Aqueous ionomer dispersions and methods thereof

Stable aqueous ionomer dispersions are achieved by neutralizing ethylene acid copolymers with monovalent and zinc cations, addressing dispersibility issues and enhancing electrostatic properties for coating applications.

JP7582948B2Active Publication Date: 2024-11-13DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021534817
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-20
Filing Date
2019-12-17
Publication Date
2024-11-13
Estimated Expiration
2039-12-17

AI Technical Summary

Technical Problem

Ionomers neutralized with polyvalent cations form polymeric crosslinks, making them less dispersible in water, while those neutralized with monovalent salts like potassium or sodium have high melt viscosity and hydrophobicity, hindering their aqueous dispersion.

Method used

Aqueous ionomer dispersions comprising ethylene acid copolymers with 70-85% ethylene and 15-30% monocarboxylic acid, neutralized with 70-100% monovalent cations and 15-50% zinc cations, combined with up to 80% polyolefin, to form stable dispersions.

Benefits of technology

The solution enables the formation of stable, easily dispersible ionomer dispersions with improved electrostatic properties and enhanced powder retention, suitable for coating various substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582948000007
    Figure 0007582948000007
  • Figure 0007582948000008
    Figure 0007582948000008
  • Figure 0007582948000009
    Figure 0007582948000009
Patent Text Reader

Abstract

An aqueous ionomer dispersion and method for producing the same, comprising an ionomer composition and water, wherein the ionomer composition comprises: a) at least 20 wt. % of an ionomer, based on the total weight percent of the ionomer composition; and b) up to 80 wt. % of a polyolefin, based on the total weight percent of the ionomer composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE Embodiments described herein relate generally to aqueous dispersions of ionomers and methods of forming aqueous dispersions of ionomers. More specifically, embodiments of the aqueous dispersions described herein can be used to coat a substrate. [Background technology]

[0002] Ionomers can be prepared by reacting metal salts with poly(ethylene (meth)acrylic acid) copolymers (base resins). Ionomers neutralized with multivalent cations such as divalent and trivalent cations have been found to be difficult to disperse in water due to the tendency of the multivalent cations to form polymeric crosslinks. On the other hand, ionomers neutralized with monovalent salts of volatile bases such as potassium, sodium, or ammonia are also difficult to disperse in water due to increased melt viscosity and hydrophobicity.

[0003] It would therefore be desirable to have alternative ionomer compositions that more readily form aqueous dispersions of the ionomer. Summary of the Invention

[0004] An aqueous ionomer dispersion is disclosed in the present embodiment. The aqueous ionomer dispersion includes an ionomer composition and water, the ionomer composition includes: a) at least 20 wt% of an ionomer based on the total weight percent of the ionomer composition, the ionomer being an at least partially neutralized ethylene acid copolymer, the ethylene acid copolymer being a polymerization reaction product of 70-85 wt% ethylene and 15-30 wt% monocarboxylic acid based on the total weight of monomers present in the ethylene acid copolymer, at least 70 mol% of the total acid units of the ethylene acid copolymer are neutralized, 15 mol%-50 mol% of the total acid units of the ethylene acid copolymer are neutralized with zinc cations, and 40 mol% of the total acid units of the ethylene acid copolymer are neutralized with monovalent cations, and b) up to 80 wt% of a polyolefin based on the total weight percent of the ionomer composition.

[0005] Also disclosed in embodiments herein is a method for producing an aqueous ionomer dispersion. The method includes providing an ionomer composition comprising: a) at least 20 weight percent of an ionomer, based on the total weight percent of the ionomer composition, the ionomer being an at least partially neutralized ethylene acid copolymer, the ethylene acid copolymer being a polymerization reaction product of 70 to 85 weight percent ethylene and 15 to 30 weight percent monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer, and wherein 15 mol % to 50 mol % of the total acid units of the ethylene acid copolymer are neutralized with zinc cations; and b) up to 80 weight percent of a polyolefin, based on the total weight percent of the ionomer composition; and mixing the ionomer composition with an aqueous composition comprising water and a monovalent cation to form an aqueous ionomer dispersion, the ionomer in the aqueous ionomer dispersion having at least 70 mol % of the total acid units of the ethylene acid copolymer neutralized and at least 40 mol % of the total acid units of the ethylene acid copolymer neutralized with monovalent cations.

[0006] Further disclosed in embodiments herein is a method of forming a coated article. The method includes coating a substrate with an aqueous ionomer dispersion as described in one or more embodiments herein to form a coated substrate, and drying the coated substrate to form a coated article. The coated article formed by the method described herein.

[0007] Further disclosed in embodiments herein is a coated article. The coated article can include a substrate and an ionomer composition coated on the substrate.

[0008] In one or more embodiments herein, the aqueous ionomer dispersion comprises 10-60 wt.% of the ionomer composition. In one or more embodiments herein, the ethylene acid copolymer is a polymerization reaction product of 75-85 wt.% ethylene and 15-25 wt.% monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer. In one or more embodiments herein, 20 mol.% to 50 mol.% of the total acid units of the ethylene acid copolymer are neutralized with zinc cations. In one or more embodiments herein, the ionomer composition comprises 10-80 wt.% polyolefin. In one or more embodiments herein, the polyolefin is selected from the group consisting of polyethylene or polypropylene. In one or more embodiments herein, the polyolefin is an ethylene / α-olefin copolymer having a melt index I2 (2.16 kg at 190° C.) of 0.1 to 100.0 g / 10 min, measured according to ASTM D1238.

[0009] In some embodiments herein, the ionomer composition is formed by providing an ethylene acid copolymer, neutralizing 15 mol % to 50 mol % of the total acid units of the ethylene acid copolymer with zinc cations to form an ionomer, and combining the ionomer with a polyolefin to form the ionomer composition. In other embodiments herein, the ionomer composition is formed by combining an ethylene acid copolymer with a polyolefin to form a mixture, and adding zinc cations to the mixture in an amount sufficient to neutralize 15 mol % to 50 mol % of the total acid units of the ethylene acid copolymer to form the ionomer composition. In one or more embodiments herein, the mixing is performed at a temperature of 100 degrees Celsius to 300 degrees Celsius.

[0010] Additional features and advantages of the embodiments are set forth in the detailed description that follows, and in part will be readily apparent to those skilled in the art from that description or will be learned by practicing the embodiments described herein, including the detailed description. It is to be understood that both the foregoing and the following description are intended to provide an overview or framework for describing the various embodiments and for understanding the nature and characteristics of the claimed subject matter. [Brief description of the drawings]

[0011] The following detailed description of specific embodiments of the present disclosure can be best understood when read in conjunction with the following drawings, where like structure is indicated with like reference numerals and in which:

[0012] [Figure 1A] 1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and static charge measurements for coated substrates according to one or more embodiments of the present disclosure. [Figure 1B] 1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and static charge measurements for coated substrates according to one or more embodiments of the present disclosure. [Figure 1C]1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and static charge measurements for coated substrates according to one or more embodiments of the present disclosure. [Figure 2A] 1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and stain application for coated substrates according to one or more embodiments of the present disclosure. [Figure 2B] 1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and stain application for coated substrates according to one or more embodiments of the present disclosure. [Figure 2C] 1 graphically illustrates "zero" static charge measurements, mechanical static charge transfer, and stain application for coated substrates according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Reference will now be made in detail to embodiments of the aqueous ionomer dispersion and the method for making the aqueous ionomer dispersion. The aqueous ionomer dispersion may be used to coat substrates such as flooring, plastic parts, wood, textiles, metals, ceramics, textiles, glass, or paper. However, it should be noted that this is merely an exemplary implementation of the embodiments disclosed herein. The embodiments are also applicable to other technologies that are susceptible to similar problems as those described above. For example, the aqueous ionomer dispersion described herein may be used as an additive in paints (or other coatings), concrete / cement, paper, plastics, composites, electrodes, adhesives, and as adhesives or binders (asphalt, bitumen, paper, textile, plastics).

[0014] In embodiments herein, the aqueous ionomer dispersion comprises an ionomer composition and water. In some embodiments, the aqueous ionomer dispersion comprises 10 wt% to 60 wt% of the ionomer composition. All individual values ​​and subranges from 10 wt% to 60 wt% are included and disclosed herein. For example, in some embodiments, the aqueous ionomer dispersion comprises 10 wt% to 55 wt%, 15 wt% to 55 wt%, 15 wt% to 50 wt%, or 15 wt% to 45 wt% of the ionomer composition. In embodiments herein, the aqueous ionomer dispersion may also comprise 40 wt% to 90 wt% water. All individual values ​​and subranges from 40 wt% to 90 wt% water are included and disclosed herein. For example, in some embodiments, the aqueous ionomer dispersion comprises 45% to 90% by weight, 45% to 85% by weight, 50% to 85% by weight, or 55% to 85% by weight water.

[0015] The aqueous ionomer dispersions described herein have particles dispersed in an aqueous solution. The particles present in the aqueous ionomer dispersions can have an average particle size of 4 μm or less. All individual values ​​and subranges are included and disclosed herein. For example, the aqueous ionomer dispersions can have an average particle size of 3.5 μm or less, 3.0 μm or less, 0.1-4 μm, 0.1-3.5 μm, or 0.1-3.0 μm. The aqueous dispersions described herein can also have a total resin content of 10-60 wt%, 15-60 wt%, 20-60 wt%, 25-60 wt%, or 30-60 wt%.

[0016] Ionomer Composition The ionomer composition comprises an ionomer and a polyolefin. In embodiments herein, the ionomer composition comprises at least 20 wt% ionomer, based on the total weight percent of the ionomer composition, and up to 80 wt% polyolefin, based on the total weight percent of the ionomer composition. All individual values ​​and subranges are included and disclosed herein. For example, in some embodiments, the ionomer composition comprises 20 wt%-90 wt% (alternatively, 20 wt%-85 wt%, 20 wt%-80 wt%, or 20 wt%-60%) ionomer and 10 wt%-80 wt% (alternatively, 15 wt%-80 wt%, 20 wt%-80 wt%, or 40 wt%-80 wt%) polyolefin.

[0017] The ionomeric composition, ionomer, and / or polyolefin may also contain other additives known in the art. Examples of additives include, but are not limited to, processing aids, flow improvers, lubricants, pigments, dyes, flame retardants, impact modifiers, nucleating agents, antiblocking agents such as silica, heat stabilizers, UV absorbers, UV stabilizers, surfactants, chelating agents, and coupling agents. Additives may be used in amounts ranging from about 0.01% to about 10% by weight, based on the weight of the material in the ionomeric composition, ionomer, or polyolefin.

[0018] Ionomer The ionomer is an at least partially neutralized ethylene acid copolymer. The ethylene acid copolymer is a polymerization reaction product of 70-85% by weight ethylene and 15-30% by weight monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer. All individual values ​​and subranges are included and disclosed herein. For example, in some embodiments, the ethylene acid copolymer is a polymerization reaction product of 72-85% by weight ethylene and 15-28% by weight monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer. In other embodiments, the ethylene acid copolymer is a polymerization reaction product of 75-85% by weight ethylene and 15-25% by weight monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer. The ethylene acid copolymer may be polymerized according to the processes disclosed in U.S. Pat. Nos. 3,404,134, 5,028,674, 6,500,888, and 6,518,365. In some embodiments, a mixture of two or more ethylene acid copolymers can be used, provided that the aggregate composition and properties of the mixture are within the limits set forth above for ethylene acid copolymers. For example, two ethylene methacrylic acid copolymers can be used, such that the total weight percent of methacrylic acid is 15% to 30% by weight of the total polymeric material.

[0019] When referring to total acid units neutralized, the calculation of percent neutralization is based on the number of acid units believed to be present based on the known number of moles of monocarboxylic acid comonomer and the number of metal equivalents added. In embodiments herein, at least 70 mole percent of the total acid units of the ethylene acid copolymer are neutralized to form an ionomer, between 15 mole percent and 50 mole percent of the total acid units of the ethylene acid copolymer are neutralized with zinc cations, and at least 40 mole percent of the total acid units of the ethylene acid copolymer are neutralized with monovalent cations. All individual values ​​and subranges are included and disclosed herein. For example, in some embodiments, at least 70 mol% (alternatively, at least 75 mol%, at least 80 mol%, or at least 85 mol%) of the total acid units of the ethylene acid copolymer are neutralized to form an ionomer, 15 mol% to 50 mol% (alternatively, 15 mol% to 45 mol%, 15 mol% to 40 mol%, 20 mol% to 50 mol%, 20 mol% to 45 mol%, or 20 mol% to 40 mol%) of the total acid units of the ethylene acid copolymer are neutralized with zinc cations, and at least 40 mol% (alternatively, at least 45 mol%, at least 50 mol%, 40 mol% to 100 mol%, 40 mol% to 95 mol%, 40 mol% to 85 mol%, or 40 mol% to 80 mol%) of the total acid units of the ethylene acid copolymer are neutralized with monovalent cations. The ethylene acid copolymers may be neutralized using methods disclosed, for example, in U.S. Pat. No. 3,404,134. In other embodiments, at least 70 mol% (alternatively, at least 75 mol%) of the total acid units of the ethylene acid copolymer are neutralized to form an ionomer, 15 mol% to 50 mol% (alternatively, 20 mol% to 50 mol%, or 20 mol% to 45 mol%) of the total acid units of the ethylene acid copolymer are neutralized with zinc cations, and at least 40 mol% (alternatively, at least 45 mol%, at least 50 mol%, 40 mol% to 100 mol%, 40 mol% to 95 mol%, 40 mol% to 85 mol%, or 40 mol% to 80 mol%) of the total acid units of the ethylene acid copolymer are neutralized with monovalent cations.

[0020] Exemplary monovalent cations include sodium, potassium, lithium, amines (e.g., dimethylethanolamine (DMEA), trimethylamine, ammonia, etc.), or combinations thereof. In some embodiments herein, the monovalent cation is selected from the group consisting of sodium, potassium, lithium, ammonia, or combinations thereof. In one or more embodiments herein, the monovalent cation is sodium, potassium, ammonia, or combinations thereof.

[0021] In some embodiments herein, the ionomers may have a melt index (I2) of 1 to 100 g / 10 min. All individual values ​​and subranges are included and disclosed herein. For example, in some embodiments, the ionomers may have a melt index (I2) of 1 to 75 g / 10 min. or 1 to 50 g / 10 min. I2 is measured at 190° C. and 2.16 kg according to ASTM D1238.

[0022] Polyolefin As described above, the ionomeric composition according to the embodiments herein comprises a polyolefin. The polyolefin may be selected from the group consisting of polyethylene or polypropylene. In some embodiments, the polyolefin is a polyethylene. The polyethylene is a reaction product of ethylene and, optionally, one or more α-olefin comonomers. In other embodiments, the polyolefin is an ethylene / α-olefin copolymer. As used herein, the term "ethylene / α-olefin copolymer" refers to the reaction product of ethylene and one or more α-olefin comonomers.

[0023] The ethylene / α-olefin copolymer is (a) 55% by weight or more, for example, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, 92% by weight or more, 95% by weight or more, 97% by weight or more, 98% by weight or more, 99% by weight or more, 99.5% by weight or more, more than 50% by weight to 99% by weight, more than 50% by weight to 97% by weight, more than 50% by weight to 94% by weight, more than 50% by weight to 90% by weight, 70% by weight to 99.5% by weight, 70% by weight to 99% by weight, 70% by weight to 97% by weight, 70% by weight to 94% by weight, 80% by weight ~99.5wt%, 80wt%~99wt%, 80wt%~97wt%, 80wt%~94wt%, 80wt%~90wt%, 85wt%~99.5wt%, 85wt%~99wt%, 85wt%~97wt%, 88wt%~99.9wt%, 88wt%~99.7wt%, 88wt%~99.5wt%, 88wt%~99wt%, 88wt%~98wt%, 88wt%~97wt%, 88wt%~95wt%, 88wt%~94wt%, 90wt%~99.9wt%, 90wt%~99.5wt%, 90wt%~99wt%, 90wt%~97wt %, 90% to 95% by weight, 93% to 99.9% by weight, 93% to 99.5% by weight, 93% to 99% by weight, or 93% to 97% by weight of units derived from ethylene; and (b) less than 30 weight percent, e.g., less than 25 weight percent, or less than 20 weight percent, less than 18 weight%, less than 15 weight%, less than 12 weight%, less than 10 weight%, less than 8 weight%, less than 5 weight%, less than 4 weight%, less than 3 weight%, less than 2 weight%, less than 1 weight%, 0.1 to 20 weight%, 0.1 to 15 weight%, 0.1 to 12 weight%, 0.1 to 10 weight%, 0.1 %.Comonomer content can be measured using any suitable technique, such as nuclear magnetic resonance ("NMR") spectroscopy and techniques based on 13C NMR analysis, such as those described in U.S. Pat. No. 7,498,282, incorporated herein by reference.

[0024] Suitable α-olefin comonomers typically have 20 or fewer carbon atoms. The one or more α-olefins may be selected from the group consisting of C3-C20 acetylenically unsaturated monomers and C4-C18 diolefins. For example, in some embodiments, the α-olefin comonomer may have 3-10 carbon atoms or 3-8 carbon atoms. Exemplary α-olefin comonomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 4-methyl-1-pentene. The one or more α-olefin comonomers may be selected, for example, from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene, or alternatively, from the group consisting of 1-butene, 1-hexene, and 1-octene.

[0025] In some embodiments described herein, the ethylene / α-olefin copolymer may have a density of 0.850 g / cc to 0.910 g / cc. All individual values ​​and subranges from at least 0.850 g / cc to 0.910 g / cc are included and disclosed herein. For example, in some embodiments, the ethylene / α-olefin copolymer has a density of 0.855 to 0.905 g / cc, 0.855 to 0.900 g / cc, 0.855 to 0.900 g / cc, or 0.865 to 0.895 g / cc. Density can be measured according to ASTM D792.

[0026] In addition to density, the ethylene / α-olefin copolymer may have a melt index I2 of 0.1 g / 10 min to 100.0 g / 10 min. All individual values ​​and subranges of 0.1 g / 10 min to 100.0 g / 10 min are included and disclosed herein. For example, in some embodiments, the ethylene / α-olefin copolymer may have a melt index I2 ranging from a lower limit of 0.1, 0.5, 1.0, 1.5, 2.5, or 5.0 to an upper limit of 100.0, 75, 0, 50.0, 35.0, 25.0, or 20.0 g / 10 min. In other embodiments, the ethylene / α-olefin copolymer may have a melt index I2 of 0.5g / 10min to 100.0g / 10min, 1.0g / 10min to 100.0g / 10min, 2.0g / 10min to 100.0g / 10min, 5.0g / 10min to 100.0g / 10min, 1.0g / 10min to 75.0g / 10min, 5.0g / 10min to 75.0g / 10min, 1.0g / 10min to 50.0g / 10min, or 5.0g / 10min to 50.0g / 10min. The melt index I2 can be measured according to ASTM D1238 (190°C and 2.16kg).

[0027] method Also provided herein is a method of making an aqueous ionomer dispersion. The method includes preparing an ionomer composition and mixing the ionomer composition with an aqueous composition comprising water and monovalent cations to form an aqueous ionomer dispersion. The mixing of the ionomer composition with the aqueous composition is performed at a temperature between 100°C and 300°C. A heated aqueous ionomer dispersion results. A further optional step may include cooling the heated aqueous ionomer dispersion to a temperature between 20°C and 30°C, with the ionomer remaining dispersed in the liquid phase. As used herein, "disperse," "dispersing," and related terms refer to solid articles, such as pellets of a polymer, that are mixed with water and dissipate into the liquid phase within a short period of time.

[0028] Aspects of the ionomer composition and the amount of water in the aqueous ionomer dispersion have been previously described in embodiments herein. The ionomer composition includes an ionomer and a polyolefin. The polyolefin has been previously described in embodiments herein. The amount of the ionomer and the polyolefin in the ionomer composition has also been previously described in embodiments herein. The ionomer is an at least partially neutralized ethylene acid copolymer. The ethylene acid copolymer and the neutralization of the ethylene acid copolymer have been previously described in embodiments herein.

[0029] As previously mentioned, the ionomer composition is mixed with an aqueous composition comprising water and monovalent cations to form an aqueous ionomer dispersion. In embodiments herein, the aqueous composition may comprise a sufficient amount of monovalent cations to neutralize all acid units of the ethylene acid copolymer with the monovalent cations.

[0030] In some embodiments herein, the ionomer composition is formed by providing an ethylene acid copolymer, neutralizing 15 mol % to 50 mol % of the total acid units of the ethylene acid copolymer with zinc cations to form an ionomer, and combining the ionomer with a polyolefin to form the ionomer composition.

[0031] In some embodiments herein, the ionomer composition is formed by combining an ethylene acid copolymer with a polyolefin to form a mixture, and adding to the mixture zinc cations in an amount sufficient to neutralize 15 mol % to 50 mol % of the total acid units of the ethylene acid copolymer to form the ionomer composition.

[0032] Purpose The aqueous dispersions described herein can be used to coat a substrate. Suitable substrates can include paperboard, cardboard, pulp molded shapes, woven fabrics, nonwoven fabrics, films, open-cell foams, closed-cell foams, or metal foils. In some embodiments herein, a method for coating a substrate includes providing an aqueous ionomer dispersion as described in embodiments herein and applying the aqueous ionomer dispersion to a substrate to form a coated substrate. Application can be performed by dipping, spraying, roll coating, doctor blade, flow coating, or other suitable methods for applying liquid coatings known in the art. The method can further include a drying step.

[0033] In other embodiments herein, a method of forming a coated article includes coating an aqueous ionomer dispersion, as described in one or more embodiments herein, onto a substrate to form a coated substrate, and drying the coated substrate to form the coated article.

[0034] The coated article comprises an ionomer composition layer as described herein formed on at least one surface of a substrate. The ionomer composition layer comprises an ionomer composition comprising: a) at least 20 wt. % of an ionomer, based on the total weight percent of the ionomer composition, as described in embodiments herein; and b) up to 80 wt. % of a polyolefin, based on the total weight percent of the ionomer composition, as described in embodiments herein.

[0035] In embodiments herein, the coated articles may exhibit improved static charge as compared to uncoated articles.

[0036] Test Method density Density was measured in accordance with ASTM D-792 and is reported in grams per cubic centimeter (g / cc).

[0037] Melt Index / Melt Flow Rate Melt index (I2) was measured according to ASTM D-1238, procedure B (condition 190°C / 2.16 kg) for ethylene-based polymers and is reported in grams dissolved per 10 minutes (g / 10 min). Melt index (MFR) was measured according to ASTM D-1238, procedure B (condition 230°C / 2.16 kg) for ethylene-propylene-based polymers and is reported in grams dissolved per 10 minutes (g / 10 min).

[0038] Average Particle Size The average particle size is defined by the volume-average particle diameter measured with a Beckman Coulter LS13-320 laser light scattering particle size analyzer (Beckman Coulter Inc., Fullerton, California) implementing an epoxy particle model (real fluid refractive index = 1.332, real sample refractive index = 1.5, virtual sample refractive index = 0). Samples are diluted in aqueous KOH solution with pH > 10 before measurement.

[0039] kinematic viscosity Kinematic viscosity is measured via a Brookfield CAP2000+ parallel plate viscometer equipped with spindle 10. Approximately 0.5 mL of the dispersion is loaded into the device and measured at the appropriate rpm to obtain a stable viscosity value for 15 seconds before recording the kinematic viscosity.

[0040] Static Charge Measurement Electrostatic charge measurements are performed as seen in Figures 1A-1C. Referring to Figure 1A, a Keyence SK-H050 electrostatic probe is mounted on an adjustable metal stand on a large metal plate to measure the temperature and humidity % of the laboratory. Electrical leads are then attached to the meter and plate to electrically ground the system. The height of the probe is then adjusted to focus on the test swatch sample. Once the probe is in focus, a "zero" electrostatic charge measurement is obtained. Next, to induce a static charge via the triboelectric effect, the test swatch is moved and affixed to a plastic plate and a plastic block covered with rabbit fur is rubbed over the test film with a constant force for 15 strokes as shown in Figure 1B. The fur-coated block is then removed from the area and the electrostatic charge is quickly measured and recorded as seen in Figure 1C. Once the initial static measurement is complete, the test swatch is returned to the grounded metal plate to discharge and the measurement process (A-C) is repeated 2-3 more times for each test swatch. The results are normalized to the swatch surface area and reported in V / cm in Table 6. 2 It is reported as follows.

[0041] Electrostatic powder retention measurement Hershey's unsweetened cocoa powder is used as the soil simulant for all static charge powder retention measurements. Coated polypropylene nonwoven swatches are tested in a similar manner to the static charge measurements, and the laboratory temperature and % humidity are measured and recorded.

[0042] The electrostatic charge powder retention measurements are performed as seen in Figures 2A-2C. First, the test swatch is pre-weighed and placed on a grounded metal plate, as seen in Figure 2A. Then, the swatch is transferred and affixed to a plastic plate, and a plastic block covered with rabbit fur is rubbed with constant force for 15 strokes on the test swatch to induce a static charge, as seen in Figure 2B. Next, a stainless steel mesh strainer pre-loaded with cocoa powder is shaken over the test film, such that a fine powder layer uniformly covers the film, as seen in Figure 2C. Then, finally, the covered swatch is removed from the plastic plate, held vertically, mechanically shaken 9, 15, and 30 times, and weighed again to measure powder retention. The results are summarized in Table 6. EXAMPLES

[0043] The polyolefin dispersions outlined in Table 3 are prepared using a Berstorff (KraussMaffei) extruder (48 L / D with 25 mm screw diameter rotating at 450 rpm) according to the procedures and conditions outlined in Table 4. The base polyolefin resin and ionomer surfactant are fed to the extruder feed throat via a Schenck Mechatron weight loss feeder and a K-Tron pellet feeder, respectively, as described in Tables 1 and 2 below. The polyolefin resin and ionomer surfactant are melt blended and emulsified in the presence of a first water stream to form an emulsion phase. The first water stream comprises water and a solution of a monovalent cation. The monovalent cation solution can be a 30 wt% solution of potassium hydroxide, a 50 wt% solution of sodium hydroxide, or a 100 wt% solution of dimethylethanolamine (DMEA). The emulsion phase is then conveyed to the dilution and cooling zone of the extruder where additional dilution water is added to form an aqueous dispersion having a solids level as outlined in Table 3. The extruder barrel temperature is set at 150° C., except for the first two barrel segments, which are set at 25° C. and 90° C., respectively. After the dispersion exits the extruder, it is further cooled and filtered through a bag filter with a mesh size of 200 μm.

[0044] In Table 5 below, materials that did not form a dispersion at the indicated temperature are designated with a "No" and materials that formed a dispersion at the indicated temperature are designated with a "Yes." An "aqueous dispersion" is formed when (i) greater than 95% of the solids have been converted to fine particles 4 μm or less in diameter, and (ii) the dispersion is stable and the cloudy or milky liquid with substantially no visible solids at the manufacturing temperature shows no visual change after initial cooling to room temperature.

[0045] The ionomer surfactants are summarized below in Table 1 and are prepared from ethylene acid copolymers, which are the polymerization reaction products of ethylene and methacrylic acid (MAA). The amount of MAA is provided below in Table 1. Additional aspects of the ionomers are provided below.

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] [Table 4]

[0050] [Table 5]

[0051] Preparation of Coated Articles Dispersion Examples B and 2 were diluted to 5% solids in glass jars with deionized water. Polypropylene nonwoven fabric was cut into 3" x 5" swatches and completely submerged in the diluted dispersion and gently rolled for 10 seconds. The wet swatches were removed from the dispersion, laid flat to dry for 24 hours, then submerged in the dispersion and air dried again. The swatches were annealed at 110°C for 5 minutes in a forced air oven and stored in resealable plastic bags before testing for static charge and static charge powder retention.

[0052] [Table 6]

[0053] As shown by the dispersion results in Tables 5 and 6, Comparative Example A did not form an aqueous dispersion. Comparative Example B formed a dispersion, but at a lower solids content, with lower static charge and lower retention of static charge powder. Inventive Examples 1-10 all formed dispersions at solids contents greater than 30%. The inventive dispersions had greater than 95% of the solids converted to particulates having diameters of 4 μm or less. The dispersions were also stable, with the cloudy or milky liquid with virtually no visible solids at the manufacturing temperature showing no visual change after initial cooling to room temperature. Additionally, inventive Example 2 showed higher static charge and higher retention of static charge powder.

[0054] The dimensions and values ​​disclosed herein should not be understood to be strictly limited to the exact numerical values ​​recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm."

[0055] All documents cited herein, including any cross-referenced or related patents or applications, if any, and any patent applications or patents to which this application claims priority or benefit, are incorporated herein by reference in their entirety, unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein, or that it teaches, suggests, or discloses such invention, either alone or in any combination with any other reference. Furthermore, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall apply.

[0056] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended in the appended claims to cover all such changes and modifications that are within the scope of this invention.

Claims

1. An aqueous ionomer dispersion comprising an ionomer composition and water, The ionomer composition comprises: a) at least 20 weight percent of an ionomer, based on a total weight percent of the ionomer composition, the ionomer being an at least partially neutralized ethylene acid copolymer, the ethylene acid copolymer having a molecular weight of: 70 to 85% by weight of ethylene; A polymerization reaction product with 15 to 30% by weight of a monocarboxylic acid, an ionomer, wherein at least 70 mole percent of the total acid units of said ethylene acid copolymer are neutralized, wherein 15 mole percent to 50 mole percent of the total acid units of said ethylene acid copolymer are neutralized with zinc cations, and wherein at least 40 mole percent of the total acid units of said ethylene acid copolymer are neutralized with a monovalent cation; b) up to 80 weight percent of a polyolefin, based on the total weight percent of the ionomer composition.

2. 10. The aqueous ionomer dispersion of claim 1, wherein the aqueous ionomer dispersion comprises 10 to 60 weight percent of the ionomer composition.

3. 3. The aqueous ionomer dispersion of claim 1 or 2, wherein the ethylene acid copolymer is the polymerization reaction product of 75 to 85 weight percent ethylene and 15 to 25 weight percent of the monocarboxylic acid, based on the total weight of monomers present in the ethylene acid copolymer.

4. The aqueous ionomer dispersion of claims 1-3, wherein 20 mole % to 50 mole % of the total acid units of the ethylene acid copolymer are neutralized with zinc cations.

5. The aqueous ionomer dispersion of claims 1 to 4, wherein the ionomer composition comprises 10 to 80 wt. % of the polyolefin.

6. The aqueous ionomer dispersion of claims 1 to 5, wherein the polyolefin is selected from the group consisting of polyethylene or polypropylene.

7. 7. The aqueous ionomer dispersion of claims 1 to 6, wherein the polyolefin is an ethylene / α-olefin copolymer having a melt index I2 of 0.1 to 100.0 g / 10 min, determined according to ASTM D1238 (2.16 kg at 190° C.).

8. 1. A method for producing an aqueous ionomer dispersion, comprising: Providing an ionomer composition; and forming an aqueous ionomer dispersion by mixing the ionomer composition with an aqueous composition comprising water and monovalent cations; The ionomer composition comprises: a) at least 20 weight percent of an ionomer, based on a total weight percent of the ionomer composition, the ionomer being an at least partially neutralized ethylene acid copolymer, the ethylene acid copolymer having, based on the total weight of monomers present in the ethylene acid copolymer, 70 to 85% by weight of ethylene; A polymerization reaction product with 15 to 30% by weight of a monocarboxylic acid, an ionomer in which 15 mol % to 50 mol % of the total acid units of said ethylene acid copolymer are neutralized with zinc cations; b) up to 80 wt. % of a polyolefin, based on the total weight percent of the ionomer composition; The ionomer in the aqueous ionomer dispersion has at least 70 mole percent of the total acid units of the ethylene acid copolymer neutralized and at least 40 mole percent of the total acid units of the ethylene acid copolymer neutralized with a monovalent cation.

9. The ionomer composition comprises: providing the ethylene acid copolymer and neutralizing 15 mole percent to 50 mole percent of the total acid units of the ethylene acid copolymer with the zinc cations to form an ionomer; and combining said ionomer with said polyolefin to form said ionomer composition.

10. The ionomer composition comprises: combining said ethylene acid copolymer and said polyolefin to form a mixture; 9. The method of claim 8, wherein said ionomer composition is formed by adding to said mixture a sufficient amount of said zinc cations to neutralize 15 mole percent to 50 mole percent of the total acid units of said ethylene acid copolymer.

11. The method of any one of claims 8 to 10, wherein mixing the ionomer composition with an aqueous composition comprising water and monovalent cations is carried out at a temperature of from 100 degrees Celsius to 300 degrees Celsius.

12. 1. A method of forming a coated article, comprising: Coating the aqueous ionomer dispersion of any one of claims 1 to 7 onto a substrate to form a coated substrate; and drying the coated substrate to form a coated article.

13. 13. A coated article formed according to the method of claim 12.

Citation Information

Patent Citations

  • Preparation of aqueous dispersion of polyolefin composition

    JP1977013539A

  • Aqueous dispersion and its preparation

    JP1999263848A

  • Rust preventive treating agent for metallic surface and surface treated metallic product

    JP2000273659A

  • Water-based dispersion and heat-sealable film coated therewith

    JP2001139737A

  • Water borne polyolefin dispersion coatings, and methods of making the same

    JP2016186071A