Refining lance and method for refining molten iron
The refining lance with integrated gas paths and adjustable suction holes allows for controlled oxygen supply adjustments, improving refining efficiency and reducing splash and corrosion by using an ejector effect and coherent jet.
Patent Information
- Application Number
- JP2022188405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-11-25
AI Technical Summary
Existing refining lances struggle to adjust oxygen supply conditions during the decarburization process in steelmaking, leading to inefficiencies and increased iron oxide production, splash, and lance corrosion, due to limitations in controlling dynamic pressure and flow rate.
A refining lance with a mainstream gas supply path and atmospheric gas supply path, allowing for the mixing of gases to increase flow rate without changing the oxygen flow rate, using an ejector effect and coherent jet to control dynamic pressure and flow direction.
Enhances refining efficiency by increasing flow rate and dynamic pressure without increasing oxygen flow rate, reducing splash and iron oxide production, and extending lance life.
Smart Images

Figure 0007582286000004 
Figure 0007582286000005 
Figure 0007582286000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a refining lance and a method for refining molten iron. [Background technology]
[0002] In the oxidation refining process of molten iron, from the viewpoint of improving reaction efficiency, there is a demand for a practical oxygen supply means that can simultaneously control the jet flow velocity and gas flow rate of the oxygen-containing gas (top-blown gas) injected from a refining lance (also called a top-blown lance) at the molten iron bath surface.
[0003] For example, in the steelmaking process of iron and steel refining, decarburization is performed by top-blowing oxygen into molten steel. This decarburization process is divided into an initial stage, a peak stage, and a final stage depending on the change in the composition of the molten steel during refining. It is known that the preferable operating conditions at each stage of the decarburization process are different.
[0004] For example, at the peak of decarburization, the carbon concentration is high, so the oxygen gas jet injected from the refining lance reacts easily with carbon when it collides with the molten steel interface. Therefore, the refining process speed is determined by the oxygen supply, that is, the decarburization rate increases as the oxygen flow rate, which is the flow rate of oxygen gas, increases. Therefore, in order to shorten the refining process time, the operating condition at the peak of decarburization should be increased as much as possible. However, if the oxygen flow rate is increased, the flow rate of the jet on the molten iron bath surface increases and the bath surface dynamic pressure increases, so that the amount of iron scattered outside the furnace as dust increases, and the amount of splashing of molten steel and slag increases, causing the adhesion and accumulation of molten steel and slag on the furnace wall and around the furnace throat. If the amount of dust and splash increases, the iron yield decreases, leading to increased costs. In addition, if a large amount of splash adheres to the lance and the inner wall of the converter, the work of removing the ingot is required, which hinders operation. In other words, there is a trade-off between the increase in oxygen flow rate and the amount of dust and splash generation. Therefore, during the peak of decarburization, it is desirable to have operating conditions that do not increase the bath surface flow velocity (dynamic pressure) even if the oxygen flow rate is increased.
[0005] On the other hand, in the final stage of decarburization, the carbon concentration has decreased to a certain extent, and the probability that the oxygen injected from the refining lance will combine with carbon at the hot point on the bath surface decreases, so that the decarburization rate is unlikely to increase even if the oxygen flow rate is increased. Furthermore, if the oxygen flow rate is increased in the final stage of decarburization, iron will combine with oxygen instead of carbon, and iron oxide will be easily generated. Although iron oxide is a substance that reacts with carbon in molten steel to cause a decarburization reaction, simply accumulating near the bath surface does not contribute to decarburization, so it is necessary to stir the molten steel to increase the probability that the iron oxide will react with the carbon in the molten steel. In other words, in the final stage of decarburization, oxygen supply conditions are required that strengthen the stirring force of the molten metal while preventing the amount of iron oxide generated from increasing too much, so that operating conditions that strengthen stirring by increasing the flow rate of the top blown gas without increasing the oxygen flow rate are desirable.
[0006] Generally, the method of adjusting the flow rate at the bath surface independently of the adjustment of the oxygen flow rate is to adjust the lance height. However, if the lance height is too low, the lance life is significantly reduced due to the melting damage caused by the scattered molten iron. If the lance height is too high, the secondary combustion rate of carbon monoxide generated by the decarburization reaction increases and the secondary combustion heat transfer efficiency decreases, which increases the gas temperature in the furnace and reduces the refractory life. In other words, there is a limit to the range of flow rate adjustment by the lance height. For this reason, the realization of a refining lance that can adjust the injection speed independently of the oxygen flow rate has been expected.
[0007] In the steelmaking process, in order to reduce the amount of steelmaking slag generated in the converter and to reduce the total cost of the steelmaking process, a method is used in which silicon and phosphorus contained in molten iron are removed by oxidation refining before decarburization blowing in the converter. One such method is dephosphorization blowing using a converter as the treatment vessel.
[0008] In general, dephosphorization blowing using a converter involves adding a refining agent such as lime (hereinafter referred to as flux) to the molten pig iron while blowing oxygen-containing gas from above the bath surface of the molten pig iron using a refining lance, similar to decarburization blowing. In this case, too, a method is used to control the T.Fe concentration (total iron concentration) in the slag generated during dephosphorization blowing by adjusting the flow rate of the oxygen-containing gas jet supplied from the refining lance.
[0009] Thus, in a refining process using a refining lance, the required operating conditions differ depending on the type and timing of the process. For example, in the peak and final stages of the decarburization process, the operating conditions are such that a refining lance with a straight nozzle that can suppress the increase in flow rate should be used in the peak decarburization stage, and a refining lance with a Laval nozzle that can increase the flow rate should be used in the final stage of the decarburization process. However, since it is difficult to replace the lance during the refining process, it is necessary to operate with one lance.
[0010] As a technique for controlling the nozzle shape of a refining lance during blowing, for example, Patent Document 1 discloses a technique for a refining lance in a vacuum degassing vessel in which the nozzle shape is mechanically changed. As one method of jet control, there is the use of a control flow separate from the main jet of the lance nozzle. For example, Patent Document 2 discloses a method of controlling the jet direction by providing a pair of openings for a control gas on the side wall of a fluid jet passage. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 8-260029 [Patent Document 2] JP 2005-113200 A Summary of the Invention [Problem to be solved by the invention]
[0012] Conventionally, when dynamic pressure was increased to strengthen stirring at the end of decarburization, the dynamic pressure was increased by increasing the oxygen flow rate because it was difficult to change the tip of the refining lance during the refining process. This resulted in an excessive supply of oxygen to the molten steel, which led to a decrease in refining efficiency due to an increase in iron oxide.
[0013] The technology described in Patent Document 1 proposes a technology for mechanically changing the inner diameter of the lance, which makes it possible to change the dynamic pressure during the refining process. However, in the final stage of decarburization, the inner diameter of the lance is reduced for operation, and the flow area becomes narrow, resulting in a decrease in flow rate and insufficient stirring power. In order to strengthen the stirring power, the oxygen flow rate must be increased, but as mentioned above, this leads to an increase in iron oxide.
[0014] Furthermore, the technology described in Patent Document 2 requires the provision of equipment for supplying and controlling a control gas separate from the main jet, which increases the costs required for implementation and maintenance.
[0015] Therefore, the present invention has been made with attention to the above-mentioned problems, and aims to provide a refining lance and a method for refining molten iron that can change the oxygen supply conditions during the refining process in a simple manner. [Means for solving the problem]
[0016] (1) According to one aspect of the present invention, there is provided a refining lance for use in a steel refining process, comprising: an injection hole formed at a lower end of the refining lance; a mainstream supply passage formed inside the refining lance and supplying a mainstream gas containing oxygen gas to the injection hole; a suction port formed on a peripheral side of the refining lance; and an atmospheric gas supply passage connected respectively to the mainstream supply passage and the suction port and supplying atmospheric gas sucked in from the suction port to the mainstream supply passage, wherein the refining lance injects from the injection hole a top blown gas which is a mixture of the mainstream gas and the sucked atmospheric gas.
[0017] (2) In the refining lance described above in (1), the atmospheric gas supply passage supplies the atmospheric gas uniformly from the circumferential direction to the mainstream supply passage at a connection portion between the mainstream supply passage and the atmospheric gas supply passage.
[0018] (3) In the refining lance of (1) or (2) above, at a connection between the main gas supply path and the atmospheric gas supply path, an angle between the flow direction of the main gas and the flow direction of the atmospheric gas is 0° or more and 20° or less.
[0019] (4) In the refining lance of any one of (1) to (3) above, the main supply path has a main branch path at a lower end of the refining lance, which branch into multiple paths, and the atmospheric gas supply path is connected to the multiple main branch paths.
[0020] (5) The refining lance according to (4) above is provided with a plurality of the atmospheric gas supply paths, and each of the plurality of the main branch paths is connected to one of the atmospheric gas supply paths.
[0021] (6) In the refining lance of any one of (1) to (5) above, the mainstream supply path has a nozzle at an outlet side of the mainstream gas having a Laval shape, and a connection part between the mainstream supply path and the atmospheric gas supply path is provided at an outlet of the Laval shape.
[0022] (7) The refining lance according to any one of (1) to (6) above, further comprising an opening adjustment mechanism capable of adjusting the opening of the suction hole.
[0023] (8) According to one aspect of the present invention, there is provided a method for refining molten iron by subjecting molten iron to an oxidative refining treatment, the method using the refining lance described above in (1).
[0024] (9) In the method for refining molten iron described above in (8), the refining lance is a refining lance further including an opening adjustment mechanism capable of adjusting the opening of the suction hole, and the opening is adjusted during the oxidation refining treatment in accordance with the timing of the oxidation refining treatment.
[0025] (10) In the method for refining molten iron according to (8) or (9) above, the oxidative refining treatment is a decarburization treatment of the molten iron, and the aperture at the end of the decarburization stage is made larger than the aperture at the peak of the decarburization stage. Effect of the Invention
[0026] According to one aspect of the present invention, there is provided a refining lance and a method for refining molten iron, which are capable of changing oxygen supply conditions during refining treatment in a simple manner. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a schematic diagram showing a converter in one embodiment of the present invention. [Diagram 2] FIG. 2 is a bottom view showing a refining lance according to an embodiment of the present invention. [Diagram 3] 2 is a cross-sectional view showing a refining lance according to one embodiment of the present invention, taken along line II in FIG. [Figure 4] 3 is a schematic diagram showing a main branch path, an ambient gas supply path, and a suction hole. FIG. [Diagram 5] FIG. 4 is an explanatory diagram showing the relationship between the flow direction of a mainstream gas and the flow direction of an ambient gas at a connection portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] In the following detailed description, an embodiment of the present invention will be described with reference to the drawings. In the description of the drawings, identical or similar parts are given identical or similar symbols, and duplicated explanations are omitted. Each drawing is schematic and may differ from the actual one. In addition, the embodiments shown below are examples of devices and methods for embodying the technical idea of the present invention, and the technical idea of the present invention does not specify the materials, structures, arrangements, etc. of the components as described below. The technical idea of the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.
[0029] <Refining lance> A refining lance 1 according to an embodiment of the present invention will be described with reference to Figs. 1 to 3. The refining lance 1 is a top-blown lance used in an oxidation refining process, which is one of the refining processes for steel, and is used, for example, in a refining process in a converter 2 shown in Fig. 1. In this embodiment, as an example, a decarburization process of molten pig iron is performed as a refining process in the converter 2. In the decarburization process in the converter 2, a top-blown gas 3 containing oxygen gas is injected from the refining lance 1 into the molten pig iron charged in the converter 2, and the molten pig iron is oxidized and decarburized by the oxygen gas contained in the top-blown gas 3, thereby producing molten steel. The molten pig iron and molten steel are also collectively referred to as molten iron 5. In the decarburization process, a slag forming agent such as CaO is added to the converter 2 to remove impurities such as phosphorus from the molten iron 5. The slag forming agent melts to become slag 4, and forms a slag layer on the molten iron 5.
[0030] The refining lance 1 has a porous structure having a plurality of injection holes 10 at its lower end. In the example shown in Fig. 2, the refining lance 1 has four injection holes 10. In addition, the refining lance 1 includes a main flow supply path 11, a plurality of atmospheric gas supply paths 12, a plurality of suction holes 13, and an opening adjustment mechanism 14 as shown in Fig. 3.
[0031] The mainstream supply passage 11 is a passage formed inside the refining lance 1 and supplies a mainstream gas containing oxygen gas to the multiple injection holes 10. The mainstream gas contains at least oxygen gas and accounts for at least the majority of the top blown gas 3. The mainstream gas is supplied from a mainstream supply device (not shown) to an inlet of the mainstream supply passage 11 provided on the upper end side of the refining lance 1. The mainstream supply passage 11 has multiple mainstream branch passages 110, which are paths branched into multiple paths, on the lower end side of the refining lance 1. The number of the mainstream branch passages 110 is the same as the number of the injection holes 10. In the example shown in Figures 2 and 3, the mainstream supply passage 11 has four mainstream branch passages 110. In such a mainstream supply passage 11, the mainstream gas supplied from the mainstream supply device flows through the mainstream supply passage 11 from the upper end side to the lower end side of the refining lance 1, branches at the multiple mainstream branch passages 110, and is injected from the multiple injection holes 10.
[0032] In addition, the nozzle of the mainstream gas outlet side of the mainstream supply passage 11, i.e., the mainstream branch passage 110, has a Laval shape. The Laval shape is a shape in which the passage contracts and expands, and the fluid flowing through the passage can obtain a high flow velocity. In FIG. 3, the outlet area (Laval outlet area) of the Laval shape of the mainstream branch passage 110 is defined as A1 (mm 2 ), and the outlet area of the main branch path 110 (nozzle outlet area) is A2 (mm 2 ), the outlet diameter of the Laval shape of the main branch path 110 (Laval outlet diameter) is D1 (mm), the nozzle outlet diameter is D2 (mm), and the distance (outlet distance) from the outlet of the Laval shape to the outlet of the main branch path 110 (nozzle outlet) is D t Shown in (mm).
[0033] The plurality of ambient gas supply paths 12 are provided in a number corresponding to the plurality of mainstream branch paths 110, and are each formed in a ring shape surrounding the plurality of mainstream branch paths 110. The ambient gas supply path 12 has a rectangular cross section perpendicular to the radial direction of the ring shape, and a part of the inner side as viewed in this cross section is connected to the mainstream branch path 110. The point where the ambient gas supply path 12 is connected to the mainstream branch path 110 is called a connection part 111, and the connection part 111 is formed around the entire circumference of the mainstream branch path 110 in the circumferential direction.
[0034] In addition, it is preferable that the atmospheric gas supply path 12 uniformly supplies the atmospheric gas to the mainstream supply path 11 from the circumferential direction at the connection part 111 between the mainstream supply path 11 and the atmospheric gas supply path 12. In order to make the flow rate of the atmospheric gas discharged from the connection part 111 uniform in the circumferential direction, it is necessary to secure a wide space for the atmospheric gas supply path 12. If the space of the supply path 12 is too narrow, the atmospheric gas sucked from the suction hole 13 will be discharged from the connection part 111 without spreading over the entire circumferential direction of the supply path 12, and will be discharged with a biased flow rate distribution such that the flow rate on the side closer to the suction hole 13 is higher. This causes problems such as a change in the flow direction of the mainstream gas. In the case of a perforated lance, the suction hole 13 of the atmospheric gas can only be set on the outside of the nozzle (the outer wall surface of the refining lance 1), so it is difficult to make the flow rate in the circumferential direction at the connection part 111 uniform. For this reason, the setting of the supply path 12 is particularly important. Although the provision of the supply path 12 is not essential for a single-hole lance, it is believed that the flow rate in the circumferential direction can be made more uniform if a supply path 12 is provided.
[0035] In order to efficiently obtain the ejector effect described later, the connection part 111 is preferably formed at a portion of the main branch passage 110 where the flow velocity of the mainstream gas is high (where the pressure is low), and may be formed at the outlet of the main branch passage 110 having a Laval shape, as shown in FIG. 3, for example. The dimensions and shape of the connection part 111 are appropriately set according to conditions such as the degree of ejector effect required and the flow velocity of the mainstream gas. At the junction of the mainstream gas and the ambient gas, the outlet area of the ambient gas flow path and the size of the gap (for example, the length of the connection part in FIG. 3) have a large effect on the injection flow velocity. If the outlet area of the ambient gas is too small or the gap is too narrow, the amount of ambient gas sucked in may not be sufficient, and the flow velocity may not be improved. On the other hand, if the outlet area of the ambient gas is too large or the gap is too wide, the situation is the same as that in which a lance is arranged in an open space, and the ejector effect may not be generated. However, since the optimal values of the outlet area and gap of the connection part 111 vary depending on the amount of ambient gas suction, which varies depending on the flow rate of the mainstream gas, the size of the refining lance 1, etc., the optimal values of the outlet area and gap of the connection part 111 should be determined according to the shape of each refining lance 1.
[0036] The plurality of suction holes 13 are openings formed in the plurality of atmospheric gas supply paths 12, respectively. The suction holes 13 connect the outside of the refining lance 1 to the atmospheric gas supply path 12, and take in the atmospheric gas outside the refining lance 1 into the atmospheric gas supply path 12. The atmospheric gas is the gas (furnace gas) in the converter 2, and during the oxidation refining process, the gas has a lower oxygen concentration than the mainstream gas. Particularly during the decarburization process, the atmospheric gas contains almost no oxygen gas. The suction holes 13 are formed in a part of the outer circumferential surface of the atmospheric gas supply path 12, as shown in FIG. 4. The shape of the suction holes 13 is not particularly limited, but may be rectangular in order to facilitate the adjustment of the suction amount described later.
[0037] The opening adjustment mechanism 14 has a partition plate attached to the suction hole 13, and is provided so that the opening of the suction hole 13 can be adjusted by moving the partition plate. For example, the opening adjustment mechanism 14 may be configured so that the partition plate can move in the extension direction of the main branch path 110, as shown in FIG. 3. The opening adjustment mechanism 14 may also adjust the opening of the suction hole 13 by moving the partition plate in another direction. Furthermore, the opening adjustment mechanism 14 may be a mechanism other than a mechanism that moves a partition plate, as long as it is capable of adjusting the opening of the suction hole 13.
[0038] Although not shown, the refining lance 1 has a cooling water flow passage formed therein through which cooling water flows.
[0039] In the refining lance 1 according to this embodiment, when the top blown gas 3 is injected, the mainstream gas is supplied from a mainstream supply device to the mainstream supply passage 11. The supplied mainstream gas flows through the mainstream supply passage 11 toward the lower end of the refining lance 1 and flows into the multiple mainstream branch passages 110. The mainstream gas then flows through the mainstream branch passages 110 and is injected from the injection hole 10 as the top blown gas 3.
[0040] At this time, in the main branch passage 110, as shown in FIG. 4, the ambient gas is drawn from the suction hole 13 to the ambient gas supply passage 12 by the ejector effect. Then, the ambient gas is drawn from the ambient gas supply passage 12 to the main branch passage 110 through the connection part 111. Then, a mixture of the mainstream gas and the ambient gas is injected from the injection hole 10 as the top blown gas 3. Although the purpose of this embodiment is not to create a vacuum, the ambient gas drawn in by the ejector effect, that is, the ambient gas in the ambient gas supply passage 12, can increase the flow rate of the top blown gas 3 and increase the flow rate. In addition, this ejector effect can increase the flow rate of the top blown gas without changing the flow rate of the mainstream gas. Therefore, the flow rate of the top blown gas can be increased without changing the flow rate of the oxygen gas, and the dynamic pressure of the top blown gas at the bath surface can be increased.
[0041] In order to generate the ejector effect efficiently, it is desirable for the shape of the lance to minimize the pressure loss during the suction of the ambient gas around the refining lance 1 and to allow smooth suction. To achieve this, the area of the flow passage from when the ambient gas is suctioned until it joins the mainstream gas should be sufficiently large, and a flow passage design in which the flow direction changes suddenly should be avoided.
[0042] Moreover, the shape of the mainstream branch passage 110 is preferably a Laval shape. The mainstream branch passage 110, which is the outlet side of the mainstream supply passage 11, may have a simple cylindrical shape. However, in order to increase the amount of gas suction due to the ejector effect, it is better for the flow velocity of the mainstream gas to be high, and therefore a Laval shape capable of generating a supersonic speed is preferable because it can increase the amount of ambient gas suction. Furthermore, when using a Laval shape as shown in FIG. 3, it is preferable that the ratio (A2 / A1) of the nozzle outlet area A2 to the Laval outlet area A1 is 1.1 or more and 3.0 or less, and the outlet distance D t Ratio of nozzle outlet diameter D2 to (D2 / D t ) is preferably 0.5 or more and 2.0 or less, and more preferably 1 or more and 1.5 or less. By setting each ratio within this range, a higher ejector effect can be obtained.
[0043] In the converter 2, the ambient gas sucked in from the suction hole 13 is mainly CO and CO2. When CO mixes with the oxygen in the mainstream gas in the nozzle, a secondary combustion reaction (2CO+O2→2CO2) occurs. A flame is generated by the secondary combustion, and by using this flame, a coherent jet effect is generated, which can further increase the molten metal surface flow rate. Coherent jet is a technology that suppresses the attenuation of the mainstream gas flow rate by surrounding the mainstream gas with a flame. The reason why the attenuation of the mainstream gas can be suppressed is that when gas flowing in the same direction as the mainstream gas is present around the mainstream gas, the attenuation of the mainstream gas flow rate is smaller than when the surrounding gas is stopped.
[0044] To form a coherent jet, the ambient gas needs to be discharged uniformly around the mainstream gas in the circumferential direction at the connection part 111. If the ambient gas is not discharged uniformly in the circumferential direction, problems such as a decrease in the flow velocity attenuation effect and bending of the jet flow direction occur.
[0045] In order to obtain the mainstream flow velocity attenuation effect by the coherent jet, the flame generated by the secondary combustion needs to surround the mainstream, but as shown in FIG. 5, the angle θ between the flow direction of the ambient gas (discharge direction) at the connection part 111 and the flow direction of the mainstream gas is important. If this angle θ is large, the mainstream gas and the ambient gas collide and mix, so that the flame occurs inside the mainstream, and the ambient gas does not surround the mainstream gas. To prevent this, the angle θ needs to be small, and the angle θ is preferably 0° or more and 20° or less. To maximize the mainstream flow velocity attenuation effect by the coherent jet, the angle θ needs to be 0°, that is, the mainstream gas and the ambient gas need to flow in the same direction. In addition, to fully obtain the mainstream flow velocity attenuation effect by the coherent jet, the angle θ is preferably 20° or less.
[0046] When a flame is generated in the secondary combustion, the mainstream gas is heated, so the temperature at the position where the mainstream gas collides with the molten iron 5 can be increased compared to when there is no flame. This makes it possible to maintain a high temperature of the molten iron 5, and is expected to improve the processing efficiency by increasing the refining reaction rate.
[0047] Moreover, in the refining lance 1 according to this embodiment, the amount of atmospheric gas taken into the atmospheric gas supply path 12 can be adjusted by adjusting the aperture of the suction hole 13 with the aperture adjustment mechanism 14. Therefore, the flow rate of the top blown gas 3 can also be adjusted by adjusting the aperture of the suction hole 13, and the flow rate of the top blown gas can be adjusted depending on the content and timing of the refining process.
[0048] <Method of refining molten iron> Next, a method for refining molten iron 5 according to this embodiment will be described. In this embodiment, as an example, a refining method for producing molten steel by subjecting molten pig iron, which is molten iron 5, to an oxidation refining process is described. In this refining method, a top-blown gas 3 containing oxygen gas is injected from a refining lance 1 into the molten pig iron charged in a converter 2, thereby decarburizing the molten pig iron as an oxidation refining process. At this time, auxiliary materials such as a slag forming agent may be added into the converter 2 to perform the refining process. Also, an inert gas for stirring may be blown in from a tuyere provided at the bottom of the converter 2.
[0049] The decarburization process is divided into an initial stage, a peak stage, and a final stage according to the carbon concentration in the molten iron. These stages are estimated, for example, by the total amount of oxygen gas injected during the decarburization process, the gas components and amount of exhaust gas discharged, etc. In this embodiment, the opening degree of the suction hole 13 is adjusted using the opening degree adjustment mechanism 14 depending on the timing of the decarburization treatment. Specifically, for the peak and final stages of the decarburization treatment, the opening degree of the suction hole 13 in the final stage of decarburization is set to be larger than the opening degree of the suction hole 13 in the peak stage of decarburization. In this case, the opening degree in each stage may be set depending on the desired amount of atmospheric gas to be sucked, or the suction hole 13 may be controlled so as to be closed in the peak stage of decarburization and open in the final stage of decarburization.
[0050] As described above, the peak of decarburization is a period when the decarburization reaction mainly occurs as an oxidation reaction of the molten iron 5, and the decarburization rate is rate-determined by the oxygen supply. In addition, as an appropriate operating condition in the peak of decarburization, it is preferable to increase the oxygen flow rate as much as possible while preventing the bath surface dynamic pressure from increasing. For this reason, in the operation of the refining lance 1, the opening of the suction hole 13 can be narrowed or closed to increase the proportion of oxygen gas (i.e., mainstream gas) contained in the top blown gas 3 while decreasing the flow rate of the top blown gas 3. This makes it possible to reduce the amount of dust and splash generated while maintaining a high decarburization rate in the peak of decarburization.
[0051] On the other hand, in the final stage of decarburization, the decarburization rate becomes the stirring rate-determining period. In addition, in the final stage of decarburization, it is necessary to increase the flow rate of the top-blown gas while decreasing the flow rate of the oxygen gas, thereby strengthening the stirring force of the molten iron 5. For this reason, in the operation of the refining lance 1, the ratio of the atmospheric gas contained in the top-blown gas 3 can be increased by increasing or opening the opening of the suction hole 13. By increasing the ratio of the atmospheric gas, it is possible to increase the flow rate of the top-blown gas 3 without changing the flow rate of the oxygen gas contained in the top-blown gas 3. As a result, in the final stage of decarburization, it is possible to suppress the generation of iron oxide while maintaining a high decarburization rate.
[0052] Furthermore, at the peak and final stages of decarburization, in addition to adjusting the opening of the suction hole 13, the dynamic pressure of the bath surface of the top blown gas 3 may be adjusted by adjusting the lance height of the refining lance 1.
[0053] In the early stage of decarburization, the de-Si reaction and the de-Mn reaction proceed preferentially, and the decarburization reaction rate is also slow because this is the period before the decarburization progresses and the temperature of the molten iron rises. The oxygen supply conditions in the early stage of decarburization are not particularly limited, but may be set in consideration of the reaction rates of the de-Si reaction and the de-Mn reaction and the amount of splash generation according to the initial component composition of the molten iron, etc. For example, the oxygen supply conditions in the early stage of decarburization may be set so as to increase the reaction rates of the de-Si reaction and the de-Mn reaction.
[0054] According to the refining lance 1 and the method for refining molten iron of this embodiment, there is no need to replace the refining lance as in Patent Document 1, nor is there a need to provide equipment for supplying and controlling a control gas different from the mainstream gas as in Patent Document 2, so that the oxygen supply conditions can be changed during the refining process in a simpler manner.
[0055] <Modification> Although the present invention has been described above with reference to specific embodiments, it is not intended that the invention be limited by these descriptions. By referring to the description of the present invention, other embodiments of the present invention including various modifications in addition to the disclosed embodiments will be apparent to those skilled in the art. Therefore, it should be understood that the embodiments of the invention described in the claims also include embodiments including these modifications described herein, either alone or in combination.
[0056] For example, in the above embodiment, the atmospheric gas supply path 12 and the suction hole 13 are provided individually in each of the plurality of main branch paths 110, but the present invention is not limited to such an example. For example, a configuration may be adopted in which the number of suction holes 13 is smaller than the number of main branch paths 110, and the atmospheric gas is supplied to the main branch path 110 through at least one of the suction holes 13 through the atmospheric gas supply path 12. In addition, the atmospheric gas supply path 12 is not limited to the shape and number of the atmospheric gas supply path 12 as long as it supplies the atmospheric gas sucked from at least one suction hole 13 to the plurality of main branch paths 110. Since the space of the metal part of the refining lance 1 is limited, for example, the plurality of atmospheric gas supply paths 12 in the above embodiment may be connected. In this case, the atmospheric gases sucked from the separate suction holes 13 are mixed before merging with the mainstream gas.
[0057] In the above embodiment, the connection portion 111 is formed around the entire circumferential direction of the main branch path 110, but the present invention is not limited to this example. For example, the connection portion 111 may be a plurality of connection ports formed at a predetermined interval in the circumferential direction of the main branch path 110. When the mainstream gas and the ambient gas are joined, the ambient gas is supplied evenly from the periphery of the mainstream gas to join the gases, thereby preventing the deflection of the jet and the occurrence of a difference in flow speed. For this reason, it is preferable that the connection portion 111 is formed in a circular shape around the entire circumferential direction of the main branch path 110 as in the above embodiment.
[0058] Furthermore, in the above embodiment, the refining lance 1 has a plurality of injection holes 10, but the present invention is not limited to such an example. For example, the refining lance 1 may be a lance with a single nozzle hole 10. In this case, an atmospheric gas supply path 12 and a suction hole 13 are provided for a nozzle on the outlet side of the mainstream supply path 11. Furthermore, the refining lance 1 may be configured to use other gases together with oxygen gas as the mainstream gas, and may be configured to inject powdered auxiliary materials and the like from the injection hole 10 together with the top blown gas 3.
[0059] Furthermore, in the above embodiment, the decarburization process is performed as the oxidation refining process of the molten iron 5, but the present invention is not limited to this example. For example, the dephosphorization process may be performed as the oxidation refining process of the molten iron 5. In the dephosphorization process, a method is adopted in which the concentration of T.Fe in the slag is controlled to be equal to or lower than a predetermined value while increasing the stirring force. In contrast, according to the refining lance 1 according to the above embodiment, the ratio of oxygen gas contained in the injected gas can be adjusted while increasing the flow rate of the injected gas by adjusting the opening degree and the flow rate of the mainstream gas. Therefore, the stirring force can be increased without increasing the concentration of T.Fe in the slag during the dephosphorization process more than necessary.
[0060] Furthermore, in the above embodiment, a partition plate that is attached to the suction hole 13 and mechanically adjusts the opening of the suction hole 13 is used as the opening adjustment mechanism 14, but the present invention is not limited to this example. The opening adjustment mechanism 14 may be set at any point in the flow path from the suction hole 13 to the junction with the mainstream gas. Also, a mechanism other than a partition plate may be used as the mechanism for adjusting the opening.
[0061] Furthermore, in the above embodiment, the refining lance 1 is used in the converter 2, but the present invention is not limited to such an example. The refining lance 1 may be used in equipment other than the converter 2 as long as it is a top-blowing lance used in a refining process. For example, the refining lance 1 may be a top-blowing lance used in an electric furnace, an RH vacuum degassing equipment, or the like. EXAMPLES
[0062] An example carried out by the present inventors will be described. In the example, the effect of the refining lance 1 according to the above embodiment was verified by numerical calculation. Specifically, an analysis model was created in which a flow path (atmospheric gas supply path 12 and suction hole 13) for sucking in atmospheric gas was provided around each nozzle hole (main stream branch path 110) of the refining lance 1 shown in Figs. 2 to 4, which is a multi-hole lance used in a converter 2. The presence or absence of suction of atmospheric gas is controlled by opening and closing a partition, which is an opening adjustment mechanism 14. When the partition is open, the ejector effect is effective, and when it is closed, it is ineffective. The nozzle shape is a Laval shape, and the Laval inlet diameter is 55 mm, the Laval outlet diameter D1 is 70 mm, and the nozzle outlet diameter D2 is 100 mm. The number of holes in the injection hole 10 is four. Oxygen gas is used as the mainstream gas, and the flow rate of the mainstream gas is 20,000 Nm 3 / Hr~40000Nm 3 / Hr, and the angle θ between the flow direction of the mainstream gas and the flow direction of the atmospheric gas was set to 0°. The flow velocity of the molten iron (molten steel) bath surface (molten metal surface flow velocity) was compared before and after switching the ejector effect on and off.
[0063] Table 1 shows the flow velocity comparison results at the molten steel bath surface position (position 2 m away from the injection hole 10). It was confirmed that the flow velocity at the molten steel bath surface was improved by about 10% when the ejector effect was used compared to when there was no ejector effect.
[0064] [Table 1]
[0065] Next, the flow rate of the mainstream gas is increased to 40,000 Nm 3 / Hr, the aperture of the suction hole 13 was adjusted using the aperture adjustment mechanism 14, and the change in the molten steel surface velocity was examined. The results are shown in Table 2. The aperture of the suction hole 13 was set to 1 when it was fully open, and 0 when it was fully closed. Table 2 also shows the results of level 6 in Table 1 as a comparison result when the aperture was fully open. As shown in Table 2, the bath surface velocity of the molten steel was almost the same when the aperture was 1 to 0.5. However, when the aperture was reduced to 0.3 and 0.1, the molten steel surface velocity decreased. From this, it was confirmed that the lance exhibited a nonlinear behavior in which the flow velocity did not change if the aperture was large to a certain extent. Note that this result is a tendency of the lance shape of this embodiment, and it is considered that the results would be different for lances of different shapes.
[0066] [Table 2]
[0067] Next, the flow rate of the mainstream gas is increased to 40,000 Nm 3 The effect of changing the flow direction of the atmospheric gas at the confluence point of the mainstream gas and the atmospheric gas (the angle θ between the flow directions of the mainstream gas and the atmospheric gas) was investigated while fixing the opening angle of the suction hole 13 at 1 at a running time of 1000 / Hr. The results are shown in Table 3. When the angle θ was between 0° and 20°, the change in the molten metal surface flow velocity was small, and when the angle θ was 30° or more, the flow velocity dropped significantly.
[0068] [Table 3] [Explanation of symbols]
[0069] 1 Refining Lance 10 injection hole 11 Main supply channels 110 Main Branch Route 111 Connection 12 Atmospheric gas supply path 13 Suction hole 14 Opening adjustment mechanism 2 Converter 3. Top-blown gas 4. Slug 5. Molten Iron
Claims
1. A refining lance for use in a steel refining process, comprising: an injection hole formed at a lower end of the refining lance; a mainstream supply passage formed inside the refining lance for supplying a mainstream gas containing oxygen gas to the injection hole; A suction hole formed on a peripheral side surface of the refining lance; an atmospheric gas supply path that is connected to the main supply path and the suction hole, and that supplies the atmospheric gas sucked through the suction hole to the main supply path; an opening adjustment mechanism capable of adjusting the opening of the suction hole; Equipped with A refining lance that injects, from the injection hole, a top-blown gas obtained by mixing the mainstream gas and the aspirated atmospheric gas.
2. The refining lance according to claim 1 , wherein the atmospheric gas supply passage supplies the atmospheric gas uniformly from a circumferential direction to the mainstream supply passage at a connection portion between the mainstream supply passage and the atmospheric gas supply passage.
3. 2. The refining lance according to claim 1, wherein an angle between a flow direction of the mainstream gas and a flow direction of the atmospheric gas at a connection portion between the mainstream supply path and the atmospheric gas supply path is 0° or more and 20° or less.
4. The main supply path has a main branch path that branches into a plurality of paths at a lower end side of the refining lance, The refining lance according to claim 1 , wherein the atmospheric gas supply passage is connected to a plurality of the main branch passages.
5. A plurality of the atmospheric gas supply paths are provided, The refining lance according to claim 4 , wherein the plurality of atmospheric gas supply paths are connected to each of the plurality of main branch paths.
6. The mainstream supply path has a nozzle on an outlet side of the mainstream gas having a Laval shape, 2. The refining lance of claim 1, wherein a connection between the main supply passage and the atmospheric gas supply passage is provided at the Laval-shaped outlet.
7. A method for refining molten iron by oxidizing and refining molten iron, comprising the steps of: Using the refining lance according to claim 1, The method for refining molten iron comprises adjusting the opening during the oxidation refining treatment depending on a timing of the oxidation refining treatment.
8. As the oxidation refining treatment, a decarburization treatment of the molten iron is performed, The method for refining molten iron according to claim 7, wherein the aperture in the final stage of decarburization is set to be larger than the aperture in the maximum stage of decarburization.
Citation Information
Patent Citations
Top-blowing oxygen lance for secondary combustion in vacuum degassing vessel
JP1996260029A
Laval nozzle for converter blowing and operation using this
JP2000234116A
Nozzle structure in burner or lance, and method for melting and refining metal
JP2005113200A
Top-blown lance and method for operating converter using this lance
JP2007077489A
Top-blown lance for refinement and method for refining molten iron