Method for modifying substances, method for refining molten iron, and method for manufacturing slag material
By introducing a powdered substance onto molten slag and stirring it with a slurry, the method achieves homogeneous mixing and reforming of non-compliant slag, ensuring compliance with quality standards and environmental safety.
Patent Information
- Application Number
- JP2022079120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-14
- Filing Date
- 2022-05-13
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-05-13
AI Technical Summary
Existing methods for refining molten iron and reforming slag fail to achieve homogeneous mixing and often require large-scale equipment, leading to inconsistencies in slag quality and potential environmental impacts due to non-compliant components.
Introduce a powdered substance onto molten slag during discharge and stir it to ensure homogeneous mixing, using a slurry made by mixing the powder with water and an inert gas to enhance melting and distribution.
The method reliably reforms non-compliant slag into a homogeneous material meeting quality standards, converting difficult-to-use by-products into reusable slag products.
Smart Images

Figure 0007582249000003 
Figure 0007582249000004 
Figure 0007582249000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for modifying a substance using molten slag, a method for refining molten iron, and a method for producing a slag material. [Background technology]
[0002] In the smelting process of molten iron, slag is generated during the refining process, and this slag is ultimately used as aggregate for asphalt concrete, raw material for roadbed materials, and other products.
[0003] Slag products generally need to meet various quality control standards, such as chemical composition, expansion stability (free lime concentration, etc.), strength (corrected CBR value, etc.), particle size, and environmental leaching standards set out in Environment Agency Notification No. 14 and Environment Ministry Notification No. 46. In order to meet these quality control standards, the slag components and processing methods are controlled during the refining process, and if the slag generated by the refining process does not meet the quality control standards as is, the slag is modified.
[0004] Furthermore, even if a slag product as a whole lot complies with the quality control standards, if there are parts within the lot that do not comply with the quality control standards due to quality variations, construction defects and adverse effects on the environment may occur after the slag product is used. Therefore, in terms of quality control of slag products, it is generally important for slag products to have a certain degree of homogeneity at the microscopic level.
[0005] Regarding the control of the refining process, Patent Document 1 discloses a method for adjusting the basicity of the auxiliary materials and slag added during the refining process. Regarding the modification process of slag, Patent Document 2 discloses a technology for rendering harmless slag that exceeds environmental standards by adding it during another refining process. Similarly, regarding the modification process of slag, Patent Documents 3 to 5 disclose technologies for modifying slag discharged from a refining vessel in a discharge vessel (slag ladle) or on a cooling yard. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-99148 A [Patent Document 2] Patent No. 6025602 [Patent Document 3] Patent No. 6443463 [Patent Document 4] Patent No. 5341849 [Patent Document 5] Japanese Patent Application Publication No. 06-329451 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the method of adjusting the basicity of the auxiliary materials and slag added during the refining process, such as the technology disclosed in Patent Document 1, the reactivity characteristics of the slag inevitably change, and it becomes necessary to consider the impact of this on the refining process.
[0008] In addition, in the technology disclosed in Patent Document 2, by-products containing Pb are introduced into the preliminary treatment process to render the Pb contained in the discharged slag harmless. As such, as in Patent Document 1, it becomes necessary to consider the impact of introducing by-products on the refining characteristics of the preliminary treatment process.
[0009] In the technology disclosed in Patent Document 3, oxygen-containing gas is blown from an immersion lance onto the molten slag in the discharge vessel to perform the reforming treatment, so that a large-scale facility is required for the gas blowing and there is a possibility that the handling process of the slag treatment is affected. In the technology disclosed in Patent Document 4, the inner surface of the slag vessel is coated with molten pig iron slag in advance, and ladle refining slag is further poured into the slag vessel to mix the two slags. However, since the two slags are not sufficiently stirred in the slag vessel, it is difficult to homogenously reform the entire slag in the slag vessel. In the technology disclosed in Patent Document 5, converter slag and blast furnace slag or desiliconization slag are discharged to a yard and mixed in a molten or semi-molten state to reform the slag. However, since the molten or semi-molten slag is mixed at a hot temperature, restrictions are placed on the slag logistics process, and it is not certain whether the slag can be homogenously mixed.
[0010] The present invention has been made in light of the above-mentioned problems, and aims to provide a method for modifying a material, a method for refining molten iron, and a method for producing a slag material, which can easily and reliably homogeneously modify powdery materials such as steelmaking slag that do not meet predetermined quality control standards. [Means for solving the problem]
[0011] The means for solving the above problems are as follows. [1] A method for modifying a material, comprising projecting a powdered substance onto the slag in a slag discharge vessel during or immediately after the molten slag generated by a refining process is discharged into the slag discharge vessel, thereby causing the powdered substance to penetrate into the slag and melt and mix. [2] A method for modifying a material described in [1], comprising projecting a slurry obtained by mixing the powdered material with water onto the molten slag. [3] The method for modifying a material described in [1], wherein slag that does not meet specified quality control standards is used as the powdered material. [4] A method for modifying a material described in [2], in which slag that does not meet specified quality control standards is used as the powdered material. [5] The method for modifying a substance according to [3], wherein the slag contains 5 ppm or more of selenium. [6] The method for modifying a substance according to [4], wherein the slag contains 5 ppm or more of selenium. [7] A method for refining molten iron, comprising: a refining process for refining molten iron in a refining vessel; and a slag discharge process for discharging slag generated by the refining process from the refining vessel to a slag pan, wherein in the slag discharge process, a powdered substance is projected onto the slag discharged into the slag pan to melt and mix it, using a substance modification method described in any one of [1] to [6]. [8] A method for refining molten iron, comprising: a first refining step of desiliconizing and dephosphorizing molten iron in a converter; a slag removal step of discharging slag generated by the first refining step from the converter to a slag pan; and a second refining step of decarburizing the molten iron after the slag removal step in the converter, wherein in the slag removal step, a powdered substance is projected onto the slag discharged into the slag pan to melt and mix it, using a substance modification method described in any one of [1] to [6]. [9] A method for producing a slag material, comprising melt-mixing the powdered substance with the molten slag using the method for modifying a substance described in any one of [1] to [6] to produce a slag material. Effect of the Invention
[0012] According to the method for modifying a substance, the method for refining molten iron, and the method for producing a slag material of the present invention, powdery substances such as steelmaking slag that do not meet the specified quality control standards can be homogeneously modified in a short time and reliably in a discharge container in association with the slag discharge process in which the molten slag generated by the refining process is discharged.
[0013] In addition, by using slag or by-products that are difficult to use as slag products such as aggregate for asphalt concrete or raw materials for roadbed materials as the powdered material to be projected onto the slag and melted and mixed, these slag and by-products can be modified into reusable slag. Examples of slag and by-products that are difficult to use as slag products as they are include those that exceed environmental standards (content and elution standards for selenium, lead, fluorine, hexavalent chromium, etc.) and those that do not meet the specified standards for particle size distribution, strength properties, expansion properties, etc. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing an example of a method for modifying a substance, a method for refining molten iron, and a method for producing a slag material according to the present invention. [Diagram 2] FIG. 2 is a SEM image showing the effects of the method for modifying substances, the method for refining molten iron, and the method for producing slag material of the present invention. [Diagram 3] FIG. 3 is a SEM-EDX element mapping image showing the effects of the method for modifying a substance, the method for refining molten iron, and the method for producing a slag material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the method for modifying a substance, the method for refining molten iron, and the method for producing a slag material of the present invention will be specifically described with reference to the drawings.
[0016] The method for modifying a substance, the method for refining molten iron, and the method for producing a slag material according to the present embodiment are shown in Fig. 1. The method for modifying a substance according to the present embodiment is applied to a slag removal process in which molten slag 3, which is generated when refining molten iron 2 in a converter (refining vessel) 1, is discharged from the converter 1 to a slag ladle 4.
[0017] Specifically, in the slag removal process, after the molten slag 3 starts to be discharged from the converter 1, a powdery substance 6 is projected by a projection device 5 onto the slag 3 being discharged from the converter 1 to the slag pan (slag removal container) 4 or into the slag 3 in the slag pan 4 immediately after discharge, and the powdery substance 6 penetrates into the slag 3 and melts and mixes it. "Immediately after discharge" means a time when the molten slag 3 discharged from the converter 1 to the slag pan 4 is still largely fluid in the slag pan 4 and can be expected to be sufficiently melted and mixed when a powdery substance is projected onto it, for example, a time before the slag pan 4 is transported to a slag treatment plant. If the slag 3 is not discharged or immediately after discharge, the momentum of the slag 3 discharged into the slag pan (slag removal container) 4 decreases, and sufficient melting and mixing cannot be achieved.
[0018] The slag ladle 4 may be empty before the slag 3 is discharged, or may contain the slag 3 discharged from a previous refining process. The projection of the powdered material 6 onto the slag 3 may continue after the discharge of the slag 3 is completed.
[0019] 1, the projection device 5 has a dispenser tank 51 and a spray pipe 52. The dispenser tank 51 contains a powdery substance 6.
[0020] The powdered material 6 includes steel slag generated in the steelmaking process, as well as powdered by-products such as blast furnace slag and dust, sludge, etc., other than steel slag. If steel slag not meeting a predetermined quality control standard, for example steel slag containing 5 ppm or more of selenium, is used as the powdered material 6, the selenium can be homogeneously mixed in the mixed slag obtained by projecting the powdered material 6 onto the slag 3, as described below, and can be rendered harmless. Alternatively, even if the powdered material 6 does not meet the predetermined standards in terms of particle size distribution, strength characteristics, expansion characteristics, etc., the powdered material 6 is homogeneously melted and mixed in the mixed slag, so that the particle size distribution, strength characteristics, expansion characteristics, etc. of the mixed slag can be made to meet the standards. The upper limit of the selenium content in the powdered material 6 is preferably 20 ppm or less, more preferably 10 ppm or less. In this way, the amount of selenium leaching from the mixed slag obtained by projecting powdered substance 6 onto slag 3 can be made to satisfy the standard of 0.01 mg / L or less specified in Environment Agency Notification No. 14 and Environment Ministry Notification No. 46.
[0021] The powdered material 6 is preferably crushed or sieved in advance to a maximum particle size of 5 mm or less in order to reduce the possibility of clogging the pipes during blasting and to facilitate melting when it comes into contact with the slag 3.
[0022] In addition, the powdery material 6 is preferably mixed with water to form a slurry in the shot material 7, and then projected from the spray piping 52 using a carrier gas made of an inert gas. By projecting the shot material 7, which is a slurry made by mixing water with the powdery material 6, the propulsion force during projection is increased, promoting the stirring of the slag 3 in the dregs pan 4, and reducing the scattering of the powdery material 6 to the surroundings during projection.
[0023] The method for refining molten iron of this embodiment is a method for applying the above-mentioned substance modification method to a refining process including a refining process for refining molten iron 2 in a converter (refining vessel) 1 and a slag discharging process for discharging slag 3 generated by the refining process from the converter 1 to a slag pan 4. Alternatively, the method for refining molten iron of this embodiment may be a method for applying the above-mentioned substance modification method to a refining process including a first refining process for desiliconizing and dephosphorizing molten iron in a converter, a slag discharging process for discharging slag generated by the first refining process from the converter to a slag pan, and a second refining process for decarburizing the molten iron after the slag discharging process in the converter. Then, in the slag discharging process, a powdery substance 6 is projected onto the slag 3 discharged into the slag pan 4 to melt and mix, thereby implementing the method for refining molten iron of this embodiment.
[0024] The method for producing slag according to the present embodiment produces slag 3 in which powdery material 6 is melt-mixed, using the above-mentioned method for modifying a material. EXAMPLES
[0025] Hereinafter, specific examples of the method for modifying a substance, the method for refining molten iron, and the method for producing a slag material according to the present invention will be described. In this example, pre-treated slag that does not meet the quality control standards is modified using converter desiliconization slag, and the molten mixture is produced as a roadbed material raw material. In this example, as in the above-mentioned embodiment, in the slag removal process in which the molten slag 3 generated when refining molten iron 2 in a converter 1 is discharged from the converter 1 to a slag pan 4, a powdered substance 6 is projected onto the slag 3 in the slag pan 4 using a projection device 5.
[0026] In this embodiment, the refining process is a desiliconization process, and the slag 3 is a desiliconization slag generated by the desiliconization process. The powdery material 6 is a slag powder obtained by sieving a pre-treated slag generated in a refining process other than the above refining process through a 5 mm sieve. This powdery material 6 contains 5 ppm or more of selenium, exceeding the elution standard (0.01 mg / L) of selenium stipulated in Notification No. 46 of the Ministry of the Environment. The powdery material 6 is then mixed with an inert gas and water in the spray pipe 52 to form a slurry-like blast material 7, which is then blasted at a speed of 200 to 400 kg / min.
[0027] Then, the slag 3 in which the powdery material 6 was melted and mixed in the slag pan 4 was observed for microstructure and various evaluations were performed as a roadbed material raw material. In this embodiment, for convenience of handling in the processing process, the above evaluations were performed by sampling multiple locations from a lot in which mixed slag generated in the refining process of multiple charges was collected at a slag processing plant.
[0028] Table 1 shows the amount of slag 3 discharged into the slag pan 4, the amount of powdered material 6 blasted, the mixing ratio of powdered material 6 in the mixed slag, and the blasting speed of powdered material 6 in each charge. As shown in Table 1, the amount of slag 3 discharged was set to 6.6 to 12.5 t / charge, the amount of powdered material 6 blasted was set to 0.5 to 1.4 t / charge, and the mixing ratio of powdered material 6 in the mixed slag was changed in the range of 6 to 18%. In addition, the blasting speed of powdered material 6 was changed in the range of 100 to 300 kg / min.
[0029] [Table 1]
[0030] Table 2 shows the results of microstructural observation and various evaluations as a roadbed material for the slag 3 before the powdery material 6 is projected, the powdery material 6, and the mixed slag (example of the invention) obtained by projecting the powdery material 6 onto the slag 3 discharged into the dregs pan 4. Figures 2 and 3 show SEM (scanning electron microscope) images and SEM-EDX (energy dispersive X-ray spectroscopy) element mapping images of the slag 3 before the powdery material 6 is projected, the powdery material 6, and the mixed slag (example of the invention), respectively.
[0031] [Table 2]
[0032] As shown in the SEM image of FIG. 2, the shape of the fine particles of the mixed slag (invention example) had characteristics similar to those of slag 3 in multiple fields of view, and the shape of powdery material 6 was not observed.
[0033] As shown in the SEM-EDX element mapping image of Figure 3, the distribution of the components of the mixed slag (example of the invention) also had characteristics similar to those of slag 3 in multiple fields of view. Specifically, while a concentrated phase of Si and Mn was present in powdered material 6, no concentrated phase of Si and Mn was observed in the mixed slag, and it was confirmed that powdered material 6 was melted and mixed in slag 3.
[0034] As shown in Table 2, the amount of melilite phase observed by XRD (X-ray diffraction) measurement was small in slag 3 and large in powdered material 6, while it was moderate in the mixed slag (example of the invention), and it was confirmed that powdered material 6 was homogeneously melted and mixed in the mixed slag. Regarding the quality control standards for roadbed material raw materials, the amount of selenium eluted from powdered material 6 exceeded the standard (0.01 mg / L) specified in Notification No. 46 of the Ministry of the Environment, while the amount of selenium eluted from the mixed slag (example of the invention) was less than 0.002 mg / L, confirming that selenium was rendered harmless. Regarding other quality control standards such as strength (corrected CBR value) and expansion stability, the measured values of the mixed slag (example of the invention) were confirmed to meet the standards for roadbed material raw materials.
[0035] From the above results, it has been confirmed that according to the method for modifying a substance, the method for refining molten iron, and the method for producing a slag material of the present invention, the powdered substance 6 projected onto the molten slag 3 is melted and mixed homogeneously into the mixed slag, and the mixed slag can be modified to meet quality control standards. [Explanation of symbols]
[0036] 1 Refining vessel (converter) 2. Molten Iron 3. Slug 4 Slag pot 5 Projection device 51 Dispenser tank 52 Spray piping 6 Powdery substances 7 Projection material
Claims
1. A method for modifying a material, in which a powdered material consisting of slag containing 5 ppm or more of selenium is projected onto and stirred in a slag discharge container during or immediately after the discharge of molten slag generated by a refining process into the slag discharge container, thereby causing the powdered material to penetrate and melt and mix with the slag, thereby homogeneously mixing the selenium into the mixed slag and rendering it harmless.
2. 2. The method for modifying a substance according to claim 1, further comprising the step of projecting a slurry obtained by mixing the powdered substance with water onto the molten slag.
3. A method for refining molten iron, comprising: a refining process for refining molten iron in a refining vessel; and a slag discharging process for discharging slag generated by the refining process from the refining vessel to a slag pan, wherein in the slag discharging process, a powdered substance is projected onto the slag discharged into the slag pan to melt and mix it, using a substance modification method as defined in claim 1 or 2.
4. A method for refining molten iron, comprising: a first refining process for desiliconizing and dephosphorizing molten iron in a converter; a slag discharging process for discharging slag generated by the first refining process from the converter to a slag pan; and a second refining process for decarburizing the molten iron after the slag discharging process in the converter, wherein in the slag discharging process, a powdered substance is projected onto the slag discharged into the slag pan to melt and mix it, using the method for modifying a substance as defined in claim 1 or 2.
5. A method for producing a slag material, comprising melt-mixing the powdered substance with the molten slag by using the method for modifying a substance according to claim 1 or 2 to produce a slag material.
Citation Information
Patent Citations
Absorption refrigerator
JP1978041849A
Treatment of desulfurizing slag
JP1983042712A
Positioning mechanism for tool post of NC lathe
JP1985025602A