Peelable coating film and paint set

A water-dispersed resin composition with immobilized silica particles and an inorganic binder creates a hydrophilic and peelable coating film, addressing appearance degradation and solvent risks, achieving effective antifouling and easy removal.

JP7582787B2Active Publication Date: 2024-11-13NITTO DENKO CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020049418
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-27
Filing Date
2020-03-19
Publication Date
2024-11-13
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Existing methods for making peelable coating films hydrophilic either degrade the film's appearance or pose health risks due to solvent use, and fail to form a stable hydrophilic surface when using crosslinking agents.

Method used

A water-dispersed resin composition with immobilized silica particles on the coating film surface via an inorganic binder, using colloidal silica, a binder, and an aqueous solvent to create a hydrophilic and peelable coating without organic solvents.

Benefits of technology

The solution provides a peelable coating film with high hydrophilicity and good surface appearance, facilitating easy removal and enhancing antifouling properties while avoiding solvent-related issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582787000002
    Figure 0007582787000002
  • Figure 0007582787000003
    Figure 0007582787000003
  • Figure 0007582787000001
    Figure 0007582787000001
Patent Text Reader

Abstract

To provide a peelable coated film which can be given hydrophilicity without degradation of the surface appearance.SOLUTION: A peelable coated film is formed of a water dispersible resin composition, in which silica particles are immobilized onto a surface of the coated film. The silica particles are immobilized to the surface of the coated film through a binder, and the binder is an inorganic binder and is at least one selected from alkali metal silicate, aluminosilicate, borosilicate, alkali metal salt, and boric acid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a peelable coating film, a coating set, and a coating material for forming a hydrophilic coating film. [Background technology]

[0002] Conventionally, in order to prevent adhesion of dirt and scratches to structures, a method of protecting the surface of the structure with a coating film has been used. In addition, a technique of making the coating film surface hydrophilic in order to enhance the antifouling effect is known.

[0003] Patent Document 1 discloses that an anti-fouling and anti-soiling agent containing methanol and / or ethanol, isopropyl alcohol, normal propyl alcohol or glycol ether, organosilica sol, tetrahydrofuran, and boric acid can be applied to the surface of an acrylic substrate, a polycarbonate substrate, or the like to form an inorganic cured coating film that has high hydrophilicity, hardness, adhesion strength to organic substrates, and water resistance and is excellent in anti-fouling and anti-fogging performance.

[0004] Patent Document 2 discloses that a hydrophilic coating film having excellent stain resistance, weather resistance, and hot water resistance can be formed by using a composition containing a swellable layered silicate, colloidal silica, and a crosslinking agent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-203774 A [Patent Document 2] JP 2014-070138 A Summary of the Invention [Problem to be solved by the invention]

[0006] From the viewpoint of antifouling properties and easy exchangeability, it is desirable for an antifouling coating film to adhere to a structure to protect the surface until a certain time and to be easily peelable at an appropriate time. Examples of such peelable coating films (hereinafter also referred to as peelable coating films) include coating films formed from water-dispersed resin compositions.

[0007] Therefore, the present inventors have attempted to hydrophilize the coating surface of the peelable coating film. However, as in the above Patent Document 1, when the coating surface was hydrophilized using a solvent-based paint containing an organic solvent as a solvent, the peelable coating film was not able to withstand the solvent and was deformed, and the appearance was deteriorated, so it was found that this method is not suitable for hydrophilizing the peelable coating film. In addition, when a solvent-based paint is used, there is a concern about the effect of the evaporated organic solvent on the human body, so it is desirable to hydrophilize the coating surface without using a solvent-based paint.

[0008] Furthermore, even when using an aqueous coating material using water or the like as a solvent as in Patent Document 2, when a crosslinking agent is used to crosslink silica particles to the coating surface to make it hydrophilic, it was found that in the case of a peelable coating, a crosslinked structure cannot be formed between the coating and the silica particles, and the surface of the peelable coating cannot be made hydrophilic.

[0009] Therefore, the present inventors have conducted extensive research into a method for hydrophilizing the surface of a peelable coating film, and as a result, have found that by using a coating material containing colloidal silica, a binder, and an aqueous solvent, silica particles can be fixed to the coating film surface via the binder without deteriorating the surface appearance, thereby making it possible to hydrophilize the peelable coating film surface, thereby completing the present invention. [Means for solving the problem]

[0010] That is, the present invention is as follows: [1] to

[14] . [1] A peelable coating film formed from a water-dispersible resin composition, A peelable coating film having silica particles fixed on the surface of the coating film. [2] The peelable coating film according to [1], wherein the silica particles are fixed on the surface of the coating film via a binder. [3] The peelable coating film according to [2], wherein the binder is an inorganic binder. [4] The peelable coating film according to [3], wherein the inorganic binder contains at least one binder selected from the group consisting of alkali metal silicates, aluminosilicates, borosilicates, alkali metal salts, and boric acid. [5] The peelable coating film according to any one of [1] to [4], wherein an antibacterial agent is immobilized on the surface of the coating film. [6] A paint for forming a peelable coating film, which is made of a water-dispersible resin composition, and and a hydrophilic coating film-forming coating material containing colloidal silica, a binder and an aqueous solvent, for forming a hydrophilic coating film on the peelable coating film. [7] The paint set according to [6], wherein the binder is an inorganic binder. [8] The paint set according to [7], wherein the inorganic binder contains at least one binder selected from the group consisting of alkali metal silicates, aluminosilicates, borosilicates, alkali metal salts, and boric acid. [9] The paint set according to any one of [6] to [8], wherein the paint for forming a hydrophilic coating film further contains an antibacterial agent.

[10] The paint set according to any one of [6] to [9], wherein the paint for forming a hydrophilic coating film further contains a wetting agent.

[11] The paint set according to any one of [6] to

[10] , wherein the paint for forming a hydrophilic coating film contains 0.1 to 30 parts by weight of colloidal silica (solid content) and 0.01 to 10 parts by weight of a binder per 100 parts by weight of an aqueous solvent.

[12] A coating material for forming a hydrophilic coating film, containing colloidal silica, alkali metal silicate, and a water-based solvent.

[13] The coating material for forming a hydrophilic coating film according to

[12] , further comprising an antibacterial agent.

[14] The coating material for forming a hydrophilic coating film according to

[12] or

[13] , further comprising a wetting agent. Effect of the Invention

[0011] The present invention can provide a peelable coating film having a highly hydrophilic coating surface and a good surface appearance. Furthermore, the present invention can provide a paint set capable of forming a peelable coating film having a highly hydrophilic coating film surface and a good surface appearance. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing a state in which a hydrophilic coating film is formed on a peelable coating film of the embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a state in which a hydrophilized peelable coating film is formed on an adherend. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail. In this specification, percentages based on mass and the like are synonymous with percentages based on weight and the like.

[0014] <Removable coating film with silica particles fixed> The peelable coating film of this embodiment has silica particles fixed on the surface of the coating film, which makes the surface of the peelable coating film exhibit excellent hydrophilicity.

[0015] In the peelable coating film of this embodiment, silica particles can be fixed on the surface of the coating film by applying a paint containing colloidal silica, a binder and an aqueous solvent (a paint for forming a hydrophilic coating film, described later) onto the peelable coating film 31 to form a hydrophilic coating film 21 on the coating film surface, as shown in Fig. 1. This allows the silica particles to be fixed on the surface of the peelable coating film via the binder.

[0016] [Removable coating film] The peelable coating film in this embodiment refers to a coating film that can be peeled off in a sheet form without cracking. The peelable coating film can be formed by applying and drying a paint for forming a peelable coating film made of a water-dispersible resin composition, and since it can be peeled off in sheets, the removal work can be made easy.

[0017] In the peelable coating film of this embodiment, the ratio of the film's breaking strength (tensile breaking strength) in a tensile test to the adhesive strength between the coating film and a SUS plate (SUS304) when the coating film is formed on the SUS plate can be used as an index of the peelability of the coating film. The tensile breaking strength is a strength indicating how difficult the coating film is to break when pulled. If the tensile breaking strength is low, the coating film breaks when peeling it from the adherend, making peeling difficult. In addition, if the adhesive strength is high, the force required to peel the coating film from the adherend becomes large, and as a result, the coating film becomes more likely to break. Therefore, in order to easily peel the coating film without breaking it, it is necessary for the ratio of the tensile breaking strength to the adhesive strength to be high.

[0018] The peelable coating film in this embodiment may satisfy the following criteria. That is, the ratio of the tensile breaking strength (N / 20 mm) to the adhesive strength (N / 20 mm) (peelability index) is 1.5 or more. From the viewpoint of ease of peeling, the peelability index is preferably 2.5 or more, more preferably 3.0 or more, and even more preferably 5.0 or more.

[0019] The tensile breaking strength means a value measured by the following method. A paint for forming a peelable coating film made of a water-dispersible resin composition is applied to the surface of a PET film (product name "Lumirror (registered trademark) S10", manufactured by Toray Industries, Inc., thickness 75 μm) with an applicator, and dried at 25 ° C for 12 hours to prepare a sample with a thickness (tensile film thickness) of 100 μm. The obtained film is further dried at 35 ° C for 4 hours, and then cut into a size of 20 mm × 80 mm, and the tensile breaking strength is measured using a tensile tester with an initial length of 60 mm and a tensile speed of 300 mm / min. The value converted assuming the width of the sample is 20 mm is taken as the tensile breaking strength (N / 20 mm).

[0020] The adhesive strength refers to a value measured by the following method. A peelable coating film-forming paint made of a water-dispersible resin composition is applied to the surface of a SUS plate (SUS304) with an applicator, dried at 25°C for 12 hours, and then dried at 35°C for 4 hours to prepare a sample with a thickness (peel film thickness) of 100 μm. Next, the remaining part is removed so that the coating film has a size of 20 mm x 100 mm. Using a tensile tester, the force when the coating film is peeled off from the SUS substrate at a peel angle of 180 degrees and a peel speed of 300 mm / min is measured as the adhesive strength. The value converted assuming the width of the sample is 20 mm is taken as the adhesive strength (N / 20 mm).

[0021] The tensile breaking strength is preferably 2.0N / 20mm or more, more preferably 2.5N / 20mm or more, and even more preferably 3.0N / 20mm or more. If the tensile breaking strength of the coating film is 2.0N / 20mm or more, the strength of the coating film is sufficiently high and the coating film can be peeled off. In addition, deformation of the coating film due to external force is prevented.

[0022] From the viewpoint of adhesion, the adhesive strength is preferably 0.5 N / 20 mm or more, and more preferably 1.0 N / 20 mm or more. From the viewpoint of workability during peeling, the adhesive strength is preferably 15 N or less, more preferably 10 N / 20 mm or less, and even more preferably 5 N / 20 mm or less.

[0023] The peelable coating film in this embodiment is formed by applying and drying a paint for forming a peelable coating film made of a water-dispersible resin composition. The water-dispersible resin composition is excellent in handleability because it can be formed into a film at room temperature (25°C). In addition, the coating film formed from the water-dispersible resin composition swells to a certain extent, so that the silica particles described below can be fixed to the coating film surface via a binder, and since it does not swell too much, even if dirt adheres to the coating film, it prevents the dirt from penetrating into the coating film, thereby exhibiting an excellent anti-fouling effect. In addition, it is also possible to wash the surface of the coating film with water or the like.

[0024] In this embodiment, the water content of the peelable coating film can be used as an index of swelling property, and there is a correlation between the swelling property of the coating film and the antifouling effect.

[0025] In order for the coating film to exhibit an excellent antifouling effect, the moisture content of the peelable coating film is preferably 200% or less, more preferably 120% or less. When an acrylic emulsion is used as the water-dispersible resin composition, the moisture content is preferably 120% or less, more preferably 110% or less. On the other hand, when a urethane emulsion is used as the water-dispersible resin composition, the moisture content is preferably 200% or less, more preferably 120% or less.

[0026] From the viewpoint of fixing the silica particles to the coating surface via the binder, the moisture content is preferably 103% or more, and more preferably 105% or more. The closer the moisture content is to 100%, the lower the swelling property is. Here, the moisture content refers to the mass change rate when the initial value is taken as 100%.

[0027] In this embodiment, the water content of the peelable coating film can be calculated by immersing the coating film in a 5% aqueous ethanol solution at 25° C. for 2 hours, measuring the mass before and after immersion, and using the following formula (1). Formula (1): Moisture content (%) = 100 + [(mass after immersion - mass before immersion) / mass before immersion] × 100

[0028] The peelability and swelling of the peelable coating film of this embodiment can be adjusted by the composition of the coating material for forming a hydrophilic coating film made of a water-dispersible resin composition, for example, by the type and content of the resin that can be contained, the type and content of the release agent or film-forming assistant that can be used in combination with the resin, etc.

[0029] The water-dispersed resin composition is an aqueous dispersion in which at least a resin is dispersed in water. As the aqueous dispersion, one in which the resin is dispersed in the presence of a surfactant is usually used, but if the resin is dispersed in water, one in which the resin is dispersed in water by the self-dispersion of a self-dispersing resin can be used.

[0030] (resin) In the water-dispersed resin composition, various resins can be used, such as acrylic resins, polyurethane resins, polystyrene resins, rubber resins, silicone resins, vinyl alkyl ether resins, polyvinyl alcohol resins, polyvinylpyrrolidone resins, polyacrylamide resins, cellulose resins, polyester resins, fluorine resins, etc. At least one selected from acrylic resins, polyurethane resins, polystyrene resins, and rubber resins is preferred, and acrylic resins and polyurethane resins are more preferred.

[0031] The acrylic resin is preferably one obtained by emulsion polymerization of a monomer component containing an alkyl (meth)acrylate, for example.

[0032] Examples of alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, and tetradecyl (meth)acrylate. These alkyl (meth)acrylates can be used alone or in combination of two or more. Among them, preferred alkyl (meth)acrylates include n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA).

[0033] In this specification, "(meth)acrylic" means acrylic and / or methacrylic. Acrylic resins include those containing acrylic acid or a derivative thereof as a constituent monomer component, and those containing methacrylic acid or a derivative thereof as a constituent monomer component.

[0034] The proportion of alkyl (meth)acrylate in all monomer components used in the synthesis of the acrylic resin is preferably 70% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more. The upper limit of the proportion of alkyl (meth)acrylate is not particularly limited, but it is usually preferably 99.5% by mass or less (for example, 99% by mass or less). Alternatively, the acrylic resin may be substantially a polymer of only alkyl (meth)acrylate.

[0035] The polyurethane resin is typically a reaction product of a polyol and a polyisocyanate. As the polyol component, a polymer polyol such as a polyacrylic polyol, a polyester polyol, or a polyether polyol is preferably used.

[0036] Polyacrylic polyol is typically obtained by polymerization of (meth)acrylic acid ester and hydroxyl group-containing monomer. Examples of (meth)acrylic acid ester include methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. Examples of hydroxyl group-containing monomer include hydroxyalkyl ester of (meth)acrylic acid such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypentyl (meth)acrylate, etc.; (meth)acrylic acid monoester of polyhydric alcohol such as glycerin and trimethylolpropane; N-methylol (meth)acrylamide, etc.

[0037] The polyester polyol is typically obtained by the reaction of a polybasic acid with a polyol. Examples of the polybasic acid include aromatic dicarboxylic acids such as orthophthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyldicarboxylic acid, and tetrahydrophthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, dodecanedicarboxylic acid, octadecanedicarboxylic acid, tartaric acid, alkyl succinic acid, linoleic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, tetrahydrophthalic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and reactive derivatives thereof such as acid anhydrides, alkyl esters, and acid halides.

[0038] Polyether polyols are typically obtained by adding alkylene oxides to polyhydric alcohols through ring-opening polymerization. Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerin, trimethylolpropane, etc. Examples of alkylene oxides include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, tetrahydrofuran, etc.

[0039] Examples of polyisocyanates include aliphatic diisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, 1,4-butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate; isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-cyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclo. Examples of the diisocyanate include alicyclic diisocyanates such as hexane; aromatic diisocyanates such as tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate; and aromatic aliphatic diisocyanates such as dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, and α,α,α,α-tetramethylxylylene diisocyanate.

[0040] Examples of polystyrene-based resins that can be used include SBS (styrene-butadiene block copolymer), SIS (styrene-isoprene block copolymer), SEBS (styrene-ethylene-butylene-styrene block copolymer), SEPS (styrene-ethylene-propylene-styrene block copolymer), and SEEPS (styrene-ethylene-ethylene-propylene-styrene block copolymer).

[0041] Examples of the rubber-based resin include acrylic rubber, diene rubber, butyl rubber, nitrile rubber, hydrogenated nitrile rubber, fluororubber, silicone rubber, ethylene propylene rubber, chloroprene rubber, urethane rubber, and epichlorohydrin rubber, and it is particularly preferable to use acrylic rubber, diene rubber, and urethane rubber. Examples of the diene-based rubber include natural rubber, isoprene rubber, butadiene rubber, styrene butadiene rubber, chloroprene rubber, and acrylonitrile butadiene rubber, and it is preferable to use styrene butadiene rubber.

[0042] The water-dispersed resin composition may contain a compound containing a polar group. Examples of such compounds include the resin containing the polar group, a silane coupling agent, a crosslinking agent, and silicone oil. Examples of the resin containing a polar group include an ionomer, a rosin resin, and a silicone resin.

[0043] The content of the above compound in the resin components in the water-dispersed resin composition is preferably 0.1 to 95 mass %, more preferably 0.5 to 60 mass %, even more preferably 0.5 to 40 mass %, particularly preferably 0.5 to 20 mass %, and most preferably 1 to 20 mass %, relative to the total mass of the resin components.

[0044] The content of the resin component in the water-dispersed resin composition is preferably 5 to 95 mass%, more preferably 10 to 90 mass%, even more preferably 15 to 80 mass%, particularly preferably 20 to 70 mass%, and most preferably 25 to 60 mass%.

[0045] The water-dispersed resin composition may be an emulsion, and is preferably an emulsion-type resin composition using a polymer emulsion obtained by emulsion polymerization.

[0046] The emulsion-type resin composition may be, for example, an emulsion containing the above-mentioned resin components, and an acrylic emulsion containing an acrylic resin or a urethane emulsion containing a urethane rubber is preferred.

[0047] Emulsion polymerization is carried out by emulsifying a monomer component in water by a conventional method, followed by emulsion polymerization. This prepares an aqueous dispersion (polymer emulsion). In emulsion polymerization, for example, a surfactant (emulsifier), a radical polymerization initiator, and optionally a chain transfer agent are appropriately mixed together with the monomer component. More specifically, for example, known emulsion polymerization methods such as a batch charging method (batch polymerization method), a monomer dropping method, and a monomer emulsion dropping method can be adopted.

[0048] In the monomer dropping method and monomer emulsion dropping method, continuous dropping or divided dropping is appropriately selected. These methods can be combined appropriately. The reaction conditions are appropriately selected, but the polymerization temperature is preferably about 40 to 95°C, and the polymerization time is preferably about 30 minutes to 24 hours.

[0049] The initiator used in emulsion polymerization can be appropriately selected from conventionally known polymerization initiators. For example, azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile can be preferably used. Other examples of polymerization initiators include persulfates such as potassium persulfate; peroxide-based initiators such as benzoyl peroxide and hydrogen peroxide; substituted ethane-based initiators such as phenyl-substituted ethane; aromatic carbonyl compounds; and the like.

[0050] Further examples of the polymerization initiator include redox initiators that are a combination of a peroxide and a reducing agent. Such polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator used may be a normal amount, and can be selected from the range of about 0.005 to 1 part by mass (typically 0.01 to 1 part by mass) per 100 parts by mass of the monomer raw material.

[0051] As the emulsifier, any of anionic, nonionic, and cationic emulsifiers can be used. These can be used alone or in combination of two or more. Usually, it is preferable to use anionic or nonionic emulsifiers.

[0052] Examples of the anionic emulsifier include sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkyl phenyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, and the like.

[0053] Examples of the nonionic emulsifier include polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers.

[0054] A radically polymerizable emulsifier (reactive emulsifier) ​​having a structure in which a radically polymerizable group such as a propenyl group is introduced into the anionic or nonionic emulsifier as described above may be used. Although not particularly limited, from the viewpoint of polymerization stability during synthesis of the resin and storage stability of the adhesive composition, an embodiment in which only an emulsifier having no radically polymerizable group is used may be preferably adopted.

[0055] In the above polymerization, various conventionally known chain transfer agents (which may also be understood as molecular weight regulators or polymerization degree regulators) may be used as necessary. Such chain transfer agents may be, for example, one or more selected from mercaptans such as n-lauryl mercaptan, tert-lauryl mercaptan, glycidyl mercaptan, and 2-mercaptoethanol. Among them, preferred chain transfer agents include n-lauryl mercaptan and tert-lauryl mercaptan.

[0056] When a chain transfer agent is used in the polymerization of the monomer raw material, the amount of the agent used is not particularly limited. For example, the amount may be about 0.001 to 0.5 parts by mass, and usually, it is preferably 0.01 to 0.1 parts by mass, per 100 parts by mass of the monomer raw material.

[0057] The Mw of the resulting resin is typically 10×10 4 or more, usually 20×10 4 From the viewpoint of achieving a good balance between adhesive strength and cohesive strength, Mw is 30×10 4 It is preferable that the value is 40×10 or more. 4 or more (e.g. 50×10 4 The upper limit of Mw is not particularly limited, and may be, for example, 500×10 4 Below, typically 200×10 4 Less than or equal to 150×10 4 It can be the following:

[0058] Mw can be adjusted, for example, by the type and amount of polymerization initiator, polymerization temperature, type and amount of emulsifier, whether or not a chain transfer agent is used and the type and amount of a chain transfer agent if used, the composition of the monomer raw material, the type and degree of crosslinking (gel fraction), etc.

[0059] (Removal agent and film forming aid) The water-dispersed resin composition may contain a release agent or a film-forming auxiliary. The release agent is an additive that adjusts the adhesive strength of the formed coating film and aids in peeling from the adherend. By including the release agent, the coating film formed from the water-dispersed resin composition has an appropriate adhesion to the adherend to be protected, and when peeling the coating film, the function of being able to peel the coating film completely without damaging the coating film can be easily maintained for a long period of time.

[0060] As the release agent, at least one compound selected from surfactants, polyhydric alcohols, waxes, etc. can be suitably used. These can be used in any form, whether dissolved or dispersed in water, or in powder form.

[0061] Examples of anionic surfactants include fatty acid salts such as sodium oleate, semi-hardened beef tallow soda, and potassium oleate; higher alcohol sulfate salts such as sodium lauryl sulfate, sodium higher alcohol sulfate, lauryl alcohol sulfate triethanolamine salt, and lauryl alcohol sulfate ammonium salt; alkyl benzene sulfonates such as sodium dodecyl benzene sulfonate; alkyl naphthalene sulfonates such as sodium alkyl naphthalene sulfonate; naphthalene sulfonic acid formalin condensates; dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate; alkyl phosphates; and the above-mentioned anionic surfactants to which ethylene oxide has been added. These may be used alone or in combination of two or more.

[0062] In particular, a phosphate ester type surfactant (for example, Phosphanol RS-410 (manufactured by Toho Chemical Industry Co., Ltd.)) is preferred, and the amount used is 0.001 to 5 mass %, preferably 0.005 to 3 mass %, and more preferably 0.005 to 1 mass % in the water-dispersible resin composition of the present invention.

[0063] In addition, the above anionic surfactants can also be used in combination with nonionic surfactants, for example, polyoxyethylene alkyl ethers such as polyoxyethylene oleyl ether and polyoxyethylene lauryl ether, polyoxyethylene alkyl phenyl ethers such as polyoxyethylene nonylphenyl ether and polyoxyethylene octylphenyl ether, polyoxyethylene alkyl esters such as polyoxyethylene monolaurate and polyoxyethylene monostearate, sorbitan esters such as sorbitan monolaurate and sorbitan monostearate, polyoxyethylene sorbitan alkyl esters such as polyoxyethylene sorbitan monolaurate, and polyoxyethylene polypropylene block polymers.

[0064] Furthermore, amphoteric surfactants, for example, betaine-type amphoteric surfactants such as dimethyl alkyl betaine, lauryl betaine, and stearyl betaine, and small amounts of cationic surfactants can also be used in combination.

[0065] Examples of polyhydric alcohols include ethylene glycol, propylene glycol, glycerin, catechol, butanediol, pentanediol, erythritol, glycerin monoalkyl esters, polyethylene glycol, and polypropylene glycol, and preferred are ethylene glycol, propylene glycol, and glycerin.

[0066] Specific examples of waxes include plant-based waxes such as candelabra wax, carnauba wax, rice wax, Japan wax, and jojoba oil; animal-based waxes such as beeswax, lanolin, and spermaceti; mineral-based waxes such as montan wax, ozokerite, and ceresin; petroleum-based waxes such as paraffin wax, microcrystalline wax, and petrolatum; synthetic hydrocarbon-based waxes such as Fischer-Tropsch wax, oxidized polyethylene wax, polyethylene wax, and acrylic-ethylene copolymer wax; modified wax-based waxes such as montan wax derivatives, paraffin wax derivatives, and microcrystalline wax derivatives; hydrogen-based waxes; hydrogenated castor oil and hydrogenated castor oil derivatives; and others such as 12-hydroxystearic acid, stearic acid amide, phthalic anhydride imide, bisamide, amide, glycerin ester, sorbitan ester, higher alcohol (C12 or more, preferably C16 or more), and higher fatty acid (C12 or more, preferably C16 or more).

[0067] The film-forming aid is an additive that aids in the formation of a coating film. After the coating film is formed, the film-forming aid evaporates relatively quickly and serves as a temporary plasticizing function that improves the strength of the coating film. An organic solvent with a boiling point of 110 to 200°C is preferably used.

[0068] For example, when the water-dispersed resin composition is an emulsion containing a resin component, by blending a film-forming aid, it becomes possible to form a film in a room temperature environment even if the resin component has an MFT above room temperature (15 to 35°C), and a highly uniform coating film can be obtained.

[0069] Specific examples include Texanol, propylene glycol monobutyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol monobutyl ether, diethylene glycol diethyl ether, dipropylene glycol monopropyl ether, carbitol, butyl carbitol, dibutyl carbitol, benzyl alcohol, etc. Among these, Texanol is particularly preferred because it has a high film-forming auxiliary effect even in a small amount.

[0070] The film-forming auxiliary is preferably contained in the water-dispersed resin composition in an amount of 0.5 to 15% by mass.

[0071] When the water-dispersed resin composition contains, for example, an acrylic resin as the resin (resin component), it preferably contains Texanol as a film-forming aid, or a phosphate ester surfactant as a release agent.

[0072] It is preferable that the water-dispersed resin composition contains an acrylic resin as the resin and further contains a release agent.

[0073] The water-dispersed resin composition may contain any suitable oil within the range that does not impair the effects of the present invention. Examples of such oils include silicone oil, liquid paraffin, surfactants, liquid hydrocarbons, fluorinated oils, waxes, petrolatum, animal fats, and fatty acids. These may be used alone or in combination of two or more kinds.

[0074] When the water-dispersed resin composition contains such an oil, the antifouling effect of the coating film may be more fully exhibited. Also, the adhesion of dirt may be more effectively prevented for a long period of time. Therefore, the appearance characteristics and mechanical properties of the coating film may be more fully exhibited.

[0075] Examples of the surfactant include anionic surfactants, nonionic surfactants, amphoteric surfactants, and cationic surfactants.

[0076] Examples of anionic surfactants include alkylbenzenesulfonates, alkyl or alkenyl ether sulfates, alkyl or alkenyl sulfates, α-olefinsulfonates, α-sulfofatty acids or ester salts, alkanesulfonates, saturated or unsaturated fatty acid salts, alkyl or alkenyl ether carboxylates, amino acid surfactants, N-acylamino acid surfactants, alkyl or alkenyl phosphates or salts thereof, etc. The anionic surfactants may be of only one type, or of two or more types.

[0077] Examples of nonionic surfactants include polyoxyalkylene alkyl or alkenyl ethers, polyoxyethylene alkylphenyl ethers, higher fatty acid alkanolamides or their alkylene oxide adducts, sucrose fatty acid esters, alkyl glycoxides, fatty acid glycerin monoesters, alkylamine oxides, etc. Only one type of nonionic surfactant may be used, or two or more types may be used.

[0078] Examples of the amphoteric surfactant include carboxy-type and sulfobetaine-type amphoteric surfactants, etc. The amphoteric surfactant may be one type only, or two or more types may be used.

[0079] Examples of cationic surfactants include quaternary ammonium salts, etc. The cationic surfactant may be one type only, or two or more types may be used.

[0080] The water-dispersible resin composition may contain any other appropriate additives within the scope of not impairing the effects of the present invention. Examples of such other additives include thickeners (e.g., association type, synthetic polymer type, alkali thickening type, etc.), colorants, weather resistance agents such as ultraviolet absorbers, light stabilizers, antibacterial agents, antioxidants, antifoaming agents, diatom adhesion inhibitors, agricultural chemicals, pharmaceuticals (medetomidine, etc.), enzyme activity inhibitors (alkylphenols, alkylresorcinols, etc.), biological repellents, fillers, etc.

[0081] As the antibacterial agent, any appropriate antibacterial agent can be used as long as it does not impair the effects of the present invention. Examples of such antibacterial agents include so-called antibacterial agents and antifungal agents.

[0082] Examples of so-called antibacterial agents include azoxystrobin, benalaxyl, benomyl, bitertanol, bromuconazole, captafol, captan, carbendazim, quinomethionate, chlorothalonil, chlozolinate, cyprodinil, dichlofluanid, diclofen, diclomedine, dicloran, diethofencarb, dimethomorph, diniconazole, dithianon, epoxyconazole, famoxadone, fenarimol, fenbuconazole, fenfuram, fenpiclonil, fentin, fluazinam, fludioxonil, fluorimide, fluquinconazole, flusulfamide, flutolanil, folpet, hexaclo These include bromobenzene, hexaconazole, imibenconazole, ipoconazole, iprodione, kresoxim methyl, manzeb, maneb, mepanipyrim, mepronil, metconazole, metiram, nickel bis(dimethyldithiocarbamate), nuarimol, oxine copper, oxolinic acid, pencycuron, phthalide, procymidone, propineb, quintozene, sulfur, tebuconazole, tecloftalam, tecnazene, thifluzamide, thiophenate methyl, thiram, tolclofos methyl, tolylfluanid, triadimefon, triadimenol, triazoxide, triforine, triticonazole, vinclozolin, zineb, and ziram.

[0083] In addition, examples of natural antibacterial agents include Chinese herbal medicines such as moso bamboo extract, hinokitiol, garlic extract, and licorice. In addition, examples of inorganic antibacterial agents include silver, copper, zinc, tin, lead, and gold. In addition, zeolite, hydroxyapatite, calcium carbonate, aluminum calcium silicate, polysiloxane compounds, zirconium phosphate, zirconium sulfate, ion exchangers, zinc oxide, and the like can be used as carriers for these inorganic antibacterial agents, if necessary.

[0084] Synthetic antibacterial agents include, for example, 2-pyridinethiol-1-oxide, p-chloro-m-cresol, polyhexamethylene hyguanide, hydrochloride, benzethonium chloride, alkylpolyaminoethylglycine, benzisothiazoline, 5-chloro-2-methyl-4-isothiazolin-3-one, 1,2-benzisothiazolin-3-one, 2,2'-dithio-bis-(pyridine-1-oxide), and the like.

[0085] Examples of the antifungal agent include sodium dehydroacetate, sodium benzoate, sodium pyridinethione-1-oxide, p-hydroxybenzoic acid ethyl ester, 1,2-benzisothiazolin-3-one and salts thereof.

[0086] Fillers and the like can be added to the water-dispersed resin composition to improve strength. Examples of fillers include silica particles, mica, kaolin, talc, and diatomaceous earth. The particle size is preferably 5 nm to 300 nm in average particle size. By adjusting the particle size within the above range, sufficient strength can be imparted to the coating film, and the particles can be uniformly dispersed in the coating film, making it difficult for cracks to occur when the coating film is subjected to an impact. In addition, the adhesion between the coating film and the adherend can be improved. The amount of particles added is preferably 0.1% by mass to 10% by mass with respect to the total mass of the resin components.

[0087] [Silica particles] In the peelable coating film of this embodiment, silica particles are fixed on the surface of the coating film. To fix the silica particles on the surface of the coating film, a paint (a paint for forming a hydrophilic coating film) containing colloidal silica, a binder and an aqueous solvent is applied to the surface of the peelable coating film and dried to form a hydrophilic coating film on the surface of the coating film. This allows the silica particles to be fixed on the surface of the peelable coating film via the binder.

[0088] Colloidal silica can impart hydrophilicity to the coating film and improve the antifouling properties. Examples of colloidal silica include colloidal fine particles of silicon dioxide (anhydrous silicic acid), as described in, for example, JP-A-53-112732, JP-B-57-9051, and JP-B-57-51653.

[0089] Furthermore, the colloidal silica may contain, for example, alumina, sodium aluminate, etc., as necessary, and may also contain, as necessary, a stabilizer such as an inorganic base (e.g., sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, etc.) or an organic base (e.g., tetramethylammonium, etc.).

[0090] Such colloidal silica can be produced by any known sol-gel method, specifically, for example, the sol-gel methods described in Werner Stober et al., J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al., Langmuir, 6, 792-801 (1990), and Journal of the Color Materials Association, 61[9], 488-493 (1988).

[0091] From the viewpoint of antifouling, it is preferable to use water-dispersed colloidal silica in which spherical silica particles are dispersed in water. The spherical silica particles dispersed in the colloidal silica preferably have an average particle size of 5 to 100 nm. If the average particle size is less than 5 nm, the adhesion to the peelable coating film, which is the undercoat layer, is insufficient and the film is easily peeled off, while if it exceeds 100 nm, the transparency of the film tends to be impaired.

[0092] The viscosity of the colloidal silica is preferably 1 to 25 mPa·s. The pH of the colloidal silica is preferably 7-12, and more preferably 8-10.

[0093] In addition, as such colloidal silica, commercially available products can be used. Specific examples thereof include products sold under the trade names "Snowtex (registered trademark)-XL", "Snowtex (registered trademark)-YL", "Snowtex (registered trademark)-ZL", "PST-2", "Snowtex (registered trademark)-20", "Snowtex (registered trademark)-30", "Snowtex (registered trademark)-30L", "Snowtex (registered trademark)-C", "Snowtex (registered trademark)-O", "Snowtex (registered trademark)-OS", "Snowtex (registered trademark)-OL", and "Snowtex (registered trademark)-50" (all manufactured by Nissan Chemical Industries, Ltd.), and product names "Adelite (registered trademark) AT-30", "Adelite (registered trademark) AT-40", and "Adelite (registered trademark) AT-50" (all manufactured by Nippon Aerosil Co., Ltd.).

[0094] There are no particular limitations on the binder as long as it has the function of fixing silica particles and the like to the surface of the peelable coating film, but from the viewpoint of fixing the silica particles to the peelable coating film, it is preferable that the binder be an inorganic binder having a silanol group.

[0095] Examples of inorganic binders include alkali metal silicates, aluminosilicates, borosilicates, alkali metal salts, and boric acid. Among these, alkali metal silicates are preferred from the viewpoint of fixing silica particles to a peelable coating film. Examples of alkali metal silicates include sodium silicate, potassium silicate, and lithium silicate. Moreover, cellulose nanofibers may be used as the binder.

[0096] As the aqueous solvent, a solution containing water can be used. Here, the solution containing water may be pure water, or may be a mixed solution or mixed solvent of water and a substance other than water. An example of the substance other than water is alcohol such as ethanol.

[0097] The thickness of the peelable coating film may be any appropriate thickness depending on the application and the environment of use. The thickness of the peelable coating film is preferably 10 μm to 1000 μm. When the thickness of the coating film falls within the above range, the antifouling effect is sufficiently long and effective. When the thickness of the peelable coating film is 10 μm or more, the antifouling effect is effectively exhibited and it is practical. When the thickness of the coating film is 1000 μm or less, the work efficiency is excellent.

[0098] From the viewpoints of durability and adhesion to the peelable coating film, the thickness of the hydrophilic coating film is preferably 0.01 μm to 1 μm. A thickness of 0.01 μm or more provides sufficient durability to the coating film surface, while a thickness of 1 μm or less provides excellent adhesion to the peelable coating film. The thickness of the coating film can be measured, for example, using RI-205 manufactured by PEAKOCK.

[0099] In the peelable coating film having silica particles fixed thereto in this embodiment, when 2 μm of water is dropped onto the coating surface and after 5 minutes, the contact angle of the coating surface is measured by the sessile drop method according to JIS R 3257:1999, and is preferably 40° or less, more preferably 20° or less, and even more preferably 10° or less.

[0100] <Paint set> The paint set of this embodiment includes a paint for forming a peelable coating film, which is made of a water-dispersible resin composition, and a paint for forming a hydrophilic coating film, which contains colloidal silica, a binder and an aqueous solvent, and is for forming a hydrophilic coating film on the peelable coating film.

[0101] [Paint for forming peelable coating film] The paint for forming a peelable coating film is made of the above-mentioned water-dispersible resin composition, and the above-mentioned ones can be used.

[0102] The paint for forming a peelable coating film can be applied to an adherend 41 and dried to form a peelable coating film 31, as shown in Figure 2. A highly uniform coating film can be obtained even when dried at room temperature (25°C).

[0103] The composition can be applied directly to any substrate by any known application method such as spraying, brushing, roller, curtain flow, roll, dip, or coater.

[0104] The drying method can be, for example, at a temperature of 0°C to 250°C (preferably, room temperature (25°C) to 180°C, more preferably, room temperature to 160°C), for example, for 2 minutes to 12 hours (first drying).

[0105] If necessary, the coating can be further dried (second drying) for, for example, 2 minutes to 12 hours at a temperature of 0°C to 250°C (preferably, room temperature (25°C) to 180°C, more preferably, room temperature to 160°C). This promotes fusion of grain boundaries and increases the uniformity of the coating film, making it possible to form a coating film that is less prone to swelling and has excellent antifouling properties.

[0106] The second drying is preferably performed at a temperature 0 to 20° C. higher than the first drying temperature for a shorter time than the first drying temperature.

[0107] Specific examples of the adherend include various structures such as metal products, wood products, plastic products, glass products, medical components (e.g., catheters, stents, gloves, tweezers, containers, guides, trays, etc.), buildings (interior and exterior wall surfaces, floor surfaces, and ceiling surfaces), electronic devices, and transportation equipment (e.g., automobiles, motorcycles, railway vehicles, and ships, etc.).

[0108] Since the content of organic solvents in the water-dispersed resin composition is extremely small, it can be used for applications such as cell culture dishes, plates such as microwells, carrier trays, containers, tanks, guides, food manufacturing equipment, walls and tables of hospitals, nursing homes and kindergartens, and coatings in places where food is handled. It can be used to form antifouling coating films for medical equipment, etc.

[0109] [Paint for forming hydrophilic coatings] The coating material for forming a hydrophilic coating film contains colloidal silica, a binder and an aqueous solvent, and these can be those described above.

[0110] The content of colloidal silica (solid content) in the coating material for forming a hydrophilic coating film is preferably 0.1 parts by weight or more, more preferably 0.5 parts by weight or more, and even more preferably 1 part by weight or more, relative to 100 parts by weight of the aqueous solvent. By being 0.1 parts by weight or more, a highly uniform silica-containing layer can be formed regardless of the coating method. In addition, it is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, and even more preferably 15 parts by weight or less. By being 30 parts by weight or less, deterioration of the coating film appearance can be prevented.

[0111] The content of the binder in the coating material for forming a hydrophilic coating film is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and even more preferably 0.1 parts by weight or more, relative to 100 parts by weight of the aqueous solvent. By being 0.01 parts by weight or more, the adhesion of the silica particles is increased. In addition, it is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 1 part by weight or less. By being 10 parts by weight or less, instability of the coating composition such as gelation can be prevented.

[0112] The coating material for forming a hydrophilic coating film may contain a wetting agent. By containing a wetting agent in the coating material for forming a hydrophilic coating film, the wettability of the surface can be improved when the coating material is applied onto the surface of a peelable coating film, and the coating material can be applied without liquid unevenness.

[0113] The wetting agent is not particularly limited, and various surfactants such as anionic, nonionic, amphoteric, and cationic surfactants can be used. Specifically, examples of anionic surfactants having a carboxyl group or a sulfonic group as a hydrophilic group include fatty acid soaps and alkylbenzene sulfonates. Other examples include cationic surfactants having a quaternary ammonium group, amphoteric surfactants having both cations and anions in the same molecule such as long-chain alkyl amino acids, and nonionic surfactants having a nonionic polar group such as polyoxyethylene nonylphenyl ether.

[0114] The content of the wetting agent in the coating material for forming a hydrophilic coating film is preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, and even more preferably 1 part by weight or more, based on 100 parts by weight of the aqueous solvent. By being 0.01 parts by weight or more, the wettability of the surface of the peelable coating film can be sufficiently improved. In addition, it is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 2.5 parts by weight or less. By being 10 parts by weight or less, the stability of the colloidal silica can be maintained.

[0115] The paint for forming a hydrophilic coating film may contain an antibacterial agent. By containing an antibacterial agent in the paint for forming a hydrophilic coating film, when a hydrophilic coating film is formed on the peelable coating film, the antibacterial agent can be fixed on the surface of the peelable coating film via the above-mentioned binder or the like. This allows the antibacterial effect to be exerted on the coating film surface. The antibacterial property of the antibacterial agent can be evaluated, for example, by JIS Z 2801:2010.

[0116] As the antibacterial agent, any suitable antibacterial agent can be adopted as long as it does not impair the effects of the present invention. Examples of such antibacterial agents include so-called antibacterial agents and antifungal agents. Specifically, the same antibacterial agents as those that can be contained in the above-mentioned water-dispersed resin composition can be used.

[0117] The content of the antibacterial agent in the coating material for forming a hydrophilic coating film is preferably 0.001 parts by weight or more, more preferably 0.01 parts by weight or more, and even more preferably 0.1 parts by weight or more, relative to 100 parts by weight of the aqueous solvent. By being 0.001 parts by weight or more, a good antibacterial effect can be obtained. In addition, it is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less. By being 20 parts by weight or less, the storage stability of the coating material for forming a hydrophilic coating film in a liquid state is increased, and the impact on the appearance after application is reduced.

[0118] The coating material for forming a hydrophilic coating film may contain any other suitable additives, such as an ultraviolet absorber, a light stabilizer, a filler, etc.

[0119] There is no particular limitation on the method for applying the coating material containing colloidal silica, a binder, and an aqueous solvent to the surface of the peelable coating film, and the coating material can be directly applied onto the peelable coating film by a known application method such as spray coating, dip coating, spin coating, brush coating, sponge coating, roller coating, curtain flow coating, roll coating, coater coating, etc. In this way, the hydrophilic coating film 21 can be formed on the peelable coating film 31.

[0120] The drying method can be, for example, at a temperature of 0°C to 250°C (preferably, room temperature (25°C) to 180°C, more preferably, room temperature to 160°C), for example, for 2 minutes to 12 hours (first drying).

[0121] If necessary, it can be further dried (second drying) at a temperature of, for example, 0°C to 250°C (preferably, room temperature (25°C) to 180°C, more preferably, room temperature to 160°C), for example, for 2 minutes to 12 hours.

[0122] The second drying is preferably performed at a temperature 0 to 20° C. higher than the first drying temperature for a shorter time than the first drying temperature. EXAMPLES

[0123] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.

[0124] Example 1 [Creating the base layer] Example 1 was prepared by mixing 100 parts by weight of an acrylic resin (acrylic resin, product name "AP-609LN", manufactured by Showa Denko K.K.) and 0.01 parts by weight of a release agent as an additive (phosphate ester type surfactant, product name "Phosphanol RS-410", manufactured by Toho Chemical Industry Co., Ltd.), stirring the mixture at a rotation speed of 3000 rpm in a disper for 3 minutes or more, and vacuum degassing the mixture at 2200 rpm for 5 minutes in a Thinky Mixer, thereby preparing a water-dispersible resin composition (paint for forming a peelable coating film) of Example 1. The water-dispersed resin composition prepared above was applied to the surface of a 75 μm-thick PET film (product name "Lumirror (registered trademark) S10", manufactured by Toray Industries, Inc.) with a wet thickness of 250 μm using an applicator. The film was dried at room temperature (25° C.) for 12 hours, and the formed coating film was further dried at 35° C. for 4 hours to prepare a base layer on the PET film, which was used as a laminate sample. [Hydrophilic treatment] A hydrophilic coating film-forming paint was prepared by mixing 3 parts by weight (solid content) of colloidal silica (product name "Snowtex (registered trademark)-30", manufactured by Nissan Chemical Industries, Ltd.), 0.3 parts by weight of sodium silicate (manufactured by Fuji Chemical Industries, Ltd.) as a binder, 0.2 parts by weight of a nonionic surfactant (product name "SN Wet 366", manufactured by San Nopco Ltd.) as a wetting agent, and 100 parts by weight of water as an aqueous solvent. The laminate sample prepared above was immersed in the coating material for forming a hydrophilic coating film for about 5 seconds and then pulled out. The sample was placed at an angle of 45 degrees and dried at 25°C for 10 minutes, then turned upside down and left to stand at 25°C for 24 hours, dried, and hydrophilized. Water was then dropped onto the surface of the peelable coating film, and the surface was scrubbed with a paper wiper three times to remove the wetting agent on the coating film surface and any components not adhering to the sample.

[0125] (Examples 2 to 10) Laminate samples of Examples 2 to 10 were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1, and were subjected to a hydrophilization treatment.

[0126] (Examples 11 to 16) Laminate samples of Examples 11 to 16 were prepared and subjected to hydrophilization treatment in the same manner as in Example 1, except that an antibacterial agent was added as shown in Table 1 and the types and amounts of other components were changed as shown in Table 1.

[0127] (Comparative Examples 1 to 6) Laminate samples of Comparative Examples 1 to 6 were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1, and were subjected to a hydrophilization treatment.

[0128] (Comparative Examples 7 to 9) Instead of preparing a peelable coating film, a plate as shown in Table 1 was used, and the plate was subjected to a hydrophilization treatment in the same manner as in Example 1.

[0129] [Evaluation of peelability] For the coating films produced using "AP-609LN" in Examples 1, 3 to 9, 11, 13, and 15 and Comparative Examples 1 to 6, the coating film produced using "WLS210" in Example 2, and the coating films produced using "WS-6021" in Examples 10, 12, 14, and 16, the tensile breaking strength and adhesive strength were measured to evaluate the peelability, and the ratio of the tensile breaking strength (N / 20 mm) to the adhesive strength (N / 20 mm) (peelability index) was calculated. (Measurement of tensile breaking strength) The water-dispersed resin compositions in Examples 1 to 16 and Comparative Examples 1 to 6 were applied to the surface of a PET film (product name "Lumirror (registered trademark) S10", manufactured by Toray Industries, Inc., thickness 75 μm) using an applicator, and dried at 25° C. for 12 hours to prepare a sample with a thickness (tensile film thickness) of 100 μm. The obtained film was further dried at 35° C. for 4 hours, and then cut into a size of 20 mm x 80 mm, and the tensile breaking strength was measured using a tensile tester (device name "AUTOGRAPH AGS-X", manufactured by Shimadzu Corporation) with an initial length of 60 mm and a pulling speed of 300 mm / min. The value converted assuming the width of the sample to be 20 mm was taken as the tensile breaking strength (N / 20 mm).

[0130] (Method of measuring adhesive strength) A coating film was prepared by the following method, and the adhesive strength was measured. The water-dispersed resin composition in Examples 1 to 16 and Comparative Examples 1 to 6 was applied to the surface of a SUS plate (SUS304) with an applicator, dried at 25°C for 12 hours, and further dried at 35°C for 4 hours to prepare a sample with a thickness (peel film thickness) of 100 μm. Next, the remaining part was removed so that the coating film had a size of 20 mm x 100 mm. Using a tensile tester (AUTOGRAPH AGS-X, manufactured by Shimadzu Corporation), the force when the coating film was peeled off from the SUS substrate at a peel angle of 180 degrees and a peel speed of 300 mm / min was measured as the adhesive strength. The value converted assuming the width of the sample to be 20 mm was taken as the tensile breaking strength (N / 20 mm). As a result of the measurement, the peelability index of the coating films in Examples 1, 3 to 9, 11, 13, and 15 and Comparative Examples 1 to 6 prepared using "AP-609LN" was 2.4, the peelability index of the coating film in Example 2 prepared using "WLS210" was 77, and the peelability index of the coating films in Examples 10, 12, 14, and 16 prepared using "WS-6021" was 11.4. That is, all of the coating films had a peelability index of 1.5 or more, indicating peelability.

[0131] [Moisture content measurement] The water-dispersed resin composition containing "AP-609LN" used in Examples 1, 3 to 9, 11, 13, 15 and Comparative Examples 1 to 6, the water-dispersed resin composition containing the resin "WLS210" used in Example 2, and the water-dispersed resin composition containing "WS-6021" used in Examples 10, 12, 14, 16 were applied to the surface of a PET substrate film (product name "Lumirror (registered trademark) S10", manufactured by Toray Industries, Inc.) having a thickness of 75 μm with an applicator, dried at 25 ° C for 12 hours, and a sample having a thickness (tensile film thickness) of 100 μm was prepared. After further drying at 35 ° C for 4 hours, the obtained coating film was cut to a size of 20 mm × 20 mm, and the mass was measured without peeling it off from the PET substrate. The sample was placed in a glass bottle containing a solution (5% aqueous ethanol solution) and left to stand (immersed) at 25 ° C for 2 hours. After 2 hours, the sample was taken out, the water droplets on the surface were quickly wiped off, and the mass was measured to determine the mass before and after immersion. In addition, the mass (W PET ) was measured, and the moisture content was calculated according to the following formula (1). Formula (1): Moisture content (%) = 100 + [((mass after immersion - W PET )-(mass before immersion-W PET )) / (mass before immersion-W PET ) x 100 As a result of the measurements, the moisture content of the coating films in Examples 1, 3 to 9, 11, 13, and 15 and Comparative Examples 1 to 6 prepared using "AP-609LN" was 107%, the moisture content of the coating film in Example 2 prepared using "WLS210" was 184%, and the moisture content of the coating films in Examples 10, 12, 14, and 16 prepared using "WS-6021" was 103%.

[0132] [Contact angle measurement] For the samples obtained by carrying out the hydrophilization treatments of the Examples and Comparative Examples, 2 μL of water was dropped onto the coating surface, and the contact angle of the coating surface after 5 minutes was measured using a contact angle measuring device (DropMaster, manufactured by Kyowa Interface Science Co., Ltd.) by the sessile drop method according to JIS R 3257. The results are shown in Table 1.

[0133] [Appearance evaluation] The change in appearance before and after the hydrophilization treatment was evaluated as ◯ if there was no change, and × if there was a change. The results are shown in Table 1.

[0134] [Antibacterial evaluation] The antibacterial activity values ​​of the samples obtained by carrying out the hydrophilization treatments of Examples 9 to 16 were determined according to JIS Z 2801:2010. In addition, an antibacterial activity value of 2.0 or more was evaluated as ◯, and an antibacterial activity value of less than 2.0 was evaluated as ×. The results are shown in Table 1.

[0135] The component compositions and the measurement and test results for each of the examples and comparative examples are summarized in Table 1.

[0136] [Table 1]

[0137] Details of the product names in Table 1 above are as follows: [Base layer] (resin) AP-609LN (Showa Denko Co., Ltd., acrylic emulsion) WLS210 (DIC Corporation, urethane dispersion) WS-6021 (Mitsui Chemicals, urethane dispersion) (board) PMMA plate (made by Nippon Test Panel Co., Ltd.) ABS board (made by Nippon Test Panel Co., Ltd.) POM plate (manufactured by Nippon Test Panel Co., Ltd.)

[0138] [Paint for forming hydrophilic coatings] (Colloidal Silica) Snowtex (registered trademark)-30 (Nissan Chemical Industries, Ltd., water-dispersed colloidal silica, Solid content (SiO2) 30% by mass, particle size 10~15nm, pH9.5~10.5, viscosity 1.0~6.0mPa·s) Snowtex (registered trademark)-30L (Nissan Chemical Co., Ltd., water-dispersed colloidal silica, solid content (SiO2) 30 mass%, particle size 40-50 nm, pH 9.5-10.5, viscosity 1.0-6.0 mPa·s) Snowtex (registered trademark)-C (Nissan Chemical Co., Ltd., water-dispersed colloidal silica, solid content (SiO2) 20 mass%, particle size 10 to 15 nm, pH 8.5 to 9.0, viscosity 1.0 to 10.0 mPa s) (Binder) Sodium silicate (manufactured by Fuji Chemical Co., Ltd., sodium silicate) Lithium silicate (Nissan Chemical Co., Ltd., lithium silicate) MS51 (Mitsubishi Chemical Corporation, methyl silicate) K-2010E (Mitsubishi Chemical Corporation, oxazoline crosslinking agent) V-02 (Nisshinbo Chemical Co., Ltd., carbodiimide crosslinking agent) KBM402 (Shin-Etsu Chemical Co., Ltd., epoxy group-containing silane coupling agent) Cellenpia (registered trademark) (Nippon Paper Industries Co., Ltd., cellulose nanofiber) Aluminum(III) acetylacetonate (TCI Corporation, cross-linking agent) A-21S (Mica, manufactured by Yamaguchi Mica Co., Ltd.) (Antibacterial agent) Silver nanoparticles (manufactured by Skyspring Nanomaterials, a silver-based inorganic antibacterial agent) Ion Pure (Ishizuka Glass Co., Ltd., silver-based inorganic antibacterial agent) Zeomic (Sinanen Zeomic Co., Ltd., silver-based inorganic antibacterial agent) (Wetting agent) SN Wet 366 (San Nopco Ltd., non-ionic surfactant) Polyethylene glycol monolaurate (TCI Corporation, wetting agent)

[0139] As can be seen from the results in Table 1, the use of a water-based paint containing colloidal silica and a binder made it possible to hydrophilize the peelable coating film surface without deteriorating the surface appearance. Note that in Comparative Examples 1 and 3 to 6, fixation of silica was not confirmed. Furthermore, the hydrophilic coating material in Examples 11 to 16 contained an antibacterial agent, thereby imparting antibacterial properties to the peelable coating film surface.

[0140] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the present invention. [Explanation of symbols]

[0141] 1. Hydrophilic surface, peelable coating film 21 Hydrophilic coating 31 Peelable coating 41 Adherent

Claims

1. A peelable coating film formed from a water-dispersible resin composition, Silica particles are fixed on the surface of the coating film via an inorganic binder, The peelable coating film, wherein the inorganic binder contains at least one binder selected from the group consisting of alkali metal silicates, aluminosilicates, borosilicates, alkali metal salts, and boric acid.

2. The peelable coating of claim 1 , wherein an antimicrobial agent is immobilized on the surface of the coating.

3. A paint for forming a peelable coating film, which is made of a water-dispersible resin composition, and a coating material for forming a hydrophilic coating film, the coating material containing colloidal silica, an inorganic binder and an aqueous solvent, for forming a hydrophilic coating film on the peelable coating film; The paint set, wherein the inorganic binder contains at least one binder selected from the group consisting of alkali metal silicates, aluminosilicates, borosilicates, alkali metal salts, and boric acid.

4. The paint set according to claim 3 , wherein the paint for forming a hydrophilic coating film further contains an antibacterial agent.

5. 5. The paint set according to claim 3, wherein the paint for forming a hydrophilic coating film further comprises a wetting agent.

6. The paint set according to any one of claims 3 to 5, wherein the paint for forming a hydrophilic coating film contains 0.1 to 30 parts by weight of the colloidal silica (solid content) and 0.01 to 10 parts by weight of the inorganic binder relative to 100 parts by weight of the aqueous solvent.

Citation Information

Patent Citations

  • Demolding coating for slag pot and preparation method thereof

    CN109054468A

  • Inorganic water-based coating material composition and formation of inorganic coating film using the same

    JP2000109722A

  • Composite sheet and method for manufacturing plastic molding using the same

    JP2002011821A

  • Surface-treated metallic sheet with outstanding press scoring resistance and coil deformation resistance and manufacturing method therefor

    JP2002210866A

  • Separate film for aqueous gel sheet

    JP2003320621A