Method for producing film adhesive for semiconductors

The film adhesive for semiconductors, with a flux-containing first layer and flux-free second layer, addresses connection reliability issues by ensuring rapid curing and stable bonding, enhancing productivity and reliability in flip-chip packages with high integration and narrow pitches.

JP7582425B2Active Publication Date: 2024-11-13RESONAC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023181615
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-23
Publication Date
2024-11-13
Estimated Expiration
2037-06-07

AI Technical Summary

Technical Problem

Conventional semiconductor connection methods face challenges with reduced connection reliability due to oxide film formation and impurities, leading to issues such as poor connectivity and decreased insulation reliability, especially in flip-chip packages with narrower pitches and higher integration, and the need for faster assembly processes.

Method used

A film adhesive for semiconductors comprising a first layer with a flux compound and a second layer without flux, utilizing a radically polymerizable compound and thermal radical generator, allowing for rapid curing even at high temperatures and short crimping times, thereby ensuring excellent connection reliability and insulation.

Benefits of technology

The film adhesive provides superior connection reliability and insulation properties, reducing void formation and improving productivity by enabling rapid curing and stable bonding, even under demanding conditions of high temperature and short crimping times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582425000009
    Figure 0007582425000009
  • Figure 0007582425000010
    Figure 0007582425000010
  • Figure 0007582425000011
    Figure 0007582425000011
Patent Text Reader

Abstract

To provide a method for manufacturing a film-like adhesive for a semiconductor which can obtain excellent connection reliability even when pressure-fitting time is shortened.SOLUTION: A method for manufacturing a film-like adhesive for a semiconductor which includes a first layer made of a first adhesive and a second layer made of a second adhesive includes a step of preparing a first resin varnish prepared by adding and dissolving or dispersing at least one kind of a thermosetting resin selected from a group consisting of an epoxy resin, a phenolic resin, and a polyimide resin, a curing agent, and a flux compound in an organic solvent, a step of preparing a second resin varnish prepared by adding and dissolving or dispersing at least a radically polymerizable compound and a thermal radical generator in an organic solvent, and a step of forming a first layer and a second layer using the first resin varnish and the second resin varnish.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film-like adhesive for semiconductors, a method for manufacturing a semiconductor device, and a semiconductor device. [Background technology]

[0002] Conventionally, wire bonding using thin metal wires such as gold wires has been widely used to connect semiconductor chips and substrates. On the other hand, in order to meet the demands for higher performance, higher integration, higher speed, etc. for semiconductor devices, flip chip connection (FC connection) in which conductive protrusions called bumps are formed on the semiconductor chip or substrate to directly connect the semiconductor chip and substrate is becoming more widespread.

[0003] For example, the COB (Chip On Board) type connection method, which is widely used for BGA (Ball Grid Array), CSP (Chip Size Package), etc., in connection between semiconductor chips and substrates, also corresponds to the FC connection method. The FC connection method is also widely used in the COC (Chip On Chip) type connection method, which forms connection parts (e.g., bumps and wiring) on ​​semiconductor chips to connect between semiconductor chips.

[0004] In addition, for packages that are strongly required to be even smaller, thinner, and more functional, chip-stack packages, POP (Package On Package), TSV (Through-Silicon Via), etc., which stack and multi-layer chips using the above-mentioned connection method, are beginning to become widespread. These stacking and multi-layering technologies arrange semiconductor chips and other components three-dimensionally, making the package smaller than methods that arrange them two-dimensionally. In addition, they are also effective in improving semiconductor performance, reducing noise, reducing mounting area, and saving power, and are therefore attracting attention as the next-generation semiconductor wiring technology.

[0005] Generally, metal bonding is used to connect the connecting parts from the viewpoint of ensuring sufficient connection reliability (e.g., insulation reliability). The main metals used for the above-mentioned connecting parts (e.g., bumps and wiring) include solder, tin, gold, silver, copper, nickel, etc., and conductive materials containing a plurality of these metals are also used. The metals used for the connecting parts may have impurities on the connecting surfaces of the connecting parts due to the surface being oxidized to form an oxide film, and impurities such as oxides adhering to the surface. If such impurities remain, the connection reliability (e.g., insulation reliability) between the semiconductor chip and the substrate, or between two semiconductor chips, may decrease, and there is a concern that the advantage of adopting the above-mentioned connecting method may be lost.

[0006] In addition, one method of suppressing the generation of these impurities is to coat the connection parts with an oxidation-preventing film, known as OSP (Organic Solderbility Preservatives) treatment, but this oxidation-preventing film can sometimes cause a decrease in solder wettability and connectivity during the connection process.

[0007] In view of this, a method has been proposed for removing the above-mentioned oxide film and impurities, in which a single layer film containing a flux agent is used in a semiconductor material (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2013 / 125086 Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, flip chip packages have become more and more highly functional and integrated. As the functionality and integration become more advanced, the pitch between wirings becomes narrower, which makes the connection reliability more likely to decrease.

[0010] In addition, in recent years, from the viewpoint of improving productivity, there is a demand for shortening the bonding time during assembly of flip chip packages. When the bonding time is shortened, if the film-like adhesive for semiconductors does not cure sufficiently during bonding, the connection cannot be sufficiently protected, and a connection failure occurs when the pressure during bonding is released. Furthermore, when solder is used for the connection, if the film-like adhesive for semiconductors does not cure sufficiently in a temperature range lower than the solder melting temperature during bonding, when the temperature during bonding reaches the solder melting temperature, the solder will scatter and flow, causing a connection failure. On the other hand, if the film-like adhesive for semiconductors cures before the connection parts come into contact with each other by bonding, the adhesive will be interposed between the connection parts, causing a connection failure.

[0011] Therefore, an object of the present invention is to provide a film-like adhesive for semiconductors that can provide excellent connection reliability even when the pressure-bonding time is shortened. Another object of the present invention is to provide a semiconductor device using such a film-like adhesive for semiconductors and a method for manufacturing the same. [Means for solving the problem]

[0012] The film-like adhesive for semiconductors of the present invention comprises a first layer made of a first adhesive containing a flux compound, and a second layer provided on the first layer and made of a second adhesive that is substantially free of a flux compound.

[0013] According to the film-like adhesive for semiconductors of the present invention, the second layer is not easily affected by the flux compound, and therefore the second layer can cause the connection parts to quickly and sufficiently harden after contact, and excellent connection reliability (e.g., insulation reliability) can be obtained even when pressure bonding is performed at high temperature for a short time. Furthermore, according to the film-like adhesive for semiconductors of the present invention, the pressure bonding time can be shortened, and therefore productivity can be improved. Furthermore, according to the film-like adhesive for semiconductors of the present invention, flip chip packages can be easily made highly functional and highly integrated.

[0014] However, in conventional semiconductor adhesives, voids may occur when the semiconductor adhesive is subjected to high temperature compression bonding in a state where the semiconductor adhesive is not sufficiently cured. In contrast, the film-like semiconductor adhesive of the present invention can be sufficiently cured in a short period of time, making it easy to prevent the occurrence of voids.

[0015] In recent years, for the purpose of reducing costs, solder, copper, etc., have tended to be used as the metal of the connection part instead of gold, etc., which is resistant to corrosion. Furthermore, for the surface treatment of wiring and bumps, there is a tendency to use solder, copper, etc., instead of gold, etc., which is resistant to corrosion, and to perform treatment such as OSP (Organic Solderability Preservative) treatment, etc., for the purpose of reducing costs. In flip chip packages, in addition to narrowing pitches and increasing the number of pins, such cost reductions are progressing, so there is a tendency to use metals that are easily corroded and have poor insulation properties, and insulation reliability is easily reduced. In contrast, the film-like adhesive for semiconductors of the present invention can suppress the deterioration of insulation reliability for the above metals.

[0016] The second adhesive preferably has a curing reaction rate of 80% or more when held for 5 seconds at 200° C. In this case, even when pressure bonding is performed at high temperature for a short period of time, better connection reliability can be obtained.

[0017] The second adhesive preferably contains a radical polymerizable compound and a thermal radical generator, and in this case, since the curing speed is very high, voids are unlikely to occur even when pressure bonding is performed at high temperature for a short time, and more excellent connection reliability can be obtained.

[0018] The thermal radical generator is preferably a peroxide, in which case better handling properties and storage stability can be obtained, and therefore better connection reliability can be easily obtained.

[0019] The radical polymerizable compound is preferably a (meth)acrylic compound, in which case even better connection reliability is likely to be obtained.

[0020] The (meth)acrylic compound preferably has a fluorene skeleton, which makes it easier to obtain even better connection reliability.

[0021] The flux compound preferably has a carboxyl group, and more preferably has two or more carboxyl groups, which makes it easier to obtain even better connection reliability.

[0022] The flux compound is preferably a compound represented by the following formula (2), in which case even better connection reliability is likely to be obtained. [ka] [In formula (2), R 1 and R 2 each independently represents a hydrogen atom or an electron-donating group, and n represents 0 or an integer of 1 or more.

[0023] The melting point of the flux compound is preferably 150° C. or less. In this case, the flux melts before the adhesive hardens during thermocompression bonding, and the oxide film of the solder, etc. is reduced and removed, making it easier to obtain even better connection reliability.

[0024] The method for manufacturing a semiconductor device of the present invention is a method for manufacturing a semiconductor device in which the connection parts of a semiconductor chip and a wiring circuit board are electrically connected to each other, or a semiconductor device in which the connection parts of a plurality of semiconductor chips are electrically connected to each other, and includes a step of sealing at least a part of the connection parts using the above-mentioned film-like adhesive for semiconductors. According to the method for manufacturing a semiconductor device of the present invention, a semiconductor device having excellent connection reliability (e.g., insulation reliability) can be obtained even when pressure bonding is performed at high temperature and in a short time. In other words, according to the manufacturing method of the present invention, a semiconductor device having excellent connection reliability (e.g., insulation reliability) can be manufactured in a short time.

[0025] The semiconductor device of the present invention is a semiconductor device in which the connection parts of a semiconductor chip and a wiring circuit board are electrically connected to each other, or a semiconductor device in which the connection parts of a plurality of semiconductor chips are electrically connected to each other, and at least a part of the connection parts is sealed with the cured product of the film-like adhesive for semiconductors described above. This semiconductor device has excellent connection reliability (e.g., insulation reliability). Effect of the Invention

[0026] According to the present invention, it is possible to provide a film-like adhesive for semiconductors that can obtain excellent connection reliability even when the pressure bonding time is shortened. Furthermore, according to the present invention, it is possible to provide a semiconductor device using such a film-like adhesive for semiconductors and a method for manufacturing the same. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a semiconductor device of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present invention. [Figure 4] 4A to 4C are cross-sectional views illustrating steps of a method for manufacturing a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] In this specification, "(meth)acrylate" means at least one of acrylate and the corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl" and "(meth)acrylic acid". Furthermore, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively.

[0029] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings where necessary. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicate explanations are omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, right, etc. are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.

[0030] <Film adhesive for semiconductors> The film-like adhesive for semiconductors of this embodiment comprises a first layer (flux-containing layer) made of a first adhesive containing a flux compound, and a second layer (flux-free layer) provided on the first layer and made of a second adhesive that contains substantially no flux compound.

[0031] The film-like adhesive for semiconductors of this embodiment is used, for example, in a semiconductor device in which the respective connection portions of a semiconductor chip and a wiring circuit board are electrically connected to each other, or in a semiconductor device in which the respective connection portions of multiple semiconductor chips are electrically connected to each other, to seal at least a portion of the connection portions.

[0032] According to the film-type adhesive for semiconductors of this embodiment, excellent connection reliability can be obtained even when the compression bonding time (e.g., the compression bonding time in the compression bonding process for joining the semiconductor chip and the wiring circuit board) is shortened (e.g., when the compression bonding time is set to 5 seconds or less) in the manufacture of the above-mentioned semiconductor device.

[0033] (First adhesive) The first adhesive contains, for example, a thermosetting component and a flux compound. Examples of the thermosetting component include a thermosetting resin and a curing agent. Examples of the thermosetting resin include an epoxy resin, a phenolic resin (except when contained as a curing agent), and a polyimide resin. Among these, it is preferable that the thermosetting resin is an epoxy resin. In addition, the film-like adhesive for semiconductors of this embodiment may contain a polymer component having a weight average molecular weight of 10,000 or more and a filler, if necessary.

[0034] Hereinafter, an embodiment will be described in which the first adhesive contains an epoxy resin (hereinafter sometimes referred to as "component (a)"), a curing agent (hereinafter sometimes referred to as "component (b)"), a flux compound (hereinafter sometimes referred to as "component (c)"), and, as necessary, a polymer component having a weight average molecular weight of 10,000 or more (hereinafter sometimes referred to as "component (d)") and a filler (hereinafter sometimes referred to as "component (e)").

[0035] [Component (a): epoxy resin] The epoxy resin can be used without any particular limitation as long as it has two or more epoxy groups in the molecule. As the component (a), for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, dicyclopentadiene type epoxy resin, and various polyfunctional epoxy resins can be used. These can be used alone or as a mixture of two or more kinds.

[0036] For component (a), from the viewpoint of preventing decomposition and generation of volatile components during connection at high temperatures, it is preferable to use an epoxy resin having a thermal weight loss rate of 5% or less at 250°C when the temperature during connection is 250°C, and it is preferable to use an epoxy resin having a thermal weight loss rate of 5% or less at 300°C when the temperature during connection is 300°C.

[0037] The content of component (a) is, for example, 5 to 75 mass %, preferably 10 to 50 mass %, and more preferably 15 to 35 mass %, based on the total amount of the first adhesive.

[0038] [Component (b): Hardener] Examples of the (b) component include phenolic resin-based curing agents, acid anhydride-based curing agents, amine-based curing agents, imidazole-based curing agents, and phosphine-based curing agents. When the (b) component contains a phenolic hydroxyl group, acid anhydrides, amines, or imidazoles, it exhibits flux activity that suppresses the formation of an oxide film at the connection, and can improve connection reliability and insulation reliability. Each curing agent will be described below.

[0039] (i) Phenolic resin-based hardener The phenolic resin-based curing agent is not particularly limited as long as it has two or more phenolic hydroxyl groups in the molecule, and examples thereof include phenol novolac resin, cresol novolac resin, phenol aralkyl resin, cresol naphthol formaldehyde polycondensate, triphenylmethane type polyfunctional phenolic resin, and various polyfunctional phenolic resins. These can be used alone or in a mixture of two or more kinds.

[0040] The equivalent ratio of the phenolic resin curing agent to the component (a) (the number of moles of phenolic hydroxyl groups in the phenolic resin curing agent / the number of moles of epoxy groups in the component (a)) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or more, the curability tends to improve and the adhesive strength tends to improve, and when it is 1.5 or less, there is no excess of unreacted phenolic hydroxyl groups remaining, the water absorption rate is kept low, and insulation reliability tends to improve.

[0041] (ii) Acid anhydride curing agent Examples of acid anhydride curing agents that can be used include methylcyclohexanetetracarboxylic dianhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and ethylene glycol bisanhydrotrimellitate. These can be used alone or in combination of two or more.

[0042] The equivalent ratio of the acid anhydride curing agent to the above component (a) (the number of moles of acid anhydride groups in the acid anhydride curing agent / the number of moles of epoxy groups in the component (a)) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or more, the curability tends to improve and the adhesion tends to improve, and when it is 1.5 or less, there is no excess of unreacted acid anhydride remaining, the water absorption rate is kept low, and the insulation reliability tends to improve.

[0043] (iii) Amine-based hardener As the amine-based curing agent, for example, dicyandiamide can be used.

[0044] The equivalent ratio of the amine curing agent to the component (a) (the number of moles of active hydrogen groups in the amine curing agent / the number of moles of epoxy groups in the component (a)) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, and even more preferably 0.5 to 1.0, from the viewpoint of good curability, adhesion, and storage stability. When the equivalent ratio is 0.3 or more, the curability tends to improve and the adhesion tends to improve, and when it is 1.5 or less, no excessive unreacted amine remains, and the insulation reliability tends to improve.

[0045] (iv) Imidazole-based curing agents Examples of the imidazole-based curing agent include 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, and 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. -[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and imidazoles. Among these, from the viewpoints of excellent curing properties, storage stability and connection reliability, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole are preferred. These may be used alone or in combination of two or more kinds. They may also be microencapsulated to form latent curing agents.

[0046] The content of the imidazole-based curing agent is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the component (a). When the content of the imidazole-based curing agent is 0.1 parts by mass or more, the curing property tends to be improved. When the content of the imidazole-based curing agent is 20 parts by mass or less, the fluidity of the first adhesive during pressure bonding can be ensured, and the first adhesive between the connection parts can be sufficiently removed. As a result, the first adhesive is prevented from curing while being interposed between the solder and the connection part, so that connection failure tends to be less likely to occur.

[0047] (v) Phosphine-based curing agents Examples of phosphine-based curing agents include triphenylphosphine, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra(4-methylphenyl)borate, and tetraphenylphosphonium(4-fluorophenyl)borate.

[0048] The content of the phosphine-based curing agent is preferably 0.1 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of component (a). When the content of the phosphine-based curing agent is 0.1 part by mass or more, the curability tends to be improved, and when it is 10 parts by mass or less, the first adhesive does not cure before the metal bond is formed, and connection failure tends to be less likely to occur.

[0049] The phenolic resin-based curing agent, the acid anhydride-based curing agent, and the amine-based curing agent can each be used alone or in combination of two or more. The imidazole-based curing agent and the phosphine-based curing agent can each be used alone, or can be used together with the phenolic resin-based curing agent, the acid anhydride-based curing agent, or the amine-based curing agent.

[0050] When the first adhesive contains a phenol resin-based curing agent, an acid anhydride-based curing agent, or an amine-based curing agent as the component (b), it exhibits flux activity for removing an oxide film, and connection reliability can be further improved.

[0051] [Component (c): Flux compound] The component (c) is a compound having flux activity, and functions as a flux agent in the first adhesive. As the component (c), any known compound can be used without particular limitation, so long as it reduces and removes an oxide film on the surface of solder or the like, and facilitates metal bonding. As the component (c), one type of flux compound may be used alone, or two or more types of flux compounds may be used in combination. However, the component (c) does not include the curing agent, which is the component (b).

[0052] From the viewpoint of obtaining sufficient flux activity and obtaining better connection reliability, the flux compound preferably has a carboxyl group, and more preferably has two or more carboxyl groups. Among these, a compound having two carboxyl groups is preferable. A compound having two carboxyl groups is less likely to volatilize even at high temperatures during connection compared to a compound having one carboxyl group (monocarboxylic acid), and can further suppress the occurrence of voids. In addition, when a compound having two carboxyl groups is used, the viscosity increase of the film-like adhesive for semiconductors during storage, connection work, etc. can be further suppressed compared to when a compound having three or more carboxyl groups is used, and the connection reliability of the semiconductor device can be further improved.

[0053] As the flux compound having a carboxyl group, a compound having a group represented by the following formula (1) is preferably used. [ka]

[0054] In formula (1), R 1 represents a hydrogen atom or an electron-donating group.

[0055] From the viewpoint of excellent reflow resistance and even better connection reliability, R 1 In this embodiment, the first adhesive contains an epoxy resin and a curing agent, and further contains a compound having a group represented by formula (1), R 1By further containing a compound in which the compound is an electron-donating group, it is possible to produce a semiconductor device that has excellent reflow resistance and connection reliability, even when used as a film-like adhesive for semiconductors in a flip-chip connection method for metal bonding.

[0056] In order to improve reflow resistance, it is necessary to suppress the decrease in adhesive strength after moisture absorption at high temperatures. Carboxylic acids have been used as flux compounds in the past, but the present inventors believe that the decrease in adhesive strength occurs in conventional flux compounds for the following reasons.

[0057] Usually, the epoxy resin reacts with the curing agent to proceed with the curing reaction, and at this time, the carboxylic acid, which is a flux compound, is incorporated into the curing reaction. That is, an ester bond may be formed by the reaction between the epoxy group of the epoxy resin and the carboxyl group of the flux compound. This ester bond is prone to hydrolysis due to moisture absorption, etc., and the decomposition of this ester bond is thought to be one of the causes of the decrease in adhesive strength after moisture absorption.

[0058] In contrast, among compounds having a group represented by formula (1), R 1 In the case of a compound having a group where the carboxyl group is an electron donating group, that is, a compound having a carboxyl group with an electron donating group nearby, the flux activity is sufficiently obtained by the carboxyl group, and even if the above-mentioned ester bond is formed, the electron donating group increases the electron density of the ester bond, suppressing the decomposition of the ester bond. In addition, since a substituent (electron donating group) exists near the carboxyl group, it is considered that the reaction between the carboxyl group and the epoxy resin is suppressed due to steric hindrance, making it difficult to form an ester bond.

[0059] For these reasons, among the compounds having a group represented by formula (1), R 1In the case of using a first adhesive further containing a compound in which is an electron donating group, the composition is less likely to change due to moisture absorption, etc., and excellent adhesive strength is maintained. In addition, the above-mentioned action can also be said to be that the curing reaction between the epoxy resin and the curing agent is less likely to be inhibited by the flux compound, and this action can be expected to have the effect of improving connection reliability by sufficient progress of the curing reaction between the epoxy resin and the curing agent.

[0060] When the electron-donating property of the electron-donating group is strong, the effect of suppressing the decomposition of the ester bond described above tends to be easily obtained. Also, when the steric hindrance of the electron-donating group is large, the effect of suppressing the reaction between the carboxyl group and the epoxy resin described above tends to be easily obtained. It is preferable that the electron-donating group has a good balance between the electron-donating property and the steric hindrance.

[0061] Examples of the electron-donating group include an alkyl group, a hydroxyl group, an amino group, an alkoxy group, and an alkylamino group. As the electron-donating group, a group that is difficult to react with other components (for example, the epoxy resin of the component (a)) is preferable, and specifically, an alkyl group, a hydroxyl group, or an alkoxy group is preferable, and an alkyl group is more preferable.

[0062] The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms. The greater the number of carbon atoms in the alkyl group, the greater the electron donating property and steric hindrance. Since an alkyl group having a carbon number within the above range has an excellent balance between electron donating property and steric hindrance, the effect of the present invention is more pronounced when using such an alkyl group.

[0063] The alkyl group may be linear or branched, and is preferably linear. When the alkyl group is linear, the number of carbon atoms of the alkyl group is preferably equal to or less than the number of carbon atoms in the main chain of the flux compound, from the viewpoint of the balance between electron donating property and steric hindrance. For example, when the flux compound is a compound represented by the following formula (2) and the electron donating group is a linear alkyl group, the number of carbon atoms of the alkyl group is preferably equal to or less than the number of carbon atoms (n+1) in the main chain of the flux compound.

[0064] The alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms. The larger the carbon number of the alkoxy group, the greater the electron donating property and steric hindrance tend to be. An alkoxy group having a carbon number within the above range has an excellent balance between electron donating property and steric hindrance, and therefore, when such an alkoxy group is used, the effects of the present invention are more pronounced.

[0065] The alkyl group portion of the alkoxy group may be linear or branched, and is preferably linear. When the alkoxy group is linear, the carbon number of the alkoxy group is preferably equal to or less than the carbon number of the main chain of the flux compound, from the viewpoint of the balance between electron donating property and steric hindrance. For example, when the flux compound is a compound represented by the following formula (2) and the electron donating group is a linear alkoxy group, the carbon number of the alkoxy group is preferably equal to or less than the carbon number (n+1) of the main chain of the flux compound.

[0066] Examples of the alkylamino group include a monoalkylamino group and a dialkylamino group. The monoalkylamino group is preferably a monoalkylamino group having 1 to 10 carbon atoms, and more preferably a monoalkylamino group having 1 to 5 carbon atoms. The alkyl group portion of the monoalkylamino group may be linear or branched, and is preferably linear.

[0067] The dialkylamino group is preferably a dialkylamino group having 2 to 20 carbon atoms, and more preferably a dialkylamino group having 2 to 10 carbon atoms. The alkyl group portion of the dialkylamino group may be linear or branched, and is preferably linear.

[0068] As a flux compound having two carboxyl groups, a compound represented by the following formula (2) can be suitably used. The compound represented by the following formula (2) can further improve the reflow resistance and connection reliability of a semiconductor device.

[0069] [ka]

[0070] In formula (2), R 1 and R 2 each independently represents a hydrogen atom or an electron donating group, and n represents an integer of 0 or 1 or more. 2 may be the same or different from each other.

[0071] R 1 is the same as formula (1). 2 The electron donating property indicated by R 1 For the same reason as that explained in formula (1), R in formula (2) is 1 is preferably an electron donating group.

[0072] In formula (2), n is preferably 1 or more. When n is 1 or more, the flux compound is less likely to volatilize even at high temperatures during connection, and the generation of voids can be further suppressed, compared with the case where n is 0. Furthermore, in formula (2), n is preferably 15 or less, more preferably 11 or less, and may be 6 or less or 4 or less. When n is 15 or less, even better connection reliability can be obtained.

[0073] Moreover, as the flux compound, a compound represented by the following formula (3) is more preferable. The compound represented by the following formula (3) can further improve the reflow resistance and connection reliability of the semiconductor device.

[0074] [ka]

[0075] In formula (3), R 1 and R 2 each independently represents a hydrogen atom or an electron-donating group, and m represents 0 or an integer of 1 or more.

[0076] In the formula (3), m is preferably equal to or less than 10, more preferably equal to or less than 5, and even more preferably equal to or less than 3. When m is equal to or less than 10, even better connection reliability can be obtained.

[0077] In formula (3), R 1 and R 2 may be a hydrogen atom or an electron donating group. From the viewpoint of obtaining even better connection reliability, R 1 and R 2 At least one of R is preferably an electron donating group. 1 is an electron donating group, R 2 When R is a hydrogen atom, the melting point tends to be low, and the connection reliability of the semiconductor device can be improved in some cases. 1 and R 2 and R are different electron donating groups. 1 and R 2 In comparison with the case where the electron-donating group is the same as that of the compound having the same structure, the melting point tends to be lower, and the connection reliability of the semiconductor device can be improved in some cases.

[0078] In addition, in formula (3), R 1 and R 2 When R is the same electron donating group, the structure becomes symmetrical and the melting point tends to be high. However, even in this case, the effect of the present invention can be sufficiently obtained. In particular, when the melting point is sufficiently low, ie, 150° C. or less, R 1 and R 2 Even if and are the same group, R 1 and R 2 In this case, the same level of connection reliability can be obtained as when the groups are different from each other.

[0079] As the flux compound, for example, a dicarboxylic acid selected from succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, and a compound in which an electron donating group is substituted at the 2-position of these dicarboxylic acids can be used.

[0080] The melting point of the flux compound is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 130°C or lower. Such a flux compound is likely to fully exhibit flux activity before the curing reaction between the epoxy resin and the curing agent occurs. Therefore, a semiconductor device with even more excellent connection reliability can be realized by using a film-like adhesive for semiconductors that uses a first adhesive containing such a flux compound. In addition, the melting point of the flux compound is preferably 25°C or higher, and more preferably 50°C or higher. In addition, the flux compound is preferably one that is solid at room temperature (25°C).

[0081] The melting point of the flux compound can be measured using a general melting point measurement device. The sample to be measured is ground into a fine powder and a small amount is used to reduce the temperature deviation inside the sample. A capillary tube with one end closed is often used as the container for the sample, but some measurement devices use a container sandwiched between two microscope cover glasses. In addition, if the temperature is increased suddenly, a temperature gradient will occur between the sample and the thermometer, causing measurement errors, so it is desirable to increase the temperature at the time of measuring the melting point at a rate of less than 1°C per minute.

[0082] As mentioned above, the material to be measured for melting point is prepared as a fine powder, so the sample before melting is opaque due to diffuse reflection from the surface. The temperature at which the sample begins to become transparent is usually taken as the lower limit of the melting point, and the temperature at which the sample is completely melted is usually taken as the upper limit. There are various types of measuring devices, but the most classic device is a device in which a capillary tube filled with the sample is attached to a double-tube thermometer and heated in a hot bath. A highly viscous liquid is used as the hot bath liquid in order to attach the capillary tube to the double-tube thermometer, and concentrated sulfuric acid or silicone oil is often used, and the sample is attached so that it is close to the reservoir at the tip of the thermometer. Alternatively, a melting point measuring device can be used that uses a metal heat block for heating, and automatically determines the melting point by adjusting the heating while measuring the light transmittance.

[0083] In this specification, a melting point of 150°C or lower means that the upper limit of the melting point is 150°C or lower, and a melting point of 25°C or higher means that the lower limit of the melting point is 25°C or higher.

[0084] The content of component (c) is preferably 0.5 to 10 mass %, and more preferably 0.5 to 5 mass %, based on the total amount of the first adhesive.

[0085] [Component (d): Polymer component having a weight-average molecular weight of 10,000 or more] If necessary, the first adhesive may contain a polymer component (component (d)) having a weight average molecular weight of at least 10,000. The first adhesive containing component (d) has even more excellent heat resistance and film formability.

[0086] Examples of the (d) component include phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, and acrylic rubber. Among these, from the viewpoint of excellent heat resistance and film formability, phenoxy resin, polyimide resin, acrylic rubber, cyanate ester resin, and polycarbodiimide resin are preferred, and phenoxy resin, polyimide resin, and acrylic rubber are more preferred. These (d) components can be used alone or as a mixture or copolymer of two or more kinds. However, the (d) component does not include a compound corresponding to the (a) component or a compound corresponding to the (e) component.

[0087] The weight average molecular weight of component (d) is, for example, not less than 10,000, preferably not less than 20,000, and more preferably not less than 30,000. Such component (d) can further improve the heat resistance and film formability of the first adhesive.

[0088] Furthermore, the weight average molecular weight of the component (d) is preferably not more than 1,000,000, and more preferably not more than 500,000. Such a component (d) can further improve the heat resistance of the first adhesive.

[0089] In this specification, the weight average molecular weight means a weight average molecular weight measured in terms of polystyrene using high performance liquid chromatography (manufactured by Shimadzu Corporation, product name: C-R4A). For example, the following conditions can be used for the measurement. Detector: LV4000 UV Detector (product name, manufactured by Hitachi, Ltd.) Pump: L6000 Pump (product name, manufactured by Hitachi, Ltd.) Column: Gelpack GL-S300MDT-5 (total of 2) (Hitachi Chemical Co., Ltd., product name) Eluent: THF / DMF=1 / 1 (volume ratio) + LiBr (0.03mol / L) + H3PO4 (0.06mol / L) Flow rate: 1mL / min

[0090] When the first adhesive contains the component (d), the content C of the component (d) d Content of component (a) relative to C a Ratio of C a / C d The mass ratio is preferably 0.01 to 5, more preferably 0.05 to 3, and further preferably 0.1 to 2. a / C d By making the ratio C 0.01 or more, better curing properties and adhesive strength can be obtained. a / C d By setting the value to 5 or less, better film formability can be obtained.

[0091] [(e) Component: Filler] The first adhesive may contain a filler (component (e)) as necessary. Component (e) can control the viscosity of the first adhesive, the physical properties of the cured product of the first adhesive, etc. Specifically, component (e) can, for example, suppress the generation of voids during connection, reduce the moisture absorption rate of the cured product of the first adhesive, etc.

[0092] Examples of the (e) component include inorganic fillers (inorganic particles) and organic fillers (organic particles). Examples of the inorganic fillers include insulating inorganic fillers such as glass, silica, alumina, titanium oxide, mica, and boron nitride. Among these, at least one selected from the group consisting of silica, alumina, titanium oxide, and boron nitride is preferred, and at least one selected from the group consisting of silica, alumina, and boron nitride is more preferred. The insulating inorganic filler may be whiskers. Examples of whiskers include aluminum borate, aluminum titanate, zinc oxide, calcium silicate, and boron nitride. Examples of organic fillers include resin fillers (resin particles). Examples of resin fillers include polyurethane and polyimide. Compared to inorganic fillers, resin fillers can provide flexibility at high temperatures such as 260°C, so they are suitable for improving reflow resistance, and are also effective in improving film formability because they can provide flexibility.

[0093] From the viewpoint of achieving even better insulation reliability, it is preferable that the component (e) is insulating. It is preferable that the first adhesive does not contain a conductive metal filler (metal particles) such as a silver filler or a solder filler, or a conductive inorganic filler such as carbon black.

[0094] The physical properties of the component (e) may be appropriately adjusted by surface treatment. From the viewpoint of improving dispersibility or adhesive strength, the component (e) is preferably a filler that has been subjected to a surface treatment. Examples of the surface treatment agent include glycidyl-based (epoxy-based), amine-based, phenyl-based, phenylamino-based, (meth)acrylic-based, and vinyl-based compounds.

[0095] As the surface treatment, silane treatment using a silane compound such as an epoxysilane, aminosilane, or acrylicsilane is preferred from the viewpoint of ease of surface treatment. As the surface treatment agent, from the viewpoint of excellent dispersibility, fluidity, and adhesive strength, at least one selected from the group consisting of a glycidyl compound, a phenylamino compound, and a (meth)acrylic compound is preferred. As the surface treatment agent, from the viewpoint of excellent storage stability, at least one selected from the group consisting of a phenyl compound and a (meth)acrylic compound is preferred.

[0096] The average particle size of component (e) is preferably 1.5 μm or less from the viewpoint of preventing jamming during flip chip connection, and more preferably 1.0 μm or less from the viewpoint of excellent visibility (transparency).

[0097] The content of the (e) component is preferably 30% by mass or more, and more preferably 40% by mass or more, based on the total amount of the first adhesive, from the viewpoint of suppressing a decrease in heat dissipation and of tending to easily suppress the occurrence of voids and an increase in moisture absorption rate. The content of the (e) component is preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the first adhesive, from the viewpoint of easily suppressing an increase in viscosity and a decrease in the fluidity of the first adhesive, and of easily suppressing the occurrence of filler trapping in the connection portion, and of tending to easily suppress a decrease in connection reliability. From these viewpoints, the content of the (e) component is preferably 30 to 90% by mass, and more preferably 40 to 80% by mass, based on the total amount of the first adhesive.

[0098] [Other ingredients] The first adhesive may contain additives such as antioxidants, silane coupling agents, titanium coupling agents, leveling agents, and ion trapping agents. These may be used alone or in combination of two or more. The amounts of these additives may be appropriately adjusted so that the effects of each additive are exerted.

[0099] (Second adhesive) The second adhesive is substantially free of flux compounds. "Substantially free" means that the content of the flux compounds in the second adhesive is less than 0.5 mass % based on the total amount of the second adhesive.

[0100] From the viewpoint of obtaining the effects of the present invention remarkably, the second adhesive preferably has a curing reaction rate of 80% or more when held at 200°C for 5 seconds. An example of such a second adhesive is a radical curing adhesive. The reason why such an adhesive provides the effects of the present invention remarkably is not clear, but the present inventors speculate as follows.

[0101] That is, in the conventional film-like adhesive containing a flux compound, the flux component deactivates the radicals, so that a radical curing system cannot be applied, and a cationic curing system using epoxy or the like is often applied. In this curing system (reaction system), the curing proceeds by a nucleophilic addition reaction, so the curing speed is slow, and voids may occur after compression bonding. In the conventional film-like adhesive, it is presumed that the voids during mounting caused problems (for example, peeling of the semiconductor material at a reflow temperature of about 260 ° C, poor connection of the connection part, etc.). On the other hand, since the above-mentioned second adhesive does not substantially contain a flux compound, the curing system can be a radical curing system, and a sufficient curing speed can be obtained. Therefore, it is presumed that by using the above-mentioned second adhesive in the second layer, voids are unlikely to occur even when compression bonding is performed at a high temperature and for a short time, and the effect of the present invention is remarkable. In addition, since a sufficient curing speed can be obtained in this embodiment, for example, even when solder is used in the connection part, the film-like adhesive can be cured in a temperature range lower than the solder melting temperature. Therefore, it is possible to sufficiently prevent the solder from scattering or flowing, which would otherwise cause poor connection.

[0102] Hereinafter, an embodiment will be described in which the second adhesive contains a radical polymerizable compound (hereinafter sometimes referred to as "component (A)"), a thermal radical generator (hereinafter sometimes referred to as "component (B)"), and, optionally, a polymer component (hereinafter sometimes referred to as "component (C)") and a filler (hereinafter sometimes referred to as "component (D)").

[0103] [Component (A): radically polymerizable compound] The (A) component is a compound capable of undergoing a radical polymerization reaction with the generation of radicals due to heat, light, radiation, electrochemical action, etc. Examples of the (A) component include (meth)acrylic compounds and vinyl compounds. As the (A) component, a (meth)acrylic compound is preferable from the viewpoint of excellent durability, electrical insulation, and heat resistance. The (meth)acrylic compound is not particularly limited as long as it is a compound having one or more (meth)acrylic groups ((meth)acryloyl groups) in the molecule, and for example, (meth)acrylic compounds containing a bisphenol A type, bisphenol F type, naphthalene type, phenol novolac type, cresol novolac type, phenol aralkyl type, biphenyl type, triphenylmethane type, dicyclopentadiene type, fluorene type, adamantane type, or isocyanuric acid type skeleton; various polyfunctional (meth)acrylic compounds (excluding (meth)acrylic compounds containing the above skeleton), etc. can be used. Examples of polyfunctional (meth)acrylic compounds include pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, trimethylolpropane di(meth)acrylate, etc. The component (A) may be used alone or in combination of two or more.

[0104] From the viewpoint of excellent heat resistance, the (A) component preferably has a bisphenol A type skeleton, a bisphenol F type skeleton, a naphthalene type skeleton, a fluorene type skeleton, an adamantane type skeleton, or an isocyanuric acid type skeleton, and more preferably has a fluorene type skeleton. The (A) component is further preferably a (meth)acrylate having any of the above skeletons.

[0105] The component (A) is preferably solid at room temperature (25°C). A solid component is less likely to generate voids than a liquid component, and the second adhesive has low viscosity (tack) before curing (B stage), making it easier to handle. Examples of the component (A) that is solid at room temperature (25°C) include (meth)acrylates having a bisphenol A skeleton, a fluorene skeleton, an adamantane skeleton, or an isocyanuric acid skeleton.

[0106] The number of functional groups of the (meth)acrylic group in component (A) is preferably 3 or less. If the number of functional groups is large, the curing network may progress too quickly, and unreacted groups may remain. On the other hand, if the number of functional groups is 3 or less, the number of functional groups is not too large, and curing can easily proceed sufficiently in a short time, making it easier to prevent a decrease in the curing reaction rate.

[0107] The molecular weight of component (A) is preferably less than 2000, and more preferably not more than 1000. The smaller the molecular weight of component (A), the more easily the reaction proceeds, and the higher the curing reaction rate.

[0108] The content of the (A) component is preferably 10% by mass or more, and more preferably 15% by mass or more, based on the total amount of the second adhesive, from the viewpoint of preventing the cured component from becoming too hard and making it easy to sufficiently control the flow of the resin after curing. The content of the (A) component is preferably 50% by mass or less, and more preferably 40% by mass or less, based on the total amount of the second adhesive, from the viewpoint of preventing the cured product from becoming too hard and making it easy to prevent the package from warping too much. From these viewpoints, the content of the (A) component is preferably 10 to 50% by mass, and more preferably 15 to 40% by mass, based on the total amount of the second adhesive.

[0109] The content of the (A) component is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, per part by mass of the (C) component, from the viewpoint of easily suppressing a decrease in curability and a decrease in adhesive strength. The content of the (A) component is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, per part by mass of the (C) component, from the viewpoint of easily suppressing a decrease in film formability. From these viewpoints, the content of the (A) component is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 5 parts by mass, per part by mass of the (C) component.

[0110] [Component (B): Thermal radical generator] There are no particular limitations on the component (B) as long as it functions as a curing agent for the component (A), but from the standpoint of excellent handleability, a thermal radical generator is preferred.

[0111] Examples of the thermal radical generator include azo compounds and peroxides (organic peroxides, etc.). Examples of the thermal radical generator include peroxides, and more preferably organic peroxides. In this case, radical reaction does not proceed in the process of drying the solvent when forming the film, and the handling and storage stability are excellent. Therefore, when peroxides are used as the thermal radical generator, it is easy to obtain even better connection reliability. Examples of the organic peroxides include ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyesters, etc. From the viewpoint of excellent storage stability, the organic peroxide is preferably at least one selected from the group consisting of hydroperoxides, dialkyl peroxides, and peroxyesters. Furthermore, from the viewpoint of excellent heat resistance, the organic peroxide is preferably at least one selected from the group consisting of hydroperoxides and dialkyl peroxides. Examples of the dialkyl peroxides include dicumyl peroxide and di-tert-butyl peroxide.

[0112] The content of the (B) component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, per 100 parts by mass of the (A) component, from the viewpoint of sufficient curing progress. The content of the (B) component is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of the (A) component. When the upper limit of the (B) component content is within the above range, the curing progresses rapidly and the reaction points are prevented from increasing, thereby preventing the molecular chain from becoming short and the unreacted groups from remaining. Therefore, when the upper limit of the (B) component content is within the above range, there is a tendency that the reliability is easily prevented from decreasing. From these viewpoints, the content of the (B) component is preferably 0.5 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the (A) component.

[0113] [(C) component: polymer component] The second adhesive may further contain a polymer component. (C) component may be an epoxy resin, a phenoxy resin, a polyimide resin, a polyamide resin, a polycarbodiimide resin, a cyanate ester resin, a (meth)acrylic resin, a polyester resin, a polyethylene resin, a polyethersulfone resin, a polyetherimide resin, a polyvinyl acetal resin, a urethane resin, an acrylic rubber, or the like. Among them, from the viewpoint of excellent heat resistance and film formability, at least one selected from the group consisting of an epoxy resin, a phenoxy resin, a polyimide resin, a (meth)acrylic resin, an acrylic rubber, a cyanate ester resin, and a polycarbodiimide resin is preferable, and at least one selected from the group consisting of an epoxy resin, a phenoxy resin, a polyimide resin, a (meth)acrylic resin, and an acrylic rubber is more preferable. (C) component may be used alone or as a mixture or copolymer of two or more kinds. However, (C) component does not include a compound corresponding to (A) component and a compound corresponding to (D) component.

[0114] The glass transition temperature (Tg) of component (C) is preferably 120°C or less, more preferably 100°C or less, and even more preferably 85°C or less, from the viewpoint of excellent adhesion of the film-like adhesive for semiconductors to the substrate or chip. When it is within these ranges, it is possible to easily fill the unevenness of bumps formed on the semiconductor chip, electrodes or wiring patterns formed on the substrate, etc. with the film-like adhesive for semiconductors (it is easy to suppress the start of the curing reaction), and there is a tendency to easily suppress the occurrence of voids due to residual air bubbles. The above Tg is the Tg measured using a DSC (manufactured by PerkinElmer, product name: DSC-7 type) under the conditions of a sample amount of 10 mg, a heating rate of 10°C / min, and a measurement atmosphere: air.

[0115] The weight average molecular weight of component (C), calculated as polystyrene, is preferably 10,000 or more, and in order to exhibit good film formability alone, it is more preferably 30,000 or more, even more preferably 40,000 or more, and particularly preferably 50,000 or more. When the weight average molecular weight is 10,000 or more, there is a tendency that a decrease in film formability is easily suppressed.

[0116] [Component (D): Filler] The second adhesive may further contain a filler to control the viscosity or physical properties of the cured product, and to further suppress the generation of voids or moisture absorption rate when connecting a semiconductor chip to a substrate or connecting semiconductor chips to each other. As component (D), the same fillers as those listed as component (d) in the first adhesive can be used. Examples of preferred fillers are also the same.

[0117] The content of the (D) component is preferably 30% by mass or more, and more preferably 40% by mass or more, based on the total amount of the second adhesive, from the viewpoint of suppressing a decrease in heat dissipation and a tendency to easily suppress the occurrence of voids and an increase in moisture absorption rate. The content of the (D) component is preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the second adhesive, from the viewpoint of easily suppressing an increase in viscosity and a decrease in the fluidity of the second adhesive, and of easily suppressing the occurrence of filler trapping in the connection portion, and of easily suppressing a decrease in connection reliability. From these viewpoints, the content of the (D) component is preferably 30 to 90% by mass, and more preferably 40 to 80% by mass, based on the total amount of the second adhesive.

[0118] [Other ingredients] The second adhesive may contain polymerizable compounds other than radically polymerizable compounds (e.g., cationic polymerizable compounds and anionic polymerizable compounds). The second adhesive may contain other components similar to those in the first adhesive. These may be used alone or in combination of two or more. The amounts of these additives may be appropriately adjusted so that the effects of each additive are exerted.

[0119] The curing reaction rate when the second adhesive is held at 200°C for 5 seconds is preferably 80% or more, and more preferably 90% or more. If the curing reaction rate at 200°C (below the solder melting temperature) / 5 seconds is 80% or more, it is easy to prevent the solder from scattering and flowing at the time of connection (above the solder melting temperature) and reducing the connection reliability. The curing reaction rate can be obtained by placing 10 mg of the second adhesive (uncured flux-free layer) in an aluminum pan and then measuring the amount of heat generated using a DSC (manufactured by PerkinElmer, product name: DSC-7 type). Specifically, a measurement sample in which 10 mg of the second adhesive (uncured flux-free layer) is placed in an aluminum pan is placed on a hot plate heated to 200°C, and the measurement sample is removed from the hot plate after 5 seconds. The measurement sample after the heat treatment and the untreated measurement sample are each measured using a DSC. From the obtained amount of heat generated, the curing reaction rate is calculated using the following formula. Curing reaction rate (%) = (1 - [heat generation amount of the measured sample after heat treatment] / [heat generation amount of the untreated measured sample]) x 100

[0120] When the second resin contains an anionically polymerizable epoxy resin (particularly an epoxy resin having a weight average molecular weight of 10,000 or more), it may be difficult to adjust the curing reaction rate to 80% or more. The content of the epoxy resin is preferably 20 parts by mass or less relative to 80 parts by mass of the (A) component, and more preferably, no epoxy resin is contained.

[0121] The second layer (flux-free layer) made of the second adhesive can be pressure-bonded at high temperatures of 200°C or higher. In addition, in flip chip packages in which connections are formed by melting a metal such as solder, it exhibits even better hardening properties.

[0122] With regard to the thickness of the film-like adhesive for semiconductors of this embodiment, when the sum of the heights of the above-mentioned connection parts is x and the total thickness of the film-like adhesive for semiconductors is y, the relationship between x and y preferably satisfies 0.70x≦y≦1.3x, and more preferably satisfies 0.80x≦y≦1.2x, from the viewpoint of the connectivity during pressure bonding and the filling property of the adhesive. The total thickness of the film-like adhesive for semiconductors may be, for example, 10 to 100 μm, 10 to 80 μm, or 10 to 50 μm.

[0123] The thickness of the first layer may be, for example, 1 to 50 μm, 3 to 50 μm, 4 to 30 μm, or 5 to 20 μm.

[0124] The thickness of the second layer may be, for example, 7 to 50 μm, 8 to 45 μm, or 10 to 40 μm.

[0125] The ratio of the thickness of the second layer to the thickness of the first layer (thickness of the second layer / thickness of the first layer) may be, for example, 0.1 to 10.0, 0.5 to 6.0, or 1.0 to 4.0.

[0126] The film-like adhesive for a semiconductor of this embodiment may further comprise layers other than the first layer and the second layer, but is preferably composed of only the first layer and the second layer. The film-like adhesive for a semiconductor of this embodiment may also comprise a base film and / or a protective film on the surface of the first layer opposite the second layer and / or on the surface of the second layer opposite the first layer.

[0127] <Method of manufacturing film adhesive for semiconductors> The film-like adhesive for semiconductors of this embodiment can be obtained, for example, by preparing a first film-like adhesive having a first layer and a second film-like adhesive having a second layer, and bonding the first film-like adhesive having the first layer and the second film-like adhesive having the second layer together.

[0128] In the step of preparing the first film-like adhesive, for example, first, components (a), (b), and (c), as well as other components such as components (d) and (e) that are added as necessary, are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc. to prepare a resin varnish (coating varnish). Thereafter, the resin varnish is applied onto a release-treated substrate film using a knife coater, roll coater, applicator, etc., and the organic solvent is reduced by heating, so that a first layer made of the first adhesive can be formed on the substrate film.

[0129] The organic solvent used in the preparation of the resin varnish is preferably one that has the property of uniformly dissolving or dispersing each component, and examples thereof include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethylsulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used alone or in combination of two or more. The stirring and mixing and kneading in the preparation of the resin varnish can be performed, for example, using a stirrer, a grinding machine, a three-roll mill, a ball mill, a bead mill, or a homodisper.

[0130] The substrate film is not particularly limited as long as it has heat resistance sufficient to withstand the heating conditions when volatilizing the organic solvent, and examples thereof include polyolefin films such as polypropylene film and polymethylpentene film, polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polyimide film, and polyetherimide film. The substrate film is not limited to a single layer made of these films, and may be a multilayer film made of two or more materials.

[0131] The drying conditions for volatilizing the organic solvent from the resin varnish applied to the base film are preferably conditions that allow the organic solvent to volatilize sufficiently, specifically, heating is preferably performed for 0.1 to 90 minutes at 50 to 200° C. If there is no effect on voids or viscosity adjustment after mounting, the organic solvent is preferably removed to 1.5 mass % or less of the total amount of the first film-like adhesive.

[0132] In the step of preparing the second film-like adhesive, a second layer made of the second adhesive can be formed on the base film in the same manner as for the first layer, except that components (A) and (B) as well as other components such as component (C), which are added as necessary, are used.

[0133] Examples of the method for laminating the first film-like adhesive and the second film-like adhesive include hot pressing, roll lamination, vacuum lamination, etc. Lamination may be performed under heating conditions of, for example, 30 to 120°C.

[0134] The film-like adhesive for semiconductors of this embodiment may be obtained, for example, by forming one of the first layer or the second layer on a substrate film, and then forming the other of the first layer or the second layer on the obtained first layer or second layer. The first layer and the second layer may be formed by the same method as the method for forming the first layer and the second layer in the production of the film-like adhesive with substrate described above.

[0135] <Semiconductor device> The semiconductor device of this embodiment will be described below with reference to Figs. 1 and 2. Fig. 1 is a schematic cross-sectional view showing one embodiment of the semiconductor device of the present invention. As shown in Fig. 1(a), the semiconductor device 100 has a semiconductor chip 10 and a substrate (circuit wiring substrate) 20 facing each other, wiring 15 arranged on the surfaces of the semiconductor chip 10 and the substrate 20 facing each other, connection bumps 30 connecting the wiring 15 of the semiconductor chip 10 and the substrate 20 to each other, and a sealing portion 40 made of a hardened product of adhesives (first adhesive and second adhesive) filled without gaps in the gap between the semiconductor chip 10 and the substrate 20. The semiconductor chip 10 and the substrate 20 are flip-chip connected by the wiring 15 and the connection bumps 30. The wiring 15 and the connection bumps 30 are sealed by the hardened product of the adhesive and are isolated from the external environment. The sealing portion 40 has an upper portion 40a including the hardened product of the first adhesive and a lower portion 40b including the hardened product of the second adhesive.

[0136] As shown in FIG. 1(b), the semiconductor device 200 has a semiconductor chip 10 and a substrate 20 facing each other, bumps 32 arranged on the facing surfaces of the semiconductor chip 10 and the substrate 20, respectively, and a sealing portion 40 made of a hardened product of adhesives (first adhesive and second adhesive) that fills the gap between the semiconductor chip 10 and the substrate 20 without any gaps. The semiconductor chip 10 and the substrate 20 are flip-chip connected by connecting the facing bumps 32 to each other. The bumps 32 are sealed by the hardened product of the adhesive and are isolated from the external environment. The sealing portion 40 has an upper portion 40a including the hardened product of the first adhesive and a lower portion 40b including the hardened product of the second adhesive.

[0137] Fig. 2 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present invention. As shown in Fig. 2(a), the semiconductor device 300 is similar to the semiconductor device 100, except that two semiconductor chips 10 are flip-chip connected by wiring 15 and connection bumps 30. As shown in Fig. 2(b), the semiconductor device 400 is similar to the semiconductor device 200, except that two semiconductor chips 10 are flip-chip connected by bumps 32.

[0138] The semiconductor chip 10 is not particularly limited, and may be an elemental semiconductor composed of the same type of element, such as silicon or germanium, or a compound semiconductor, such as gallium arsenide or indium phosphide.

[0139] The substrate 20 is not particularly limited as long as it is a circuit substrate, and examples that can be used include a circuit substrate having wiring (wiring pattern) 15 formed by etching away unnecessary portions of a metal film on the surface of an insulating substrate whose main component is glass epoxy, polyimide, polyester, ceramic, epoxy, bismaleimide triazine, etc.; a circuit substrate having wiring 15 formed on the surface of the insulating substrate by metal plating or the like; and a circuit substrate having wiring 15 formed by printing a conductive material on the surface of the insulating substrate.

[0140] The connection parts such as wiring 15 and bumps 32 contain as their main components gold, silver, copper, solder (the main components being, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), nickel, tin, lead, etc., and may contain multiple metals.

[0141] Among the above metals, from the viewpoint of providing a package having excellent electrical and thermal conductivity at the connection portion, gold, silver and copper are preferred, and silver and copper are more preferred. From the viewpoint of providing a package at reduced cost, inexpensive materials such as silver, copper and solder are preferred, copper and solder are more preferred, and solder is even more preferred. Since the formation of an oxide film on the surface of a metal at room temperature can reduce productivity and increase costs, from the viewpoint of suppressing the formation of an oxide film, gold, silver, copper and solder are preferred, gold, silver and solder are more preferred, and gold and silver are even more preferred.

[0142] A metal layer mainly composed of gold, silver, copper, solder (main components are, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, etc.), tin, nickel, etc. may be formed, for example, by plating, on the surfaces of the wiring 15 and bumps 32. This metal layer may be composed of only a single component, or may be composed of multiple components. The metal layer may have a structure in which a single layer or multiple metal layers are laminated.

[0143] Furthermore, the semiconductor device of this embodiment may be a stack of a plurality of structures (packages) such as those shown in the semiconductor devices 100 to 400. In this case, the semiconductor devices 100 to 400 may be electrically connected to each other by bumps, wiring, or the like containing gold, silver, copper, solder (whose main component is, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), tin, nickel, or the like.

[0144] As a method for stacking a plurality of semiconductor devices, for example, TSV (Through-Silicon Via) technology can be mentioned as shown in FIG. 3. FIG. 3 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present invention, which is a semiconductor device using the TSV technology. In the semiconductor device 500 shown in FIG. 3, the wiring 15 formed on the interposer 50 is connected to the wiring 15 of the semiconductor chip 10 via the connection bump 30, so that the semiconductor chip 10 and the interposer 50 are flip-chip connected. The gap between the semiconductor chip 10 and the interposer 50 is filled with a hardened product of the adhesive (first adhesive and second adhesive) without any gaps, forming a sealing part 40. On the surface of the semiconductor chip 10 opposite to the interposer 50, the semiconductor chips 10 are repeatedly stacked via the wiring 15, the connection bump 30 and the sealing part 40. The wiring 15 on the pattern surfaces on the front and back of the semiconductor chip 10 are connected to each other by the through electrodes 34 filled in holes penetrating the inside of the semiconductor chip 10. The material of the through electrodes 34 can be copper, aluminum, or the like.

[0145] Such TSV technology makes it possible to obtain signals from the back surface of the semiconductor chip, which is not normally used. Furthermore, since the through electrodes 34 are vertically passed through the semiconductor chip 10, the distance between the opposing semiconductor chips 10 and between the semiconductor chip 10 and the interposer 50 can be shortened, enabling flexible connection. The film-like adhesive for semiconductors of this embodiment can be applied as a film-like adhesive for semiconductors between the opposing semiconductor chips 10 and between the semiconductor chip 10 and the interposer 50 in such TSV technology.

[0146] Furthermore, in a highly flexible bump formation method such as area bump chip technology, a semiconductor chip can be directly mounted on a motherboard without an interposer. The film-like adhesive for semiconductors of this embodiment can also be applied to such cases where a semiconductor chip is directly mounted on a motherboard. The film-like adhesive for semiconductors of this embodiment can also be applied to sealing the gap between two wiring circuit boards when the boards are stacked.

[0147] <Method of Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device according to this embodiment will be described below with reference to Fig. 4. Fig. 4 is a schematic diagram showing one embodiment of the method for manufacturing a semiconductor device according to the present invention, and Fig. 4(a), Fig. 4(b), and Fig. 4(c) each show a cross section of a semiconductor device.

[0148] First, as shown in FIG. 4(a), a solder resist 60 having openings at positions where connection bumps 30 are to be formed is formed on a substrate 20 having wiring 15. The solder resist 60 is not necessarily provided. However, by providing a solder resist on the substrate 20, it is possible to suppress the occurrence of bridges between the wiring 15 and improve connection reliability and insulation reliability. The solder resist 60 can be formed, for example, using a commercially available ink for solder resist for packaging. Specific examples of commercially available ink for solder resist for packaging include the SR series (manufactured by Hitachi Chemical Co., Ltd., product name) and the PSR4000-AUS series (manufactured by Taiyo Ink Mfg. Co., Ltd., product name).

[0149] Next, as shown in FIG. 4(a), the connection bumps 30 are formed in the openings of the solder resist 60. Then, as shown in FIG. 4(b), the film-like adhesive for semiconductors of this embodiment (hereinafter, sometimes referred to as the "film-like adhesive") 41 is attached to the substrate 20 on which the connection bumps 30 and the solder resist 60 have been formed, so that the surface of the second layer 41b containing the second adhesive faces the substrate 20. The attachment of the film-like adhesive 41 can be performed by hot pressing, roll lamination, vacuum lamination, or the like. The supply area and thickness of the film-like adhesive 41 are appropriately set depending on the sizes of the semiconductor chip 10 and the substrate 20, the height of the connection bumps 30, and the like. The attachment of the film-like adhesive 41 may be performed so that the surface of the first layer 41a containing the first adhesive faces the substrate 20.

[0150] After the film-like adhesive 41 is attached to the substrate 20 as described above, the wiring 15 of the semiconductor chip 10 and the connection bumps 30 are aligned using a connection device such as a flip chip bonder. Next, the semiconductor chip 10 and the substrate 20 are pressure-bonded while being heated at a temperature equal to or higher than the melting point of the connection bumps 30, and as shown in Fig. 4(c), the semiconductor chip 10 and the substrate 20 are connected, and the gap between the semiconductor chip 10 and the substrate 20 is sealed and filled by the sealing part 40 made of the cured product of the film-like adhesive 41. In this manner, the semiconductor device 600 is obtained.

[0151] The pressure-bonding time may be, for example, 5 seconds or less. In this embodiment, since the film-like adhesive 41 of the present embodiment described above is used, even if the pressure-bonding time is 5 seconds or less, a semiconductor device having excellent connection reliability can be obtained.

[0152] In the manufacturing method of the semiconductor device of this embodiment, after alignment, the semiconductor chips 10 and the substrate 20 may be temporarily fixed (through a film-like adhesive for semiconductors) and then heated in a reflow furnace to melt the connection bumps 30 and connect the semiconductor chips 10 and the substrate 20. Since it is not necessarily required to form a metal bond at the stage of temporary fixing, compression can be performed with a lower load, in a shorter time, and at a lower temperature than the above-mentioned method of compression bonding while heating, which improves productivity and suppresses deterioration of the connection.

[0153] In addition, after the semiconductor chip 10 and the substrate 20 are connected, a heat treatment may be performed in an oven or the like to further improve the connection reliability and insulation reliability. The heating temperature is preferably a temperature at which the film-like adhesive hardens, and more preferably a temperature at which the film-like adhesive hardens completely. The heating temperature and heating time are appropriately set.

[0154] In the method for manufacturing a semiconductor device of this embodiment, the substrate 20 may be connected after the film-like adhesive 41 is attached to the semiconductor chip 10.

[0155] From the viewpoint of improving productivity, a semiconductor film-like adhesive may be supplied to a semiconductor wafer having a plurality of semiconductor chips 10 connected thereto, and then the wafer is diced into individual pieces to obtain a structure in which the semiconductor film-like adhesive is supplied onto the semiconductor chips 10. The semiconductor film-like adhesive may be supplied so as to embed wiring, bumps, etc. on the semiconductor chips 10 by a bonding method such as hot pressing, roll lamination, and vacuum lamination. In this case, the amount of resin supplied is constant, improving productivity, and it is possible to suppress the occurrence of voids and deterioration of dicing properties due to insufficient embedding.

[0156] The connection load is set taking into consideration the variation in the number and height of the connection bumps 30, and the deformation of the connection bumps 30 due to pressure, or the wiring that receives the bumps at the connection parts. The connection temperature is preferably a temperature at the connection parts that is equal to or higher than the melting point of the connection bumps 30, but may be any temperature at which a metal bond is formed between the respective connection parts (bumps and wiring). When the connection bumps 30 are solder bumps, a temperature of about 240° C. or higher is preferable.

[0157] The connection time varies depending on the constituent metal of the connection portion, but from the viewpoint of improving productivity, the shorter the connection time, the better. When the connection bumps 30 are solder bumps, the connection time is preferably 20 seconds or less, more preferably 10 seconds or less, and even more preferably 5 seconds or less. In the case of copper-copper or copper-gold metal connection, the connection time is preferably 60 seconds or less.

[0158] The film-like adhesive for semiconductors of this embodiment also exhibits excellent reflow resistance and connection reliability in flip chip connections in the various package structures described above.

[0159] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES

[0160] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0161] <Preparation of a monolayer film with a flux-containing layer> The compounds used to prepare the monolayer films with the flux-containing layer are given below. (a) Epoxy resin - Triphenolmethane skeleton-containing multifunctional solid epoxy (Japan Epoxy Resins Co., Ltd., product name "EP1032H60") Bisphenol F type liquid epoxy (manufactured by Japan Epoxy Resin Co., Ltd., product name "YL983U") (b) Hardener 2,4-Diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct (manufactured by Shikoku Kasei Co., Ltd., product name "2MAOK-PW") (c) Fluxing agent Glutaric acid (Tokyo Chemical Industry Co., Ltd., melting point approx. 98°C) 2-Methylglutaric acid (Aldrich, melting point approx. 78°C) 3-Methylglutaric acid (Tokyo Chemical Industry Co., Ltd., melting point approx. 87°C) (d) Polymer component Phenoxy resin (manufactured by Tohto Kasei Co., Ltd., product name "ZX1356-2", Tg: approx. 71°C, weight average molecular weight Mw: approx. 63,000) (e) Filler Silica filler (Admatechs Co., Ltd., SE2050, average particle size: 0.5 μm) Epoxy silane surface treatment filler (Admatechs Co., Ltd., SE2050-SEJ, average particle size: 0.5 μm) Methacrylic surface-treated nano-silica filler (Admatechs Co., Ltd., YA050C-MJE, average particle size: approx. 50 nm) Organic filler (resin filler, Rohm and Haas Japan Co., Ltd., EXL-2655: core-shell type organic fine particles)

[0162] The epoxy resin, hardener, fluxing agent, inorganic filler, and organic filler in the amounts (unit: parts by mass) shown in Table 1 were added to an organic solvent (methyl ethyl ketone) so that the NV value ([mass of paint after drying] / [mass of paint before drying] x 100) was 60%. Then, Φ1.0 mm beads and Φ2.0 mm beads were added in the same mass as the solids (epoxy resin, hardener, fluxing agent, polymer component, inorganic filler, and organic filler), and the mixture was stirred for 30 minutes with a bead mill (Fritsch Japan Co., Ltd., planetary fine grinder P-7). After stirring, the beads were removed by filtration to prepare a coating varnish.

[0163] The obtained coating varnish was applied onto a base film (manufactured by Teijin DuPont Films Limited, product name "Purex A54") using a small precision coating device (Kanei Seiki) and dried (80°C / 10 min) in a clean oven (manufactured by ESPEC) to obtain the monolayer films (A-1), (A-2), and (A-3) shown in Table 1.

[0164] [Table 1]

[0165] <Preparation of a monolayer film with a flux-free layer> The compounds used to prepare the monolayer films with the non-flux-containing layer are shown below.

[0166] (A) (Meth)acrylic compound · Acrylate with a fluorene skeleton (Osaka Gas Chemicals Co., Ltd., EA-0200, two functional groups) · Acrylate with bisphenol A structure (Shin-Nakamura Chemical Co., Ltd., EA1020) Ethoxylated isocyanuric acid triacrylate (Shin-Nakamura Chemical Co., Ltd., A-9300)

[0167] (B) Thermal radical generator Dicumyl peroxide (NOF Corporation, Percumyl (registered trademark) D) Di-tert-butyl peroxide (NOF Corporation, Perbutyl (registered trademark) D) 1,4-bis-((tert-butylperoxy)diisopropyl)benzene (NOF Corporation, Perbutyl (registered trademark) P)

[0168] (C) Polymer component Acrylic resin (Hitachi Chemical Co., Ltd., KH-CT-865, weight average molecular weight Mw: 100,000, Tg: 10°C)

[0169] (D) Filler The same filler (component (d)) as that used in the preparation of the single-layer film having a flux-containing layer was used.

[0170] The (meth)acrylic compound, polymer component, inorganic filler and organic filler in the amounts (unit: parts by mass) shown in Table 2 were added to an organic solvent (methyl ethyl ketone) so that the NV value was 60%. Then, Φ1.0 mm beads and Φ2.0 mm beads were added in the same mass as the solid content ((meth)acrylic compound, polymer component, inorganic filler and organic filler) and stirred for 30 minutes with a bead mill (Fritsch Japan Co., Ltd., planetary fine grinder P-7). After stirring, the beads were removed by filtration. Next, a thermal radical generator was added to the obtained mixture, and the mixture was stirred and mixed to prepare a coating varnish.

[0171] The obtained coating varnish was applied onto a base film (manufactured by Teijin DuPont Films Limited, product name "Purex A54") using a small precision coating device (Kanei Seiki) and dried (80°C / 10 min) in a clean oven (manufactured by ESPEC) to obtain the monolayer films (B-1), (B-2), (B-3), (B-4), and (B-5) shown in Table 2.

[0172] [Table 2]

[0173] <Preparation of two-layer film> (Examples 1 and 2, and Comparative Examples 1 to 8) Two of the monolayer films prepared above (the first film and the second film) were laminated at 50° C. to prepare a film-like adhesive with a total thickness of 40 μm. The combination of the monolayer films was as shown in Table 3.

[0174] <Evaluation> The film-like adhesives obtained in the Examples and Comparative Examples were evaluated for initial connectivity, voids, solder wettability, and insulation reliability by the methods described below. The results are shown in Table 3.

[0175] (Initial connectivity assessment) The film-like adhesive prepared in the examples or comparative examples was cut to a predetermined size (8 mm long x 8 mm wide x 40 μm thick) to prepare an evaluation sample. Next, the evaluation sample was attached to a glass epoxy substrate (glass epoxy substrate: 420 μm thick, copper wiring: 9 μm thick), and a semiconductor chip with solder bumps (chip size: 7.3 mm long x 7.3 mm wide x 0.15 mm thick, bump height: copper pillar + solder total about 40 μm, number of bumps 328) was mounted using a flip mounting device "FCB3" (Panasonic, product name) (mounting conditions: pressure head temperature 350°C, pressure time 3 seconds, pressure pressure 0.5 MPa). As a result, a semiconductor device in which the glass epoxy substrate and the semiconductor chip with solder bumps were daisy-chain connected was prepared in the same manner as in FIG. 4. The evaluation samples of Examples 1 and 2 were attached to the glass substrate so that the flux-free layer and the glass epoxy substrate were in contact with each other.

[0176] The connection resistance of the obtained semiconductor device was measured using a multimeter (manufactured by ADVANTEST, product name "R6871E") to evaluate the initial continuity after mounting. When the connection resistance was 10.0 Ω or more and 13.5 Ω or less, the connectivity was rated as "A" (good), when the connection resistance was 13.5 Ω or more and 20 Ω or less, the connectivity was rated as "B" (poor), and when the connection resistance was more than 20 Ω, when the connection resistance was less than 10 Ω, and when no resistance value was displayed due to poor connection, the connectivity was rated as "C" (poor).

[0177] (Void evaluation) For the semiconductor device fabricated by the above method, an external image was taken with an ultrasonic imaging diagnostic device (trade name "Insight-300", manufactured by Insight), and an image of the adhesive layer (a layer made of a cured product of a film-like adhesive for semiconductors) on the chip was captured with a scanner GT-9300UF (trade name, manufactured by EPSON), and voids were identified by color correction and two-tone gradation using image processing software Adobe Photoshop (registered trademark), and the proportion of voids was calculated using a histogram. The area of ​​the adhesive part on the chip was taken as 100%, and the void occurrence rate was evaluated as "A" when it was 5% or less, "B" when it was more than 5% and less than 10%, and "C" when it was more than 10%.

[0178] (Solder wettability evaluation) The cross-sections of the connections of the semiconductor devices fabricated by the above method were observed, and the results were rated as "A" (good) if 90% or more of the solder was wetted on the top surface of the Cu wiring, and "B" (insufficient wetting) if less than 90% of the solder was wetted.

[0179] (Insulation Reliability Test [HAST Test: Highly Accelerated Storage Test]) The film-like adhesive (thickness: 40 μm) produced in the examples or comparative examples was attached to an interdigital electrode evaluation TEG (manufactured by Hitachi Chemical Co., Ltd., wiring pitch: 50 μm) and cured in a clean oven (manufactured by ESPEC) at 175° C. for 2 hours. The cured sample was placed in an accelerated life test device (manufactured by HIRAYAMA Corporation, product name "PL-422R8", conditions: 130° C. / 85% RH / 100 hours, 5 V applied) and the insulation resistance was measured. If the insulation resistance after 100 hours was 10 8 If it is Ω or more, it is marked as "A", and 10 7 Ω or more 10 8 If it is less than Ω, it is marked as "B", and if it is less than 10 7 If it was less than Ω, it was rated as "C".

[0180] [Table 3]

[0181] It was confirmed that the film-like adhesives for semiconductors of Examples 1 and 2 adequately suppressed the generation of voids, had good solder wettability, and were excellent in HAST resistance. [Explanation of symbols]

[0182] 10...semiconductor chip, 15...wiring (connection portion), 20...substrate (wired circuit board), 30...connection bump, 32...bump (connection portion), 34...through electrode, 40...sealing portion, 41...film-like adhesive for semiconductor, 50...interposer, 60...solder resist, 100, 200, 300, 400, 500, 600...semiconductor device.

Claims

1. A method for producing a film-like adhesive for semiconductors comprising a first layer made of a first adhesive and a second layer made of a second adhesive, comprising: (a) preparing a first resin varnish by adding at least one thermosetting resin selected from the group consisting of epoxy resins, phenolic resins, and polyimide resins, a curing agent, and a flux compound to an organic solvent and dissolving or dispersing the resin; (b) preparing a second resin varnish by adding at least a radical polymerizable compound and a thermal radical generator to an organic solvent and dissolving or dispersing the compound; (c) A method for producing a film-like adhesive for semiconductors, comprising the following steps (c1) to (c3), the following steps (c1) and (c4), or the following steps (c2) and (c5) (excluding the case where the second resin varnish contains an epoxy resin). (c1) A step of preparing a first film-like adhesive having the first layer by applying the first resin varnish onto a first base film and then reducing the organic solvent by heating to form the first layer. (c2) A step of preparing a second film-like adhesive having the second layer by applying the second resin varnish onto a second base film and then reducing the organic solvent by heating to form the second layer. (c3) A step of bonding the first film-like adhesive and the second film-like adhesive together. (c4) applying the second resin varnish onto the first layer, and then reducing the organic solvent by heating to form the second layer. (c5) applying the first resin varnish onto the second layer, and then reducing the organic solvent by heating to form the first layer.

2. The method for producing a film-like adhesive for semiconductors according to claim 1 , wherein the radical polymerizable compound comprises a (meth)acrylic compound.

3. The method for producing a film-like adhesive for semiconductors according to claim 2 , wherein the (meth)acrylic compound has a fluorene-type skeleton.

4. the thermosetting resin comprises an epoxy resin; The method for producing a film-like adhesive for semiconductors according to any one of claims 1 to 3, wherein the curing agent comprises at least one selected from the group consisting of a phenolic resin-based curing agent, an acid anhydride-based curing agent, and an amine-based curing agent.

5. The method for producing a film-like adhesive for semiconductors according to any one of claims 1 to 4, wherein the flux compound has two or more carboxyl groups.

6. The method for producing a film-like adhesive for semiconductors according to any one of claims 1 to 5, wherein the flux compound is a compound represented by the following formula (2): 【Chemistry 1】 [In formula (2), R 1 and R 2 each independently represents a hydrogen atom or an electron-donating group, n represents an integer of 0 or 1 or more.

7. The method for producing a film-like adhesive for semiconductors according to any one of claims 1 to 5, wherein the flux compound contains glutaric acid.

Citation Information

Patent Citations

  • Dicing tape integrated adhesive sheet, multilayer circuit board, electronic component and semiconductor device

    JP2012195414A

  • Circuit connection material, and method of manufacturing semiconductor device using the same

    JP2013211352A

  • Adhesive composition, and connection structure for circuit member

    WO2008015852A1

  • Adhesive for semiconductor, fluxing agent, manufacturing method for semiconductor device, and semiconductor device

    WO2013125086A1