Adhesives based on carbodiimide chemistry
A thermosetting resin composition using polycarbodiimide and specific polyol ratios addresses the issues of polyurethane-based adhesives, offering enhanced adhesive strength and stability for diverse bonding applications.
Patent Information
- Application Number
- JP2021553137
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-07
- Filing Date
- 2020-03-05
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-03-05
AI Technical Summary
Existing adhesives based on polyurethane and isocyanates pose environmental, health, and safety concerns, and there is a need for isocyanate-free polymers with improved adhesive properties.
A thermosetting resin composition comprising polycarbodiimide with 1 to 10 carbodiimide groups per molecule, combined with a mixture of crystalline and amorphous polyols, where the molar ratio of carbodiimide groups to hydroxyl groups ranges from 1:2 to 2:1, enhancing adhesive strength and stability.
The composition exhibits excellent adhesive failure temperature (SAFT) and mechanical properties, with improved shear force over time, making it suitable for various bonding applications.
Smart Images

Figure 0007582960000001 
Figure 0007582960000002 
Figure 0007582960000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, in particular for use as an adhesive, which is obtained or obtainable from the reaction of at least: (i) a polycarbodiimide, the number of carbodiimide groups per molecule of which ranges from 1 to 10; (ii) a mixture of a crystalline polyol and a non-crystalline polyol, in which the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the polyesterol according to (ii) ranges from 1:2 to 2:1, and at least 25% by weight of the mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight. The present invention further relates to a method for the use of said thermosetting resin composition as an adhesive, to a method for producing an adhesive, to a method for producing a component comprising an adhesive layer on at least one substrate, and to an adhesive film obtained or obtainable from one of these methods. [Background technology]
[0002] Adhesives based on polyurethanes and isocyanates are known, but in some cases are associated with environmental, health or safety issues. Polyurethanes are not a single material with a constant composition, even if they include a series of chemicals sharing similar chemical properties, but are polymers composed of organic chain units linked by urethane (-NH-C(=O)-O-) or carbamate (-NR-C(=O)-O-) bonds. That is, polyurethane polymers are formed by the reaction of isocyanate(s) with polyol(s). The isocyanates and polyols used usually contain more than one functional group per molecule.
[0003] Polymers that do not contain isocyanates are known. For example, US 5,079,326 A discloses a thermosetting resin containing a reaction product of polycarbodiimide and at least one crosslinking agent having two or more active hydrogen groups in the molecule, such as 2,4,6-triamino-1,3,5-triazine or 2,4-diamino-6-phenyl-1,3,5-triazine. It is described that this thermosetting resin has high heat resistance, high strength, flame retardancy, and good processability. When carbodiimide (CDI) is reacted with alcohol, a polymer having an iso-urea bond (-NH-C(=NR)-O-) is formed. The chemistry for preparing CDI-containing molecules is described in detail in "Chemistry and technology of carbodiimides", Henri Ulrich, Wiley, Hoboken, USA, 2007. CDI-containing molecules can also be prepared from isocyanates. Oligomeric CDI structures can be obtained when difunctional isocyanates are partially reacted with monofunctional alcohols followed by the addition of a phospholene-based catalyst (WO2015 / 123416 A1). The resulting polycarbodiimide (pCDI) polymers can be utilized, for example, in electrical and electronic packaging applications or synthetic fiber applications, coating compositions and / or inks. Oligomeric CDI structures can also be obtained starting from difunctional isocyanates combined with monofunctional isocyanates using a phospholene-based catalyst, resulting in capped polycarbodiimides (WO2015 / 127041 A1). WO2015 / 127041 A1 also discloses compositions comprising these capped polycarbodiimides and polyols. WO2015 / 127038 A1 discloses a method for producing capped polycarbodiimides and polymers comprising the reaction product of capped polycarbodiimides and monomeric acids.
[0004] What all the documents have in common is, firstly, that they disclose an extensive list of the components used and also describe a wide range of suitable mixing ratios of (capped) pCDI and reactive compounds to prepare the final resin, and secondly, all the documents make no mention of using the resin as an adhesive. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] US 5,079,326 A [Patent Document 2] WO2015 / 123416 A1 [Patent Document 3] WO2015 / 127041 A1 [Patent Document 4] WO2015 / 127038 A1 [Non-patent literature]
[0006] [Non-Patent Document 1] "Chemistry and technology of carbodiimides", Henri Ulrich, Wiley, Hoboken, USA, 2007 Summary of the Invention [Problem to be solved by the invention]
[0007] The problem underlying the present invention was to provide further isocyanate-free polymers which can be used as adhesives and which have improved adhesive properties. [Means for solving the problem]
[0008] According to the invention, this objective is at least i) polycarbodiimide (pCDI) having 1 to 10 carbodiimide groups per molecule; ii) Polyesterol wherein the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the polyesterol according to (ii) is in the range of 1:2 to 2:1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] According to a preferred embodiment, the polyesterol according to (ii) is crystalline. Preferably, the crystalline polyesterol (ii) is used in the form of a mixture of crystalline and non-crystalline polyols, where at least 25% by weight of the mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight. Thus, according to a preferred embodiment, the thermosetting resin composition comprises at least i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol wherein the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of the mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight.
[0010] Surprisingly, it has been shown that the use of certain combinations of pCDI and, in particular, crystalline polyesterols results in superior properties, for example, the resulting adhesive has a shear adhesion failure temperature (SAFT) of more than 80°C. SAFT represents the temperature at which the adhesive bond breaks, i.e., it is an index of not only the adhesive strength at room temperature, but also the stability of the adhesive bond at elevated temperatures. Furthermore, a molar ratio of carbodiimide groups in pCDI to hydroxyl groups in the crystalline polyesterol in the range of 1:2 to 2:1 clearly improves the mechanical properties of the thermoset, as evidenced, for example, by the change in shear force over time.
[0011] In one embodiment of the thermosetting resin composition, the polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3) with at least i.1) a polyisocyanate composition comprising at least one diisocyanate; i.2) monofunctional compounds selected from the group consisting of monoisocyanates, isocyanate-reactive monofunctional compounds, where the isocyanate-reactive monofunctional compounds are selected from the group consisting of monoalcohols, monothiols, monoamines, and mixtures of two or more of these isocyanate-reactive monofunctional compounds, and mixtures of monoisocyanates and isocyanate-reactive monofunctional compounds, preferably at least monoalcohols; The compound is obtained or obtainable from the reaction of
[0012] In one embodiment of the thermosetting resin composition, the polycarbodiimide according to (i) is a) mixing, at temperature T1, the polyisocyanate composition according to (i.1) with at least a portion of the monofunctional compound according to (i.2) to obtain a first mixture; b) adding a catalyst (i.3) to the first mixture obtained in (a) at a temperature T2 greater than T1 to obtain a precursor compound; c) conditioning the precursor compound obtained in (b) at a temperature T3; d) At temperature T3, the remaining portion of the monofunctional compound according to (i.2) is added to obtain the polycarbodiimide according to (i). obtained or obtainable by Here, T1 is a temperature less than 70°C, preferably in the range of 5 to less than 70°C, more preferably in the range of 5 to 69°C; T2 is a temperature of 70°C or higher, preferably in the range of 70°C or higher to 150°C, more preferably in the range of 70 to 150°C; T3 is a temperature less than 100°C, preferably in the range of 5 to 100°C, more preferably in the range of 5 to 99°C.
[0013] In one embodiment of the thermosetting resin composition, the polyesterol according to (ii) has a melting point above 30° C., preferably in the range of from 30° C. to 80° C., more preferably in the range of from 31° C. to 80° C. In a preferred embodiment, at least one crystalline polyesterol of the mixture according to (ii) has a melting point above 30° C., preferably in the range of from 30° C. to 80° C., more preferably in the range of from 31° C. to 80° C.
[0014] In one embodiment of the thermosetting resin composition, the polyesterol according to (ii) has a molecular weight in the range of 500 to 5000 g / mol. Preferably, at least one crystalline polyesterol of the mixture according to (ii) has a molecular weight in the range of 500 to 5000 g / mol.
[0015] Although the crystalline polyesterol of the present invention is known as crystalline polyesterol to those skilled in the art, it is difficult to determine its crystallinity. First, because the preferred molecular weight of the polyesterol is in the range of 500 to 5000 g / mol, preferably in the range of 750 to 3000 g / mol, and the end of the hydroxyl chain limits the crystallization of the polyol. Second, because the temperature history experienced by the sample before the measurement affects the extension of crystallization. Third, the speed at which the crystallinity determination is made may affect the measurement result. Those skilled in the art recognize crystalline polyesterol by visual inspection of the polyesterol and its rheological behavior based on the following characteristics at room temperature (temperature in the range of 20 ° C to 25 ° C): A) Crystalline polyesterol has a white to cloudy appearance because the crystals in the polyesterol have a size larger than the wavelength of visible light and therefore function as scatterers. B) Polyesterol does not flow under its own weight. C) Polyesterol has a waxy viscosity.
[0016] A polyesterol according to (ii) is considered to be crystalline so long as it satisfies at least one of the characteristics (A), (B) and (C), preferably two of the characteristics (A), (B) and (C), and more preferably all three of the characteristics (A), (B) and (C).
[0017] According to one embodiment, only one or more crystalline polyesterol(s) (ii) are used. Sometimes it is advantageous to reduce the crystallinity of the polyol phase by using a mixture of polyols, where the first polyol is at least one crystalline polyesterol (ii) and the second polyol(s) are non-crystalline. Thus, in an embodiment of the present invention, a mixture (blend) of crystalline and non-crystalline polyols can also be used, where at least 25% by weight, preferably at least 50% by weight, more preferably at least 75% by weight, based on the total weight of the mixture being 100% by weight, of the mixture is composed of one or more crystalline polyesterols. The remaining part up to 100% by weight is one or more non-crystalline polyol(s). Preferably, at least 50% by weight, more preferably at least 75% by weight, based on the total weight of the mixture being 100% by weight, of the mixture of crystalline and non-crystalline polyols is composed of at least one crystalline polyesterol, where more preferably (ii) is composed of one or more crystalline polyesterols. The term "non-crystalline polyol" includes non-crystalline polyesterols (polyester polyols) and polyetherols (polyether polyols). Such polyols are described in WO 2016 / 026807 A1, where suitable polyetherols and their synthesis are disclosed on page 7, line 23 to page 8, line 14, and suitable polyesterols and their synthesis are disclosed on page 8, line 16 to page 9, line 13. Polyesterols prepared from a single diol and a single diacid may be crystalline, whereby the melting point of said polyesterol is determined by the number of carbon atoms between the heteroatom groups. The higher the number of carbon atoms, the higher the melting point. Polyesterols prepared from branched diols and / or branched diacids and from mixtures of two or more diols and / or mixtures of two or more diacids are likely to be amorphous. When the polyesterol is at least partially crystalline, its melting point is in the range of 25 to 100°C, preferably in the range of more than 30 to 80°C, more preferably in the range of 31 to 80°C, depending on the structures of the diol and diacid described above.
[0018] In one embodiment of the thermosetting resin composition, the polyesterol according to (ii) comprises at least: (ii.1) compounds having at least two hydroxyl groups reactive towards ester formation; (ii.2) Compounds having at least two carboxyl groups reactive towards ester formation is a saturated polyesterol based on wherein the compound (ii.1) having at least two hydroxyl groups reactive towards ester formation is preferably a saturated diol, more preferably a saturated C2-C18 alkyl diol, more preferably a saturated C2-C10 alkyl diol selected from the group consisting of 1,2-ethanediol, diethylene glycol, 1,2-propanediol, dipropylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol and mixtures of two or more of these diols, and The compound (ii.2) having at least two carboxyl groups reactive towards ester formation is preferably selected from the group consisting of saturated dicarboxylic acids, anhydrides of saturated dicarboxylic acids, esters of saturated dicarboxylic acids and mixtures of two or more of these components, more preferably from the group consisting of saturated C2-C10 dicarboxylic acids and mixtures of two or more of these, more preferably from the group consisting of saturated C2-C10 dicarboxylic acids selected from the group consisting of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, maleic acid, fumaric acid, hexahydrophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, 3,6,9-trioxaundecanedioic acid and mixtures of two or more of these dicarboxylic acids. Preferably, at least one crystalline polyesterol of the mixture according to (ii) is at least: (ii.1) compounds having at least two hydroxyl groups reactive towards ester formation; (ii.2) Compounds having at least two carboxyl groups reactive towards ester formation is a saturated polyesterol based on wherein the compound (ii.1) having at least two hydroxyl groups reactive towards ester formation is preferably a saturated diol, more preferably a saturated C2-C18 alkyl diol, more preferably a saturated C2-C10 alkyl diol selected from the group consisting of 1,2-ethanediol, diethylene glycol, 1,2-propanediol, dipropylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol and mixtures of two or more of these diols, and The compound (ii.2) having at least two carboxyl groups reactive towards ester formation is preferably selected from the group consisting of saturated dicarboxylic acids, anhydrides of saturated dicarboxylic acids, esters of saturated dicarboxylic acids and mixtures of two or more of these components, more preferably saturated C2-C10 dicarboxylic acids and mixtures of two or more of these, more preferably saturated C2-C10 dicarboxylic acids selected from the group consisting of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, maleic acid, fumaric acid, hexahydrophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, 3,6,9-trioxaundecanedioic acid and mixtures of two or more of these dicarboxylic acids.
[0019] According to a preferred embodiment of the thermosetting resin composition, the polyesterol according to (ii) is a polyesterol based on a C2-C10 dicarboxylic acid selected from the group consisting of adipic acid, azelaic acid, sebacic acid, 12-dodecanedioic acid and a mixture of two or more of these dicarboxylic acids, and a diol which is hexane-1,6-diol, neopentyl glycol or a mixture of hexane-1,6-diol and neopentyl glycol.
[0020] In another embodiment of the thermosetting resin composition, the polyesterol according to (ii) is a saturated polyesterol based on at least an α-ω-hydroxy-carboxylic acid, a cyclic oligomer of an α-ω-hydroxy-carboxylic acid, or a mixture of two or more thereof, where the polyesterol according to (ii) is preferably selected from the group consisting of polycaprolactone, polylactic acid, 1,6-dioxacyclododecane-7,12-dione, oxacyclododecan-2-one, and a mixture of two or more of these compounds.
[0021] Preferably, at least one crystalline polyesterol of the mixture according to (ii) is a polyesterol based on a C2-C10 dicarboxylic acid selected from the group consisting of adipic acid, azelaic acid, sebacic acid, 12-dodecanedioic acid, and mixtures of two or more of these dicarboxylic acids, and a diol which is hexane-1,6-diol, neopentyl glycol, or a mixture of hexane-1,6-diol and neopentyl glycol; or At least one crystalline polyesterol of the mixture according to (ii) is a saturated polyesterol based on at least an α-ω-hydroxy-carboxylic acid, a cyclic oligomer of an α-ω-hydroxy-carboxylic acid, or a mixture of two or more thereof, whereby the at least one crystalline polyesterol of the mixture according to (ii) is preferably selected from the group consisting of polycaprolactone, polylactic acid, 1,6-dioxacyclododecane-7,12-dione, oxacyclododecan-2-one, and mixtures of two or more of these compounds.
[0022] The carbodiimidization catalyst (i.3) may be any type of carbodiimidization catalyst known to a person skilled in the art for producing polycarbodiimides. In one embodiment of the thermosetting resin composition, the carbodiimidization catalyst (i.3) is selected from the group consisting of tertiary amides, basic metal compounds, metal carboxylates, non-basic organometallic compounds, and phosphorus compounds. Specific carbodiimidization catalysts, which are incorporated herein by reference, are disclosed in WO 2015 / 123416 A1 in paragraphs
[0047] to
[0056] . In a preferred embodiment, the carbodiimidization catalyst (i.3) comprises at least one phospholene oxide, wherein the at least one phospholene oxide has the general formula (I): [ka] (In the formula, R 1 is a substituted or unsubstituted C1 to C15 hydrocarbon group, R 2 or R 4 is selected from the group consisting of a hydrogen atom, a halogen atom, preferably a chlorine atom (Cl), and a C1 to C12 alkyl group; R 2 , R 4 The other is R 3 forms a double bond with R 5 , R 6 , R 7 , R 8 , R 9 are independently selected from the group consisting of a hydrogen atom, a halogen atom, preferably a chlorine atom (Cl), and a C1 to C12 alkyl group.
[0023] Preferably, R 1 is selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, tert-butyl, cyclohexyl, n-dodecyl, phenyl, o-, m- or p-tolyl, xylyl, naphthyl, 4-diphenyl, 2-phenylethyl, 2-chloroethyl, 2-methoxy-ethyl, o-, m- or p-chlorophenyl, p-methoxyphenyl, and pN,N-dimethylaminophenyl. More preferably, R 1is selected from the group consisting of a C2 to C4 alkyl group, a phenyl group, or a benzyl group. 3 R does not form a double bond with 2 or R 4 is preferably H. Preferably, R 5 ~R 9 are independently selected from the group consisting of a hydrogen atom, a chlorine atom, methyl, ethyl, propyl, isopropyl, and butyl, with methyl being preferred. More preferably, R 5 ~R 9 Each of is H or methyl.
[0024] In a preferred embodiment, the phospholene oxide catalyst is selected from the group consisting of 1-methyl-1-oxo-phospholene, 1-phenyl-3-methyl-1-oxo-phospholene, 1-benzyl-3-methyl-1-oxo-phospholene, 1-ethyl-3-methyl-1-oxo-phospholene, and mixtures of two or more of these phospholene oxide catalysts. Preferred catalysts are 1-methyl-1-oxo-phospholene, 1-phenyl-3-methyl-1-oxo-phospholene (3-methyl-1-phenyl-2-phospholene 1-oxide, MPPO), and mixtures of 1-methyl-1-oxo-phospholene and MPPO, with MPPO being a particularly preferred catalyst.
[0025] In one embodiment of the thermosetting resin composition, the resin composition further comprises a catalyst (iii), which can be used as an isourea bond forming catalyst and is preferably selected from the group of metal-containing catalysts, more preferably from the group consisting of alcoholates, carboxylates, acetoacetates and / or 2-4 pentanediones of alkali metals or alkaline earth metals, preferably Na, K and / or Li, or metals from the group Ti, Zr, Hf, V, Cu, Hg, Zn, Sn, Hg, Bi and Pb. More preferably, the catalyst (iii) is selected from the group consisting of dimethyltin carboxylate, dimethyltin dineodecane, tetraisopropyl orthotitanate, titanium isopropoxide and bismuth trimeodecanate.
[0026] The diisocyanate compound contains two isocyanate groups and is selected from the group consisting of aliphatic diisocyanates, aromatic diisocyanates, and mixtures of two or more of these diisocyanates. Specific examples of aliphatic diisocyanate compounds include isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), dicyclohexylmethane diisocyanate (HMDI), cyclohexyl diisocyanate (CHDI), tetramethylxylylene diisocyanate (TMXDI), and combinations thereof, and any isomers of these aliphatic diisocyanate compounds. However, typically, the diisocyanate compound contains an aromatic diisocyanate compound. In one embodiment of the thermosetting resin composition, the diisocyanate contained in the polyisocyanate composition according to (i) is an aromatic diisocyanate, preferably selected from the group consisting of 2,2'-diphenylmethane diisocyanate (2,2'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI), 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), and mixtures of two or more of these diisocyanates, more preferably selected from the group consisting of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, and mixtures of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
[0027] In the synthesis of the polycarbodiimide (i), a monofunctional compound (i.2) is used which is a monofunctional compound selected from the group consisting of monoisocyanates, isocyanate-reactive monofunctional compounds and mixtures of monoisocyanates and isocyanate-reactive monofunctional compounds. Monoisocyanates refer to organic molecules having one isocyanate group, while isocyanate-reactive monofunctional compounds are organic molecules having one isocyanate-reactive group. The amount of monofunctional compound is necessary to adjust the molecular weight of the polycarbodiimide; the more monofunctional compound used in the preparation of the polycarbodiimide, the lower its molecular weight. The monoisocyanate can be aromatic or aliphatic, preferably aromatic. The monoisocyanate may be selected from the group consisting of phenyl isocyanate, toluyl isocyanate, naphthalene isocyanate and mixtures of two or more of these monoisocyanates. The compound having an isocyanate-reactive group is selected from the group consisting of monoalcohols, monothiols, monoamines, and mixtures of two or more of these isocyanate-reactive monofunctional compounds, i.e. the compound having an isocyanate-reactive group is an organic molecule having one group selected from alcohols, amines and thiols. The organic substituents may be aromatic or aliphatic, preferably aliphatic, including linear, branched and cyclic aliphatic. The aliphatic substituents may preferably contain one or more heteroelement atoms selected from the group consisting of nitrogen atoms, oxygen atoms and sulfur atoms, preferably oxygen atoms. The isocyanate-reactive group is preferably an alcohol, i.e. the isocyanate-reactive monofunctional compound is preferably a monoalcohol, more preferably the monofunctional compound (i.2) is at least a monoalcohol. The number of carbon atoms and the number of heteroelement atoms of the organic substituents may vary in total from 1 to 50, preferably from 2 to 20.In a preferred embodiment, the monoalcohol is selected from the group consisting of ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, 2-methyl-propan-1-ol, propan-2-ol, 2-ethyl-hexan-1-ol, cyclohexanol, 2-(2-ethoxyethoxy)ethanol, and mixtures of two or more of these monoalcohols, preferably from the group consisting of butanol, hexanol, 2-ethylhexan-1-ol, and mixtures of two or more of these monoalcohols, and more preferably the monoalcohol comprises at least 2 ethylhexan-1-ol, more preferably is at least 2 ethylhexan-1-ol.
[0028] According to one embodiment, the thermosetting resin composition comprises at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) Polyesterol and wherein the molar ratio of carbodiimide groups in the polycarbodiimide (i) to hydroxyl groups in the polyesterol (ii) is in the range of 1:2 to 2:1; - the polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3), preferably 3-methyl-1-phenyl-2-phospholene 1-oxide (MPPO), with at least: i.1) a polyisocyanate composition comprising at least TDI; i.2) A monofunctional compound that is 2-ethylhexan-1-ol is a toluene diisocyanate-based polycarbodiimide obtained or obtainable from the reaction of The polyesterols according to (ii) are crystalline saturated copolyesters based on hexane-1,6-dicarboxylic acid and hexane-1,6-diol.
[0029] Preferably, the thermosetting resin composition according to any one of claims 1 to 8 is prepared by subjecting the composition to at least the following reaction, optionally in the presence of a catalyst (iii), preferably dimethyltin carboxylate: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol and wherein the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of the mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight; - the polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3), preferably 3-methyl-1-phenyl-2-phospholene 1-oxide (MPPO), with at least: i.1) a polyisocyanate composition comprising at least TDI; i.2) A monofunctional compound that is 2-ethylhexan-1-ol is a toluene diisocyanate-based polycarbodiimide obtained or obtainable from the reaction of - at least one crystalline polyesterol of the mixture according to (ii) is a crystalline saturated copolyester based on hexane-1,6-dicarboxylic acid and hexane-1,6-diol.
[0030] Method of using the thermosetting resin composition The present invention further relates to the use of the above-described thermosetting resin composition as an adhesive.
[0031] The thermosetting resin composition is used as a two-component adhesive (2K) or a one-component adhesive (1K), preferably as a 1K adhesive, more preferably as a 1K adhesive in the form of an adhesive film.
[0032] When used as an adhesive, it shows that the use of a specific combination of pCDI and crystalline polyesterol can provide excellent properties, e.g., SAFT above 80° C., preferably above 100° C., more preferably above 120° C. Secondly, by setting a specific molar ratio of carbodiimide groups in pCDI to hydroxyl groups in the crystalline polyesterol in the range of 1:2 to 2:1, the mechanical properties of the thermosetting resin were obviously improved, which was evident, for example, from the change in shear force over time.
[0033] The adhesive of the present invention can be used universally to bond a wide variety of substrates, in particular when bonding foil to foil or foil to substrate. A further embodiment is the application of a 1K adhesive film cast onto a foil to which the adhesive adheres well. The foil thus prepared can be stored for a long time, heat activated and applied as required. Upon cooling, a bond is formed and a stable composite is obtained. A further embodiment is that the foil is a decorative foil.
[0034] Adhesive manufacturing method The present invention further relates to a first method for producing an adhesive, preferably a 2K adhesive, comprising the steps of: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) Polyesterol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in the polycarbodiimide by (i) to hydroxyl groups in the polyesterol by (ii) is in the range of 1:2 to 2:1, and the mixing by (a) is carried out at a temperature above the melting point Tm of the polyesterol (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b) applying the mixture resulting from step (a) to at least one substrate, the substrate having a temperature above 0°C, the applying step being carried out at a temperature of the mixture above the melting point Tm of polyesterol (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; c) optionally curing the mixture on at least one substrate at a temperature above the melting point Tm of the polyesterol (ii), preferably in the range above Tm to 200°C, preferably in the range of Tm+1°C to 200°C, more preferably in the range of 50°C to 150°C, to obtain a component comprising an adhesive layer on at least one substrate; Includes.
[0035] Preferably, the first method for producing an adhesive, preferably a 2K adhesive, comprises the steps of: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of the mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight, and the mixing according to (a) is carried out at a temperature above the melting point Tm of the polyesterol (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b) applying the mixture resulting from step (a) to at least one substrate, the substrate having a temperature above 0° C., the applying step being carried out at a temperature of the mixture above the melting point Tm of at least one crystalline polyesterol of the mixture according to (ii), preferably at a temperature of Tm+10° C. or higher, more preferably at a temperature in the range of Tm+10° C. to Tm+50° C., more preferably at a temperature in the range of Tm+20° C. to Tm+40° C.; c) optionally curing the mixture on at least one substrate at a temperature above the melting point Tm of at least one crystalline polyesterol of the mixture according to (ii), preferably in the range of from Tm to 200°C, preferably in the range of from Tm+1°C to 200°C, more preferably in the range of from 50°C to 150°C, to obtain a component comprising an adhesive layer on the at least one substrate; Including, Here, the curing according to (c) is preferably carried out for a period of more than 1 minute, more preferably for a period of more than 10 minutes, more preferably for a period of more than 20 minutes.
[0036] In one embodiment of this first method for making the adhesive, curing according to (c) is carried out for a period of more than 1 minute, preferably more than 10 minutes, more preferably more than 20 minutes.
[0037] In one embodiment of this first method of making an adhesive, the at least one substrate comprises a first substrate and a second substrate, wherein step (b) comprises: b.1) at least partially applying the mixture obtained from step (a) to at least one surface of a first substrate to obtain a first substrate having a surface at least partially coated with the mixture obtained from step (a), the substrate having a temperature above 0°C, the application being carried out at a temperature of the mixture above the melting point Tm of polyesterol (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b.2) placing a second substrate at least partially on the coated surface of the first substrate to obtain a component comprising the first substrate, the second substrate, and the mixture obtained from step (a) therebetween; Including, Step (c) includes curing the mixture between the first substrate and the second substrate at a temperature exceeding the melting point Tm of the polyesterol (ii), preferably in the range of above Tm to 200°C, preferably in the range of Tm+1°C to 200°C, more preferably in the range of 50°C to 150°C, to obtain a component including the first substrate, the second substrate, and an adhesive layer therebetween.
[0038] Preferably, the at least one substrate comprises a first substrate and a second substrate, wherein step (b) comprises: b.1) at least partially applying the mixture obtained from step (a) to at least one surface of a first substrate to obtain a first substrate having a surface at least partially coated with the mixture obtained from step (a), the substrate having a temperature above 0°C, the application being carried out at a temperature of the mixture above the melting point Tm of at least one crystalline polyesterol of the mixture according to (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b.2) placing a second substrate at least partially on the coated surface of the first substrate to obtain a component comprising the first substrate, the second substrate, and the mixture obtained from step (a) therebetween; Including, Step (c) comprises curing the mixture between the first substrate and the second substrate at a temperature above the melting point Tm of at least one crystalline polyesterol of the mixture according to (ii), preferably in the range of above Tm to 200°C, preferably in the range of Tm+1°C to 200°C, more preferably in the range of 50°C to 150°C, to obtain a component comprising the first substrate, the second substrate, and an adhesive layer therebetween.
[0039] Another embodiment of the present invention is a second method for producing an adhesive, preferably a 1K adhesive, comprising: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) Polyesterol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in the polycarbodiimide by (i) to hydroxyl groups in the polyesterol by (ii) is in the range of 1:2 to 2:1, and the mixing by (a) is carried out at a temperature above the melting point Tm of the polyesterol (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b') casting the mixture obtained according to step (a) onto the surface of at least one substrate having a temperature in the range of 0 to 150°C to obtain an adhesive film on the surface; c') optionally removing the adhesive film obtained according to step (b') from the surface. Includes.
[0040] Preferably, the second method for producing an adhesive, preferably a 1K adhesive, comprises the steps of: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in the polycarbodiimide according to (i) to hydroxyl groups in the mixture according to (ii) is in the range of 1:2 to 2:1, and the mixing according to (a) is carried out at a temperature above the melting point Tm of the crystalline polyesterol of the mixture according to (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b') casting the mixture obtained according to step (a) onto the surface of at least one substrate having a temperature in the range of 0 to 150°C to obtain an adhesive film on the surface; c') optionally removing the adhesive film obtained according to step (b') from the surface. Including, Here, the casting in step (b') is preferably carried out at a temperature ranging from 0°C to the melting point Tm of at least one crystalline polyesterol in the mixture in (ii), more preferably at a temperature ranging from 5°C to Tm-10°C, more preferably at a temperature ranging from 10 to 30°C.
[0041] In one embodiment of the second manufacturing method of this adhesive, the casting in step (b') is carried out at a temperature ranging from 0°C to the melting point Tm of polyesterol (ii), preferably at a temperature ranging from 5°C to Tm-10°C, and more preferably at a temperature ranging from 10 to 30°C.
[0042] In one embodiment of this second method of making an adhesive, the at least one substrate comprises at least a first substrate and a second substrate, the method further comprising: d) applying the film obtained according to step (b') or (c') at least partially onto at least one surface of a first substrate to obtain a first substrate having a surface at least partially covered with the film obtained according to step (b') or (c'); e) placing a second substrate at least partially on the covered surface of the first substrate to obtain a component comprising the first substrate, the second substrate and, between them, the film obtained according to step (b') or (c'); f) curing the film between the first substrate and the second substrate at a temperature exceeding the melting point Tm of the polyesterol (ii), preferably in the range of more than Tm to 200°C, preferably in the range of Tm+1°C to 200°C, more preferably in the range of 50°C to 150°C, to obtain a component including the first substrate, the second substrate, and an adhesive layer therebetween; Includes.
[0043] The present invention further relates to a component comprising an adhesive layer on at least one substrate, obtained or obtainable from the first method described above or from the second method described above, preferably a component comprising a first substrate, a second substrate and an adhesive layer therebetween.
[0044] The present invention further relates to an adhesive film obtained or obtainable from the second process described above.
[0045] The present invention is further described by the following embodiments and combinations according to the embodiments, as indicated by the respective dependencies and back references. In particular, in each instance where a range according to the embodiments is mentioned, it is to be noted that in the context of a term such as "described in any one of embodiments 1 to 4," it is meant that all embodiments within this range are expressly disclosed to a person skilled in the art, i.e., the wording of this term is understood by a person skilled in the art to be equivalent to "described in any one of embodiments 1, 2, 3, 4." Furthermore, it is to be expressly noted that the following set of embodiments represents a properly structured part of the description directed to the general and preferred aspects of the present invention, rather than a set of claims determining the scope of protection.
[0046] 1. At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol A thermosetting resin composition, particularly for use as an adhesive, obtained or obtainable from the reaction of 1. A thermosetting resin composition, wherein a molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by mass of said mixture according to (ii) consists of at least one crystalline polyesterol, based on a total mass of said mixture being 100% by mass.
[0047] 2. The polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3) with at least: i.1) a polyisocyanate composition comprising at least one diisocyanate; i.2) Monofunctional compounds selected from the group consisting of monoisocyanates, isocyanate-reactive monofunctional compounds, and mixtures of monoisocyanates with isocyanate-reactive monofunctional compounds, preferably at least monoalcohols, wherein the isocyanate-reactive monofunctional compounds are selected from the group consisting of monoalcohols, monothiols, monoamines, and mixtures of two or more of these isocyanate-reactive monofunctional compounds. 2. The thermosetting resin composition of embodiment 1, obtained or obtainable from the reaction of
[0048] 3. The polycarbodiimide according to (i) a) mixing, at a temperature T1, said polyisocyanate composition according to (i.1) with at least a portion of said monofunctional compound according to (i.2) to obtain a first mixture; b) adding said catalyst (i.3) to said first mixture obtained in (a) at a temperature T2 greater than T1 to obtain a precursor compound; b) conditioning the precursor compound obtained in (b) at a temperature T3; c) adding the remaining portion of said monofunctional compound according to (i.2) at temperature T3 to obtain said polycarbodiimide according to (i). obtained or obtainable by T1 is a temperature less than 70°C, preferably in the range of 5 to less than 70°C, more preferably in the range of 5 to 69°C; T2 is a temperature of 70°C or higher, preferably a temperature in the range of 70°C or higher to 150°C; The thermosetting resin composition according to embodiment 2, wherein T3 is a temperature below 100°C, preferably in the range of 5 to 100°C, more preferably in the range of 5 to 99°C.
[0049] 4. The thermosetting resin composition according to any one of the preceding claims, wherein the at least one crystalline polyesterol of the mixture according to (ii) has a melting point greater than 30°C, preferably greater than 30°C to 80°C, more preferably in the range of 31°C to 80°C.
[0050] 5. The thermosetting resin composition according to any one of the preceding claims, wherein the at least one crystalline polyesterol of the mixture according to (ii) has a molecular weight in the range of 500 to 5000 g / mol.
[0051] 6. The thermosetting resin composition according to any one of the preceding claims, wherein at least 50% by weight, more preferably at least 75% by weight, of the mixture of crystalline polyol and non-crystalline polyol, based on the total weight of the mixture being 100% by weight, is made up of at least one crystalline polyesterol, more preferably (ii) is made up of one or more crystalline polyesterols.
[0052] 7. The at least one crystalline polyesterol of the mixture according to (ii) comprises at least: (ii.1) compounds having at least two hydroxyl groups reactive towards ester formation; (ii.2) Compounds having at least two carboxyl groups reactive towards ester formation is a saturated polyesterol based on said compound (ii.1) having at least two hydroxyl groups reactive towards ester formation is preferably a saturated diol, more preferably a saturated C2-C18 alkyl diol, more preferably a saturated C2-C10 alkyl diol selected from the group consisting of 1,2-ethanediol, diethylene glycol, 1,2-propanediol, dipropylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol and mixtures of two or more of these diols, and 7. The thermosetting resin composition according to any one of the preceding claims, wherein the compound (ii.2) having at least two carboxyl groups reactive towards ester formation is preferably selected from the group consisting of saturated dicarboxylic acids, anhydrides of saturated dicarboxylic acids, esters of saturated dicarboxylic acids, and mixtures of two or more of these components, more preferably saturated C2-C10 dicarboxylic acids and mixtures of two or more of these, more preferably saturated C2-C10 dicarboxylic acids selected from the group consisting of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, maleic acid, fumaric acid, hexahydrophthalic acid, hexahydroisophthalic acid, hexahydroterephthalic acid, 3,6,9-trioxaundecanedioic acid, and mixtures of two or more of these dicarboxylic acids.
[0053] 8. The thermosetting resin composition according to any one of the preceding claims, wherein the at least one crystalline polyesterol of the mixture according to (ii) is a polyesterol based on a C2-C10 dicarboxylic acid selected from the group consisting of adipic acid, azelaic acid, sebacic acid, 12-dodecanedioic acid and mixtures of two or more of these dicarboxylic acids, and a diol which is hexane-1,6-diol, neopentyl glycol or a mixture of hexane-1,6-diol and neopentyl glycol.
[0054] 9. The thermosetting resin composition according to any one of the preceding claims, wherein the at least one crystalline polyesterol of the mixture according to (ii) is a saturated polyesterol based on at least an α-ω-hydroxy-carboxylic acid, a cyclic oligomer of an α-ω-hydroxy-carboxylic acid, or a mixture of two or more thereof, and the at least one crystalline polyesterol of the mixture according to (ii) is preferably selected from the group consisting of polycaprolactone, polylactic acid, 1,6-dioxacyclododecane-7,12-dione, oxacyclododecan-2-one, and mixtures of two or more of these compounds.
[0055] 10. The carbodiimidization catalyst (i.3) is selected from the group consisting of tertiary amides, basic metal compounds, metal carboxylates, non-basic organometallic compounds and phosphorus compounds, preferably, the carbodiimidization catalyst (i.3) comprises at least one phospholene oxide, the at least one phospholene oxide having the general formula (I): [ka] (In the formula, R 1 is a substituted or unsubstituted C1 to C15 hydrocarbon group, R 2 or R 4 is selected from the group consisting of a hydrogen atom, a halogen atom, preferably Cl, and a C1-C12 alkyl group; R 2 , R 4 The other is R 3 forms a double bond with R 5 , R 6 , R 7 , R 8 , R 9 is selected from the group consisting of a hydrogen atom, a halogen atom, preferably a chlorine atom, and a C1 to C12 alkyl group),
[0056] 11. The thermosetting resin composition according to any one of the preceding claims, further comprising a catalyst (iii), which is usable as an isourea bond forming catalyst and is preferably selected from the group of metal-containing catalysts, more preferably from the group consisting of alcoholates, carboxylates, acetoacetates and / or 2-4-pentanedione of alkali metals or alkaline earth metals, preferably Na, K and / or Li, or metals from the group Ti, Zr, Hf, V, Cu, Hg, Zn, Sn, Hg, Bi and Pb, more preferably the catalyst (iii) is selected from the group consisting of dimethyltin carboxylate, dimethyltin dineodecane, tetraisopropyl orthotitanate, titanium isopropoxide and bismuth trimeodecanate.
[0057] 12. The thermosetting resin composition according to any one of the preceding claims, wherein the diisocyanate contained in the polyisocyanate composition according to (i) is an aromatic diisocyanate, preferably selected from the group consisting of 2,2'-diphenylmethane diisocyanate (2,2'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI), 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), and mixtures of two or more of these diisocyanates, more preferably selected from the group consisting of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, and mixtures of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
[0058] 13. Optionally in the presence of a catalyst (iii), which is preferably dimethyltin carboxylate, at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol and the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight; - said polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3), preferably 3-methyl-1-phenyl-2-phospholene 1-oxide (MPPO), with at least: i.1) a polyisocyanate composition comprising at least TDI; i.2) A monofunctional compound that is 2-ethylhexan-1-ol is a toluene diisocyanate-based polycarbodiimide obtained or obtainable from the reaction of 13. The thermosetting resin composition according to any one of the preceding claims, wherein the at least one crystalline polyesterol of the mixture according to (ii) is a crystalline saturated copolyester based on hexane-1,6-dicarboxylic acid and hexane-1,6-diol.
[0059] 14. Use of the thermosetting resin composition according to any one of claims 1 to 13 as an adhesive.
[0060] 15. Use according to embodiment 14 as a two-component adhesive (2K) or one-component adhesive (1K), preferably as a 1K adhesive, more preferably as a 1K adhesive in the form of an adhesive film.
[0061] 16. A method for producing an adhesive, preferably a 2K adhesive, comprising the steps of: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight; said mixing according to (a) is carried out at a temperature above the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii), preferably at a temperature equal to or higher than Tm+10°C, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b) applying the mixture resulting from step (a) to at least one substrate, the substrate having a temperature above 0°C and the applying step being carried out at a temperature of the mixture above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; c) optionally curing said mixture on said at least one substrate at a temperature above the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii), preferably in the range of from Tm to 200°C, preferably in the range of from Tm+1°C to 200°C, more preferably in the range of from 50°C to 150°C, to obtain a component comprising an adhesive layer on said at least one substrate; A method comprising:
[0062] 17. The method according to embodiment 16, wherein the curing according to (c) is carried out for a period of more than 1 minute, preferably more than 10 minutes, more preferably more than 20 minutes.
[0063] 18. The at least one substrate comprises a first substrate and a second substrate, and step (b) comprises: b.1) at least partially applying the mixture resulting from step (a) to at least one surface of the first substrate to obtain a first substrate having a surface at least partially coated with the mixture resulting from step (a), the substrate having a temperature above 0°C and the application being carried out at a temperature of the mixture above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii), preferably at a temperature of Tm+10°C or higher, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b.2) placing said second substrate at least partially on the coated surface of said first substrate to obtain a component comprising said first substrate, said second substrate and said mixture obtained from step (a) therebetween; Including, 18. The method according to embodiment 16 or 17, wherein step (c) comprises curing the mixture between a first substrate and a second substrate at a temperature above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii), preferably in the range of from above Tm to 200°C, preferably in the range of from Tm+1°C to 200°C, more preferably in the range of from 50°C to 150°C, to obtain a component comprising a first substrate, a second substrate, and an adhesive layer therebetween.
[0064] 19. A method for producing an adhesive, preferably a 1K adhesive, comprising the steps of: a) At least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) a catalyst, preferably an isourea-forming catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight; said mixing according to (a) is carried out at a temperature above the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii), preferably at a temperature equal to or higher than Tm+10°C, more preferably at a temperature in the range of Tm+10°C to Tm+50°C, more preferably at a temperature in the range of Tm+20°C to Tm+40°C; b') casting the mixture obtained according to step (a) onto the surface of at least one substrate having a temperature in the range of 0 to 150°C to obtain an adhesive film on the surface; c') optionally removing the adhesive film obtained according to step (b') from the surface. A method comprising:
[0065] 20. The method according to embodiment 19, wherein the casting according to step (b') is carried out at a temperature ranging from 0°C to below the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii), preferably at a temperature ranging from 5°C to Tm-10°C, more preferably at a temperature ranging from 10 to 30°C.
[0066] 21. The at least one substrate comprises at least a first substrate and a second substrate; d) applying the film obtained according to step (b') or (c') at least partially onto at least one surface of the first substrate to obtain a first substrate having a surface at least partially covered with the film obtained according to step (b') or (c'); e) placing said second substrate at least partially on the covered surface of said first substrate to obtain a component comprising said first substrate, said second substrate and, between them, said film obtained according to step (b') or (c'); f) curing the film between the first substrate and the second substrate at a temperature above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii), preferably in the range of from above Tm to 200°C, preferably in the range of from Tm+1°C to 200°C, more preferably in the range of from 50°C to 150°C, to obtain a component comprising the first substrate, the second substrate, and an adhesive layer therebetween; 21. The method of embodiment 19 or 20, comprising:
[0067] 22. A component comprising an adhesive layer on at least one substrate, preferably a first substrate, a second substrate and an adhesive layer therebetween, obtained or obtainable from the method according to any one of embodiments 16 to 18 or from the method according to any one of embodiments 19 to 21.
[0068] 23. An adhesive film obtained or obtainable by the method according to embodiment 19 or 20.
[0069] The present invention will be further described with reference to the following Reference Examples, Comparative Examples and Examples. EXAMPLES
[0070] 1. Chemicals
[0071] [Table 1]
[0072] 2.Measurement method Hydroxyl number (HV): DIN 53240 Acid value (AV): DIN EN ISO 14898 NCO content: DIN EN ISO 14896 N=C=N content: Oxalic acid method published by W. Adam and F. Yany, 676 Analytical Chemistry, Vol. 49, No. 4, April 1977 Residual TDI monomer: DIN EN ISO 10283 Lap shear strength: Sample preparation according to ISO 4587 / DIN EN 1465, measurement according to ISO 4587 / DIN EN 6060 Tensile strength: ISO 4587 / DIN EN 6060 Shear Adhesion Failure Temperature (SAFT): Similar to ASTM D4498 using an air circulating oven.
[0073] 3. Reference Examples, Examples and Comparative Examples Reference Example 1 - Preparation of toluene diisocyanate-based polycarbodiimide (pCDI) An 80:20 mixture of 2,4- and 2,6-isomers of toluene diisocyanate (TDI) (500.0 g) was placed in a flask and cooled in a water / ice bath. With stirring, 2-ethylhexan-1-ol (157.2 g) was added dropwise to maintain the temperature below 25° C. After the reaction was complete, the contents of the flask were heated to 100° C. When 75° C. was reached, 30.0 g of catalyst 1 (3-methyl-1-phenyl-2-phospholene 1-oxide, MPPO) solution (5% by weight in butyl acetate) was added, and after reaching 100° C., the mixture was stirred at a constant temperature of 100° C. for 75 minutes. The product was cooled to below 50° C. and the NCO content (determined according to DIN EN ISO 14896: Plastics - Polyurethane raw materials - Determination of isocyanate content) was determined to be 9.49% by weight. Based on the NCO content, a further 178.6 g of 2-ethylhexan-1-ol was added dropwise while maintaining the temperature below 70° C. to reach a theoretical NCO content of 0.0% by weight. After the addition was complete, the mixture was stirred at 60° C. until the reaction was complete. The material was left at room temperature overnight. It was heated to 70° C. for transfer. The N=C=N content (determined according to the oxalic acid method published by W. Adam and F. Yany, 676 Analytical Chemistry, Vol. 49, No. 4, April 1977) was determined to be 6.90% by weight, the NCO content was 0.17% by weight, and the residual TDI monomer (determined according to DIN EN ISO 10283: Binders for paints and varnishes - Determination of monomeric diisocyanates in polyisocyanate resins) was less than 0.01% by weight. The butyl acetate was removed using a rotary evaporator at 10 mbar and an oil bath of 100° C.
[0074] Examples 2 to 7-2K Adhesive Description of 2K Experimental Procedure: Samples for determining the lap shear strength (lap shear strength 0.3 mm) were prepared in strict accordance with ISO 4587 / DIN EN 1465; their composition is shown in Table 2. The adhesive composition according to Table 2 was prepared by conditioning both polyesterol 1 and pCDI of Reference Example 1 at 90°C. Catalyst 2 was added to polyesterol 1 and premixed with a spatula. pCDI was added and the blend was homogenized for 30 seconds at 1600 rpm with a Speedmixer™ (Hauschild Engineering, Germany). Subsequently, a sufficient amount of the reaction mixture to slightly overfill the 25 mm x 12.5 mm x 0.3 mm joint of the bond was placed on a wooden test bar (beech, 100 mm x 25 mm x 5 mm, Rochell GmbH, Germany) and a second wooden test bar was pressed with low force onto the adhesive. The joint was assembled by placing the test bars with a 12.5 mm overlap. The thickness of the adhesive layer was set to 0.3 mm using a metal spacer. The test specimens were fixed in the mold by placing a 434 g weight on the joint and cured in an oven at 130 °C for 30 min. After cooling to room temperature, the weight was removed and the samples were left at room temperature for at least one week before testing. The lap shear strength was determined at a crosshead speed of 5 mm / min and calculated by dividing the measured tensile force by the overlap area. For each series, the average value of the lap shear strength was recorded and the experimental error was generally around 10%. Sample systems 4, 5 and 6 were also tested using steel plates (100 mm x 25 mm x 1 mm, Rochell GmbH, Germany). The determination of SAFT (shear adhesion failure temperature) was performed similarly to ASTM D4498 using an air circulating oven. The oven was preheated to 80 °C before the determination. One end of the lap shear test specimen was fixed and held in a vertical position and a 100 g weight was attached to the other end (lower end). The adhesive joints were held at 80°C for 30 minutes, with the temperature increasing stepwise at 10°C intervals and the samples held at each temperature for 30 minutes until the bond broke. The highest temperature at which the bond was stable for 30 minutes was recorded as the SAFT. The mechanical and SAFT property results are shown in Table 3. The abbreviation nd stands for not yet determined.
[0075] [Table 2]
[0076] [Table 3]
[0077] It is clear that Examples 3 to 6, in which the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the polyesterol is in the range of 1:2 to 2:1, have superior mechanical properties (especially SAFT) compared with Examples 2 and 7, in which the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the polyesterol is outside the range of 1:2 to 2:1.
[0078] For samples 3, 4, 5 and 6, wooden test bars were used to determine the change in bond joint strength as a function of time. The sample preparation procedure for the lap shear test specimens was the same as described above, except that the samples were not cured at 130°C for 30 minutes. Instead, the change in strength as a function of time was measured for fresh test specimens. The results are shown in Table 4.
[0079] [Table 4]
[0080] Examples 3-6 show that strength build-up of the adhesive bond occurs over a moderate time span, with the strength increasing to about 30-40% of its final strength after about 4 minutes.
[0081] Comparative Examples 1 to 5-2K Adhesive In the comparative examples, wooden test bars were used. The adhesive formulations are shown in Table 5. The polyols used in Comparative Examples 1-3 were non-crystalline. In Comparative Example 4, Linear Polyesterol 1 was used to prepare the bond joints, and in Comparative Example 5, Linear pCDI was used. In the preparation of Comparative Examples 4 and 5, Polyesterol 1 and pCDI were pre-conditioned and applied at 90°C. The strength build-up of Comparative Examples 1-4 is shown in Table 6. The lap shear strength and SAFT of Comparative Examples 4 and 5 are shown in Table 7.
[0082] [Table 5]
[0083] [Table 6]
[0084] [Table 7]
[0085] From the comparison of Examples 3 to 6 and Comparative Examples 1 to 5, it is clear that a specific combination of pCDI and a crystalline polyester polyol (here, polyester polyol 1) has excellent properties, especially when the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the crystalline polyester polyol is in the range of 1:2 to 2:1, a clearly high shear force is obtained. In the case of a polyesterol different from the crystalline polyesterol, the development of the shear force was inferior even when the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the polyesterol is in the range of 1:2 to 2:1.
[0086] Examples 8 to 11-1K Adhesive / Adhesive Film Description of 1K Experimental Procedure: Both polyesterol 1 and pCDI of Reference Example 1 were prepared at 90°C. Catalyst 2 was added to polyesterol 1 and premixed with a spatula. pCDI was added and the blend was homogenized with a Speedmixer™ at 1600 rpm for 30 seconds. Using a doctor blade, the mixture thus obtained was drawn into a film having a thickness of 500 μm onto a preheated Teflon® sheet fixed on a hot plate having a temperature of 130°C. The film was cured at this temperature (130°C) for 30 minutes. Afterwards, the Teflon sheet was removed from the hot plate and cooled to room temperature. The film could be easily removed from the Teflon sheet. A dry, tack-free and flexible film was obtained. A sample with dimensions of 25 mm x 12.5 mm was cut from the film and placed between two wooden test bars with an overlap of 12.5 mm. The assembly was fixed using a universal double clip and placed in an air-circulating oven at a temperature of 130°C for 30 minutes. After cooling, the clamps were removed. The test samples were stored in the laboratory for at least two weeks before testing. The film compositions and corresponding adhesive properties are shown in Tables 8 and 9, respectively.
[0087] [Table 8]
[0088] [Table 9]
[0089] It is clear that Examples 9 and 10, in which the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the polyesterol is in the range of 1:2 to 2:1, have superior mechanical properties (especially SAFT) compared with Examples 8 and 11, in which the molar ratio of the carbodiimide groups in pCDI to the hydroxyl groups in the polyesterol is outside the range of 1:2 to 2:1.
[0090] Examples 12 to 14 The adhesive films of Examples 12-14 were prepared as described above for Examples 8-11, except that the stretching temperature was room temperature (temperatures in the range of 20-25° C.). Dry, tack-free, flexible films were obtained. Adhesive joints were prepared as described above for Examples 8-11. The film compositions and corresponding adhesion and SAFT properties are shown in Tables 10 and 11, respectively.
[0091] [Table 10]
[0092] [Table 11]
[0093] It is clear that in Examples 12-14, firstly where the molar ratio of carbodiimide groups in pCDI to hydroxyl groups in polyesterol is in the range of 1:2 to 2:1, and secondly where the temperature at which the film is prepared is below the melting point of the polyesterol (stretching at room temperature instead of 130°C), further improved properties were obtained compared to Experiments 9-11 where the films were prepared at temperatures above the melting point of the polyesterol.
[0094] Comparative Examples 6 to 8 - Comparative 1K Adhesive The compositions of the adhesive films of Comparative Examples 6-8 are shown in Table 12. The polyol used was non-crystalline. The adhesive films of Comparative Examples 6-8 were prepared according to the procedure described above for Examples 8-11.
[0095] [Table 12]
[0096] The obtained films of Comparative Examples 6 to 8 were soft and sticky and were not suitable for adhesive applications. When stretched at room temperature, the films of Comparative Examples 6 to 8 remained liquid and could not be removed from the Teflon sheet.
[0097] As a result, it is clear that even if the molar ratio of carbodiimide groups in pCDI to hydroxyl groups in polyol was in the range of 1:2 to 2:1, the mechanical properties (especially SAFT) were inferior when a polyol different from polyesterol was used.
[0098] Overall, it is clear from the Examples and Comparative Examples that the use of a particular combination of pCDI and crystalline polyesterol resulted in excellent properties, e.g., SAFTs above 80° C., preferably above 100° C., and more preferably above 120° C. Secondly, a particular molar ratio of carbodiimide groups in pCDI to hydroxyl groups in the crystalline polyesterol in the range of 1:2 to 2:1 clearly improved the mechanical properties of the thermosetting resin, as evidenced, for example, by the change in shear force over time.
[0099] References US 5,079,326 A Chemistry and technology of carbodiimides, Henri Ulrich, Wiley, Hoboken, USA, 2007 WO 2015 / 127041 A1 WO 2015 / 123416 A1 EP 0 381 324 A1 W. Adam and F. Yany, Analytical Chemistry, Vol. 49, No. 4, April 1977, 676 WO2016 / 026807 A1 WO 2015 / 127038 A1
Claims
1. at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol A thermosetting resin composition obtained or obtainable from the reaction of 1. A thermosetting resin composition comprising: a polycarbodiimide having a molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) ranging from 1:2 to 2:1; and at least 25% by weight of said mixture according to (ii) consisting of at least one crystalline polyesterol, based on a total weight of said mixture being 100% by weight.
2. The polycarbodiimide according to (i) is reacted in the presence of a carbodiimidization catalyst (i.3) with at least i. 1) a polyisocyanate composition comprising at least one diisocyanate; 2) A monofunctional compound selected from the group consisting of monoisocyanates, isocyanate-reactive monofunctional compounds, and mixtures of monoisocyanates and isocyanate-reactive monofunctional compounds, wherein the isocyanate-reactive monofunctional compound is obtained or obtainable from the reaction of a monofunctional compound selected from the group consisting of monoalcohols, monothiols, monoamines, and mixtures of two or more of these isocyanate-reactive monofunctional compounds.
3. The polycarbodiimide according to (i) is a) Temperature T 1 mixing the polyisocyanate composition according to (i.1) with at least a portion of the monofunctional compound according to (i.2) to obtain a first mixture; b) T 1 Temperature T 2 adding a catalyst (i.3) to said first mixture obtained in (a) to obtain a precursor compound; b) Temperature T 3 conditioning the precursor compound obtained in (b); c) Temperature T 3 and adding the remaining portion of said monofunctional compound according to (i.2) to obtain said polycarbodiimide according to (i). obtained or obtainable by T 1 is a temperature less than 70° C., T 2 is a temperature of 70° C. or higher, T 3 The thermosetting resin composition according to claim 1 or 2, wherein the temperature is less than 100°C.
4. 4. The thermosetting resin composition according to claim 1, wherein the at least one crystalline polyesterol of the mixture according to (ii) has a melting point above 30°C.
5. 5. The thermosetting resin composition according to claim 1, wherein the at least one crystalline polyesterol of the mixture according to (ii) has a molecular weight in the range of 500 to 5000 g / mol.
6. 6. The thermosetting resin composition according to claim 1, wherein at least 50% by weight of the mixture of crystalline polyol and non-crystalline polyol is comprised of at least one crystalline polyesterol, based on the total weight of the mixture being 100% by weight.
7. The at least one crystalline polyesterol of the mixture according to (ii) comprises at least: (ii.1) a compound having at least two hydroxyl groups reactive towards ester formation; (ii.2) Compounds having at least two carboxyl groups reactive towards ester formation is a saturated polyesterol based on the compound (ii.1) having at least two hydroxyl groups reactive towards ester formation is a saturated diol, and 7. The thermosetting resin composition according to any one of claims 1 to 6, wherein the compound (ii.2) having at least two carboxyl groups reactive towards ester formation is selected from the group consisting of saturated dicarboxylic acids, anhydrides of saturated dicarboxylic acids, esters of saturated dicarboxylic acids, and mixtures of two or more of these components.
8. 8. The thermosetting resin composition according to any one of claims 1 to 7, wherein the at least one crystalline polyesterol of the mixture according to (ii) is a polyesterol based on a C2 to C10 dicarboxylic acid selected from the group consisting of adipic acid, azelaic acid, sebacic acid, 12-dodecanedioic acid and mixtures of two or more of these dicarboxylic acids, and a diol which is hexane-1,6-diol, neopentyl glycol or a mixture of hexane-1,6-diol and neopentyl glycol, or the at least one crystalline polyesterol of the mixture according to (ii) is a saturated polyesterol based on at least α-ω-hydroxy-carboxylic acids, cyclic oligomers of α-ω-hydroxy-carboxylic acids, or a mixture of two or more thereof.
9. Optionally in the presence of a catalyst (iii), comprising at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol and the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight, said polycarbodiimide according to (i) being reacted in the presence of a carbodiimidization catalyst (i.3) with at least: i. 1) a polyisocyanate composition comprising at least TDI; i.2) A monofunctional compound which is 2-ethylhexan-1-ol is a toluene diisocyanate-based polycarbodiimide obtained or obtainable from the reaction of 9. A thermosetting resin composition according to claim 1, wherein the at least one crystalline polyesterol of the mixture according to (ii) is a crystalline saturated copolyester based on hexane-1,6-dicarboxylic acid and hexane-1,6-diol.
10. 10. Use of the thermosetting resin composition according to any one of claims 1 to 9 as an adhesive.
11. A method for producing an adhesive, comprising the steps of: a) at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) Catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said polyesterol according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight, and said mixing according to (a) is carried out at a temperature above the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii); b) applying the mixture resulting from step (a) to at least one substrate, the substrate having a temperature above 0° C., the applying step being carried out at a temperature of the mixture above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii); c) optionally curing said mixture on said at least one substrate at a temperature above the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii) to obtain a component comprising an adhesive layer on at least one substrate; A method comprising:
12. The at least one substrate comprises a first substrate and a second substrate, and step (b) comprises: b. 1) at least partially applying the mixture resulting from step (a) to at least one surface of the first substrate to obtain a first substrate having a surface at least partially coated with the mixture resulting from step (a), the substrate having a temperature above 0° C., and the application is performed at a temperature of the mixture above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii); b. 2) at least partially disposing said second substrate on the coated surface of said first substrate to obtain a component comprising said first substrate, said second substrate, and said mixture obtained from step (a) therebetween; Including, 12. The method according to claim 11, wherein step (c) comprises curing the mixture between a first substrate and a second substrate at a temperature above the melting point Tm of the at least one crystalline polyesterol of the mixture according to (ii) to obtain a component comprising a first substrate, a second substrate, and an adhesive layer therebetween.
13. A method for producing an adhesive, comprising the steps of: a) at least: i) a polycarbodiimide having 1 to 10 carbodiimide groups per molecule; ii) A mixture of a crystalline polyol and a non-crystalline polyol iii) Catalyst to obtain a mixture, wherein the molar ratio of carbodiimide groups in said polycarbodiimide according to (i) to hydroxyl groups in said mixture according to (ii) is in the range of 1:2 to 2:1, and at least 25% by weight of said mixture according to (ii) consists of at least one crystalline polyesterol, based on the total weight of said mixture being 100% by weight, and said mixing according to (a) is carried out at a temperature above the melting point Tm of the crystalline polyesterol of said mixture according to (ii); b') casting the mixture obtained according to step (a) onto the surface of at least one substrate having a temperature ranging from 0 to 150°C to obtain an adhesive film on said surface; c') optionally removing the adhesive film obtained according to step (b') from the surface. wherein said casting according to step (b') is carried out at a temperature ranging from 0°C to below the melting point Tm of said at least one crystalline polyesterol of said mixture according to (ii).
Citation Information
Patent Citations
Decorative sheet
JP1996060109A
Aqueous adhesive and resin sheet-covered metal plate
JP2008260831A
Polyisourea
JP2017507213A
Thermosetting resin and a method for producing it
US5079326A
Method of preparing a polycarbodiimide polymer and polycarbodiimide polymer prepared thereby
WO2015123416A1