basic compounds> In the present production method, the polymerization step may be carried out in the presence of a basic compound. The binder containing the present polymer thus obtained can exhibit high binding properties. In addition, when a monomer composition containing an ethylenically unsaturated carboxylic acid monomer is polymerized in the presence of a basic compound, the polymerization stability is improved, and the present polymer can be stably produced even at a high monomer concentration.

[0061] By carrying out the polymerization reaction in the presence of a basic compound, the polymerization reaction can be stably carried out even under high monomer concentration conditions, such as a monomer concentration exceeding 13.0% by mass. The polymer obtained by polymerization at such a high monomer concentration has a high molecular weight (long primary chain length) and therefore has excellent binding properties.

[0062] The base compound is a so-called alkaline compound, and may be either an inorganic base compound or an organic base compound. Examples of the inorganic base compound include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkaline earth metal hydroxides such as calcium hydroxide and magnesium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, and alkali metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate. One or more of these may be used. Examples of the organic base compound include, in addition to ammonia, N-alkyl-substituted amines such as monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, monobutylamine, dibutylamine, tributylamine, monohexylamine, dihexylamine, trihexylamine, trioctylamine and tridodecylamine; (alkyl)alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, propanolamine, dimethylethanolamine and N,N-dimethylethanolamine; cyclic amines such as pyridine, piperidine, piperazine, 1,8-bis(dimethylamino)naphthalene, morpholine and diazabicycloundecene (DBU); and organic amine compounds such as diethylenetriamine and N,N-dimethylbenzylamine, and one or more of these can be used. Among these, organic amine compounds other than ammonia are preferred from the viewpoint of binding property.

[0063] When a basic compound is used in the polymerization step, it is preferable to use 0.001 mol% or more of the basic compound relative to the ethylenically unsaturated carboxylic acid monomer. By carrying out the polymerization reaction in the presence of 0.001 mol% or more of the basic compound, the polymerization stability can be improved, and the polymerization reaction proceeds smoothly even under high monomer concentration conditions. The amount of the basic compound used relative to the ethylenically unsaturated carboxylic acid monomer is preferably 0.01 mol% or more, more preferably 0.03 mol% or more, and even more preferably 0.05 mol% or more. The amount of the basic compound used may be 0.3 mol% or more, or may be 0.5 mol% or more. In addition, the upper limit of the amount of the basic compound used is preferably 4.0 mol% or less. By carrying out the polymerization reaction in the presence of 4.0 mol% or less of the basic compound, the polymerization stability can be improved, and the polymerization reaction proceeds smoothly even under high monomer concentration conditions. The amount of the basic compound used relative to the ethylenically unsaturated carboxylic acid monomer is preferably 3.0 mol% or less, more preferably 2.0 mol% or less, and even more preferably 1.0 mol% or less. In this specification, the amount of the basic compound used represents the molar concentration of the basic compound used relative to the ethylenically unsaturated carboxylic acid monomer, and does not mean the degree of neutralization. In other words, the valence of the basic compound used is not taken into consideration.

[0064] <Polymerization initiator> The polymerization initiator may be any known polymerization initiator such as an azo compound, an organic peroxide, or an inorganic peroxide, but is not particularly limited. The conditions of use may be adjusted so that an appropriate amount of radicals is generated by known methods such as thermal initiation, redox initiation using a reducing agent, or UV initiation. In order to obtain a crosslinked polymer with a long primary chain length, it is preferable to set the conditions so that the amount of radicals generated is as small as possible within the allowable range of production time.

[0065] Examples of the azo compound include 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(N-butyl-2-methylpropionamide), 2-(tert-butylazo)-2-cyanopropane, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), and the like. One or more of these may be used.

[0066] Examples of the organic peroxides include 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane (manufactured by NOF Corporation, trade name "Pertetra A"), 1,1-di(t-hexylperoxy)cyclohexane (manufactured by NOF Corporation, trade name "Perhexa HC"), 1,1-di(t-butylperoxy)cyclohexane (manufactured by NOF Corporation, trade name "Perhexa C"), n-butyl-4,4-di(t-butylperoxy)valerate (manufactured by NOF Corporation, trade name "Perhexa V"), 2,2-di(t-butylperoxy)butane (manufactured by NOF Corporation, trade name "Perhexa 22"), t-Butyl hydroperoxide ("Perbutyl H"), cumene hydroperoxide (manufactured by NOF Corporation, trade name "Percumyl H"), 1,1,3,3-tetramethylbutyl hydroperoxide ("Perocta H"), t-butylcumyl peroxide ("Perbutyl C"), di-t-butyl peroxide ("Perbutyl D"), di-t-hexyl peroxide ("Perhexyl D"), di(3,5,5-trimethylhexanoyl) peroxide ("Perbutyl H"), Peroyl 355), dilauroyl peroxide (Peroyl L), bis(4-t-butylcyclohexyl) peroxydicarbonate (Peroyl TCP), di-2-ethylhexyl peroxydicarbonate (Peroyl OPP), di-sec-butyl peroxydicarbonate (Peroyl SBP), cumyl peroxyneodecanoate (Percumyl ND), 1,1,3,3-tetramethylbutyl peroxyneodecanoate (Peroyl SBP), Octa ND), t-hexyl peroxyneodecanoate (Perhexyl ND), t-butyl peroxyneodecanoate (Perbutyl ND), t-butyl peroxyneoheptanoate (Perbutyl NHP), t-hexyl peroxypivalate (Perhexyl PV), t-butyl peroxypivalate (Perbutyl PV), 2,5-dimethyl-2,5-di(2-ethylhexanoyl)hexane (Perhexa 250), 1,1,3,3-Tetramethylbutylperoxy-2-ethylhexanoate (Perocta O), t-hexylperoxy-2-ethylhexanoate (Perhexyl O), t-butylperoxy-2-ethylhexanoate (Perbutyl O), t-butylperoxylaurate (Perbutyl L), t-butylperoxy-3,5,5-trimethylhexanoate (Perbutyl 355), t-hexylperoxyisopropyl monocarbonate t-butylperoxyisopropyl monocarbonate ("Perbutyl I"), t-butylperoxy-2-ethylhexyl monocarbonate ("Perbutyl E"), t-butylperoxyacetate ("Perbutyl A"), t-hexylperoxybenzoate ("Perhexyl Z") and t-butylperoxybenzoate ("Perbutyl Z"), and one or more of these can be used.

[0067] Examples of the inorganic peroxide include potassium persulfate, sodium persulfate, ammonium persulfate, etc. In the case of redox initiation, sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, sulfurous acid gas (SO2), ferrous sulfate, etc. can be used as a reducing agent.

[0068] The amount of the polymerization initiator used is preferably, for example, 0.001 to 2 parts by mass, or, for example, 0.005 to 1 part by mass, or, for example, 0.01 to 0.1 part by mass, when the total amount of the monomers used is 100 parts by mass. If the amount of the polymerization initiator used is 0.001 part by mass or more, the polymerization reaction can be stably carried out, and if it is 2 parts by mass or less, a polymer having a long primary chain length is easily obtained.

[0069] <Polymerization temperature, etc.> The polymerization temperature varies depending on conditions such as the type and concentration of the monomers used, but is preferably 0 to 100° C., more preferably 20 to 80° C. The polymerization temperature may be constant or may vary during the polymerization reaction. The polymerization time is preferably 1 minute to 20 hours, more preferably 1 hour to 10 hours.

[0070] <Drying process etc.> Prior to the drying step, it is preferable to provide a solid-liquid separation step such as centrifugation and filtration, and a washing step using water, methanol, acetonitrile, or the same solvent as the polymerization solvent, etc., following the polymerization step, for the purpose of removing unreacted monomers or their salts, impurities derived from the initiator, etc. When the above washing step is provided, even if the present polymer undergoes secondary aggregation, it is easy to disintegrate during use, and further, since the remaining unreacted monomers are removed, it is advantageous in terms of binding properties and battery characteristics.

[0071] <Neutralization process> In the present production method, when an unneutralized or partially neutralized salt is used as the ethylenically unsaturated carboxylic acid monomer, an alkaline compound may be added to the polymer dispersion obtained by the polymerization step to neutralize the polymer (hereinafter also referred to as "process neutralization"), and then the solvent may be removed in the drying step described above to obtain the present polymer in a solid state. Alternatively, a drying step may be performed in the unneutralized or partially neutralized salt state to obtain the present polymer in a solid state such as a powder, and then an alkaline compound for forming a salt when preparing the electrode mixture layer slurry may be added to neutralize the polymer (hereinafter also referred to as "post-neutralization"). Of the above, process neutralization is preferred because it tends to break up secondary aggregates more easily.

[0072] The alkaline compound that can be used in the neutralization step such as the neutralization step is not particularly limited, and various alkaline compounds that can be used in the polymerization step described above can be used. For example, LiOH, NaOH, KOH, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, etc. are included. From the viewpoint of battery performance when a Li salt is used, LiOH is preferred because it can provide the Li salt of the present polymer.

[0073] <Composition for secondary battery electrode and method for producing same> The composition is a composition for an electrode (mixture layer) of a secondary battery, and can contain a binder containing the polymer, an active material, and water. The amount of the polymer used in the composition is, for example, 0.1% by mass or more and 20% by mass or less, based on the total amount of the active material. The amount used is, for example, 0.2% by mass or more and 10% by mass or less, for example, 0.3% by mass or more and 8% by mass or less, and for example, 0.4% by mass or more and 5% by mass or less. When the amount of the polymer and its salt used is less than 0.1% by mass, sufficient binding property may not be obtained. In addition, the dispersion stability of the active material may become insufficient, and the uniformity of the mixture layer formed may decrease. On the other hand, when the amount of the polymer and its salt used exceeds 20% by mass, the electrode mixture layer composition may become highly viscous and the coatability to the current collector may decrease. As a result, bumps and unevenness may occur in the obtained mixture layer, which may adversely affect the electrode characteristics.

[0074] The present specification also provides a method for producing a composition for a secondary battery electrode, comprising the steps of preparing the present polymer and preparing the present composition using the present polymer.

[0075] When the amount of the present polymer and its salt is within the above range, the present composition has a sufficiently low slurry viscosity, and a mixture layer having extremely high adhesion to the current collector and therefore high binding property can be obtained, resulting in improved durability of the battery. Furthermore, the present polymer and its salt exhibit sufficiently high binding property even in a small amount (for example, 5 mass % or less) to the active material, and since they have carboxy anions, an electrode having low interface resistance and excellent high-rate characteristics can be obtained.

[0076] Among the above active materials, lithium salts of transition metal oxides are mainly used as the positive electrode active material. For example, layered rock salt type and spinel type lithium-containing metal oxides can be used. Specific compounds of the layered rock salt type positive electrode active material include lithium cobalt oxide, lithium nickel oxide, and NCM{Li(Ni x ,Co y ,Mn z ), x+y+z=1} and NCA{Li(Ni 1-a-b Coa Al b )}, etc. Examples of the spinel-type positive electrode active material include lithium manganate, etc. In addition to oxides, phosphates, silicates, sulfur, etc. are used, and examples of the phosphates include olivine-type lithium iron phosphate, etc. As the positive electrode active material, one of the above may be used alone, or two or more may be combined to be used as a mixture or composite.

[0077] In addition, when a positive electrode active material containing a layered rock salt type lithium-containing metal oxide is dispersed in water, the lithium ions on the active material surface are exchanged with hydrogen ions in the water, and the dispersion liquid becomes alkaline. Therefore, there is a risk that aluminum foil (Al), which is a common positive electrode current collector material, may be corroded. In such a case, it is preferable to neutralize the alkali content eluted from the active material by using the unneutralized or partially neutralized present polymer as a binder. In addition, it is preferable to use the unneutralized or partially neutralized present polymer in an amount such that the amount of unneutralized carboxyl groups of the present polymer is equivalent to or greater than the amount of alkali eluted from the active material.

[0078] Since all positive electrode active materials have low electrical conductivity, they are generally used with the addition of a conductive assistant. Examples of the conductive assistant include carbon-based materials such as carbon black, carbon nanotubes, carbon fiber, graphite powder, and carbon fiber. Of these, carbon black, carbon nanotubes, and carbon fiber are preferred because they are easy to obtain excellent electrical conductivity. As carbon black, ketjen black and acetylene black are preferred. The conductive assistant may be one of the above alone or two or more may be used in combination. The amount of the conductive assistant may be, for example, 0.2 to 20% by mass, or, for example, 0.2 to 10% by mass, based on the total amount of the active material, from the viewpoint of achieving both electrical conductivity and energy density. The positive electrode active material may be surface-coated with a carbon-based material having electrical conductivity.

[0079] On the other hand, examples of the negative electrode active material include carbon-based materials, lithium metal, lithium alloys, and metal oxides, and one or more of these can be used in combination. Among these, active materials made of carbon-based materials such as natural graphite, artificial graphite, hard carbon, and soft carbon (hereinafter also referred to as "carbon-based active materials") are preferred, and graphite such as natural graphite and artificial graphite, and hard carbon are more preferred. In the case of graphite, spherical graphite is preferably used from the viewpoint of battery performance, and the preferred range of the particle size is, for example, 1 to 20 μm, and also, for example, 5 to 15 μm. In addition, in order to increase the energy density, metals or metal oxides capable of occluding lithium, such as silicon and tin, can also be used as the negative electrode active material. Among them, silicon has a higher capacity than graphite, and active materials made of silicon-based materials such as silicon, silicon alloys, and silicon oxides such as silicon monoxide (SiO) (hereinafter also referred to as "silicon-based active materials") can be used. However, while the silicon-based active material has a high capacity, it undergoes a large volume change during charging and discharging. For this reason, it is preferable to use it in combination with the carbon-based active material. In this case, if the amount of silicon-based active material is large, the electrode material may collapse, and the cycle characteristics (durability) may be significantly reduced. From this point of view, when the silicon-based active material is used in combination, the amount of the silicon-based active material is, for example, 60% by mass or less, or, for example, 30% by mass or less, relative to the carbon-based active material.

[0080] The binder containing the present polymer has a structural unit (component (a)) derived from an ethylenically unsaturated carboxylic acid monomer. Here, component (a) has a high affinity for silicon-based active materials and exhibits good binding properties. Therefore, the present binder exhibits excellent binding properties even when a high-capacity active material containing a silicon-based active material is used, and is therefore considered to be effective in improving the durability of the resulting electrode.

[0081] Since the carbon-based active material itself has good electrical conductivity, it is not necessary to add a conductive additive. When a conductive additive is added for the purpose of further reducing resistance, the amount of the conductive additive used is, for example, 10% by mass or less, or, for example, 5% by weight or less, based on the total amount of the active material, from the viewpoint of energy density.

[0082] When the composition is in a slurry state, the amount of the active material used is, for example, in the range of 10 to 75 mass %, or, for example, in the range of 30 to 65 mass %, based on the total amount of the composition. If the amount of the active material used is 10 mass % or more, migration of the binder, etc. is suppressed, and it is also advantageous in terms of the drying cost of the medium. On the other hand, if it is 75 mass % or less, the fluidity and coatability of the composition can be ensured, and a uniform mixture layer can be formed.

[0083] When the present composition is prepared in a wet powder state, the amount of the active material used is, for example, in the range of 60 to 97 mass %, or, for example, in the range of 70 to 90 mass %, based on the total amount of the present composition. From the viewpoint of energy density, the amount of non-volatile components other than the active material, such as binders and conductive assistants, should be as small as possible within the range that ensures the necessary binding property and conductivity.

[0084] The composition uses water as a medium. In order to adjust the properties and drying property of the composition, the composition may be mixed with lower alcohols such as methanol and ethanol, carbonates such as ethylene carbonate, ketones such as acetone, tetrahydrofuran, N-methylpyrrolidone, and other water-soluble organic solvents. The proportion of water in the mixed medium is, for example, 50% by mass or more, and, for example, 70% by mass or more.

[0085] When the composition is in a coatable slurry state, the content of the water-containing medium in the entire composition can be, for example, in the range of 25 to 90 mass %, or, for example, in the range of 35 to 70 mass %, from the viewpoints of the coatability of the slurry, the energy cost required for drying, and productivity. When the composition is in a pressable wet powder state, the content of the medium can be, for example, in the range of 3 to 40 mass %, or, for example, in the range of 10 to 30 mass %, from the viewpoints of the uniformity of the mixture layer after pressing.

[0086] The binder component contained in the present composition may be composed of only the present polymer, but may also be used in combination with other binder components such as styrene / butadiene latex (SBR), acrylic latex, and polyvinylidene fluoride latex. When other binder components are used in combination, the amount of the binder components used may be, for example, 0.1 to 5% by mass or less, for example, 0.1 to 2% by mass or less, or for example, 0.1 to 1% by mass or less, based on the active material. If the amount of the other binder components used exceeds 5% by mass, the resistance increases, and high-rate characteristics may become insufficient. Among the above, styrene / butadiene latex is preferred in terms of excellent balance between binding property and flex resistance.

[0087] The present composition is essentially composed of the active material, water and binder, and is obtained by mixing the components using known means. The method of mixing the components is not particularly limited, and known methods can be adopted, but a method of dry-blending the powder components such as the active material, the conductive assistant and the present polymer as the binder, and then mixing with a dispersion medium such as water and kneading the mixture is preferred. When the present composition is obtained in a slurry state, it is preferable to finish the slurry without poor dispersion or aggregation. As a mixing means, known mixers such as a planetary mixer, a thin film swirling mixer and a self-revolving mixer can be used, but it is preferable to use a thin film swirling mixer in order to obtain a good dispersion state in a short time. In addition, when using a thin film swirling mixer, it is preferable to perform preliminary dispersion in advance using a stirrer such as a disperser.

[0088] The viscosity of the slurry of this composition is 60 s at 25 °C. -1 The shear viscosity of the composition can be, for example, in the range of 500 to 100,000 mPa·s, and can be, for example, in the range of 1,000 to 50,000 mPa·s. For example, the slurry viscosity of the composition is preferably in the range of 500 to 10,000 mPa·s, more preferably 500 to 7,000 mPa·s, even more preferably 500 to 6,000 mPa·s, still more preferably 500 to 5,000 mPa·s, even more preferably 500 to 4,000 mPa·s, still more preferably 500 to 3,000 mPa·s, even more preferably 500 to 2,000 mPa·s, still more preferably 500 to 1,800 mPa·s, still more preferably 500 to 1,700 mPa·s, still more preferably 500 to 1,600 mPa·s, and still more preferably 500 to 1,500 mPa·s.

[0089] On the other hand, when the present composition is obtained in the form of a wet powder, it is preferable to knead the composition to a uniform state without unevenness in concentration using a Henschel mixer, blender, planetary mixer, twin-screw kneader, or the like.

[0090] <Secondary battery electrode> The electrode comprises a mixture layer formed from the composition on the surface of a current collector such as copper or aluminum. The mixture layer is formed by applying the composition to the surface of the current collector and then drying and removing the medium such as water. The method for applying the composition is not particularly limited, and known methods such as doctor blade method, dip method, roll coating method, comma coating method, curtain coating method, gravure coating method and extrusion method can be adopted. The drying can be performed by known methods such as hot air blowing, decompression, (far) infrared radiation, and microwave irradiation. Usually, the mixture layer obtained after drying is subjected to a compression treatment using a mold press, roll press, etc. The active material and the binder are adhered by compression, and the strength of the mixture layer and the adhesion to the current collector can be improved. The thickness of the mixture layer can be adjusted by compression to, for example, about 30 to 80% of the thickness before compression, and the thickness of the mixture layer after compression is generally about 4 to 200 μm.

[0091] The present specification also provides a method for producing a secondary battery electrode, the method including the steps of preparing the present polymer, preparing the present composition using the present polymer, and preparing a secondary battery electrode using the present composition.

[0092] By providing this electrode with a separator and a non-aqueous electrolyte, a secondary battery can be produced. The separator is disposed between the positive and negative electrodes of the battery, and serves to prevent short circuits caused by contact between the two electrodes and to retain the electrolyte to ensure ionic conductivity. The separator is preferably a film-like insulating microporous membrane having good ion permeability and mechanical strength. Specific materials that can be used include polyolefins such as polyethylene and polypropylene, and polytetrafluoroethylene.

[0093] The non-aqueous electrolyte may be any known solvent generally used in secondary batteries. Specific examples of the solvent include cyclic carbonates with high dielectric constants and high electrolyte dissolving ability, such as propylene carbonate and ethylene carbonate, and chain carbonates with low viscosity, such as ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate, which may be used alone or as a mixed solvent. The non-aqueous electrolyte is used by dissolving lithium salts, such as LiPF6, LiSbF6, LiBF4, LiClO4, and LiAlO4, in these solvents. The secondary battery is obtained by storing a positive electrode plate and a negative electrode plate separated by a separator in a spiral or stacked structure in a case or the like.

[0094] As described above, the binder for secondary battery electrodes disclosed in this specification can achieve both excellent binding properties and reduced viscosity of the mixture layer slurry. A secondary battery equipped with an electrode obtained using the binder is expected to ensure good integrity and exhibit good durability (cycle characteristics) even after repeated charging and discharging, and is suitable for, for example, vehicle-mounted secondary batteries. EXAMPLES

[0095] The production and use of the present polymer disclosed in this specification will be specifically illustrated below, but the disclosure of this specification is not limited to the following examples. In the following, unless otherwise specified, "parts" and "%" mean parts by mass and % by mass, respectively.

[0096] <Production Example of This Polymer> <Production Example 1: Production of Crosslinked Polymer Salt R-1> For the polymerization, a reactor equipped with a stirring blade, a thermometer, a reflux condenser, and a nitrogen inlet tube was used. 567 parts of acetonitrile, 2.20 parts of ion-exchanged water, 100 parts of acrylic acid (hereinafter referred to as "AA"), 0.20 parts of 2-hydroxy-3-acryloyloxypropyl methacrylate (manufactured by Kyoeisha Chemical Co., Ltd., Light Ester G-201P), and triethylamine equivalent to 1.0 mol% relative to the AA were charged into the reactor. After the inside of the reactor was sufficiently replaced with nitrogen, the inside temperature was raised to 55°C by heating. After confirming that the inside temperature was stable at 55°C, 0.040 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., trade name "V-65") was added as a polymerization initiator, and the reaction liquid became cloudy, so this point was determined to be the polymerization initiation point. The monomer concentration was calculated to be 15.0%.

[0097] The polymerization reaction was continued while maintaining the internal temperature at 55°C by adjusting the external temperature (water bath temperature), and the internal temperature was raised to 65°C 6 hours after the polymerization initiation point. The internal temperature was maintained at 65°C, and cooling of the reaction solution was started 12 hours after the reaction initiation point. After the internal temperature had dropped to 25°C, 52.5 parts of lithium hydroxide monohydrate (hereinafter referred to as "LiOH·H2O") powder was added. After the addition, stirring was continued for 12 hours at room temperature, and a slurry-like polymerization reaction solution in which particles of crosslinked polymer salt R-1 (Li salt, neutralization degree 90 mol%) were dispersed in the medium was obtained.

[0098] The obtained polymerization reaction solution was centrifuged to settle the polymer particles, and the supernatant was removed. The precipitate was then redispersed in acetonitrile of the same weight as the polymerization reaction solution, and the operation of settling the polymer particles by centrifugation and removing the supernatant was repeated twice. The precipitate was collected and dried at 80°C for 3 hours under reduced pressure conditions to remove the volatile matter, thereby obtaining a powder of crosslinked polymer salt R-1. Since crosslinked polymer salt R-1 is hygroscopic, it was sealed and stored in a container with water vapor barrier properties. The powder of crosslinked polymer salt R-1 was subjected to IR measurement, and the degree of neutralization was calculated from the intensity ratio of the peak derived from the C=O group of the carboxylic acid and the peak derived from the C=O of the carboxylic acid Li, which was 90 mol%, which was equal to the calculated value from the charge.

[0099] <Production Examples 2 to 15: Production of Crosslinked Polymer Salts R-2 to R-15> The same operation as in Production Example 1 was carried out, except that the amount of each raw material was as shown in Table 1, to obtain a polymerization reaction solution containing crosslinked polymer salts R-2 to R-15. Next, the same operation as in Production Example 1 was carried out for each polymerization reaction solution to obtain powdered crosslinked polymer salts R-2 to R-15. Each crosslinked polymer salt was sealed and stored in a container with water vapor barrier properties. In Production Example 9, a crosslinked polymer Na salt (neutralization degree 90 mol%) was obtained by using NaOH instead of LiOH·H2O powder.

[0100] [Table 1]

[0101] The notations shown in Table 1 are explained below. AA: Acrylic acid DMAA: Dimethylacrylamide HAPMA: 2-hydroxy-3-acryloyloxypropyl methacrylate (Light Ester G-201P, Kyoeisha Chemical) GDMA: Glycerin dimethacrylate (Light Ester G-101P, Kyoeisha Chemical) EGDMA: Ethylene dimethacrylate (Fujifilm Wako Pure Chemical Industries, Ltd.) T-20: Trimethylolpropane diallyl ether (Osaka Soda) TEA: Triethylamine AcCN: Acetonitrile V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) (Wako Pure Chemical Industries, Ltd.)

[0102] <Example> <Example 1> 3.2 parts of powdered crosslinked polymer Li salt R-1 was weighed out into 100 parts of natural graphite and mixed thoroughly in advance, then 160 parts of ion-exchanged water was added and pre-dispersed with a disperser, and then main dispersion was performed for 15 seconds at a peripheral speed of 20 m / sec using a thin film rotary mixer (FM-56-30, manufactured by Primix Corporation), to obtain a slurry-like negative electrode mixture layer composition. The slurry concentration (solid content) was calculated to be 39.2%.

[0103] <Measurement of electrode slurry viscosity> The negative electrode mixture layer composition (slurry) obtained above was subjected to a shear rate of 60 s at 25°C using a CP25-5 cone plate (diameter 25 mm, cone angle 5°) using an Anton Paar rheometer (Physica MCR301). -1 The slurry viscosity was measured.

[0104] <90° peel strength (bonding)> The mixture layer composition was applied to a copper foil (manufactured by Nippon Foil Co., Ltd.) having a thickness of 20 μm using a variable applicator, and then dried in a ventilated dryer at 100° C. for 15 minutes to form a mixture layer. After that, the thickness of the mixture layer was 70±5 μm and the packing density was 1.70±0.20 g / cm. 3 The negative electrode was then rolled to a width of 25 mm to prepare a negative electrode. The negative electrode obtained above was cut into a strip of 25 mm width, and the composite layer surface of the sample was attached to double-sided tape fixed to a horizontal surface to prepare a peel test sample. The test sample was dried at 60°C overnight under reduced pressure, and then peeled at 90° at a tensile speed of 50 mm / min to measure the peel strength between the composite layer and the copper foil. The peel strength was high at 15.8 N / m, which was good.

[0105] <Examples 2 to 15 and Comparative Examples 1 to 3> A negative electrode mixture layer composition was prepared in the same manner as in Example 1, except that the active material and the crosslinked polymer salt used as the binder were used as shown in Table 2. In Examples 3 and 4, natural graphite and silicon particles were stirred at 400 rpm for 1 hour using a planetary ball mill (FRITSCH, P-5), and 3.2 parts of powdered crosslinked polymer Li salt R-2 were weighed into the resulting mixture, and the mixture was thoroughly mixed in advance. The mixture layer composition was prepared by performing the same operation as in Example 1. The slurry viscosity and 90° peel strength of each mixture layer composition were evaluated. The results are shown in Table 2.

[0106] [Table 2]

[0107] As shown in Table 2, in Examples 1 to 15 using crosslinked polymers R-1 to R-13 using crosslinkable monomers having two or more (meth)acryloyl groups and hydroxyl groups, the viscosity of the mixture layer slurry was 330 to 1800 mPa·s, which showed extremely good viscosity. Furthermore, the peel strength of these Examples 1 to 15 was 14.4 to 19.1 N / m, which showed sufficient electrode binding. In contrast, in Comparative Example 1 using the non-crosslinked polymer of Production Example 14, the viscosity was high but the binding was low, and in Comparative Example 2 using the crosslinked polymer of Production Example 15 using a crosslinkable monomer having two acryloyl groups but no hydroxyl groups, the binding was good, but the slurry viscosity was still quite high, and in Comparative Example 3 using the crosslinked polymer of Production Example 16 using a crosslinkable monomer having two allyl groups and a hydroxyl group, the binding was low and the slurry viscosity was still high.

[0108] From the above, it was found that by polymerizing an ethylenically unsaturated carboxylic acid monomer with a crosslinkable monomer having two (meth)acryloyl groups and a hydroxyl group, and providing a crosslinked structure derived from such a crosslinkable monomer, it is possible to achieve both good binding properties and good slurry viscosity.

[0109] Moreover, according to Examples 1-2 and 5-7, it was found that a crosslinked polymer with good binding properties can be obtained when the amount of the crosslinkable monomer used is about 0.1 to 10 parts relative to 100 parts of the non-crosslinkable monomer, and a crosslinked polymer with even better binding properties can be obtained when the amount of the crosslinkable monomer used is about 0.2 to 9 parts, 0.2 to 5 parts, 0.2 to 2 parts, or 0.2 to 1 part. It was also found that a crosslinked polymer with sufficiently low slurry viscosity can be obtained when the amount of the crosslinkable monomer used is about 0.1 to 10 parts.

[0110] Also, according to Examples 3 and 4, it was found that even if silicon particles were contained as an active material, both stable binding property and slurry viscosity could be achieved. Furthermore, according to Example 8, it was found that even if the crosslinked polymer of Production Example 6, which uses a crosslinkable monomer having a structure different from those of Production Examples 1 to 5, was used, excellent binding property and slurry viscosity could be obtained.

[0111] Furthermore, according to Examples 9 to 12, it was found that stable binding properties and slurry viscosity could be ensured regardless of the degree of neutralization of the salt (85%, 70% and 90%) or the type of salt to be neutralized (Li, Na, K). Furthermore, according to Examples 13 to 15, it was found that excellent binding properties and slurry viscosity could be ensured even by using dimethylacrylamide as a non-crosslinkable monomer. In addition, the use of dimethylacrylamide also tended to reduce the slurry viscosity.

Claims

1. A binder for a secondary battery electrode comprising a crosslinked polymer or a salt thereof, The crosslinked polymer (excluding those that dissolve in an amount of 5 g or more in 100 g of each of methanol, ethanol, isopropanol and tetrahydrofuran at 25° C.) or a salt thereof has a non-crosslinked structural unit and a crosslinked structural unit, the non-crosslinked structural unit is derived from an ethylenically unsaturated carboxylic acid monomer having a carboxy group which is a free acid and / or a salt, and includes an ethylenically unsaturated carboxylic acid non-crosslinked structural unit having a carboxy group which is a free acid and / or a salt, the crosslinked structural unit includes a crosslinked structural unit derived from a crosslinkable monomer having two or more (meth)acryloyl groups and a hydroxyl group in one molecule, the amount of the crosslinked structural unit is 0.01 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the total amount of the non-crosslinked structural units, The binder contains the ethylenically unsaturated carboxylic acid non-crosslinked structural units in an amount of 30% by mass or more and 100% by mass or less based on the total amount of the non-crosslinked structural units.

2. A composition for a secondary battery electrode, The binder for a secondary battery electrode according to claim 1 ; An active material; Water, A composition comprising:

3. A secondary battery electrode, The binder for a secondary battery electrode according to claim 1 ; An active material; An electrode comprising:

4. 4. The electrode of claim 3 further comprising: the active material being a silicon-containing material.

5. A method for producing a binder for a secondary battery electrode, comprising: a step of polymerizing a monomer composition containing an ethylenically unsaturated carboxylic acid monomer and a crosslinkable monomer having two or more (meth)acryloyl groups and a hydroxyl group in one molecule to obtain a crosslinked polymer (excluding those which dissolve in an amount of 5 g or more in 100 g each of methanol, ethanol, isopropanol and tetrahydrofuran at 25° C.) or a salt thereof; Equipped with The crosslinked polymer or salt thereof has a non-crosslinked structural unit and a crosslinked structural unit, the non-crosslinked structural unit is derived from an ethylenically unsaturated carboxylic acid monomer having a carboxy group which is a free acid and / or a salt, and includes an ethylenically unsaturated carboxylic acid non-crosslinked structural unit having a carboxy group which is a free acid and / or a salt, the crosslinked structural unit includes a crosslinked structural unit derived from a crosslinkable monomer having two or more (meth)acryloyl groups and a hydroxyl group in one molecule, the amount of the crosslinked structural unit is 0.01 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the total amount of the non-crosslinked structural units, The ethylenically unsaturated carboxylic acid non-crosslinked structural unit is contained in an amount of 30% by mass or more and 100% by mass or less based on the total amount of the non-crosslinked structural units.

Citation Information

Patent Citations

  • Battery

    JP2004311306A

  • Binder for battery electrode, electrode using the same, and battery

    JP2014160638A

  • Soluble polyfunctional vinyl copolymer method for producing the same, curable resin composition containing the same, and coated film and cured product of the same

    JP2018076446A

  • Binder for lithium cell, composition for producing electrode, and electrode

    WO2014065407A1

  • Binder for nonaqueous electrolyte secondary cell electrode, method for producing binder, and use thereof

    WO2017073589A1