Polychloroprene Latex Composition
The polychloroprene latex composition with an aromatic compound inhibits crystallization, maintaining flexibility and comfort in molded products like gloves at low temperatures.
Patent Information
- Application Number
- JP2022573103
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-28
- Filing Date
- 2021-12-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Chloroprene polymers crystallize at low temperatures, leading to hardening and discomfort in products like gloves, with existing methods failing to address this issue effectively.
A polychloroprene latex composition containing a chloroprene (co)polymer and an aromatic compound with 7 to 10 carbon atoms, in specific proportions, is used to inhibit crystallization and maintain flexibility at low temperatures.
The composition ensures molded products, such as gloves, retain flexibility and comfort even at low temperatures, preventing hardening and enhancing user experience.
Smart Images

Figure 0007582334000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a latex composition based on a polymer of 2-chloro-1,3-butadiene (chloroprene) or a copolymer of 2-chloro-1,3-butadiene and a comonomer, and to a molded product, particularly a dipped product, obtained from the latex composition. [Background technology]
[0002] Chloroprene rubber (hereinafter sometimes abbreviated as "CR") has good general rubber properties, weather resistance, heat resistance, chemical resistance, etc., and is therefore widely used in dipped products such as gloves, pressure sensitive adhesives, adhesives, elastic asphalt (modified asphalt), elastic cement, and other civil engineering and construction applications. In particular, for disposable medical gloves, especially surgical gloves, chloroprene rubber is used to prevent shock symptoms (anaphylaxis) caused by allergies to natural rubber, because the flexibility and mechanical properties of chloroprene rubber are relatively close to those of natural rubber, and chloroprene rubber can be produced relatively inexpensively. Gloves made from chloroprene rubber have excellent features, such as a good fit (comfort) similar to that of natural rubber, and the gloves can follow the fine movements of the user's fingertips well (following ability). However, since chloroprene polymer crystallizes at low temperatures and becomes hard, gloves made of chloroprene rubber have a problem of poor usability at low temperatures.
[0003] The crystallization of chloroprene polymers may be hindered by the presence of impurities in chloroprene latex. As an example of a chloroprene latex containing impurities, a chloroprene latex containing a chloroprene dimer is known (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5525684 [Patent Document 2] Japanese Patent Application Publication No. 3-203609 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the technology described in Patent Document 1 provides a method for suppressing the amount of chloroprene dimer produced during the production of chloroprene latex in order to deal with the odor of chloroprene latex, and evaluation of the flexibility of molded products containing impurities has not been performed. Patent Document 2 proposes a method for removing impurities such as dimers from extrusion-molded polychloroprene, but Patent Document 2 is also a document related to odor countermeasures and does not describe the functions of molded products obtained from chloroprene rubber. Furthermore, no technology is known for suppressing the crystallization of chloroprene polymers. For this reason, it is currently difficult to prevent the crystallization of chloroprene polymers at low temperatures, and chloroprene rubber that can maintain flexibility even at low temperatures has not yet been obtained. As described above, conventional chloroprene rubber becomes hard due to the progress of crystallization of chloroprene polymers at low temperatures, so there is a problem that gloves, rubber threads, etc. manufactured from conventional chloroprene rubber have a poor feel when used at low temperatures.
[0006] An object of the present invention is to provide a molded product which can maintain its flexibility at low temperatures (e.g., -10°C) and can be suitably used as, for example, gloves, rubber threads, etc. even at low temperatures, and to provide a latex composition which can be used for producing such a molded product. [Means for solving the problem]
[0007] Means for Solving the Problem As a result of intensive research by the present inventors, it was found that a chloroprene rubber produced from a polychloroprene latex composition containing a specific substance does not harden even at low temperatures, and can be formed into a molded product that does not impair the feel when used.
[0008] That is, the present invention relates to the following polychloroprene latex composition.
[0009] [1] A polychloroprene latex composition comprising a chloroprene (co)polymer (A) and an aromatic compound having 7 to 10 carbon atoms (B), The polychloroprene latex composition, wherein the proportion of the aromatic compound (B) having 7 to 10 carbon atoms is 0.0012 to 0.15 parts by mass per 100 parts by mass of the solid content of the polychloroprene latex composition.
[0010] [2] The polychloroprene latex composition according to [1], wherein the aromatic compound (B) having 7 to 10 carbon atoms is a compound in which one or more hydrogen atoms bonded to an aromatic ring are substituted with a chlorine atom or a substituent containing a chlorine atom.
[0011] [3] The polychloroprene latex composition according to [1] or [2], wherein the aromatic compound (B) having 7 to 10 carbon atoms is a di-substituted aromatic compound.
[0012] [4] The polychloroprene latex composition according to any one of [1] to [3], wherein the aromatic compound (B) having 7 to 10 carbon atoms has a molecular weight of 100 to 200.
[0013] [5] The polychloroprene latex composition according to any one of [1] to [4], comprising 4-chlorovinylbenzene as the aromatic compound (B) having 7 to 10 carbon atoms.
[0014] [6] The polychloroprene latex composition according to any one of [1] to [5], wherein the aromatic compound (B) having 7 to 10 carbon atoms contains at least one of 2-methylbenzyl chloride and 3-methylbenzyl chloride.
[0015] [7] The polychloroprene latex composition according to any of [1] to [6], wherein a ratio of the chloroprene (co)polymer (A) is 40 to 99.9 parts by mass per 100 parts by mass of a solid content of the polychloroprene latex composition.
[0016] [8] The polychloroprene latex composition according to any one of [1] to [7], further containing a vulcanization accelerator, a metal oxide, and an antioxidant.
[0017] [9] The polychloroprene latex composition according to any one of [1] to [8], further comprising a tackifier.
[0018]
[10] A dipping product obtained by molding the polychloroprene latex composition according to any one of [1] to [8] by a dipping method and curing it.
[0019]
[11] A pressure-sensitive adhesive comprising the polychloroprene latex composition according to any one of [1] to [9].
[0020]
[12] An adhesive comprising the polychloroprene latex composition according to any one of [1] to [9].
[0021]
[13] An adhesive product comprising: a first adherend; a layer of solid content of the polychloroprene latex composition according to any one of [1] to [9] adhered to a part of the first adherend; and a second adherend laminated on the layer of solid content. Effect of the Invention
[0022] It is possible to provide a molded product which can maintain flexibility even at low temperatures and is suitable for use in, for example, gloves, rubber threads, etc., and a latex composition which can be used for producing such molded products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described in detail below, but the present invention is not limited to the configuration of the following embodiment. In the claims and the description of this specification, the term "to" specifying a numerical range means a value equal to or greater than the lower limit and equal to or less than the upper limit.
[0024] <Polychloroprene latex composition> The polychloroprene latex composition of the present invention contains at least a chloroprene (co)polymer (A) and an aromatic compound (B) having 7 to 10 carbon atoms. The proportion of the aromatic compound (B) having 7 to 10 carbon atoms is 0.0012 to 0.15 parts by mass when the solid content of the polychloroprene latex composition is 100 parts by mass. In the following description, the aromatic compound (B) having 7 to 10 carbon atoms may be simply referred to as "aromatic compound (B)". The polychloroprene latex composition may be produced by adding the aromatic compound (B) to polychloroprene latex. The polychloroprene latex composition may also be produced by emulsion polymerization of monomers constituting the chloroprene (co)polymer (A) under conditions in which the aromatic compound (B) is produced as a by-product. In this specification, only polychloroprene latex or polychloroprene latex to which aromatic compound (B) is added is referred to as "polychloroprene latex composition a". On the other hand, one to which at least one of tackifier, surfactant (other than that used in polymerization of chloroprene (co)polymer (A)), vulcanization accelerator, metal oxide such as zinc oxide dispersion, acid acceptor, antioxidant, filler, pigment, colorant, wetting agent, defoamer, thickener, etc. is added is referred to as "polychloroprene latex composition b".
[0025] [Polychloroprene latex] Polychloroprene latex is a latex in which a chloroprene (co)polymer (A) is dispersed in a dispersion medium such as water. The chloroprene (co)polymer (A) is a polymer whose main monomer component is 2-chloro-1,3-butadiene (hereinafter also referred to as "chloroprene"). Specifically, (1) 2-chloro-1,3-butadiene (A-1) homopolymer, (2) Copolymer of 2-chloro-1,3-butadiene (A-1) and 2,3-dichloro-1,3-butadiene (A-2) (3) A copolymer of 2-chloro-1,3-butadiene (A-1), 2,3-dichloro-1,3-butadiene (A-2), and a monomer (A-3) described below, and (4) Copolymer of 2-chloro-1,3-butadiene (A-1) and monomer (A-3) described later or a mixture of two or more of the above (1) to (4). In the present invention, the "polychloroprene latex" refers to a latex in which any one or more of the above (co)polymers (1) to (4) are dispersed in a dispersion medium.
[0026] In the chloroprene (co)polymer (A), the ratio of the mass of the structure (monomer unit) derived from 2-chloro-1,3-butadiene (A-1) to the mass of the monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2) (mass of monomer units derived from (A-1):mass of monomer units derived from (A-2)) is preferably 100:0 to 70:30, more preferably 100:0 to 75:25, and even more preferably 100:0 to 80:20. When the total amount of the monomer units derived from 2-chloro-1,3-butadiene (A-1) and the monomer units derived from 2,3-dichloro-1,3-butadiene (A-2) is taken as 100 parts by mass, if the amount of the monomer units derived from 2-chloro-1,3-butadiene (A-1) is 70 parts by mass or more, the tensile strength of the molded product is good, which is preferable.
[0027] The chloroprene (co)polymer (A) preferably contains a monomer unit derived from 2-chloro-1,3-butadiene (A-1) and a monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2). When the chloroprene (co)polymer (A) contains a monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2), it is preferable because it has excellent flexibility at room temperature (25°C). When the chloroprene (co)polymer (A) contains a monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2), the amount of the monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2) is preferably 0.01 parts by mass or more, more preferably 5 parts by mass or more, when the total of the monomer unit derived from 2-chloro-1,3-butadiene (A-1) and the monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2) is taken as 100 parts by mass. When the amount of the monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2) is 30 parts by mass or less, the molded product has excellent flexibility, which is preferable. The flexibility of the molded product is measured by the durometer hardness A in the examples described later, and the durometer hardness A is preferably 20 to 65, more preferably 20 to 60, so that the molded product has excellent flexibility.
[0028] The chloroprene (co)polymer (A) may contain a monomer unit derived from a monomer (A-3) in addition to a monomer unit derived from 2-chloro-1,3-butadiene (A-1) and an optional monomer unit derived from 2,3-dichloro-1,3-butadiene (A-2). Here, the monomer (A-3) is a monomer other than 2-chloro-1,3-butadiene (A-1) and 2,3-dichloro-1,3-butadiene (A-2) and is copolymerizable with at least one of 2-chloro-1,3-butadiene (A-1) and 2,3-dichloro-1,3-butadiene (A-2). The monomer (A-3) may be a monomer copolymerizable with both 2-chloro-1,3-butadiene (A-1) and 2,3-dichloro-1,3-butadiene (A-2). However, the monomer (A-3) does not include a compound corresponding to the aromatic compound (B) described later. Examples of the monomer (A-3) include 1-chloro-1,3-butadiene, butadiene, isoprene, styrene, acrylonitrile, acrylic acid and its esters, methacrylic acid and its esters, etc. The chloroprene (co)polymer (A) may contain structures derived from two or more types of monomers as structures derived from the monomer (A-3) as necessary.
[0029] In the chloroprene (co)polymer (A), the ratio of the mass of the monomer units derived from 2-chloro-1,3-butadiene (A-1) to the mass of the monomer units derived from the monomer (A-3) (mass of the monomer units derived from (A-1):mass of the monomer units derived from (A-3)) is preferably 100:0 to 90:10, more preferably 100:0 to 92:8, and even more preferably 100:0 to 94:6. When the chloroprene (co)polymer (A) contains monomer units derived from monomer (A-3), the amount of monomer units derived from monomer (A-3) is 0.01 parts by mass or more when the total of monomer units derived from 2-chloro-1,3-butadiene (A-1) and monomer units derived from monomer (A-3) is 100 parts by mass. When the ratio of monomer units derived from monomer (A-3) is 10 parts by mass or less, the molded product has good tensile strength and elongation, and the molded product has good flexibility stability over time.
[0030] <Production method of polychloroprene latex> The polychloroprene latex is preferably produced by radically polymerizing a monomer in an aqueous emulsion, which produces a polychloroprene latex in which particles of a chloroprene (co)polymer (A) are dispersed in a dispersion medium such as water.
[0031] Anionic surfactants are preferred as emulsifiers in emulsion polymerization. Examples of anionic surfactants include rosin acid soap, sodium salt of naphthalenesulfonic acid condensate, sodium salt of dodecylbenzenesulfonic acid, and sodium salt of dodecylsulfuric acid. For dipping product applications, a normal rosin acid soap can be used, particularly because of the ease of the coagulation operation. In particular, it is preferred to use sodium or potassium salt of disproportionated rosin acid, from the viewpoint of color stability.
[0032] The amount of the emulsifier used is preferably 1 to 30 parts by mass when the total of all monomers including 2-chloro-1,3-butadiene (A-1), 2,3-dichloro-1,3-butadiene (A-2), and monomer (A-3) is taken as 100 parts by mass. When the amount of the emulsifier used is 1 part by mass or more, emulsification failure is unlikely to occur, heat generation due to polymerization can be controlled, and the formation of aggregates is suppressed, so that the appearance of the molded product obtained from the polychloroprene latex tends to be good. When the amount of the emulsifier used is 30 parts by mass or less, adhesion of the chloroprene (co)polymer (A) caused by the emulsifier remaining in the polychloroprene latex is unlikely to occur, and poor peeling from the mold (former) used to obtain the molded product and adhesion of the surface of the molded product are unlikely to occur, so that deterioration of processability and operability is unlikely to occur, and deterioration of the color tone of the product is unlikely to occur, which is preferable. In addition, two or more kinds of surfactants as emulsifiers may be used as appropriate.
[0033] The chain transfer agent is not particularly limited, but xanthogen disulfide and alkyl mercaptan can be used. The alkyl mercaptan can be n-dodecyl mercaptan, n-decyl mercaptan, octyl mercaptan, or tert-dodecyl mercaptan. The xanthogen disulfide can be diisopropyl xanthogen disulfide, diethyl xanthogen disulfide, or the like. The amount of the chain transfer agent used cannot be generally determined because it varies depending on the type of chain transfer agent, the amount of 2,3-dichloro-1,3-butadiene (A-2) used, the polymerization conversion rate, and the polymerization temperature. For example, when n-dodecyl mercaptan is used, the amount is preferably in the range of 0.03 to 0.2 parts by mass, and more preferably in the range of 0.06 to 0.15 parts by mass, when the total amount of all monomers including 2-chloro-1,3-butadiene (A-1), 2,3-dichloro-1,3-butadiene (A-2), and monomer (A-3) is 100 parts by mass.
[0034] When producing polychloroprene latex, the polymerization conversion rate is preferably 80 to 100%. If the polymerization conversion rate is 80% or more, the solid content of the polychloroprene latex is sufficient, so that molding such as filming is easy and pinholes and cracks are unlikely to occur in the molded product, which is preferable. Here, the solid content of the polychloroprene latex is a component obtained by removing a dispersion medium such as water from the polychloroprene latex, and is a component obtained by drying the polychloroprene latex by leaving it in an oven at 141°C for 30 minutes. When the aromatic compound (B) is produced as a by-product of the chloroprene (co)polymer (A) simultaneously with emulsion polymerization as described below, a polymerization conversion rate of 90% or more is more preferable since it facilitates the production of the aromatic compound (B).
[0035] As the polymerization initiator, a general radical polymerization initiator can be used, and there is no particular limitation. In the case of emulsion polymerization, organic or inorganic peroxides such as benzoyl peroxide, potassium persulfate, ammonium persulfate, and azo compounds such as azobisisobutyronitrile are preferred. The polymerization initiator may be used alone or in combination of two or more kinds.
[0036] When polymerizing the chloroprene (co)polymer (A), a cocatalyst may be used together with the polymerization initiator, if desired. The cocatalyst that can be used together with the polymerization initiator is not particularly limited, and a general cocatalyst can be used. For example, a cocatalyst such as anthraquinone sulfonate, potassium sulfite, or sodium sulfite can be used in combination as appropriate. The cocatalyst may be used alone or in combination of two or more kinds.
[0037] The polymerization temperature of the chloroprene (co)polymer (A) is preferably 30 to 55°C, and more preferably in the range of 35 to 50°C. If the polymerization temperature is 30°C or higher, aromatic compounds (B) tend to be easily generated as by-products of the chloroprene (co)polymer (A). The reaction in generating the aromatic compounds (B) will be described later. If the polymerization temperature is 55°C or lower, the vapor pressure of 2-chloro-1,3-butadiene (A-1) is appropriate, so that the polymerization operation is easy, and the mechanical properties such as tensile strength of the molded product obtained by molding the chloroprene (co)polymer (A) tend to be good. The polymerization time in the emulsion polymerization is preferably 5 to 25 hours. If the polymerization temperature and polymerization time in the emulsion polymerization are in the above ranges, it is preferable because the desired polymerization conversion rate is obtained.
[0038] Usually, in the production of polychloroprene latex, it is preferable to add a polymerization terminator at the time when a predetermined polymerization conversion rate is reached to terminate the reaction in order to obtain a chloroprene (co)polymer (A) having a desired molecular weight and molecular weight distribution. A polymerization terminator may also be used in the embodiment of the present invention. There is no particular limitation on the polymerization terminator that can be used, and a commonly used terminator such as phenothiazine, para-t-butylcatechol, hydroquinone, hydroquinone monomethyl ether, diethylhydroxylamine, etc. may be used. The polymerization terminator may be used alone or in combination of two or more kinds.
[0039] [Aromatic compounds with 7 to 10 carbon atoms (B)] The polychloroprene latex composition of the present invention contains at least one aromatic compound (B) having 7 to 10 carbon atoms. Examples of the aromatic compound (B) include toluene, o-xylene, m-xylene, p-xylene, vinylbenzene, 2-ethyltoluene, 3-ethyltoluene, 4-ethyltoluene, cumene, 2-propyltoluene, 3-propyltoluene, 4-propyltoluene, 1,2-diethylbenzene, 1,3-diethylbenzene, and 1,4-diethylbenzene, and one or more of the hydrogen atoms may be substituted with a halogen (chlorine atom, bromine atom, iodine atom, or fluorine atom), a hydroxyl group, an amino group, a nitro group, a carbonyl group, a carboxyl group, or an isocyanato group. The aromatic compound (B) also includes compounds in which the number of carbon atoms in the aromatic compound before being substituted with a substituent containing a carbon atom is 6, such as salicylic acid and acetophenone.
[0040] The aromatic compound (B) having 7 to 10 carbon atoms is preferably a compound in which one or more hydrogen atoms bonded to an aromatic ring are substituted with a chlorine atom or a substituent containing a chlorine atom, more preferably a disubstituted compound in which one or more hydrogen atoms are substituted with a chlorine atom or a substituent containing a chlorine atom, still more preferably a xylene derivative substituted with a chlorine atom or a substituent containing a chlorine atom, particularly preferably any one of 4-chlorovinylbenzene, 2-methylbenzyl chloride, 3-methylbenzyl chloride, and 4-methylbenzyl chloride, and even more preferably 4-chlorovinylbenzene. The molecular weight of the aromatic compound (B) is preferably 100-200, more preferably 120-180, and further preferably 130-150, in order to achieve good compatibility with the chloroprene (co)polymer (A).
[0041] The amount of the aromatic compound (B) in the polychloroprene latex composition a is 0.0012 to 0.15 parts by mass, preferably 0.002 to 0.12 parts by mass, and more preferably 0.05 to 0.1 parts by mass, based on 100 parts by mass of the solid content of the polychloroprene latex composition a. When the amount of the aromatic compound (B) is 0.0012 parts by mass or more, the aromatic compound (B) can prevent the crystallization of the chloroprene (co)polymer (A) in a molded product produced from the polychloroprene latex composition, so that an increase in hardness of the molded product is suppressed even at low temperatures. Here, the solid content of the polychloroprene latex composition a is a value obtained by multiplying the mass of the polychloroprene latex itself or, when an aromatic compound (B) is added, the mass of the polychloroprene latex to which the aromatic compound (B) has been added (polychloroprene latex composition a) by the solid content rate determined by the method described in the Examples described later. Therefore, when calculating the solid content of the polychloroprene latex composition a, the contents of tackifiers, surfactants (other than those used in the polymerization of the chloroprene (co)polymer (A)), vulcanization accelerators, metal oxides such as zinc oxide dispersions, acid acceptors, antioxidants, fillers, pigments, colorants, wetting agents, defoamers, thickeners, etc. are not used.
[0042] When the aromatic compound (B) is added, the aromatic compound (B) can be added to the starting material for producing the polychloroprene latex before the polymerization of the chloroprene (co)polymer (A). The aromatic compound (B) can also be added to the polychloroprene latex after the polymerization of the chloroprene (co)polymer (A). Only the aromatic compound (B) having a group copolymerizable with 2-chloro-1,3-butadiene (A-1), 2,3-dichloro-1,3-butadiene (A-2), or the monomer (A-3) is added to the polychloroprene latex after the polymerization of the chloroprene (co)polymer (A) to prevent the aromatic compound (B) from being polymerized in the chloroprene (co)polymer (A). In addition, the aromatic compound (B) can be produced as a by-product from a monomer or the like used in the polymerization of the chloroprene (co)polymer (A) as a side reaction when the polymerization of the chloroprene (co)polymer (A) is carried out under certain conditions.
[0043] [Adhesives, adhesives, and adhesive products] The polychloroprene latex composition of the present embodiment thus obtained can be used not only for producing dipped products such as gloves, rubber threads, breathing bags, and blood pressure gauge bladders as described later, but also as a pressure-sensitive adhesive. Note that the pressure-sensitive adhesive refers to a pressure-sensitive adhesive and an adhesive. Furthermore, the polychloroprene latex composition is applied to a part or the whole surface of an adherend, and the polychloroprene latex composition is dried on the surface of the adherend to form a layer of solid content of the polychloroprene latex composition, thereby obtaining an adherend with an adhesive layer. Examples of the adherend include any material to which the polychloroprene latex composition can be applied, such as urethane foam, foam, sheet, film, canvas, glass, etc. A bonded product can also be produced by laminating a plurality of adherends via the polychloroprene latex composition. Here, the plurality of adherends may be the same type of adherend, or one of the adherends (hereinafter also referred to as the "first adherend") may be a different type of adherend from the other adherend (hereinafter also referred to as the "second adherend"). When producing a bonded product, one of the adherends to be laminated can be made into an adherend with an adhesive layer by producing an adhesive layer on the surface of the adherend, and then the other adherend can be laminated. Alternatively, a bonded product can be produced by providing an adhesive layer on both of the adherends to be bonded, and then laminating the adhesive layers of the adherends to bond them. Examples of bonded products include furniture, shoes, and the like.
[0044] [Other ingredients that may be included in the composition] When the polychloroprene latex composition of the present embodiment is used as a pressure-sensitive adhesive or a bonding agent, a tackifier can be added to the polychloroprene latex composition. Although the polychloroprene latex composition a to which no tackifier is added can also be used as a pressure-sensitive adhesive or a bonding agent, the addition of a tackifier can improve the adhesive strength of the polychloroprene latex composition to provide a pressure-sensitive adhesive or a bonding agent having high adhesive strength.
[0045] The type of tackifier is not particularly limited, but phenolic resins, terpene resins, rosin derivative resins, petroleum hydrocarbons, etc. can be used as tackifiers, and specific examples include hydrogenated rosin, pentaerythritol esters of hydrogenated rosin, polymerized rosin, rosin-modified resins containing rosin as the main component, alkylphenol resins, rosin-modified phenolic resins, terpene-modified phenolic resins, and natural terpene resins. One type of tackifier may be used alone, or two or more types may be used in combination.
[0046] The amount of the tackifier added is usually 10 to 60 parts by mass, preferably 20 to 40 parts by mass, based on 100 parts by mass of the solid content of the polychloroprene latex calculated from the solid content rate calculated by the method described in the examples described later and the mass of the polychloroprene latex. If the amount of the tackifier added is within the above range, the adhesion of the polychloroprene latex composition is sufficiently ensured, and the adhesive strength of the polychloroprene latex composition is sufficiently improved. The method of adding the tackifier is not particularly limited, but the tackifier may be added to the polychloroprene latex composition in the form of an emulsion in which the tackifier is emulsified and dispersed.
[0047] Furthermore, a pressure-sensitive adhesive can be obtained by further adding, as necessary, a surfactant, a vulcanization accelerator, a metal oxide such as a zinc oxide dispersion, an acid acceptor, an antioxidant, a filler, a pigment, a colorant, a wetting agent, an antifoaming agent, a thickener, or the like to the polychloroprene latex composition a of the present embodiment. Regardless of whether the polychloroprene latex composition a contains the above-mentioned addable substances such as a tackifier and a surfactant, the proportion of the chloroprene (co)polymer (A) in the polychloroprene latex composition a is preferably 30 to 99.9 parts by mass, more preferably 40 to 98 parts by mass, and particularly preferably 50 to 95 parts by mass, based on 100 parts by mass of the solid content of the polychloroprene latex composition a. Here, the solid content of the polychloroprene latex composition a refers to a component obtained by drying the polychloroprene latex composition a by leaving it in an oven at 141°C for 30 minutes, and is a component obtained by removing a dispersion medium such as water from the polychloroprene latex composition.
[0048] [Molded product] A dipping product can be obtained from the polychloroprene latex composition b according to the embodiment by a dipping processing method. That is, a mold for molding is immersed in the polychloroprene latex composition b according to the present invention, and the solid content of the polychloroprene latex composition b is precipitated on the surface of the mold for molding to form a molded product, and the molded solid content is dried and then cured to obtain a molded product. It is preferable that a coagulant is attached to the surface of the mold to be immersed in the polychloroprene latex composition b. The molded solid content can be dried, for example, by leaving it to stand in an oven at 25 to 80°C for 5 minutes to 24 hours. Before the immersion process, the polychloroprene latex composition b according to the present embodiment may be aged under a predetermined condition. The temperature condition for aging is preferably 15 to 40°C, and the aging time is preferably 15 to 72 hours. For example, a condition of aging at 23°C for 20 hours may be used. When the aromatic compound (B) is added after the production of the polychloroprene latex, the aging starts when all the substances to be blended, such as the polychloroprene latex, the aromatic compound (B), and an optional vulcanization accelerator, are mixed. On the other hand, when the aromatic compound (B) is added before the production of the polychloroprene latex, and when the aromatic compound (B) is generated as a by-product of the chloroprene (co)polymer (A), the aging starts when the polymerization of the polychloroprene latex is stopped, or when all the substances to be blended in the polychloroprene latex composition, including an optional vulcanization accelerator, are mixed, whichever is later. After maturation, the steps of immersion / coagulation, drying, and vulcanization (curing) are carried out in this order to obtain a film-like molded product.
[0049] The immersion and coagulation treatment can be carried out by submerging a plate or mold coated with a coagulant in the polychloroprene latex composition b for a predetermined period of time, and depositing the solid content in the polychloroprene latex composition b, such as the chloroprene (co)polymer (A), on the surface of the plate or mold. This is presumably because, in the polychloroprene latex, fine particles covered with a film of an emulsifier having surface activity are formed, and the film of the fine particles is destroyed by the action of the coagulant attached to the surface of the plate or mold, causing the chloroprene (co)polymer (A) and the like in the fine particles to adhere to the surface of the plate or mold. As the coagulant, a metal salt, for example, a metal nitrate, can be used. In order to avoid appearance problems of molded products, such as the formation of blisters, pinholes, etc., a drying step (rough drying step) may be carried out at a relatively low temperature of 65° C. or more and 100° C. or less before the vulcanization treatment. Regardless of whether or not the rough drying step is carried out, the drying step is carried out before the vulcanization treatment.
[0050] The vulcanization temperature in the vulcanization treatment can be, for example, 110 to 140° C. For example, the solid content in the polychloroprene latex composition b deposited by the immersion and coagulation treatment can be vulcanized at 130° C. in air. The vulcanization time in the above vulcanization temperature range can be, for example, 15 to 90 minutes, but it is preferable to perform the vulcanization treatment sufficiently within a range in which the tensile strength and tensile elongation of the molded product are not deteriorated. For example, the solid matter deposited on the surface of a plate or a mold can be vulcanized under the above-mentioned conditions to obtain a molded product.
[0051] In the molded product obtained from the polychloroprene latex composition b according to the present invention, the aromatic compound (B) prevents the crystallization of the chloroprene (co)polymer (A) even at low temperatures, so that an increase in hardness of the molded product containing the chloroprene (co)polymer (A) is suppressed. This is presumably because the aromatic compound (B) disrupts the regularity of the crystals of the chloroprene (co)polymer (A). Therefore, the molded product obtained from the polychloroprene latex composition according to the present invention can maintain its flexibility even at low temperatures. As a result, when the molded product is a glove, the comfort of the user is not deteriorated even at low temperatures. In addition, when the molded product is a blood pressure bladder, a breathing bag, rubber thread, or the like, the user can feel good when using the product even at low temperatures.
[0052] [Use of molded product] The molded product can be suitably used as gloves, particularly disposable medical gloves, blood pressure monitor bladders, breathing bags, rubber threads, etc. The modulus (M500) at 500% elongation, tensile strength, elongation at break, and durometer hardness A at low temperature of the molded product can be measured by the methods employed in the examples described later.
[0053] The modulus at 500% elongation of the molded product is preferably 1.0 to 5.0 MPa, more preferably 2.0 to 4.0 MPa, from the viewpoint of the feeling when used in gloves or the like. The tensile strength of the molded product is preferably 15 to 40 MPa, more preferably 17 to 30 MPa, in terms of resistance to breakage. The elongation at break of the molded product is preferably 500 to 1500%, more preferably 700 to 1200%, in terms of resistance to breakage. The change over time in durometer hardness A of the molded product at low temperature (-10°C) is preferably 10 to 30, and more preferably 15 to 25, in terms of embrittlement at low temperatures. EXAMPLES
[0054] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. First, methods for measuring and calculating physical properties of polychloroprene latex and polychloroprene latex composition will be described, and then individual examples will be described.
[0055] <Calculation method of polymerization conversion rate> The emulsion after the initiation of polymerization of chloroprene (co)polymer (A) was collected and dried by standing in an oven at 141°C for 30 minutes to obtain a dry solid. The dry solid obtained by the drying process contains chloroprene (co)polymer (A) and solids other than chloroprene (co)polymer (A). Therefore, the mass of the solids other than chloroprene (co)polymer (A) was calculated from the amount of polymerization raw materials charged, and was taken as the mass of the solids other than chloroprene (co)polymer (A) from the mass of the dry solid obtained by drying the emulsion after the initiation of polymerization. The polymerization conversion rate was calculated by formula (1) using the value obtained by subtracting the mass of the solids other than chloroprene (co)polymer (A) from the mass of the dry solid obtained by drying the emulsion after the initiation of polymerization as the "amount of chloroprene (co)polymer (A) produced." Polymerization conversion rate (%) = [(amount of chloroprene (co)polymer (A) produced) / (mass of all monomers charged)] × 100 (1) The "feed mass of all monomers" in formula (1) is the sum of the feed amount of 2-chloro-1,3-butadiene (A-1) contained in the amount of emulsion collected to obtain a dry product, and optionally the feed amounts of 2,3-dichloro-1,3-butadiene (A-2) and monomer (A-3).
[0056] <Solid content of polychloroprene latex (polychloroprene latex composition a) (by measurement)> A predetermined amount of polychloroprene latex (or polychloroprene latex composition a, the same applies below) was collected, and the mass of the collected polychloroprene latex was weighed. The weighed polychloroprene latex was then left to stand in an oven at 141°C for 30 minutes to dry and obtain a dried product. The solid content was calculated according to formula (2) from the mass of the latex before drying and the mass of the solid content obtained after drying. Solid content (mass%) = [(mass of solids after drying) / (mass of latex before drying)] × 100 (2)
[0057] <Content of aromatic compound (B) in polychloroprene latex composition> 2 mL (about 2.1 to 2.2 g) of the polychloroprene latex composition was placed in a 20 mL headspace vial, sealed, and heated to 100° C. for 60 minutes while shaking. The outgassing was then measured by GCMS using an autosampler. The measurement conditions were as follows: {Measurement conditions} GC: Agilent 6890N MS: JEOL Automass II Column: Agilent Technologies DB-624 320μm×30m (film thickness) 1.8μm Mobile phase: He 2.2ml / min constant flow Injection volume: 1.0mL Inlet temperature: 250℃ Injection method: Split injection method (split ratio 5:1) Analysis time: 60 minutes Interface temperature: 250℃ Ion source temperature: 200℃ Column temperature conditions: 40°C (20 min) → 240°C (20 min) (heating condition at this time is +10°C / min) Measurement mode: SCAN (m / z=35-300) Ionization method: EI Acceleration voltage: 70 eV Detector voltage: 500V Ionization current: 300μA
[0058] [Example 1] Preparation of polychloroprene latex (A1) and addition of aromatic compound (B) In a 5-liter glass reactor, 2.0 kg (100 parts by mass) of 2-chloro-1,3-butadiene (A-1) (manufactured by Tokyo Chemical Industry Co., Ltd.), 1.6 kg (80 parts by mass) of pure water, 80 g (4 parts by mass) of rosin acid (manufactured by Arakawa Chemical Industries Co., Ltd., R-300), 2 g (0.1 parts by mass) of n-dodecyl mercaptan (manufactured by Tokyo Chemical Industry Co., Ltd.), 100 g (5 parts by mass) of 20% by mass potassium hydroxide aqueous solution (manufactured by Wako Pure Chemical Industries Co., Ltd., special grade), and 16 g (0.8 parts by mass) of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation) were charged. The starting materials charged in the reactor were emulsified, and the rosin acid was converted into rosin acid soap.
[0059] 2-chloro-1,3-butadiene (A-1) was blended as a raw monomer for chloroprene polymer, and pure water was blended as a dispersion medium for emulsion polymerization. n-Dodecyl mercaptan was blended as a chain transfer agent, rosin acid and potassium hydroxide were blended as raw materials for emulsifier, and sodium salt of β-naphthalenesulfonic acid formalin condensate was blended as emulsifier. However, the blended amount of potassium hydroxide was 100g (5 parts by mass) as a 20% by mass aqueous solution, so the amount of potassium hydroxide was 20g (1 part by mass).
[0060] Potassium persulfate (first-class product manufactured by Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to the emulsion obtained by emulsifying the starting material, and polymerization was carried out for 7 hours at a temperature of 40°C under a nitrogen gas atmosphere. The polymerization was stopped when it was confirmed that the polymerization conversion rate of the monomer was 88%. Next, the unreacted monomer was removed by steam distillation. When the amount of 2-chloro-1,3-butadiene (A-1) charged in the reactor was 100 parts by mass, 0.005 parts by mass of 4-chlorovinylbenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.005 parts by mass of 2-methylbenzyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to the obtained polychloroprene latex (A1), thereby obtaining a polychloroprene latex composition (A1a). That is, 0.10 g each of 4-chlorovinylbenzene and 2-methylbenzyl chloride was added to the polychloroprene latex composition (A1a). The measured solid content of the polychloroprene latex (A1a) was 49.2% by mass.
[0061] The polychloroprene latex composition (A1a) obtained by the above method was analyzed by GCMS, and the ratio of the peak area of the reference S (retention time: 1 minute 34 seconds) to the peak area of 4-chlorovinylbenzene (retention time: 31 minutes 48 seconds) was 0.028, and the ratio of the peak area of the reference S to the peak area of 2-methylbenzyl chloride (retention time: 33 minutes 46 seconds) was 0.118. The obtained peak area ratios are shown in Table 1.
[0062] The content ratio of the aromatic compound (B) relative to the solid content of the polychloroprene latex composition (A1a) was calculated based on the solid content ratio of the polychloroprene latex composition (A1a) measured by the above-mentioned measurement method and the added amounts of 4-chlorovinylbenzene and 2-methylbenzyl chloride. The ratio of 4-chlorovinylbenzene to 100 parts by mass of the solid content of the polychloroprene latex composition (A1a) was 0.0053 parts by mass, and the ratio of 2-methylbenzyl chloride was 0.0053 parts by mass.
[0063] <Preparation of Chloroprene Copolymer Latex Composition b> In a stirring tank equipped with a three-one motor, the polychloroprene latex composition (A1a), surfactant, vulcanization accelerator, zinc oxide, and phenol-based antioxidant dispersion were charged in the amounts shown below and stirred for 30 minutes. Hereinafter, the obtained composition is referred to as polychloroprene latex composition (A1b). Solid content of polychloroprene latex composition (A1a) 100 parts by mass Surfactant 1) 1 part by weight Vulcanization accelerator 2) 1 part by mass Vulcanization accelerator 3) 1 part by mass Zinc oxide dispersion 4) 5 parts by weight Phenolic antioxidant dispersion 5) 2 parts by weight The substances used as the surfactant, vulcanization accelerator, zinc oxide, and phenol-based antioxidant dispersion are as follows: Surfactant 1): Sodium alkyl sulfate, Darvan WAQ, manufactured by RT Vanderbilt Co., Ltd. Vulcanization accelerator 2) Noccelaer (registered trademark) C, N,N'-diphenylthiourea, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 3) Noccelaer (registered trademark) D, 1,3-diphenylguanidine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Zinc oxide dispersion 4) Osaki Kogyo Co., Ltd., ZnO, AZ-SW Phenolic antioxidant dispersion 5) Oligomeric hindered phenol (butylated reaction product of DCPD and p-cresol), K-840 (Wingstay L dispersion), manufactured by Chukyo Yushi Co., Ltd.
[0064] In addition, since zinc oxide AZ-SW and the phenol-based antioxidant K-840 are in the form of a dispersion in which the active ingredients, zinc oxide and antioxidant, are dispersed in a liquid medium, the amounts of zinc oxide AZ-SW and the phenol-based antioxidant K-840 charged above are the amounts of only the active ingredients of zinc oxide AZ-SW and K-840 charged.
[0065] In the polychloroprene latex composition (A1b), a total of 10 parts by mass of surfactant, vulcanization accelerator, zinc oxide, and phenol-based antioxidant are blended with respect to 100 parts by mass of the solid content of the polychloroprene latex composition (A1a), and the total solid content is 110 parts by mass. Therefore, the ratio of the aromatic compound (B) in the polychloroprene latex composition (A1b) was calculated as 1 / 1.1 of the ratio of the aromatic compound (B) in the polychloroprene latex composition (A1a). The ratio of 4-chlorovinylbenzene in the polychloroprene latex composition (A1b) is 0.0048 parts by mass with respect to 100 parts by mass of the solid content of the polychloroprene latex composition (A1b). Similarly, the ratio of 2-methylbenzyl chloride is also 0.0048 parts by mass with respect to 100 parts by mass of the solid content of the polychloroprene latex composition (A1b). The proportion of the aromatic compound (B) in the polychloroprene latex composition (A1b) is shown in Table 1.
[0066] <Film Preparation> First, a ceramic plate 200 mm long, 100 mm wide, and 5 mm thick was prepared as a mold for the chloroprene (co)polymer film. This mold was immersed in a 30% by mass calcium nitrate aqueous solution, then removed and dried in an oven at 40°C for 5 minutes to adhere calcium nitrate, which acts as a coagulant, to the surface of the mold.
[0067] Further, the dried mold was immersed in the polychloroprene latex composition (A1b) to deposit the solid content of the polychloroprene latex composition (A1b) on the surface of the mold. After the mold was removed from the chloroprene copolymer latex composition, it was dried in an oven at 70° C. for 30 minutes. Thereafter, leaching was carried out for 2 minutes to remove water-soluble components from the solid content of the deposited polychloroprene latex composition (A1b), and the composition was further dried in an oven at 70° C. for 30 minutes.
[0068] Next, the mold with the solid matter deposited on the surface was heated in an oven at 130°C for 60 minutes to vulcanize and harden the solid matter of the polychloroprene latex composition (A1b) deposited on the surface of the mold. After cooling in the air, the hardened molded product on the surface of the mold was cut into a desired shape and size to obtain a film as a vulcanized molded product.
[0069] <Tensile test of molded product obtained by vulcanization treatment> According to JIS-K6301-1995, the vulcanized film was cut into test dumbbells to obtain test pieces. Tensile tests were performed on the film test pieces according to JIS-K6301-1995 to measure the modulus (M500) at 500% elongation at room temperature (23°C), tensile strength, and elongation at break. The results are shown in Table 1.
[0070] <Hardness measurement of molded products obtained by vulcanization treatment> The test piece was placed in a low-temperature chamber at -10°C, and the hardness of the test piece was measured immediately after placing the test piece and after leaving it to stand for 24 hours using a surface hardness durometer hardness A in accordance with JIS K6253-2012. The results are shown in Table 1.
[0071] [Example 2] Polymerization of chloroprene (co)polymer (A) was started under the same conditions as in Example 1, and the polymerization reaction was stopped after 7 hours. The polymerization conversion rate of the monomer was 88%. Unreacted monomers were removed by steam distillation to obtain polychloroprene latex (A2). When the amount of 2-chloro-1,3-butadiene (A-1) charged in the reactor was 100 parts by mass, 0.005 parts by mass of 2-methylbenzyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.005 parts by mass of 3-methylbenzyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) were blended with the obtained polychloroprene latex (A2) to obtain a polychloroprene latex composition (A2a). That is, 0.10 g each of 2-methylbenzyl chloride and 3-methylbenzyl chloride was added to the polychloroprene latex composition (A2a). Therefore, the proportion of 2-methylbenzyl chloride and the proportion of 3-methylbenzyl chloride are both 0.0053 parts by mass when the solid content of the polychloroprene latex composition (A2a) is taken as 100 parts by mass.
[0072] The polychloroprene latex composition (A2a) obtained by the above method was analyzed by GCMS under the same conditions as in Example 1. As a result, the ratio of the peak area of the reference S (retention time: 1 minute 34 seconds) to the peak area of 2-methylbenzyl chloride (retention time: 33 minutes 46 seconds) was 0.117, and the ratio of the peak area of the reference S to the peak area of 3-methylbenzyl chloride (retention time: 34 minutes 05 seconds) was 0.031.
[0073] A surfactant, a vulcanization accelerator, zinc oxide, and a phenol-based antioxidant dispersion were added to the polychloroprene latex composition (A2a) obtained by the above method in the same formulation as in Example 1, and a polychloroprene latex composition (A2b) was prepared in the same manner as in Example 1. Furthermore, using the polychloroprene latex composition (A2b), a film and a test piece were produced in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1. When the ratios of 2-methylbenzyl chloride and 3-methylbenzyl chloride were calculated in the same manner as in Example 1, each of 2-methylbenzyl chloride and 3-methylbenzyl chloride was 0.0048 parts by mass relative to 100 parts by mass of the solid content of the polychloroprene latex composition (A1b).
[0074] [Example 3] The blending of starting materials, emulsification, and addition of a polymerization initiator were carried out under the same conditions as in Example 1. The polymerization of chloroprene (co)polymer (A) was carried out for 24 hours at a temperature of 45°C under a nitrogen gas atmosphere, and then the polymerization was terminated. The polymerization conversion rate at the time of termination of the polymerization was 95%. Next, steam distillation was carried out in the same manner as in Example 1 to obtain a polychloroprene latex (A3).
[0075] When the polychloroprene latex (A3) was analyzed by GCMS under the same conditions as in Example 1, the ratio of the peak area of the reference S (retention time: 1 minute 34 seconds) to the peak area of 4-chlorovinylbenzene (retention time: 31 minutes 48 seconds) was 0.031. In addition, the ratio of the peak area of the reference S to the peak area of 2-methylbenzyl chloride (retention time: 33 minutes 46 seconds) was 0.131, and the ratio of the peak area of the reference S to the peak area of 3-methylbenzyl chloride (retention time: 34 minutes 05 seconds) was 0.035. From this result, since 4-chlorovinylbenzene (molecular weight 140.6 g / mol), 2-methylbenzyl chloride (molecular weight 140.6 g / mol), and 3-methylbenzyl chloride (molecular weight 140.61 g / mol) produced as by-products during polymerization of chloroprene (co)polymer (A) coexist as aromatic compounds (B) in polychloroprene latex (A3), it can be said that polychloroprene latex (A3) is a polychloroprene latex composition. That is, polychloroprene latex (A3) is also a polychloroprene latex composition (A3a).
[0076] Considering that the ratio of the peak area of the peak derived from the aromatic compound (B) to the peak area of the peak derived from the standard sample S is proportional to the content of the aromatic compound (B), the content of the aromatic compound (B) in the polychloroprene latex (A3) can be calculated as follows from the results of Examples 1 and 2 in which the amount of the aromatic compound (B) added is known and the GCMS analysis result: In the following formula, the contents of 4-chlorovinylbenzene and 2-methylbenzyl chloride are calculated using the peak area ratio and the added amount in Example 1, and the content of 3-methylbenzyl chloride is calculated using the peak area ratio and the added amount in Example 2. 4-Chlorovinylbenzene Content = (Peak area ratio to standard sample S in Example 3) / (Peak area ratio to standard sample S in Example 1) × (Amount added in Example 1) =0.031 / 0.028×0.1=0.111(g) 2-Methylbenzyl chloride content =0.131 / 0.118×0.1=0.111(g) 3-Methylbenzyl chloride content = (Peak area ratio to standard sample S in Example 3) / (Peak area ratio to standard sample S in Example 2) × (Amount added in Example 2) =0.035 / 0.031×0.1=0.113(g) Using these values, the content ratio of the aromatic compound (B) in the polychloroprene latex (A3) is calculated in the same manner as in Example 1. The ratio of each substance when the solid content of the polychloroprene latex (A3) is assumed to be 100 parts by mass is as follows. Ratio of 4-chlorovinylbenzene: 0.0055 parts by mass Ratio of 2-methylbenzyl chloride: 0.0055 parts by mass Proportion of 3-methylbenzyl chloride: 0.0056 parts by mass
[0077] A surfactant, a vulcanization accelerator, zinc oxide, and a phenol-based antioxidant dispersion were added to the polychloroprene latex (A3) obtained by the above method in the same formulation as in Example 1, and a polychloroprene latex composition (A3b) was prepared in the same manner as in Example 1. Furthermore, a film and a test piece were produced using the polychloroprene latex composition (A3b) in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1. From the content ratio of the aromatic compound (B) in the polychloroprene latex (A3), the ratio of the aromatic compound (B) in the polychloroprene latex composition (A3b) was calculated in the same manner as in Example 1. When the solid content of the polychloroprene latex composition (A3b) is 100 parts by mass, the ratio of the aromatic compound (B) is as follows. Ratio of 4-chlorovinylbenzene: 0.0050 parts by mass Ratio of 2-methylbenzyl chloride: 0.0050 parts by mass Proportion of 3-methylbenzyl chloride: 0.0051 parts by mass
[0078] [Comparative Example 1] Polymerization of chloroprene (co)polymer (A) was initiated under the same conditions as in Example 1, and polymerization was terminated after 7 hours. The polymerization conversion rate of the monomer was 88%. Unreacted monomer was removed by steam distillation to obtain polychloroprene latex (CA1).
[0079] When polychloroprene latex (CA1) was analyzed by GCMS under the same conditions as in Example 1, the ratio of the peak area of the reference S (retention time: 1 minute 34 seconds) to the peak area of 4-chlorovinylbenzene (retention time: 31 minutes 48 seconds) was 0.002. In addition, the ratio of the peak area of the reference S to the peak area of 2-methylbenzyl chloride (retention time: 33 minutes 46 seconds) was 0.005, and the ratio of the peak area of the reference S to the peak area of 3-methylbenzyl chloride (retention time: 34 minutes 05 seconds) was 0.003.
[0080] Using the GCMS analysis result of the polychloroprene latex (CA1), the content of the aromatic compound (B) in the polychloroprene latex (CA1) was calculated in the same manner as in Example 3, and the following value was obtained. 4-Chlorovinylbenzene content: 0.0071g 2-Methylbenzyl chloride content: 0.0042g 3-Methylbenzyl chloride content: 0.0097g From these values, the contents of the aromatic compound (B) per 100 parts by mass of the solid content of the polychloroprene latex (CA1) are calculated as follows: Ratio of 4-chlorovinylbenzene: 3.8×10 -4 Mass part Ratio of 2-methylbenzyl chloride: 2.2×10 -4 Mass part Ratio of 3-methylbenzyl chloride: 5.2×10 -4 Mass part
[0081] A surfactant, a vulcanization accelerator, zinc oxide, and a phenol-based antioxidant dispersion were added to the polychloroprene latex (CA1) obtained by the above method in the same formulation as in Example 1, and a polychloroprene latex composition (CA1b) was prepared in the same manner as in Example 1. Furthermore, using the polychloroprene latex composition (CA1b), a film and a test piece were produced in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 1. The ratio of the aromatic compound (B) in the polychloroprene latex composition (CA1b) was calculated from the content ratio of the aromatic compound (B) in the polychloroprene latex (CA1) in the same manner as in Example 1. When the solid content of the polychloroprene latex composition (CA1b) is taken as 100 parts by mass, the ratio of the aromatic compound (B) is as follows. Ratio of 4-chlorovinylbenzene: 3.5×10 -4 Mass part Ratio of 2-methylbenzyl chloride: 2.0×10 -4 Mass part Ratio of 3-methylbenzyl chloride: 4.7×10 -4 Mass part
[0082] [Table 1]
[0083] As is clear from Examples 1 to 3, when the aromatic compound (B) is contained in the polychloroprene latex composition, the increase in hardness at low temperatures (-10°C) can be suppressed. Therefore, when the polychloroprene latex composition of the present invention is molded into gloves, the gloves do not become hard even when used in cold regions, and a comfortable feel can be obtained. In addition, even if the gloves are stored at low temperatures, they can be worn immediately after being taken out at room temperature without waiting for them to become soft.
Claims
1. A polychloroprene latex composition comprising a chloroprene (co)polymer (A) and an aromatic compound having 7 to 10 carbon atoms (B), The aromatic compound (B) having 7 to 10 carbon atoms is a compound in which one or more hydrogen atoms bonded to an aromatic ring are substituted with a chlorine atom or a substituent containing a chlorine atom, A polychloroprene latex composition, wherein a ratio of the aromatic compound (B) having 7 to 10 carbon atoms is 0.0012 to 0.15 parts by mass per 100 parts by mass of a solid content of the polychloroprene latex composition.
2. The polychloroprene latex composition according to claim 1, wherein the aromatic compound (B) having 7 to 10 carbon atoms is a di-substituted aromatic compound.
3. The polychloroprene latex composition according to claim 1 or 2, wherein the aromatic compound (B) having 7 to 10 carbon atoms has a molecular weight of 100 to 200.
4. The polychloroprene latex composition according to any one of claims 1 to 3, comprising 4-chlorovinylbenzene as the aromatic compound (B) having 7 to 10 carbon atoms.
5. The polychloroprene latex composition according to any one of claims 1 to 4, wherein the aromatic compound (B) having 7 to 10 carbon atoms contains at least one of 2-methylbenzyl chloride and 3-methylbenzyl chloride.
6. The polychloroprene latex composition according to any one of claims 1 to 5, wherein a ratio of the chloroprene (co)polymer (A) is 40 to 99.9 parts by mass when a solid content of the polychloroprene latex composition is 100 parts by mass.
7. The polychloroprene latex composition according to any one of claims 1 to 6, further comprising a vulcanization accelerator, a metal oxide, and an antioxidant.
8. The polychloroprene latex composition according to any one of claims 1 to 7, wherein the polychloroprene latex composition further comprises a tackifier.
9. A dipped product obtained by molding the polychloroprene latex composition according to any one of claims 1 to 7 by a dipping method and curing the same.
10. A pressure-sensitive adhesive comprising the polychloroprene latex composition according to any one of claims 1 to 8.
11. An adhesive comprising the polychloroprene latex composition according to any one of claims 1 to 8.
12. 9. An adhesive product comprising: a first adherend; a layer of solid content of the polychloroprene latex composition according to any one of claims 1 to 8 adhered to a part of the first adherend; and a second adherend laminated on the layer of solid content.
Citation Information
Patent Citations
Method of airrspraying chemicals
JP1980025684A
Removal of chloroprene dimer from polchloroprene
JP1991203609A
Method for producing chloroprene rubber composition, chloroprene rubber composition, and adhesive using the same
JP2009173890A
Method for producing chloroprene rubber composition, chloroprene rubber composition, and adhesive using the same
JP2009173891A